Resin film

A three-layer resin film with higher viscosity polyamide 6 in the inner layer and lower viscosity polyamide 6 in the outer layers enhances both bending and abrasion resistance, addressing the compromise in existing films with soft resins.

JP2024160434APending Publication Date: 2024-11-14GUNZE LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023075402
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-01
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

Resin films containing a relatively soft resin like elastomers improve bending resistance but compromise abrasion resistance.

Method used

A resin film composed of three layers, where the first layer has a higher relative viscosity of polyamide 6 compared to the second layer, with the second layer closer to the surface, enhancing both Gelboflex test results and abrasion resistance.

Benefits of technology

The resin film achieves improved Gelboflex test results and abrasion resistance, suitable for packaging under refrigerated conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024160434000001_ABST
    Figure 2024160434000001_ABST
Patent Text Reader

Abstract

To provide a resin film that is relatively good in both Gelbo Flex test results and abrasion resistance.SOLUTION: A resin film includes at least three layers. The three layers include a first layer and a second layer. Each of the first layer and the second layer is predominantly composed of polyamide 6. The second layer is located closer to the surface than the first layer. The relative viscosity of the polyamide 6 included in the first layer is 3.5 or more, which is at least 0.5 higher than the relative viscosity of the polyamide 6 included in the second layer.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin film. [Background technology]

[0002] JP 2017-002114 A (Patent Document 1) discloses a polyamide-based film. This polyamide-based film has at least a polyamide layer containing 86 to 98% by weight of polyamide and 2 to 14% by weight of a flex resistance agent. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2017-002114 A Summary of the Invention [Problem to be solved by the invention]

[0004] In the resin film disclosed in the above Patent Document 1, the results of the Gelbo flex test (flex resistance test) are improved by including a bending agent composed of a relatively soft resin such as an elastomer. However, the inclusion of a relatively soft resin such as an elastomer may reduce the abrasion resistance of the resin film.

[0005] The present invention has been made to solve such problems, and an object of the present invention is to provide a resin film which is relatively good in both the results of the Gelbo flex test and abrasion resistance. [Means for solving the problem]

[0006] The resin film according to the present invention has at least three layers. The three layers include a first layer and a second layer. Each of the first layer and the second layer is mainly composed of polyamide 6. The second layer is located closer to the surface of the resin film than the first layer. The relative viscosity of the polyamide 6 contained in the first layer is 3.5 or more and is 0.5 or more higher than the relative viscosity of the polyamide 6 contained in the second layer.

[0007] The inventor(s) found that in a resin film, when the second layer is located on the surface side of the first layer, and the relative viscosity of the polyamide 6 contained in the first layer is 3.5 or more and is 0.5 or more higher than the relative viscosity of the polyamide 6 contained in the second layer, both the result of the Gelbo flex test and the abrasion resistance are relatively good. In the resin film according to the present invention, the second layer is located on the surface side of the first layer, and the relative viscosity of the polyamide 6 contained in the first layer is 3.5 or more and is 0.5 or more higher than the relative viscosity of the polyamide 6 contained in the second layer. Therefore, this resin film can make both the result of the Gelbo flex test and the abrasion resistance relatively good.

[0008] The resin film may further include a barrier layer.

[0009] This resin film has a barrier layer, which can suppress the permeation of oxygen and the like.

[0010] In the above resin film, the content of polyamide 6 in each of the first layer and the second layer may be 90 wt % or more, and each of the first layer and the second layer may not contain a flex resistance additive.

[0011] In the resin film, the abrasion strength measured through an abrasion resistance test may be 400 times or more, and the total number of pinholes confirmed through three Gelbo flex tests may be 5 or less when the Gelbo flex test is performed in a 25°C environment, and 10 or less when the Gelbo flex test is performed in a 5°C environment. Effect of the Invention

[0012] According to the present invention, it is possible to provide a resin film which is relatively good in both the result of the Gelbo flex test and the abrasion resistance. [Brief description of the drawings]

[0013] [Figure 1] FIG. 2 is a diagram illustrating a cross section of a resin film. [Diagram 2] FIG. 2 is a diagram showing a schematic configuration of a resin film manufacturing apparatus. [Diagram 3] FIG. 11 is a schematic cross-sectional view of a resin film according to another embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, an embodiment according to one aspect of the present invention (hereinafter also referred to as "the present embodiment") will be described in detail with reference to the drawings. Note that the same or corresponding parts in the drawings are given the same reference numerals and their description will not be repeated. Also, each drawing is drawn in a schematic manner with objects appropriately omitted or exaggerated for ease of understanding.

[0015] [1. Resin film composition] FIG. 1 is a schematic diagram showing a cross section of a resin film 10 according to the present embodiment. The resin film 10 is a polyamide-based film. As shown in FIG. 1, the resin film 10 is configured by laminating three layers, and includes a first layer 100 and second layers 110 and 120. The first layer 100 is located between the second layers 110 and 120 in the thickness direction of the resin film 10. Each of the second layers 110 and 120 is located closer to the surface of the resin film 10 than the first layer 100.

[0016] The total thickness of the resin film 10 is, for example, 10 μm to 50 μm, and preferably 10 μm to 30 μm. The ratio of the thickness of the first layer 100 to the sum of the thicknesses of the second layers 110 and 120 is, for example, 30:70 to 70:30, and more preferably 40:60 to 60:40.

[0017] Each of the first layer 100 and the second layers 110, 120 is mainly composed of polyamide 6. The content of polyamide 6 in each of the first layer 100 and the second layers 110, 120 is, for example, 90 wt% or more, preferably 95 wt% or more, more preferably 98 wt% or more, and even more preferably 99 wt% or more. Each of the first layer 100 and the second layers 110, 120 may contain a resin other than polyamide 6, such as polyamide 66.

[0018] The polyamide 6 contained in the first layer 100 (hereinafter also referred to as "first polyamide 6") and the polyamide 6 contained in each of the second layers 110, 120 (hereinafter also referred to as "second polyamide 6") are different in type. Specifically, the first polyamide 6 and the second polyamide 6 have different relative viscosities. The relationship between the relative viscosity of the first polyamide 6 and the relative viscosity of the second polyamide 6 is represented by the following formulas (1) to (3). It is not necessarily required that the polyamide 6 satisfying the following formulas (1) to (3) is contained in both the second layers 110, 120. It is sufficient that the polyamide 6 satisfying the following formulas (1) to (3) is contained in at least one of the second layers 110, 120. ηa-ηb≧0.5 (1) ηa>ηb (2) ηa≧3.5 (3)

[0019] In the above formulas (1) to (3), ηa represents the relative viscosity of the first polyamide 6, and ηb represents the relative viscosity of the second polyamide 6. That is, the relative viscosity of the first polyamide 6 is 3.5 or more and is 0.5 or more higher than the relative viscosity of the second polyamide 6. Each relative viscosity is measured by a method in accordance with JIS K-6920-2.

[0020] Each of the first layer 100 and the second layers 110, 120 may contain multiple types of polyamide 6. In this case, the relative viscosity of the polyamide 6 having the highest relative viscosity among the multiple types of polyamide 6 contained in the first layer 100 is ηa. Moreover, the relative viscosity of the polyamide 6 having the highest relative viscosity among the multiple types of polyamide 6 contained in each of the second layers 110, 120 is ηb. For example, the first layer 100 may contain a medium-viscosity polyamide 6 in addition to a high-viscosity polyamide 6 for the purpose of improving defects during extrusion molding.

[0021] When multiple types of polyamide 6 are contained in each of the first layer 100 and the second layers 110, 120, the content of polyamide 6 having the highest relative viscosity is 10 wt% or more, preferably 20 wt% or more, more preferably 30 wt% or more, and even more preferably 40 wt% or more.

[0022] In addition, the first layer 100 and the second layers 110 and 120 each do not contain a flex-resistant agent. An example of the flex-resistant agent is a thermoplastic elastomer. An example of the thermoplastic elastomer is a polyester-based elastomer, a polyamide-based elastomer, a polyolefin-based elastomer, a polystyrene-based elastomer, a polyurethane-based elastomer, a polyvinyl chloride-based elastomer, and an ionomer polymer.

[0023] Thus, in the resin film 10, the polyamide 6 contained in the first layer 100 has a high relative viscosity, and the polyamide 6 contained in each of the second layers 110, 120 has a low relative viscosity. The reason why the resin film 10 is configured in this manner will be explained below.

[0024] The Gelbo Flex test is generally known as a test for measuring the flex resistance of a resin film. When a resin film contains a relatively soft resin such as an elastomer (e.g., a flex resistance agent), the results of the Gelbo Flex test improve. This is because rubber-based components such as elastomers have a low glass transition point and maintain a flexible state even in a low temperature environment. However, the present inventor(s) found that when a resin film contains a relatively soft resin such as an elastomer, the abrasion resistance of the resin film may decrease.

[0025] The inventor(s) conducted extensive research to realize a resin film that is good in both Gelbo flex test results and abrasion resistance. As a result, the inventor(s) found that in a resin film 10, when each of the second layers 110, 120 is located on the surface layer side of the first layer 100, and the relative viscosity of the polyamide 6 contained in the first layer 100 is 3.5 or more and is 0.5 or more higher than the relative viscosity of the polyamide 6 contained in each of the second layers 110, 120, both the Gelbo flex test results and abrasion resistance are relatively good.

[0026] It is believed that the results of the Gelbo Flex test are improved by using high-viscosity polyamide 6. This is because high-viscosity polyamide 6 has a high molecular weight and a strong yet flexible structure due to entanglement of molecular chains, resulting in high bending resistance. For this reason, in the resin film 10, the first layer 100 contains high-viscosity polyamide 6.

[0027] In addition, it is considered that the abrasion resistance is improved by using medium- or low-viscosity polyamide 6. The harder the polymer, the less likely it is to wear, and the higher the crystallinity, the harder the polymer. In general, the lower the molecular weight, the higher the crystallinity. Medium- or low-viscosity polyamide 6 has a lower molecular weight than high-viscosity polyamide 6, and has a high degree of crystallinity, so has high abrasion resistance. Therefore, it is considered that the abrasion resistance is improved by using medium- or low-viscosity polyamide 6 on the surface layer side. In the resin film 10, each of the second layers 110 and 120 contains medium-viscosity polyamide 6.

[0028] Through these investigations, the inventors found that when, in a resin film 10, each of the second layers 110, 120 is located on the outer surface side of the first layer 100, and the relative viscosity of the polyamide 6 contained in the first layer 100 is 3.5 or more and is 0.5 or more higher than the relative viscosity of the polyamide 6 contained in each of the second layers 110, 120, both the results of the Gelbo flex test and the abrasion resistance are relatively good.

[0029] In resin film 10 according to the present embodiment, each of second layers 110, 120 is located closer to the surface than first layer 100, and the relative viscosity of polyamide 6 contained in first layer 100 is 3.5 or more and is 0.5 or more higher than the relative viscosity of polyamide 6 contained in each of second layers 110, 120. Therefore, resin film 10 can achieve both relatively good results in the Gelbo flex test and good abrasion resistance.

[0030] [2. Manufacturing method of resin film] 2 is a diagram showing a schematic configuration of a manufacturing apparatus 20 for the resin film 10 according to the present embodiment. The resin film 10 is manufactured by the manufacturing apparatus 20. As shown in FIG. 2, the manufacturing apparatus 20 includes a T-die 200, cast rolls 210 and 220, a longitudinal stretching machine 240, and a transverse stretching machine 250.

[0031] The T-die 200 includes a T-die body 201 and raw material input sections 230, 231, and 232. Raw material for forming the second layer 120 is input into the raw material input section 230. For example, a resin made of the second polyamide 6 is input into the raw material input section 230. Raw material for forming the first layer 100 is input into the raw material input section 231. For example, a resin made of the first polyamide 6 is input into the raw material input section 231. Raw material for forming the second layer 110 is input into the raw material input section 232. For example, a resin made of the second polyamide 6 is input into the raw material input section 232. For example, at least a part of an antiblocking agent, an antistatic agent, and an antioxidant may be further input into each of the raw material input sections 230 and 232. Also, for example, an antioxidant may be further input into the raw material input section 231.

[0032] The T-die body 201 is configured to co-extrude the raw materials fed through the raw material feed sections 230, 231, and 232, thereby fusing the molten materials fed into each raw material feed section to form a single integrated film (molten material). The cast rolls 210 and 220 are configured to cool the extruded molten material and send it downstream. The longitudinal stretching machine 240 stretches the molten material cooled by the cast rolls 210 and 220 in the machine direction (MD). The transverse stretching machine 250 stretches the resin film 10 stretched in the MD in the transverse direction (TD).

[0033] The resin film 10 that has been subjected to various stretching processes is wound up by a winding roll (not shown) located downstream. A roll of the resin film 10 is produced through the manufacturing process in the manufacturing apparatus 20.

[0034] [3. Features] As described above, in resin film 10 according to the present embodiment, each of second layers 110, 120 is located closer to the surface than first layer 100, and the relative viscosity of polyamide 6 contained in first layer 100 is 3.5 or more and is 0.5 or more higher than the relative viscosity of polyamide 6 contained in each of second layers 110, 120. Therefore, resin film 10 can achieve both relatively good results in the Gelbo flex test and good abrasion resistance.

[0035] [4. Other embodiments] The idea of ​​the above-mentioned embodiment is not limited to the embodiment described above. For example, at least a part of the configuration of any of the embodiments may be combined with at least a part of the configuration of any of the other embodiments. Hereinafter, an example of another embodiment to which the idea of ​​the above-mentioned embodiment can be applied will be described.

[0036] In the above embodiment, the resin film 10 is configured with three layers. However, the resin film 10 does not necessarily have to be configured with three layers. For example, the resin film 10 may be configured with four or more layers.

[0037] 3 is a schematic cross-sectional view of a resin film 10A according to another embodiment. As shown in FIG. 3, the resin film 10A is configured by laminating five layers, including first layers 100X and 100Y, second layers 110 and 120, and a barrier layer 130.

[0038] In the resin film 10A, the barrier layer 130 is located between the first layers 100X and 100Y. The second layer 110 is laminated on the surface of the first layer 100X opposite to the surface on which the barrier layer 130 is laminated. The second layer 120 is laminated on the surface of the first layer 100Y opposite to the surface on which the barrier layer 130 is laminated.

[0039] Each of the first layers 100X and 100Y has, for example, the same composition as the first layer 100 in the above embodiment. The barrier layer 130 is made of, for example, EVOH (ethylene vinylalcohol copolymer) or m-xylylenediamine (MXD). Since the resin film 10A has the barrier layer 130, it is possible to suppress the permeation of oxygen and the like.

[0040] The above describes the embodiments of the present invention by way of example. That is, the detailed description and the accompanying drawings are disclosed for the purpose of illustrative description. Therefore, some components described in the detailed description and the accompanying drawings may be non-essential components for solving the problem. Therefore, just because the non-essential components are described in the detailed description and the accompanying drawings, it should not be immediately determined that the non-essential components are essential.

[0041] Furthermore, the above-described embodiment is merely an example of the present invention in every respect. The above-described embodiment can be improved or modified in various ways within the scope of the present invention. In other words, in implementing the present invention, specific configurations can be appropriately adopted according to the embodiment. EXAMPLES

[0042] Examples of the present invention will be described below, but the present invention is not limited to the following examples.

[0043] [1. Examples and Comparative Examples] The resin films of Examples 1 to 5 and Comparative Examples 1 to 6 were produced by the following method. The raw material composition constituting each layer was supplied to an extruder at 250°C, and the raw material composition was extruded from a T-die at 250°C onto a chill roll through which cooling water was circulated to obtain a three-layer polyamide-based sheet. The obtained sheet was then longitudinally stretched 3.0 times by a roll stretcher at 65°C, transversely stretched 4.0 times by a tenter stretcher in an atmosphere at 110°C, and further heat-treated in an atmosphere at 210°C by the same tenter to obtain a three-layer polyamide-based film having a thickness of 15 μm. The structure of each resin film was the three-layer structure shown in FIG. 1. The total thickness of each obtained resin film was 15 μm. In each resin film, the thickness of the first layer was 8 μm, and the thickness of each second layer was 3.5 μm.

[0044] The resin film of Example 6 was produced by the following method. The raw material composition constituting each layer was supplied to an extruder at 250°C, and the raw material composition was extruded from a T-die at 250°C into a sheet shape onto a chill roll through which cooling water was circulating, thereby obtaining a five-layer polyamide-based sheet including a barrier resin layer. Next, the obtained sheet was longitudinally stretched 3.0 times by a roll stretcher at 65°C, transversely stretched 4.0 times by a tenter stretcher in an atmosphere of 110°C, and further heat-treated in an atmosphere of 210°C by the same tenter, thereby obtaining a five-layer polyamide-based film having a thickness of 15 μm. The structure of each resin film was the five-layer structure shown in FIG. 3. The total thickness of the obtained resin film was 15 μm. In the resin film, the thickness of each first layer was 3.25 μm, the thickness of each second layer was 3.5 μm, and the thickness of the barrier layer was 1.5 μm.

[0045] In each of Examples 1 to 6 and Comparative Examples 1 to 6, the relative viscosity of polyamide 6 was measured by a method in accordance with JIS K-6920-2.

[0046] In the resin film of Example 1, the relative viscosity of the polyamide 6 contained in the first layer was 4.0, and the relative viscosity of the polyamide 6 contained in each second layer was 3.2. That is, the relative viscosity difference between the first layer and the second layer was 0.8. The content of polyamide 6 having a relative viscosity of 4.0 in the first layer was 100 wt%, and the content of polyamide 6 having a relative viscosity of 3.2 in each second layer was 100 wt%. Note that the resin film of Example 1 did not contain a flex resistance additive.

[0047] In the resin film of Example 2, the relative viscosity of the polyamide 6 contained in the first layer was 3.5, and the relative viscosity of the polyamide 6 contained in each second layer was 3.0. That is, the relative viscosity difference between the first layer and the second layer was 0.5. The content of the polyamide 6 having a relative viscosity of 3.5 in the first layer was 100 wt%, and the content of the polyamide 6 having a relative viscosity of 3.0 in each second layer was 100 wt%. Note that the resin film of Example 2 did not contain a flex resistance additive.

[0048] In the resin film of Example 3, the relative viscosity of the polyamide 6 contained in the first layer was 4.0, and the relative viscosity of the polyamide 6 contained in each second layer was 3.2. That is, the relative viscosity difference between the first layer and the second layer was 0.8. The content of polyamide 6 having a relative viscosity of 4.0 in the first layer was 100wt%. The content of polyamide 6 having a relative viscosity of 3.2 in each second layer was 70wt%, and the content of polyamide 6 having a relative viscosity of 2.4 in each second layer was 30wt%. The higher relative viscosity of 3.2 was used as the relative viscosity in the second layer. Note that the resin film of Example 3 did not contain a flex resistance additive.

[0049] In the resin film of Example 4, the relative viscosity of the polyamide 6 contained in the first layer was 4.0, and the relative viscosity of the polyamide 6 contained in each second layer was 3.2. That is, the relative viscosity difference between the first layer and the second layer was 0.8. The content of the polyamide 6 having a relative viscosity of 4.0 in the first layer was 60 wt%, and the content of the polyamide 6 having a relative viscosity of 3.2 in the first layer was 40 wt%. As the relative viscosity in the first layer, the higher relative viscosity of 4.0 was used. The content of the polyamide 6 having a relative viscosity of 3.2 in each second layer was 100 wt%. Note that the resin film of Example 4 did not contain a flex resistance additive.

[0050] In the resin film of Example 5, the relative viscosity of the polyamide 6 contained in the first layer was 4.0, and the relative viscosity of the polyamide 6 contained in each second layer was 2.4. That is, the relative viscosity difference between the first layer and the second layer was 1.6. The content of polyamide 6 having a relative viscosity of 4.0 in the first layer was 100 wt%, and the content of polyamide 6 having a relative viscosity of 2.4 in each second layer was 100 wt%. Note that the resin film of Example 5 did not contain a flex resistance additive.

[0051] In the resin film of Example 6, the relative viscosity of the polyamide 6 contained in each first layer was 4.0, and the relative viscosity of the polyamide 6 contained in each second layer was 3.2. That is, the relative viscosity difference between the first layer and the second layer was 0.8. The content of the polyamide 6 having a relative viscosity of 4.0 in each first layer was 100 wt%, and the content of the polyamide 6 having a relative viscosity of 3.2 in each second layer was 100 wt%. Note that the resin film of Example 6 did not contain a flex resistance additive.

[0052] In the resin film of Comparative Example 1, the relative viscosity of the polyamide 6 contained in the first layer was 4.0, and the relative viscosity of the polyamide 6 contained in each second layer was 4.0. That is, the relative viscosity difference between the first layer and the second layer was 0. The content of the polyamide 6 having a relative viscosity of 4.0 in the first layer was 100 wt%, and the content of the polyamide 6 having a relative viscosity of 4.0 in each second layer was 100 wt%. Note that the resin film of Comparative Example 1 did not contain a flex resistance additive.

[0053] In the resin film of Comparative Example 2, the relative viscosity of the polyamide 6 contained in the first layer was 3.2, and the relative viscosity of the polyamide 6 contained in each second layer was 3.2. That is, the relative viscosity difference between the first layer and the second layer was 0. The content of the polyamide 6 having a relative viscosity of 3.2 in the first layer was 100 wt%, and the content of the polyamide 6 having a relative viscosity of 3.2 in each second layer was 100 wt%. Note that the resin film of Comparative Example 2 did not contain a flex resistance additive.

[0054] In the resin film of Comparative Example 3, the relative viscosity of the polyamide 6 contained in the first layer was 3.5, and the relative viscosity of the polyamide 6 contained in each second layer was 3.2. That is, the relative viscosity difference between the first layer and the second layer was 0.3. The content of polyamide 6 having a relative viscosity of 3.5 in the first layer was 100 wt%, and the content of polyamide 6 having a relative viscosity of 3.2 in each second layer was 100 wt%. Note that the resin film of Comparative Example 3 did not contain a flex resistance additive.

[0055] In the resin film of Comparative Example 4, the relative viscosity of the polyamide 6 contained in the first layer was 4.0, and the relative viscosity of the polyamide 6 contained in each second layer was 3.2. That is, the relative viscosity difference between the first layer and the second layer was 0.8. The content of polyamide 6 having a relative viscosity of 4.0 in the first layer was 100 wt%, and the content of polyamide 6 having a relative viscosity of 3.2 in each second layer was 100 wt%. The resin film of Comparative Example 4 contained a flex resistance agent (polyester-based elastomer).

[0056] In the resin film of Comparative Example 5, the relative viscosity of the polyamide 6 contained in the first layer was 3.2, and the relative viscosity of the polyamide 6 contained in each second layer was 2.4. That is, the relative viscosity difference between the first layer and the second layer was 0.8. The content of polyamide 6 having a relative viscosity of 3.2 in the first layer was 100 wt%, and the content of polyamide 6 having a relative viscosity of 2.4 in each second layer was 100 wt%. Note that the resin film of Comparative Example 5 did not contain a flex resistance additive.

[0057] In the resin film of Comparative Example 6, the relative viscosity of the polyamide 6 contained in the first layer was 3.2, and the relative viscosity of the polyamide 6 contained in each second layer was 4.0. That is, the relative viscosity difference between the first layer and the second layer was 0.8. The content of polyamide 6 having a relative viscosity of 3.2 in the first layer was 100 wt%, and the content of polyamide 6 having a relative viscosity of 4.0 in each second layer was 100 wt%. Note that the resin film of Comparative Example 6 did not contain a flex resistance additive.

[0058] The composition of each of the resin films in Examples 1 to 6 and Comparative Examples 1 to 6 is shown in Table 1 below.

[0059] [Table 1]

[0060] [2.Various Tests] The resin films of Examples 1 to 6 and Comparative Examples 1 to 6 were subjected to the following tests.

[0061] <2-1. Gelboflex test> Measurements were performed using a Gelbo Flex Tester manufactured by Rikagaku Kogyo Co., Ltd. A resin film bag made into a cylindrical shape with a folded diameter of 150 mm and a length of 300 mm was attached to the Gelbo Flex Tester, and a 440° twist was applied for the first 88.9 cm, followed by a linear horizontal motion for the next 63.5 cm. This was repeated 1000 times at a test speed of 40 times / min under conditions of 25°C and 5°C, and the number of pinholes was then counted using a penetrant. The number of pinholes was measured at 300 cm in the center of the sample. 2 The number of pinholes was measured for the three samples, and the total number of pinholes was recorded as the measurement result.

[0062] <2-2. Abrasion resistance test> A resin film was attached to a cone-shaped aluminum jig using tape, and the apex of the cone-shaped jig was brought into contact with cardboard (KOKUYO Campus Itame grain, for paper size 430g / m2) via the resin film. The radius of the apex was 10mm in the sliding direction.

[0063] Next, a load of 25 g was placed on the jig. Under the condition of 65% humidity, the jig was slid parallel to the cardboard at a speed of 6000 mm / min and within a range of a moving distance of 45 mm, and the number of slides was measured in increments of 25, and the number of slides at which a pinhole opened was measured. For example, if a pinhole opened after 300 slides but not after 275 slides, the number was counted as 300 slides.

[0064] The occurrence of pinholes was judged by dropping a penetrating liquid on the resin film where the apex of the jig had been in contact, and observing whether or not the liquid penetrated onto a piece of white paper.

[0065] [3. Test Results] The test results are shown in Table 2 below.

[0066] [Table 2] As shown in Table 2, for each of the resin films of Examples 1 to 6, the result of the Gelbo flex test in a 25°C environment was 2 or less (5 or less), and the result of the Gelbo flex test in a 5°C environment was 8 or less (10 or less). It was found that each of the resin films of Examples 1 to 6 is suitable for packaging foods and the like that are distributed refrigerated. Furthermore, for each of the resin films of Examples 1 to 6, the abrasion strength measured through the abrasion resistance test was 400 times or more. That is, for each of the resin films of Examples 1 to 6, both the result of the Gelbo flex test and the abrasion resistance were relatively good.

[0067] On the other hand, the resin film of Comparative Example 1 had low abrasion resistance, and the resin film of Comparative Example 2 had poor results in the Gelbo flex test in a 5° C. environment. The resin film of Comparative Example 3 had poor results in the Gelbo flex test in a 5° C. environment, and the resin film of Comparative Example 4 had low abrasion resistance. The resin film of Comparative Example 5 had poor results in the Gelbo flex test in both 25° C. and 5° C. environments, and the resin film of Comparative Example 6 had low abrasion resistance. [Explanation of symbols]

[0068] 10, 10A resin film, 20 manufacturing apparatus, 100, 100X, 100Y first layer, 110, 120 second layer, 130 barrier layer, 200 T-die, 201 T-die body, 210, 220 cast roll, 230, 231, 232 raw material input section, 240 longitudinal stretching machine, 250 transverse stretching machine.

Claims

1. A resin film having at least three layers, The three layers include a first layer and a second layer, each of the first layer and the second layer is primarily composed of polyamide 6; the second layer is located closer to a surface of the resin film than the first layer, A resin film, wherein the relative viscosity of the polyamide 6 contained in the first layer is 3.5 or more and is higher than the relative viscosity of the polyamide 6 contained in the second layer by 0.5 or more.

2. The resin film according to claim 1 , further comprising a barrier layer.

3. the content of polyamide 6 in each of the first layer and the second layer is 90 wt % or more; The resin film according to claim 1 or 2, wherein each of the first layer and the second layer does not contain a bending resistance additive.

4. The abrasion strength measured through the abrasion resistance test is 400 times or more, 3. The resin film according to claim 1, wherein the total number of pinholes confirmed through three Gelbo Flex tests is 5 or less when the Gelbo Flex test is performed in a 25°C environment, and 10 or less when the Gelbo Flex test is performed in a 5°C environment.

Citation Information

Patent Citations

  • Polyamide film

    JP2017002114A