Non-photosensitive insulation film-forming composition
A non-photosensitive insulating film forming composition with specific aromatic heterocycles and crosslinkable substituents addresses the limitations of BT resins, achieving low dielectric constant and loss tangent in cured films.
Patent Information
- Application Number
- JP2021153373
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2021-09-21
- Publication Date
- 2024-11-14
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing BT resins used in high-performance printed wiring boards face limitations in achieving low dielectric constants and low dielectric loss tangents, despite improvements in composition.
A non-photosensitive insulating film forming composition is developed using a polymer with a specific aromatic heterocycle and crosslinkable substituents, combined with a crosslinking agent, to achieve a low relative dielectric constant and dielectric loss tangent.
The composition provides a cured film with significantly reduced dielectric constant and loss tangent, outperforming BT resins in electrical performance.
Smart Images

Figure 2024160416000001 
Figure 2024160416000002 
Figure 2024160416000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a non-photosensitive insulating film-forming composition and a non-photosensitive resin film obtained from the composition. [Background technology]
[0002] Thermosetting resins using a combination of a cyanate ester compound and a bismaleimide compound (for example, Patent Document 1) are called "BT resins" and are widely used as insulating materials for high-performance printed wiring boards and the like, as thermosetting resins with excellent processability, heat resistance, and electrical properties. However, in recent years, with the increasing speed of communication devices, there is a demand for BT resins with low relative dielectric constants and low dielectric loss tangents in order to accommodate higher transmission frequencies. In response to this issue, Patent Document 2 claims that the issue of low relative dielectric constants and low dielectric loss tangents has been resolved by a thermosetting resin composition containing BT resin, a cyclic olefin resin with a glass transition temperature of 260°C or more and 310°C or less, and a curing catalyst. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Special Publication No. 54-30440 [Patent Document 2] JP 2017-88647 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, there is a limit to how much electrical properties can be improved simply by improving the composition containing BT resin.
[0005] Therefore, an object of the present invention is to provide a non-photosensitive insulating film-forming composition that can achieve a low relative dielectric constant and a low dielectric loss tangent without being restricted to BT resin, and a non-photosensitive resin film obtained from the composition. [Means for solving the problem]
[0006] Means for Solving the Problems The present inventors have conducted intensive research to achieve the above object and have found that by employing a polymer having a repeating unit structure containing a specific aromatic heterocycle and a crosslinkable substituent, a non-photosensitive resin composition that gives a cured film with a low dielectric constant and a low dielectric loss tangent can be obtained, thereby completing the present invention.
[0007] That is, the present invention includes the following. [1] The following formula (1): [ka] [In formula (1), Base A 1 teeth, [ka] represents a 5- to 8-membered aromatic heterocycle represented by the formula: The aromatic heterocycle may have a bridging substituent, Base A 2 teeth, [ka] represents a 5- to 8-membered aromatic heterocycle represented by the formula: The aromatic heterocycle may have a bridging substituent, Base B 1 represents an organic group having 6 to 40 carbon atoms and having a crosslinkable substituent, which may contain at least one heteroatom selected from N, S, and O and may contain a halogen atom; Base B 2 represents an organic group having 6 to 40 carbon atoms and no crosslinkable substituent, which may contain at least one heteroatom selected from N, S, and O and may contain a halogen atom; n 1 , n 2 are each independently a number greater than or equal to 0 and less than or equal to 1, m 1 , m 2 are each independently a number greater than or equal to 0 and less than or equal to 1, n is a number equal to or greater than 1, m is a number equal to or greater than 0, 10≦n+m≦500, However, group A 1 , group A 2 When neither of these has a crosslinkable substituent, If m ≠ 0, then n 1 and m 1 At least one of is 1, If m=0, then n 1 is 1.] A polymer having a repeating unit structure represented by the formula: solvent A non-photosensitive insulating film forming composition comprising: [2] The non-photosensitive insulating film forming composition according to [1], further comprising a crosslinking agent. [3] The non-photosensitive insulating film forming composition according to [2], wherein the crosslinking agent is a bismaleimide compound. [4] Group A 1 but, [ka] The aromatic heterocycle may have a crosslinkable substituent. [1] to [3], the non-photosensitive insulating film forming composition according to any one of the above. [5] Group A 2 but, [ka] [ka] and [ka] and wherein each of these aromatic heterocycles may have a crosslinkable substituent. [1] to [4], the non-photosensitive insulating film forming composition according to any one of the above. [6] Group B1 is at least one selected from the following: [ka] (In the formula, G represents a direct bond or any of the following formulae: [ka] L and M each independently represent a hydrogen atom, a phenyl group, or a C1-3 alkyl group. [1] to [5], the non-photosensitive insulating film forming composition according to any one of the above. [7] Group B 1 but, [ka] Represented by [1] to [6], the non-photosensitive insulating film forming composition according to any one of the above. [8] Group B 2 is at least one selected from the following: [ka] (In the formula, G represents a direct bond or any of the following formulae: [ka] L and M each independently represent a hydrogen atom, a phenyl group, or a C1-3 alkyl group. [1] to [7], the non-photosensitive insulating film forming composition according to any one of the above. [9] Group B 2 is at least one selected from the following: [ka] (In the formula, G1 and G2 each independently represent a direct bond or any of the following formulae: [ka] L and M each independently represent a hydrogen atom, a phenyl group, or a C1-3 alkyl group. [1] to [7], the non-photosensitive insulating film forming composition according to any one of the above.
[10] The non-photosensitive insulating film forming composition according to any one of [1] to [9], wherein the crosslinkable substituent contains a radical crosslinkable group.
[11] The non-photosensitive insulating film forming composition according to any one of [1] to
[10] , wherein the crosslinkable substituent comprises a (meth)acrylate group, a maleimide group, or an allyl group.
[12] The non-photosensitive insulating film forming composition according to any one of [1] to
[11] , wherein m=0.
[13] The non-photosensitive insulating film forming composition according to any one of [1] to
[12] , wherein the boiling point of the solvent is 230° C. or lower.
[14] The non-photosensitive insulating film forming composition according to any one of [1] to
[13] , wherein the boiling point of the solvent is 200° C. or lower.
[15] A non-photosensitive resin film, which is a cured product of a coating film of the non-photosensitive insulating film forming composition according to any one of [1] to
[14] .
[16] The non-photosensitive resin film according to
[15] , having a dielectric tangent of less than 0.01. Effect of the Invention
[0008] According to the present invention, it is possible to provide a non-photosensitive resin composition which gives a cured product having a low relative dielectric constant and a low dielectric loss tangent, and a non-photosensitive resin film obtained from the composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] [Non-photosensitive insulating film forming composition] The non-photosensitive insulating film forming composition of the present invention comprises The following formula (1): [ka] [In formula (1), Base A 1teeth, [ka] represents a 5- to 8-membered aromatic heterocycle represented by the formula: The aromatic heterocycle may have a bridging substituent, Base A 2 teeth, [ka] represents a 5- to 8-membered aromatic heterocycle represented by the formula: The aromatic heterocycle may have a bridging substituent, Base B 1 represents an organic group having 6 to 40 carbon atoms and having a crosslinkable substituent, which may contain at least one heteroatom selected from N, S, and O and may contain a halogen atom; Base B 2 represents an organic group having 6 to 40 carbon atoms which may contain at least one heteroatom selected from N, S, and O and which has no crosslinkable substituent which may contain a halogen atom; n 1 , n 2 are each independently a number greater than or equal to 0 and less than or equal to 1, m 1 , m 2 are each independently a number greater than or equal to 0 and less than or equal to 1, n is a number equal to or greater than 1, m is a number equal to or greater than 0, 10≦n+m≦500, However, group A 1 , group A 2 When neither of these has a crosslinkable substituent, If m ≠ 0, then n 1 and m 1 At least one of is 1, If m=0, then n 1 is 1.] A polymer having a repeating unit structure represented by the formula: solvent Includes. Here, the term "non-photosensitive" in the non-photosensitive insulating film forming composition means a composition that does not contain a photopolymerization initiator. Each component is described in turn below.
[0010] <Polymer> The polymer according to the present invention has a repeating unit structure represented by the above formula (1).
[0011] Base A 1 represents a 5- to 8-membered aromatic heterocycle that does not contain a heteroatom in the shortest series of covalent bonds between two bonds, and the aromatic heterocycle may have a bridging substituent.
[0012] Preferably, the group A 1 teeth, [ka] The aromatic heterocycle may have a crosslinkable substituent.
[0013] Base A 1 may be one type or a combination of two or more types.
[0014] In the above formula (1), the group A 2 represents a 5- to 8-membered aromatic heterocycle containing a nitrogen atom in the shortest series of covalent bonds between two bonds, and the aromatic heterocycle may have a bridging substituent.
[0015] Preferably, the group A 2 teeth, [ka] [ka] and [ka] and any of these aromatic heterocycles may have a crosslinkable substituent.
[0016] Base A 2 may be one type or a combination of two or more types.
[0017] Preferably, the crosslinkable substituent comprises a radically crosslinkable group.
[0018] Preferably, the crosslinkable substituent comprises a (meth)acrylate group, a maleimide group, or an allyl group.
[0019] Examples of the crosslinkable substituent containing a (meth)acrylate group include those represented by the following general formula (2): [ka] (In the formula, R 3 , R 4 and R 5 are each independently a hydrogen atom or a monovalent organic group having 1 to 3 carbon atoms, and m is an integer of 1 to 10. * represents the group A in general formula (1). 1 , group A 2 , or group B 1 is a bonding site with respect to the ring.
[0020] R in the above general formula (2) 3 is not limited as long as it is a hydrogen atom or a monovalent organic group having 1 to 3 carbon atoms, but is preferably a hydrogen atom or a methyl group from the viewpoint of reactivity in the radical reaction.
[0021] R in the above general formula (2) 4 and R 5 are not limited as long as they are each independently a hydrogen atom or a monovalent organic group having 1 to 3 carbon atoms, but are preferably a hydrogen atom.
[0022] In the above general formula (2), m is an integer of 1 or more and 10 or less, and preferably an integer of 1 or more and 4 or less.
[0023] Specific examples of monovalent organic groups having 1 to 3 carbon atoms include linear alkyl groups such as methyl, ethyl, and propyl groups; branched alkyl groups such as isopropyl groups; alicyclic alkyl groups such as cyclopropyl groups; alkenyl groups such as vinyl and allyl groups; alkynyl groups such as ethynyl groups; alkoxy groups such as methoxy, ethoxy, and propoxy groups; acyl groups such as acetyl groups; ester groups such as methoxycarbonyl groups; formyl groups; haloformyl groups; carbamoyl groups; cyano groups; and heterocyclic groups such as oxiranyl groups, aziridinyl groups, thietanyl groups, triazinyl groups, oxathiolanyl groups, dihydroazetyl groups, and dihydrothiazolyl groups.
[0024] In the above formula (1), the group B 1 represents an organic group having 6 to 40 carbon atoms and having a crosslinkable substituent which may contain at least one heteroatom selected from N, S, and O and may contain a halogen atom.
[0025] Preferably, the group B 1 is at least one selected from the following: [ka] (In the formula, G represents a direct bond or any of the following formulae: [ka] L and M each independently represent a hydrogen atom, a phenyl group, or a C1-3 alkyl group.
[0026] Preferably, the group B 1 teeth, [ka] It is expressed as:
[0027] In the above formula (1), the group B 2represents an organic group having 6 to 40 carbon atoms and no crosslinkable substituent, which may contain at least one heteroatom selected from N, S, and O and may contain a halogen atom.
[0028] Preferably, the group B 2 is at least one selected from the following: [ka] (In the formula, G represents a direct bond or any of the following formulae: [ka] L and M each independently represent a hydrogen atom, a phenyl group, or a C1-3 alkyl group.
[0029] In addition, group B 2 is also preferably at least one selected from the following: [ka] (In the formula, G1 and G2 each independently represent a direct bond or any of the following formulae: [ka] L and M each independently represent a hydrogen atom, a phenyl group, or a C1-3 alkyl group.
[0030] Base A 1 , group A 2 When neither of the groups has a crosslinking substituent, if m ≠ 0, then n 1 and m 1 At least one of m is 1, and if m=0, then n 1 is 1. That is, in the polymer having the repeating unit structure represented by formula (1), the group A 1 , group A 2 Even if neither of the groups has a crosslinkable substituent, the group B 1 exists.
[0031] In the polymer having the repeating unit structure represented by formula (1), the group A 2 does not necessarily have to exist. In that case, m=0 in formula (1).
[0032] [Method for preparing a polymer having a repeating unit structure represented by formula (1)] The polymer having the repeating unit structure represented by formula (1) can be prepared by a known method. For example, 1 Compounds represented by -X, XA 2 -X, HO-B 1 Compounds represented by -OH and HO-B 2 The compound represented by the formula: 1 , A 2 , B 1 , B 2 is as defined above, and X is a halogen atom. 1 Compounds represented by -X and XA 2 -X and HO-B 1 Compounds represented by -OH and HO-B 2 Each of the compounds represented by -OH may be used alone or in combination of two or more. 1 Compounds represented by -X and XA 2 -X compounds, HO-B 1 Compounds represented by -OH and HO-B 2 The total amount of the compounds represented by --OH can be set to 0.1 to 10 moles, preferably 0.1 to 2 moles.
[0033] The catalyst used in the condensation reaction may be a basic or acidic catalyst, but it is preferable to use a basic catalyst. The basic catalyst may be a solid base catalyst, such as calcium hydroxide, strontium hydroxide octahydrate, barium hydroxide octahydrate, magnesium hydroxide, sodium carbonate, or potassium carbonate. Examples of acidic catalysts that can be used include mineral acids such as sulfuric acid, phosphoric acid, and perchloric acid; organic sulfonic acids such as p-toluenesulfonic acid, p-toluenesulfonic acid monohydrate, and methanesulfonic acid; and carboxylic acids such as formic acid and oxalic acid. The amount of catalyst used varies depending on the type of catalyst used. 1 Compounds represented by -X and XA 2 The amount is usually 0.001 to 10,000 parts by mass, preferably 0.01 to 1,000 parts by mass, and more preferably 0.05 to 100 parts by mass, relative to 100 parts by mass of the total of the compounds represented by -X.
[0034] The condensation reaction can be carried out without a solvent, but is usually carried out using a solvent. The solvent is not particularly limited as long as it can dissolve the reaction substrate and does not inhibit the reaction. Examples of the solvent include 1,2-dimethoxyethane, diethylene glycol dimethyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, tetrahydrofuran, and dioxane. The condensation reaction temperature is usually 40° C. to 200° C., preferably 50° C. to 180° C. The reaction time varies depending on the reaction temperature, but is usually 5 minutes to 500 hours, preferably 5 minutes to 200 hours.
[0035] The weight average molecular weight of the polymer having the repeating unit structure represented by formula (1) is usually 500 to 100,000, and preferably 600 to 80,000, 800 to 60,000, or 1,000 to 50,000.
[0036] [solvent] As the solvent, it is preferable to use an organic solvent from the viewpoint of solubility for the polymer having the repeating unit structure represented by formula (1).Specific examples include N,N-dimethylformamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N,N-dimethylacetamide, dimethylsulfoxide, diethylene glycol dimethyl ether, cyclopentanone, cyclohexanone, γ-butyrolactone, α-acetyl-γ-butyrolactone, methyl lactate, ethyl lactate, tetramethylurea, 1,3-dimethyl-2-imidazolinone, N-cyclohexyl-2-pyrrolidone, N-methyl-2-pyrrolidinone, toluene, and methyl ethyl ketone, which can be used alone or in combination of two or more kinds.Preferably, the solvent has a boiling point of 230°C or less, and more preferably, the solvent has a boiling point of 200°C or less.
[0037] The above-mentioned solvent can be used in an amount of, for example, 30 parts by mass to 1500 parts by mass, preferably 40 parts by mass to 1000 parts by mass, and more preferably 50 parts by mass to 300 parts by mass, relative to 100 parts by mass of the polymer having a repeating unit structure represented by formula (1), depending on the desired coating film thickness and viscosity of the non-photosensitive insulating film-forming composition.
[0038] [Other ingredients] In the embodiment, the non-photosensitive insulating film forming composition may further contain components other than the polymer having the repeating unit structure represented by the above formula (1) and the solvent. Examples of the other components include resin components other than the polymer having the repeating unit structure represented by the formula (1), a thermal polymerization initiator, a hindered phenol compound, a crosslinking agent, a filler, etc.
[0039] [Resin components other than the polymer having the repeating unit structure represented by formula (1)] In an embodiment, the non-photosensitive insulating film forming composition may further contain a resin component other than the polymer having the repeating unit structure represented by the formula (1). Examples of the resin component that can be contained in the non-photosensitive insulating film forming composition include polyimide, polyoxazole, polyoxazole precursor, phenol resin, polyamide, epoxy resin, siloxane resin, and acrylic resin. When such a resin is blended, the blending amount of the resin component is preferably within the range of 0.01 to 20 parts by mass based on 100 parts by mass of the polymer having the repeating unit structure represented by formula (1).
[0040] [Thermal polymerization initiator] In an embodiment, a thermal polymerization initiator may be blended into the non-photosensitive insulating film forming composition to promote thermal polymerization and enhance curing properties. Examples of the thermal polymerization initiator include, but are not limited to, ketone peroxides (methyl ethyl ketone peroxide, cyclohexanone peroxide, etc.), diacyl peroxides (acetyl peroxide, benzoyl peroxide, etc.), hydroperoxides (hydrogen peroxide, tert-butyl hydroperoxide, cumene hydroperoxide, etc.), dialkyl peroxides (di-tert-butyl peroxide, dicumyl peroxide, dilauroyl peroxide, etc.), peroxyketals (dibutylperoxycyclohexane, etc.), alkyl peresters (peroxyneodecanoic acid-tert-butyl ester, peroxypivalic acid-tert-butyl ester, peroxy-2-ethylcyclohexanoic acid-tert-amyl ester, etc.), persulfates (potassium persulfate, sodium persulfate, ammonium persulfate, etc.), and azo compounds (azobisisobutyronitrile, 2,2'-di(2-hydroxyethyl)azobisisobutyronitrile, etc.). The thermal polymerization initiator may be a commercially available product. Such a thermal polymerization initiator may be used alone or in combination of two or more kinds.
[0041] The amount of the thermal polymerization initiator is preferably 1 to 10 parts by mass, and more preferably 1 to 5 parts by mass, based on 100 parts by mass of the polymer having the repeating unit structure represented by formula (1).
[0042] [Crosslinking agent] In the embodiment, in order to increase the crosslinking density and improve the curability, a crosslinking agent can be blended into the non-photosensitive insulating film forming composition. As such a crosslinking agent, a polyfunctional vinyl ether compound, a polyfunctional allyl ether compound, and a bismaleimide compound that undergo radical polymerization reaction by a thermal polymerization initiator are preferable. Examples of polyfunctional vinyl ether compounds include ethylene glycol divinyl ether, diethylene glycol divinyl ether, polyethylene glycol divinyl ether, propylene glycol divinyl ether, butylene glycol divinyl ether, hexanediol divinyl ether, bisphenol A alkylene oxide divinyl ether, bisphenol F alkylene oxide divinyl ether, trimethylolpropane trivinyl ether, ditrimethylolpropane tetravinyl ether, glycerin trivinyl ether, pentaerythritol tetravinyl ether, dipentaerythritol pentavinyl ether, and dipentaerythritol hexavinyl ether. Examples of compounds that can be used include, but are not limited to, polyethylene glycol divinyl ether, pentaerythritol divinyl ether, pentaerythritol trivinyl ether, vinylbenzyl ether, pentaerythritol tetravinyl ether, 4-methoxyvinylbenzyl ether, 2-methoxyvinylbenzyl ether, 1,4-divinyloxymethylbenzene, ethylene oxide-added trimethylolpropane trivinyl ether, ethylene oxide-added ditrimethylolpropane tetravinyl ether, ethylene oxide-added pentaerythritol tetravinyl ether, and ethylene oxide-added dipentaerythritol hexavinyl ether. Examples of polyfunctional allyl ether compounds include ethylene glycol diallyl ether, diethylene glycol diallyl ether, polyethylene glycol diallyl ether, propylene glycol diallyl ether, butylene glycol diallyl ether, hexanediol diallyl ether, bisphenol A alkylene oxide diallyl ether, bisphenol F alkylene oxide diallyl ether, trimethylolpropane triallyl ether, ditrimethylolpropane tetraallyl ether, glycerin triallyl ether, pentaerythritol tetraallyl ether, dipentaerythritol pentaallyl ether, and dipentaerythritol hexaallyl ether. Examples of compounds that can be used include, but are not limited to, polyethylene glycol diallyl ether, pentaerythritol diallyl ether, pentaerythritol triallyl ether, allyl benzyl ether, pentaerythritol tetraallyl ether, 4-methoxyallyl benzyl ether, 2-methoxyallyl benzyl ether, 1,4-diallyloxymethylbenzene, ethylene oxide-added trimethylolpropane triallyl ether, ethylene oxide-added ditrimethylolpropane tetraallyl ether, ethylene oxide-added pentaerythritol tetraallyl ether, and ethylene oxide-added dipentaerythritol hexaallyl ether. Examples of the bismaleimide compound include bis(4-maleimidophenyl)methane, polyphenylmethane maleimide, bis(4-maleimidophenyl)ether, bis(4-maleimidophenyl)sulfone, 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethane bismaleimide, 4-methyl-1,3-phenylene bismaleimide, m-phenylene bismaleimide, 2,2-bis(4-(4-maleimidophenoxy)phenyl)propane, biphenyl, bis(4-maleimidophenyl)methane ... Examples of compounds that can be used include, but are not limited to, bis(4-maleimidophenyl)sulfone, bis(4-maleimidophenyl)sulfide, bis(4-maleimidophenyl)ketone, 2,2-bis(4-(4-maleimidophenoxy)phenyl)propane, bis(4-(4-maleimidophenoxy)phenyl)sulfone, 4,4'-bis(3-maleimidophenoxy)biphenyl, 1,6-bismaleimido-(2,2,4-trimethyl)hexane, and the like.
[0043] The amount of the crosslinking agent added is preferably 1 to 200 parts by mass, and more preferably 1 to 100 parts by mass, based on 100 parts by mass of the polymer having the repeating unit structure represented by formula (1).
[0044] [Filler] The filler may be, for example, an inorganic filler, and specifically, may be a sol of silica, aluminum nitride, boron nitride, zirconia, alumina, or the like.
[0045] [Hindered phenol compounds] In an embodiment, a hindered phenol compound can be optionally blended in the non-photosensitive insulating film forming composition as a polymerization inhibitor for the radical crosslinking site. Examples of the hindered phenol compound include 2,6-di-t-butyl-4-methylphenol, 2,5-di-t-butyl-hydroquinone, octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, isooctyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 4,4'-methylenebis(2,6-di-t-butylphenol), 4,4'-thio-bis(3-methyl-6-t-butylphenol), 4,4'-butylidene-bis(3-methyl-6 -t-butylphenol), triethylene glycol-bis[3-(3-t-butyl-5-methyl-4-hydroxyphenyl)propionate], 1,6-hexanediol-bis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], 2,2-thio-diethylene bis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], N,N'-hexamethylene bis(3,5-di-t-butyl-4-hydroxy-hydrocinnamamide), 2,2'-methylene-bis(4-methyl -6-t-butylphenol), 2,2'-methylene-bis(4-ethyl-6-t-butylphenol), pentaerythrityl-tetrakis〔3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate〕, tris-(3,5-di-t-butyl-4-hydroxybenzyl)-isocyanurate, 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, 1,3,5-tris(3-hydroxy-2,6-dimethyl-4-isopropylbenzyl)- 1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-s-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris[4-(1-ethylpropyl)-3-hydroxy-2,6-dimethylbenzyl]-1,3,5-Triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris[4-triethylmethyl-3-hydroxy-2,6-dimethylbenzyl]-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(3-hydroxy-2,6-dimethyl-4-phenylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-3-hydroxy 1,3,5-tris(4-t-butyl-5-ethyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-6-ethyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione Trione, 1,3,5-tris(4-t-butyl-6-ethyl-3-hydroxy-2,5-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-5,6-diethyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-3-hydroxy-2-methylbenzyl)-1,3 ,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-3-hydroxy-2,5-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-5-ethyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, etc., but are not limited thereto. Among these, 1,3,5-tris(4-t-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione is particularly preferred.
[0046] The amount of the hindered phenol compound is preferably 0.1 to 20 parts by mass relative to 100 parts by mass of the polymer having the repeating unit structure represented by formula (1), and more preferably 0.5 to 10 parts by mass from the viewpoint of the reactivity of the radical crosslinking site. When the amount of the hindered phenol compound is 0.1 parts by mass or more relative to 100 parts by mass of the polymer having the repeating unit structure represented by formula (1), for example, undesired radical crosslinking reaction in a solution is prevented, while when it is 20 parts by mass or less, it is favorable for the crosslinking reaction.
[0047] The non-photosensitive insulating film forming composition of the present invention is useful not only for application to semiconductor devices but also for applications such as interlayer insulating films in multilayer circuits, cover coats for flexible copper-clad boards, solder resist films, and liquid crystal alignment films. EXAMPLES
[0048] Hereinafter, specific examples of the non-photosensitive insulating film forming composition of the present invention will be described using the following examples, but the present invention is not limited thereto.
[0049] The weight average molecular weights shown in the synthesis examples below in this specification are the results of measurements by gel permeation chromatography (hereinafter, abbreviated as GPC in this specification). The apparatus and measurement conditions used in the measurements are as follows: Equipment: GPC system manufactured by JASCO Corporation Columns: Shodex® KF-804L and KF-803L Column oven: 40℃ Flow rate: 1mL / min Eluent: Tetrahydrofuran Sample concentration: 10mg / mL Sample injection volume: 20 μL Standard material: Monodisperse polystyrene Detector: Differential refractometer
[0050] <Synthesis Example 1> (Synthesis of Polymer (1)) In a 2000 ml four-neck flask, 50.00 g (0.329 mol) of 4,6-dichloropyrimidine, 114.51 g (0.366 mol) of 2,2-bis(3-allyl-4-hydroxyphenyl)propane (Konishi Chemical Industry Co., Ltd.), 109.32 g (0.839 mol) of potassium carbonate, and 548.71 g of N-ethyl-2-pyrrolidone were added, heated to 100°C, and stirred for 42 hours. After cooling to below 30°C, 382.80 g of tetrahydrofuran was added for dilution, and the precipitate formed in the reaction solution was removed by filtration to obtain a reaction mixture. The resulting reaction mixture was adjusted to pH 4 with a 6N hydrochloric acid / N-ethyl-2-pyrrolidone (1:9) solution, and then dropped into 3241.81 g of methanol and 648.36 g of pure water to precipitate a polymer. The precipitate obtained was filtered off, and the residue was washed twice with 259.35 g of methanol and dried in vacuum to obtain a polymer. The molecular weight of this polymer was measured by GPC (standard polystyrene equivalent) to find that the weight average molecular weight (Mw) was 13,968, and the yield was 71.91%. This polymer has a repeating unit structure represented by the following formula (1).
[0051] [ka]
[0052] <Synthesis Example 2> (Synthesis of Polymer (2)) In a 1000-mL four-neck flask, 25.00 g (0.165 mol) of 4,6-dichloropyrimidine, 27.63 g (0.086 mol) of 2,2-bis(3-allyl-4-hydroxyphenyl)propane (Konishi Chemical Industry Co., Ltd.), 30.28 g (0.086 mol) of 1,3-bis[2-(4-hydroxyphenyl)-2-propyl]benzene, 54.66 g (0.420 mol) of potassium carbonate, and 194.10 g of N-ethyl-2-pyrrolidone were placed and heated to 100° C., and stirred at 100° C. for 46 hours. After cooling to below 30° C., the mixture was diluted with 275.43 g of tetrahydrofuran, and the precipitate formed in the reaction solution was removed by filtration to obtain a reaction mixture. The resulting reaction mixture was adjusted to pH 4 with a 6N hydrochloric acid / N-ethyl-2-pyrrolidone (1:9) solution, and then dropped into 819.83 g of methanol and 1168.00 g of pure water to precipitate a polymer. The resulting precipitate was filtered off, and the filter cake was washed twice with 130.60 g of methanol and dried in vacuum to obtain a polymer. The molecular weight of this polymer was measured by GPC (standard polystyrene equivalent) to find that the weight average molecular weight (Mw) was 11,778, and the yield was 88.62%. This polymer has a repeating unit structure represented by the following formula (2).
[0053] [ka]
[0054] <Synthesis Example 3> (Synthesis of Polymer (3)) In a 1000 ml four-neck flask, 20.00 g (0.132 mol) of 4,6-dichloropyrimidine, 22.34 g (0.069 mol) of 2,2-bis(3-allyl-4-hydroxyphenyl)propane (Konishi Chemical Industry Co., Ltd.), 23.81 g (0.069 mol) of spiro-bichroman, 43.73 g (0.336 mol) of potassium carbonate, and 154.73 g of N-ethyl-2-pyrrolidone were added and heated to 100°C and stirred for 44 hours. After lowering the temperature to below 30°C, 219.86 g of tetrahydrofuran was added for dilution, and the precipitate formed in the reaction solution was removed by filtration to obtain a reaction mixture. The resulting reaction mixture was adjusted to pH 4 with a 6N hydrochloric acid / N-ethyl-2-pyrrolidone (1:9) solution, and then added dropwise to 667.22 g of methanol and 911.75 g of pure water to precipitate a polymer. The precipitate obtained was filtered off, and the residue was washed twice with 104.20 g of methanol and dried in vacuum to obtain a polymer. The molecular weight of this polymer was measured by GPC (standard polystyrene equivalent) to find that the weight average molecular weight (Mw) was 14,313 and the yield was 68.00%. This polymer has a repeating unit structure represented by the following formula (3).
[0055] [ka]
[0056] <Synthesis Example 4> (Synthesis of Polymer (4)) In a 100-mL four-neck flask, 3.00 g (0.020 mol) of 4,6-dichloropyrimidine, 3.42 g (0.011 mol) of 2,2-bis(3-allyl-4-hydroxyphenyl)propane (Konishi Chemical Co., Ltd.), 3.00 g (0.011 mol) of 4,4'-(butane-1,4-diylbis(oxy))diphenol synthesized in the same manner as in a reported example (Polym. Chem. 2012, 3, 2892), 6.56 g (0.050 mol) of potassium carbonate, and 21.71 g of N-ethyl-2-pyrrolidone were placed and heated to 100°C and stirred for 49 hours. After cooling to below 30°C, 28.15 g of tetrahydrofuran was added for dilution, and the precipitate formed in the reaction solution was removed by filtration to obtain a reaction mixture. The resulting reaction mixture was adjusted to pH 4 with a 6N hydrochloric acid / N-ethyl-2-pyrrolidone (1:9) solution, and then dropped into 146.46 g of methanol and 208.11 g of pure water to precipitate a polymer. The resulting precipitate was filtered off, washed twice with 11.82 g of methanol, and dried in vacuum to obtain a polymer. The molecular weight of this polymer was measured by GPC (standard polystyrene equivalent) to find that the weight average molecular weight (Mw) was 27,735, and the yield was 80.01%. This polymer has a repeating unit structure represented by the following formula (4).
[0057] [ka]
[0058] <Synthesis Example 5> (Synthesis of Polymer (5)) In a 100-mL four-neck flask, 3.00 g (0.020 mol) of 4,6-dichloropyrimidine, 3.32 g (0.010 mol) of 2,2-bis(3-allyl-4-hydroxyphenyl)propane (Konishi Chemical Co., Ltd.), 3.20 g (0.010 mol) of 4,4'-(hexane-1,6-diylbis(oxy))diphenol synthesized in the same manner as in the reported example (Polym. Chem. 2012, 3, 2892), 6.56 g (0.050 mol) of potassium carbonate, and 22.00 g of N-ethyl-2-pyrrolidone were added and heated to 100°C and stirred for 49 hours. After cooling to below 30°C, the mixture was diluted with 89.00 g of tetrahydrofuran, and the precipitate formed in the reaction solution was removed by filtration to obtain a reaction mixture. The resulting reaction mixture was adjusted to pH 4 with a 6N hydrochloric acid / N-ethyl-2-pyrrolidone (1:9) solution, and then dropped into 151.14 g of methanol and 216.36 g of pure water to precipitate a polymer. The resulting precipitate was filtered off, washed twice with 11.92 g of methanol, and dried in vacuum to obtain a polymer. The molecular weight of this polymer was measured by GPC (standard polystyrene equivalent) to find that the weight average molecular weight (Mw) was 16,016, and the yield was 71.34%. This polymer has a repeating unit structure represented by the following formula (5).
[0059] [ka]
[0060] <Synthesis Example 6> (Synthesis of Polymer (6)) In a 100-mL four-neck flask, 3.00 g (0.020 mol) of 4,6-dichloropyrimidine, 3.35 g (0.010 mol) of 2,2-bis(3-allyl-4-hydroxyphenyl)propane (Konishi Chemical Co., Ltd.), 3.54 g (0.010 mol) of 4,4'-(octane-1,8-diylbis(oxy))diphenol synthesized in the same manner as in the reported example (Polym. Chem. 2012, 3, 2892), 6.56 g (0.050 mol) of potassium carbonate, and 23.11 g of N-ethyl-2-pyrrolidone were added and heated to 100°C and stirred for 30 hours. After cooling to below 30°C, 89.00 g of tetrahydrofuran was added for dilution, and the precipitate formed in the reaction solution was removed by filtration to obtain a reaction mixture. The resulting reaction mixture was adjusted to pH 4 with a 6N hydrochloric acid / N-ethyl-2-pyrrolidone (1:9) solution, and then dropped into 156.17 g of methanol and 215.31 g of pure water to precipitate a polymer. The resulting precipitate was filtered off, washed twice with 12.29 g of methanol, and dried in vacuum to obtain a polymer. The molecular weight of this polymer was measured by GPC (standard polystyrene equivalent) to find that the weight average molecular weight (Mw) was 28,607, and the yield was 70.57%. This polymer has a repeating unit structure represented by the following formula (6).
[0061] [ka]
[0062] <Example 1> A composition was prepared by dissolving 6.32 g of the polymer obtained in Synthesis Example 1 and 6.32 g of 2,2-bis-[4-(4-maleimidophenoxy)phenyl]propane (manufactured by K.I. Chemical Co., Ltd.) in 18.96 g of cyclohexanone. The resulting solution was then filtered using a microfilter made of polytetrafluoroethylene (hereinafter abbreviated as PTFE in this specification) with a pore size of 5 μm to prepare a non-photosensitive resin composition.
[0063] <Example 2> A composition was prepared by dissolving 15.80 g of the polymer obtained in Synthesis Example 2 and 15.80 g of 2,2-bis-[4-(4-maleimidophenoxy)phenyl]propane (manufactured by K.I. Chemical Co., Ltd.) in 47.39 g of cyclohexanone. The resulting mixture was then filtered using a PTFE microfilter with a pore size of 5 μm to prepare a non-photosensitive resin composition.
[0064] <Example 3> A composition was prepared by dissolving 6.32 g of the polymer obtained in Synthesis Example 3 and 6.32 g of 2,2-bis-[4-(4-maleimidophenoxy)phenyl]propane (manufactured by K.I. Chemical Co., Ltd.) in 18.96 g of cyclohexanone. The resulting mixture was then filtered using a PTFE microfilter with a pore size of 5 μm to prepare a non-photosensitive resin composition.
[0065] <Example 4> A composition was prepared by dissolving 2.53 g of the polymer obtained in Synthesis Example 4 and 2.53 g of 2,2-bis-[4-(4-maleimidophenoxy)phenyl]propane (manufactured by K.I. Chemical Co., Ltd.) in 7.58 g of cyclohexanone. The resulting mixture was then filtered using a PTFE microfilter having a pore size of 5 μm to prepare a non-photosensitive resin composition.
[0066] <Example 5> A composition was prepared by dissolving 2.53 g of the polymer obtained in Synthesis Example 5 and 2.53 g of 2,2-bis-[4-(4-maleimidophenoxy)phenyl]propane (manufactured by K.I. Chemical Co., Ltd.) in 7.58 g of cyclohexanone. The resulting mixture was then filtered using a PTFE microfilter having a pore size of 5 μm to prepare a non-photosensitive resin composition.
[0067] <Example 6> A composition was prepared by dissolving 2.53 g of the polymer obtained in Synthesis Example 6 and 2.53 g of 2,2-bis-[4-(4-maleimidophenoxy)phenyl]propane (manufactured by K.I. Chemical Co., Ltd.) in 7.58 g of cyclohexanone. The resulting mixture was then filtered using a PTFE microfilter having a pore size of 5 μm to prepare a non-photosensitive resin composition.
[0068] <Comparative Example 1> A solution was prepared by dissolving 9.00g of 2,2-bis(4-cyanatophenyl)propane and 1.00g of 4,4'-bismaleimidophenylmethane in 10.00g of tetrahydrofuran, and further dissolving 0.10g of iron acetylacetonate as a curing catalyst. The prepared solution was applied to aluminum foil laminated on a silicon wafer using a spin coater, prebaked at 75°C for 5 minutes, and further baked at 100°C for 1 hour in a vacuum, and then at 160°C for 4 hours to form a BT resin film with a thickness of about 10-30μm.
[0069] [Electrical property test] The non-photosensitive resin compositions prepared in Examples 1 to 6 were applied to aluminum foil laminated on a silicon wafer using a spin coater, pre-baked at 100°C for 5 minutes, and further baked at 230°C for 4 hours under nitrogen to form a film with a thickness of about 10-20 μm. The film was then immersed in 6N hydrochloric acid. The aluminum was dissolved and the film floated up, which was then collected and cut to a length of 7.5 cm and a width of 6.3 cm to obtain a free-standing film. Using this free-standing film, the relative dielectric constant and dielectric loss tangent at 10 GHz immediately after obtaining the free-standing film were calculated by a split cylinder type cavity resonance method. The hydrochloric acid treatment and cutting were also performed in the same manner for Comparative Example 1, and measurements were performed by a split cylinder type cavity resonance method. The details of the measurement method are as follows. (Measurement method) Split cylinder type cavity resonance method (Device configuration) Vector network analyzer: N5227A PNA network analyzer (Keysight Technologies, Inc.) Resonator: CR-710 (EM Lab Co., Ltd.) Measurement frequency: Approximately 10 GHz (depends on the resonant frequency of the sample)
[0070] The measurement results are shown in Table 1 below.
[0071] [Table 1] [Industrial Applicability]
[0072] The non-photosensitive insulating film forming composition according to the present invention provides a cured film that exhibits a low relative dielectric constant and a low dielectric loss tangent with respect to BT resin.
Claims
1. The following formula (1): 【Chemical 1】 [In formula (1), Group A 1 teeth, 【Chemistry 2】 represents a 5- to 8-membered aromatic heterocycle represented by the formula: The aromatic heterocycle may have a bridging substituent, Group A 2 teeth, 【Chemistry 3】 represents a 5- to 8-membered aromatic heterocycle represented by the formula: The aromatic heterocycle may have a bridging substituent, Group B 1 represents an organic group having 6 to 40 carbon atoms and having a crosslinkable substituent, which may contain at least one heteroatom selected from N, S, and O and may contain a halogen atom; Group B 2 represents an organic group having 6 to 40 carbon atoms and no crosslinkable substituent, which may contain at least one heteroatom selected from N, S, and O and may contain a halogen atom; n 1 , n 2 are each independently a number greater than or equal to 0 and less than or equal to 1, m 1 , m 2 are each independently a number greater than or equal to 0 and less than or equal to 1, n is a number equal to or greater than 1, m is a number equal to or greater than 0, 10≦n+m≦500, However, group A 1 , group A 2 When neither of these has a crosslinkable substituent, If m≠0, then n 1 and m 1 at least one of is 1, If m=0, then n 1 is 1.] A polymer having a repeating unit structure represented by the formula: solvent A non-photosensitive insulating film forming composition comprising:
2. The non-photosensitive insulating film-forming composition according to claim 1 , further comprising a crosslinking agent.
3. 3. The non-photosensitive insulating film forming composition according to claim 2, wherein the crosslinking agent is a bismaleimide compound.
4. Group A 1 but, 【Chemistry 4】 The aromatic heterocycle may have a crosslinkable substituent. The non-photosensitive insulating film forming composition according to claim 1 .
5. Group A 2 but, 【Chemistry 5】 【Chemistry 6】 and 【Chemistry 7】 and wherein each of these aromatic heterocycles may have a crosslinkable substituent. The non-photosensitive insulating film forming composition according to claim 1 .
6. Group B 1 is at least one selected from the following: 【Chemistry 8】 (In the formula, G represents a direct bond or any of the following formulae: 【Chemistry 9】 L and M each independently represent a hydrogen atom, a phenyl group, or a C1-3 alkyl group. The non-photosensitive insulating film forming composition according to claim 1 .
7. Group B 1 but, 【Chemistry 10】 is expressed as The non-photosensitive insulating film forming composition according to claim 1 .
8. Group B 2 is at least one selected from the following: 【Chemistry 11】 (In the formula, G represents a direct bond or any of the following formulae: 【Chemistry 12】 L and M each independently represent a hydrogen atom, a phenyl group, or a C1-3 alkyl group. The non-photosensitive insulating film forming composition according to claim 1 .
9. Group B 2 is at least one selected from the following: 【Chemistry 13】 (In the formula, G1 and G2 each independently represent a direct bond or any of the following formulae: 【Chemistry 14】 L and M each independently represent a hydrogen atom, a phenyl group, or a C1-3 alkyl group. The non-photosensitive insulating film forming composition according to claim 1 .
10. The non-photosensitive insulating film-forming composition according to claim 1 , wherein the crosslinkable substituent comprises a radical crosslinkable group.
11. 11. The non-photosensitive insulating film-forming composition according to claim 1, wherein the crosslinkable substituent comprises a (meth)acrylate group, a maleimide group, or an allyl group.
12. The non-photosensitive insulating film forming composition according to claim 1 , wherein m=0.
13. The non-photosensitive insulating film forming composition according to claim 1 , wherein the boiling point of the solvent is 230° C. or lower.
14. The non-photosensitive insulating film forming composition according to claim 1 , wherein the boiling point of the solvent is 200° C. or lower.
15. A non-photosensitive resin film, which is a cured product of a coating film of the non-photosensitive insulating film-forming composition according to any one of claims 1 to 14.
16. 16. The non-photosensitive resin film according to claim 15, having a dielectric loss tangent of less than 0.01.
Citation Information
Patent Citations
Inverter
JP1979030440A
Thermosetting resin composition and method for producing cured product
JP2017088647A