Laminate for packaging material, packaging bag and packaged article

The packaging laminate addresses hygiene and quality issues in high recycled resin content laminates by using chemically recycled polyolefin resins, ensuring safe and recyclable packaging with reduced impurities and thermal deterioration.

JP2024160675APending Publication Date: 2024-11-14TOPPAN HOLDINGS INC

Patent Information

Application Number
JP2023195956
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-11-17
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

Conventional packaging laminates using recycled resins face issues with hygiene due to impurities and foreign substances, and quality degradation from thermal deterioration, especially when the recycled resin content is high.

Method used

A packaging material laminate comprising an outer layer base material and a sealant layer made of polyolefin resin films, with a minimum 20% volume content of chemically recycled resin, which is less prone to impurities and thermal deterioration, and optionally including an intermediate base material to enhance strength and hygiene.

Benefits of technology

The laminate maintains improved hygiene and quality even with a high recycled resin content, ensuring safe packaging for contents like food by reducing impurities and thermal degradation, while enhancing recyclability and reducing environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024160675000001_ABST
    Figure 2024160675000001_ABST
Patent Text Reader

Abstract

To provide a laminate for packaging material that enhances the levels of hygiene and quality even with a sufficiently high content of recycled resin, packaging bag, and packaged article.SOLUTION: A laminate for packaging material includes an outer layer substrate and a sealant layer. The outer layer substrate and the sealant layer are composed of polyolefin resin films. The laminate for packaging material has a recycled resin content of 20 vol.% or more. The recycled resin is chemically recycled resin.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a laminate for packaging materials, a packaging bag, and a packaging article. [Background technology]

[0002] Packaging materials used in packaging bags and the like are required to have various properties depending on the application. Therefore, in order to simultaneously satisfy such various performance requirements, the packaging material is generally composed of a laminate including an outer layer base material and a sealant layer. Known examples of such laminates for packaging materials include a laminate including a first layer including an inner liner and a second layer including an outer sheath, where the outer sheath is made of post-consumer resin (hereinafter also referred to as "PCR") that may contain contaminants such as paper, ink, and food residues (see, for example, Patent Document 1 below). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Special Publication No. 2022-552096 Summary of the Invention [Problem to be solved by the invention]

[0004] However, the laminate described in Patent Document 1 above has the following problems when the PCR content is increased in the case where the PCR is a recycled resin containing contaminants, that is, a so-called material recycled resin. That is, in the laminate described in Patent Document 1, impurities and foreign matter may appear on the surface, and there is room for improvement in terms of hygiene. Furthermore, in the laminate described in Patent Document 1, odorous components generated due to thermal degradation of the polyolefin resin were detected, and there was also room for improvement in terms of quality.

[0005] An object of the present disclosure is to provide a laminate for packaging materials, a packaging bag, and a packaging article that can improve hygiene and quality even when the content of recycled resin is sufficiently high. [Means for solving the problem]

[0006] One aspect of the present disclosure provides a laminate for packaging material comprising an outer layer base material and a sealant layer, the outer layer base material and the sealant layer being polyolefin resin films, the content of recycled resin in the laminate for packaging material being 20% ​​by volume or more, and the recycled resin being a chemically recycled resin. The higher the ratio of recycled resin used, the more environmental load can be reduced, and the ratio of recycled resin used is generally 20% by mass or more, preferably 25% by mass or more, and more preferably 30% by mass or more. Since it is not easy to calculate the mass ratio after the laminate for packaging material is made into a packaging material, in the present disclosure, the content of recycled resin is specified in volume % so that it can be calculated by the film thickness ratio. In other words, the ratio of the film thickness of the layer using the recycled resin to the film thickness of the entire laminate can be used as the content of recycled resin (volume %). The density of polyethylene and polypropylene that constitute most of the packaging material is 0.90 to 0.95 g / cm 3 The range of the recycled resin content specified in volume percent generally satisfies the range specified in mass percent. According to the laminate for packaging material, the recycled resin is a chemically recycled resin, which is a recycled resin produced by first decomposing discarded resin into low molecular weight resins through a process such as gasification or monomerization, and then polymerizing the resin. Therefore, the chemically recycled resin is less likely to be mixed with impurities or foreign matter than the material recycled resin, which is a resin produced by cleaning and crushing resin products such as collected used packaging materials, and then melting them with heat to re-produce the raw material. In addition, unlike the material recycled resin, the chemically recycled resin is not affected by heat treatment such as melting after the recycling process, and is therefore less likely to be thermally deteriorated. Therefore, the laminate for packaging material can improve hygiene and quality even if the content of the recycled resin in the laminate for packaging material is increased to 20% by volume or more.

[0007] The content of the polyolefin resin in the laminate for packaging material may be 80% by volume or more. In this case, the content of polyolefin resin in the entire laminate is increased, and therefore the recyclability of the packaging laminate is further improved. The higher the ratio of the same resin used, the easier it is to recycle, and the ratio of the same resin used is generally 80% by mass or more, preferably 85% by mass or more, and more preferably 90% by mass or more. Since it is not easy to calculate the mass ratio after the packaging laminate is made into a packaging material, in this disclosure, the content of polyolefin resin is specified in volume % so that it can be calculated by film thickness ratio. In other words, the ratio of the film thickness of the layer using the polyolefin material to the film thickness of the entire laminate can be used as the content of polyolefin resin (volume %). The density of polyethylene and polypropylene that make up the majority of the packaging material is 0.90 to 0.95 g / cm 3 The polyolefin resin content specified in volume % generally satisfies the value specified in mass %. Moreover, the outer layer base material and the sealant layer are preferably made of the same material.

[0008] In the above laminate for packaging material, the polyolefin resin film may be a polyethylene film. In this case, both the outer layer base material and the sealant layer contain polyethylene films, improving recyclability.

[0009] The above-mentioned packaging laminate may further comprise an intermediate substrate between the outer layer substrate and the sealant layer. In this case, the outer layer base material is reinforced by the intermediate base material, thereby making it possible to further improve the strength of the laminate. The intermediate substrate is also preferably made of a polyolefin resin, and further, the outer substrate and the sealant layer are preferably made of the same material.

[0010] In the laminate for packaging materials, the recycled resin may be a post-consumer recycled resin (PCR). PCR can reduce the cost of laminates because large quantities are available on the market. The recycled resin may be a combination of PCR and post-industrial recycled resin (PIR).

[0011] In the above laminate for packaging materials, the sealant layer may be a non-recycled polyolefin resin film. The sealant layer is the layer that comes into contact with the contents when the contents are placed in a packaging bag obtained by using the laminate. If the sealant layer is a non-recycled polyolefin resin film, the possibility that impurities or foreign matter will migrate to the contents due to heating during retort or boiling treatment of the packaging bag can be further reduced. Therefore, the laminate can be used safely for packaging contents such as food. It is preferable to use a polyolefin resin film derived from biomass as the sealant layer, since the sealant layer does not use petroleum, the amount of petroleum used can be reduced.

[0012] In the above-mentioned laminate for packaging materials, the sealant layer may be composed of a plurality of layers, and the layer located farthest from the outer layer base material may be a non-recycled polyolefin resin film. The layer furthest from the outer layer substrate in the sealant layer is the layer that comes into contact with the contents when the contents are placed in a packaging bag obtained using the laminate. If this layer is a non-recycled polyolefin resin film, the possibility that impurities or foreign matter will migrate to the contents as a result of heating during retort or boiling treatment of the packaging bag can be further reduced. Therefore, the laminate can be used safely to package contents such as food.

[0013] The above-mentioned packaging laminate may further comprise a gas barrier layer between the outer layer base material and the sealant layer. In this case, the gas barrier property of the laminate is further improved, so that when the laminate is used to produce a packaging bag and contents are placed in the packaging bag, deterioration of the contents due to gases such as oxygen can be effectively suppressed.

[0014] Another aspect of the present disclosure provides a packaging bag obtained by using the above-mentioned laminate for packaging materials. According to the packaging bag, as already mentioned, chemically recycled resin is less likely to be mixed with impurities or foreign matter than material recycled resin. Moreover, unlike material recycled resin, chemically recycled resin is not affected by heat treatment such as heat melting after the recycling process, and is therefore less likely to undergo thermal degradation. Therefore, the packaging bag obtained using the above-mentioned packaging laminate can safely contain contents such as food even if the content of recycled resin in the packaging laminate is sufficiently increased to 20 volume % or more. Furthermore, since the quality of the packaging laminate can be improved, the packaging bag obtained using the packaging laminate can have improved properties such as strength.

[0015] Yet another aspect of the present disclosure provides a packaging article comprising the above-described packaging bag and contents contained within the packaging bag. According to the above-mentioned packaging article, as already mentioned, the chemically recycled resin as the recycled resin contained in the laminate is less likely to be mixed with impurities or foreign matter than the materially recycled resin. Moreover, unlike the materially recycled resin, the chemically recycled resin is not affected by heat treatment such as heat melting after the recycling process, and is therefore less likely to be thermally deteriorated. Therefore, the above-mentioned packaging article can be safely stored with the contents such as food contained therein, even if the content of the recycled resin in the packaging laminate is sufficiently high, such as 20 volume % or more. Furthermore, since the packaging laminate can improve the quality, the packaging article including the packaging bag obtained using the packaging laminate can improve the properties such as strength. Effect of the Invention

[0016] According to the present disclosure, there are provided a laminate for packaging materials, a packaging bag, and a packaging article that can improve hygiene and quality even when the content of recycled resin is sufficiently high. [Brief description of the drawings]

[0017] [Figure 1] 1 is a cross-sectional view showing an embodiment of a packaging laminate according to one aspect of the present disclosure. FIG. [Diagram 2] FIG. 2 is a cross-sectional view illustrating an embodiment of a packaging article according to another aspect of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, preferred embodiments of the present disclosure will be described in detail. In the drawings, the same or corresponding parts are denoted by the same reference numerals, and duplicated explanations will be omitted.

[0019] <Laminated body for packaging materials> First, one embodiment of a packaging laminate according to one aspect of the present disclosure will be described with reference to Fig. 1. Fig. 1 is a cross-sectional view showing one embodiment of a packaging laminate according to one aspect of the present disclosure.

[0020] As shown in FIG. 1, a laminate for packaging material (hereinafter also referred to as “laminate”) 100 includes an outer layer base material 10 and a sealant layer 30. The laminate 100 may further include an intermediate substrate 20 between the outer layer substrate 10 and the sealant layer 30 . The outer layer base material 10 and the sealant layer 30 are made of a polyolefin resin film, and the content of recycled resin in the packaging laminate 100 is 20% by volume or more. Here, the recycled resin is a chemically recycled resin.

[0021] According to the laminate 100, even if the content of recycled resin is made sufficiently high, hygiene and quality can be improved.

[0022] (Outer layer base material) The outer layer base material 10 is made of a polyolefin resin film, and the polyolefin resin film contains a resin made of a polyolefin resin.

[0023] Examples of polyolefin resins include polyethylene and polypropylene.

[0024] Polyethylene is a resin containing ethylene as a structural unit. Examples of polyethylene include ethylene homopolymers and copolymers of ethylene and other monomers. The proportion of ethylene in polyethylene is, for example, 80 mol % or more. Examples of other monomers include α-olefins, vinyl acetate, acrylic esters, and the like. The α-olefin may be an olefin having a carbon number in the range of 3 to 20. Examples of the α-olefin include propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, 1-eicosene, 3-methyl-1-butene, 4-methyl-1-pentene, and 6-methyl-1-heptene. Examples of polyethylene include high density polyethylene (HDPE), medium density polyethylene (MDPE), low density polyethylene (LDPE), linear low density polyethylene (LLDPE), very low density polyethylene (VLDPE), ethylene-vinyl acetate copolymer, ionomer resin, ethylene-acrylic acid copolymer, ethylene-methyl acrylate copolymer, ethylene-methacrylic acid copolymer, ethylene-propylene copolymer, etc. These may be used alone or in combination of two or more.

[0025] Polypropylene is a resin that contains propylene as a structural unit and does not contain ethylene as a structural unit. Examples of polypropylene include homopolypropylene, block polypropylene, and random polypropylene.

[0026] The polyolefin resin may be a non-recycled polyolefin resin, a chemically recycled polyolefin resin, or a mixture thereof. The non-recycled polyolefin resin may be a petroleum-derived polyolefin resin obtained using a petroleum-derived raw material monomer, a biomass-derived polyolefin resin obtained using a biomass-derived raw material monomer, or a mixture thereof, but from the viewpoint of reducing the environmental load, a biomass-derived polyolefin resin is preferable. The chemically recycled polyolefin resin may be composed of a single chemically recycled polyolefin resin, or may be composed of a mixture of multiple types of chemically recycled polyolefin resins.

[0027] The outer layer base material 10 may further contain additives such as a filler, an antistatic agent, a plasticizer, a lubricant, a light-shielding pigment, and an antioxidant, as necessary. When the outer layer base material 10 contains a light-shielding pigment, the outer layer base material 10 can function as a light-shielding layer.

[0028] The outer layer base material 10 may be an unstretched film or a stretched film. The stretched film may be a uniaxially stretched film or a biaxially stretched film. The outer layer base material 10 may be composed of either a stretched film or an unstretched film. When the outer layer base material 10 is a biaxially stretched film, the mechanical strength and dimensional stability of the laminate 100 can be improved.

[0029] When an adhesive layer is provided on the surface of the outer layer base material 10, in order to enhance adhesion to the adhesive layer, the surface on the adhesive layer side may be subjected to various pretreatments such as corona treatment, plasma treatment, ozone treatment, and flame treatment, or a coating layer such as an easy-adhesion layer may be provided.

[0030] The thickness of the outer layer substrate 10 is not particularly limited and is, for example, 10 μm or more and 100 μm or less. From the viewpoint of reducing materials to reduce the environmental load and from the viewpoint of obtaining excellent heat resistance, impact resistance, and gas barrier properties, the thickness of the outer layer substrate 10 may be 20 μm or more, 25 μm or more, 30 μm or more, or 40 μm or more. The thickness of the outer layer substrate 10 may also be 60 μm or less, or 50 μm or less.

[0031] (Sealant layer) The sealant layer 30 is made of a polyolefin resin film, and the polyolefin resin film contains a resin made of a polyolefin resin. As the polyolefin resin, the same resin as that used in the outer layer base material 10 can be used.

[0032] The sealant layer 30 preferably has a melting point lower than that of the outer layer base material 10. In this case, when the laminate 100 is heat-sealed, it is possible to heat-seal the sealant layer 30 while suppressing melting of the outer layer base material 10. Furthermore, by heating the laminate 100, the outer layer base material 10 and the sealant layer 30 can be easily separated, and material recycling can be easily performed for each of the outer layer base material 10 and the sealant layer 30.

[0033] The sealant layer 30 may further contain additives, such as a flame retardant, a slip agent, an antiblocking agent, an antioxidant, a light stabilizer, a tackifier, an antistatic agent, and a light-shielding pigment, as necessary. When the sealant layer 30 contains a light-shielding pigment, the sealant layer 30 can function as a light-shielding layer.

[0034] The sealant layer 30 may be composed of a single layer or multiple layers. When the sealant layer 30 is composed of a single layer, the sealant layer 30 may be a recycled polyolefin resin film or a non-recycled polyolefin resin film, but is preferably a non-recycled polyolefin resin film. The sealant layer 30 is the layer that comes into contact with the contents when the contents are placed in a packaging bag obtained by using the laminate 100. If the sealant layer 30 is a non-recycled polyolefin resin film, the possibility that impurities or foreign matter will migrate to the contents as a result of heating during retort or boiling treatment of the packaging bag can be further reduced. For this reason, the laminate 100 can be used safely to package contents such as food. When the sealant layer 30 is composed of multiple layers, all of the layers may be recycled polyolefin resin films, or non-recycled polyolefin resin films, or some of the layers may be non-recycled polyolefin resin films and the remaining layers may be recycled polyolefin resin films. When at least a portion of the sealant layer 30 is a non-recycled polyolefin resin film, it is preferable that the layer located farthest from the outer layer base material 10 is a non-recycled polyolefin resin film. The layer of the sealant layer 30 located farthest from the outer layer base material 10 is the layer that comes into contact with the contents when the contents are placed in a packaging bag obtained using the laminate 100. If this layer is a non-recycled polyolefin resin film, the possibility that impurities or foreign matter will migrate to the contents as a result of heating during retort or boiling treatment of the packaging bag can be further reduced. For this reason, the laminate 100 can be used safely to package contents such as food. When the plurality of layers is three layers, the plurality of layers may consist of a first outer layer, a middle layer, and a second outer layer. Here, the first outer layer and the second outer layer may be made of a non-recycled polyolefin resin film, and the intermediate layer may be made of a recycled polyolefin resin film.

[0035] The thickness of the sealant layer 30 is not particularly limited and is appropriately adjusted depending on the application of the laminate 100. The thickness of the sealant layer 30 may be, for example, 10 μm or more, 25 μm or more, 30 μm or more, 40 μm or more, or 50 μm or more. The thickness of the sealant layer 30 may be 100 μm or less, 80 μm or less, 60 μm or less, or 50 μm or less.

[0036] (Intermediate substrate) The intermediate base material 20 is a base material that reinforces the outer layer base material 10, and can further improve the strength of the laminate 100. The intermediate base material 20 is made of a polyolefin resin film, and the polyolefin resin film contains a resin made of a polyolefin resin. As the polyolefin resin, the same resin as that used in the outer layer base material 10 can be used.

[0037] The intermediate substrate 20 may be a single layer or a laminate of multiple layers. When the intermediate substrate 20 is composed of a single layer, the intermediate substrate 20 may be a recycled polyolefin resin film or a non-recycled polyolefin resin film. When the intermediate substrate 20 is composed of multiple layers, all of the layers may be recycled polyolefin resin films, or may be non-recycled polyolefin resin films, or some of the layers may be non-recycled polyolefin resin films and the remaining layers may be recycled polyolefin resin films. However, materials other than those mentioned above can be used as long as the recycled resin content is 20% or more by volume. For example, polyethylene terephthalate resin can be used, although the olefin resin ratio in the packaging material is lower. Also, if polyethylene terephthalate resin produced by chemical recycling is used, the recycled resin content can be increased. When the plurality of layers is three layers, the plurality of layers may consist of a first outer layer, a middle layer, and a second outer layer. Here, the first and second outer layers may be made of non-recycled polyolefin resin films, and the intermediate layer may be made of recycled polyolefin resin films. In this case, the possibility that impurities or foreign matter will migrate from the intermediate substrate 20 through the sealant layer 30 to the contents due to heating during retort or boiling treatment of the packaging bag can be further reduced. Therefore, the laminate 100 can be used safely to package contents such as food.

[0038] The thickness of the intermediate substrate 20 is not particularly limited and is appropriately adjusted depending on the application of the laminate 100. The thickness of the intermediate substrate 20 may be, for example, 10 μm or more, 25 μm or more, 30 μm or more, 40 μm or more, or 50 μm or more. The thickness of the intermediate substrate 20 may be 100 μm or less, 80 μm or less, 60 μm or less, or 50 μm or less.

[0039] (Adhesive layer) The adhesive layer may be an adhesive layer formed using an adhesive.

[0040] Examples of the adhesive include known adhesives such as urethane adhesives, polyester adhesives, polyamide adhesives, epoxy adhesives, and isocyanate adhesives.

[0041] The adhesive may or may not contain a biomass-derived component, but from the viewpoint of reducing the environmental load, it is preferable that the adhesive contains a biomass-derived component. Specific examples of the biomass-derived component include the "DIC Dry BM Series" manufactured by DIC Corporation and the "ECOAD Series" manufactured by Toyo Ink Co., Ltd.

[0042] The adhesive may be an adhesive containing an organic solvent or an adhesive containing no organic solvent, but from the viewpoint of reducing the environmental load, an adhesive containing no organic solvent (solvent-free adhesive) is preferable.

[0043] The thickness of the adhesive layer is not particularly limited and may be, for example, 1 μm or more. By making the thickness of the adhesive layer 2 μm or more, sufficient adhesive strength can be obtained. The thickness of the adhesive layer may be 2 μm or more. The thickness of the adhesive layer may be 50 μm or less, 5 μm or less, or 3 μm or less.

[0044] (Printing layer and gas barrier layer) The laminate 100 may further include at least one of a printed layer and a gas barrier layer between the outer layer substrate 10 and the intermediate substrate 20 . The print layer is a layer that displays characters, pictures, etc., and can be formed using ink. As the ink, for example, inks obtained by adding various pigments, plasticizers, drying agents, stabilizers, etc. to a binder resin such as a urethane-based, acrylic-based, nitrocellulose-based, or rubber-based ink can be used.

[0045] The ink may be either water-based or oil-based, but is preferably water-based. Water-based inks use water or alcohol as a solvent, and therefore can further reduce the environmental impact. In particular, when the adhesive is a solventless adhesive, the use of water-based ink as the ink can significantly reduce the environmental impact. In addition, the ink may be biomass ink or not, but from the viewpoint of reducing the environmental impact, it is preferable that the ink is biomass ink. Here, biomass ink refers to ink containing components obtained from biological resources (biomass) such as cotton, pulp, rice bran, vegetable oil, and angiosperm seeds. The ink may be recycled ink made by collecting and recycling used ink, or may be non-recycled ink. From the viewpoint of environmental impact, however, recycled ink is preferable.

[0046] The gas barrier layer is a layer that improves the gas barrier properties of the laminate 100 . The gas barrier layer has a barrier property against gases such as water vapor or oxygen.

[0047] As the gas barrier layer, for example, a vapor-deposited layer of a metal or a vapor-deposited layer of an inorganic compound can be used. Metals include aluminum and silicon. Inorganic oxides include aluminum oxide and silicon oxide (silica). When the gas barrier layer is a vapor-deposited layer of a metal such as aluminum, the gas barrier layer can function as a light-shielding layer.

[0048] (Other layers) The laminate 100 may further include a layer containing a resin other than the polyolefin resin (non-polyolefin resin) so long as the recycled resin content is 20% by volume or more. Examples of non-polyolefin resins include polyamide resins such as nylon, and polyester resins such as polyethylene terephthalate (PET).

[0049] (Laminate) (A) Recycled resin content In the laminate 100, the content of recycled resin in the laminate 100 is 20% by volume or more. When the recycled resin content in the polyolefin resin film containing recycled resin is 100 volume % (100 mass %), the recycled resin content in the laminate 100 can be determined as the ratio of the total thickness of the film to the total thickness of the laminate 100. However, when the recycled resin content in the polyolefin resin film containing recycled resin is X mass % (less than 100 mass %) and the thickness of the film is Y1 (μm), the recycled resin content of the film thickness Y2 (μm) is calculated as X / 100×Y1 (μm). The content of the recycled resin in the laminate 100 is preferably 30% by volume or more, and more preferably 40% by volume or more.

[0050] In the present disclosure, the above-mentioned recycled resin is a chemical recycled resin and does not include material recycled resin. The chemically recycled resin may be a post-consumer recycled resin (PCR), a post-industrial recycled resin (PIR), or a mixture thereof, but is preferably a PCR. Since PCR can be secured in large quantities on the market, if the chemically recycled resin is a PCR, the cost of the laminate 100 can be reduced.

[0051] (B) Polyolefin resin content The content of the polyolefin resin in the laminate 100 is preferably 80% by volume or more, more preferably 85% by volume or more, and particularly preferably 90% by volume or more. When the content of the polyolefin resin in the laminate 100 is 80% by volume or more, the content of the polyolefin resin in the entire laminate 100 becomes high, and therefore the recyclability of the laminate 100 is further improved.

[0052] In the laminate 100, the polyolefin resin films in the outer layer base material 10 and the sealant layer 30 may both be polyethylene films.

[0053] (C) Odor components In a total ion chromatogram obtained by subjecting laminate 100 to mass analysis using purge-and-trap gas chromatography-mass spectrometry, when the ratio of the peak area of ​​nonanal as an indicator of odor components to the sum of the peak area values ​​of all aliphatic hydrocarbon components is R1 (%) and the ratio of the peak area of ​​decanal to the sum of the peak area values ​​of all aliphatic hydrocarbon components is R2 (%), R1 is preferably less than 1.5%, more preferably 1.0% or less, and particularly preferably 0.5% or less. Furthermore, R2 is preferably less than 3.5%, more preferably 2.5% or less, and particularly preferably 1.5% or less. It is preferable that R1 is less than 1.5% and R2 is less than 3.5%, in which case thermal degradation is suppressed overall in the laminate 100, and the quality of the laminate 100 can be further improved. Specifically, the above mass spectrometry is carried out by cutting out a 1.0 gram sample from the laminate 100, placing this sample in a 20 mL vial together with a collector of odor components, heating it at 60°C for 1 hour to adsorb the volatile components from the sample onto the collector, and then analyzing the volatile components in the collector using a purge-and-trap gas chromatograph mass spectrometer.

[0054] (D) Fisheye Fisheyes refer to foreign matter such as gelled or charred spots that look like fish eyes and are found on film. If a fisheye has a diameter of 1 mm or more, it is considered a defective product. The number of fisheyes with a diameter of 0.5 mm or more but less than 1 mm is 100 per m 2 Less than or equal to 50 pieces / m 2 Less than 10 pieces / m 2 It would be better if it was less than this.

[0055] (E) Variation in kinetic friction On the surface of the outer layer base material 10 of the laminate 100, the variation (in-plane variation) of the kinetic friction force refers to the standard deviation σ of the kinetic friction force. σ is preferably less than 0.45, more preferably less than 0.35, and particularly preferably less than 0.2. When σ is less than 0.45, the transportability of the laminate 100 can be improved when the layer having σ of less than 0.45 is placed on the transport roller side. In addition, on the surface of the layer, there are regions where the dynamic friction force received from the transport roller is large and regions where it is small, and the difference in stress between the regions is small, so that the residual distortion in the layer is reduced, and the decrease in the strength of the laminate 100 caused by the residual distortion can be suppressed. From the viewpoint of the strength of the laminate, σ is preferably 0.1 or more, more preferably 0.2 or more, and particularly preferably 0.3 or more. The dynamic friction coefficient is measured for the laminate 100 using a multifunction static and dynamic friction tester TL201Tt (manufactured by Trinity Lab Co., Ltd.) and a tactile measuring probe. The standard deviation σ of the dynamic friction force is a value obtained based on JIS K 7125-ISO8295, and specifically, is determined by placing the laminate 100 on a test table with the outer layer base material 10 facing down, and moving a tactile measuring probe at a sliding speed of 10 mm / sec while contacting the laminate 100 with a load of 50 grams.

[0056] (F) Impurities The laminate 100 is analyzed by a Fourier transform infrared spectrophotometer (FT-IR: Fourier transform infrared spectroscopy) using an attenuated total reflection (ATR) measurement method. When an ATR spectrum is obtained, the 2915 cm -1 Absorption coefficients of CH inverse symmetric stretching of methylene groups near 1720 cm from polyesters and polyurethanes -1 The ratio R3 of the absorption coefficients for C=O stretching near the polyolefin is preferably less than 0.1, more preferably less than 0.05, and particularly preferably 0.01 or less, as an index showing that there are few resin components other than polyolefin. In the above analysis, a diamond prism is used as the prism to be brought into close contact with the laminate 100, and the angle of incidence with respect to the surface of the laminate 100 is set to 45°.

[0057] When the laminate 100 includes the outer layer substrate 10, the intermediate substrate 20, and the sealant layer 30, it is preferable that the outer layer substrate 10 and the sealant layer 30 are composed of a non-recycled polyolefin resin film, and the intermediate substrate 20 includes a recycled polyolefin resin film. In this case, even if impurities or foreign matter are mixed in the intermediate substrate 20, the intermediate substrate 20 is sandwiched between the outer layer substrate 10 and the sealant layer 30, and therefore even if impurities or foreign matter are present in the intermediate substrate 20, the impurities or foreign matter are unlikely to appear outside the laminate 100. Furthermore, when the laminate 100 includes an outer layer base material 10 and a sealant layer 30, at least one of the outer layer base material 10 and the sealant layer 30 may be a recycled polyolefin resin film.

[0058] <Packaged goods> Next, an embodiment of a packaging article according to another aspect of the present disclosure will be described with reference to Fig. 2. Fig. 2 is a cross-sectional view showing one embodiment of a packaging article according to another aspect of the present disclosure.

[0059] As shown in FIG. 2, the packaged article 500 includes a packaging bag 400 and a content C contained in the packaging bag 400. The packaging bag 400 is obtained by using a pair of laminates 100. The packaging bag 400 is obtained, for example, by placing the sealant layers 30 of a pair of laminates 100 facing each other and bonding the peripheral portions. The packaging bag 400 is composed of a storage section that stores the content C and an adhesive section provided around the storage section. The adhesive section is a portion formed by bonding the sealant layers 30 of opposing laminates 100 to each other, and the storage section is a portion where the sealant layers 30 of opposing laminates 100 are not bonded to each other.

[0060] According to the packaging item 500, the chemically recycled resin as the recycled resin contained in the laminate 100 is less likely to be mixed with impurities or foreign matter than the material recycled resin, which is a resin obtained by cleaning and crushing resin products such as collected used packaging materials, and then heating and melting them to re-materialize them. In addition, unlike the material recycled resin, the chemically recycled resin is not affected by heat treatment such as heating and melting after the recycling process, and is therefore less likely to be thermally deteriorated. Therefore, even if the content rate of the recycled resin in the laminate 100 is sufficiently high, such as 20 volume % or more, the packaging item 500 can safely contain the contents C such as food. In addition, since the laminate 100 can improve the quality, the packaging item 500 equipped with the packaging bag 400 obtained using the packaging laminate 100 can improve the properties such as strength.

[0061] (Contents) The contents C are not particularly limited and may be appropriately selected depending on the application of the packaging bag 400. The contents C are not particularly limited, and examples of the contents C include food, shampoo, rinse, body soap, detergent, and the like.

[0062] (packaging bag) The pair of laminates 100 constituting the packaging bag 400 may have the same configuration as each other, or may have different configurations from each other.

[0063] The packaging bag 400 may have a half-cut line, and may further have an easy-open processed part at both ends or one end of the half-cut line. Examples of the easy-open processed part include a group of scars, and a V-shaped, U-shaped, or I-shaped notch.

[0064] In the adhesive portion of the packaging bag 400, the sealant layers 30 of the pair of laminates 100 may be directly adhered to each other by heat sealing (see FIG. 2), or may be adhered to each other by an adhesive.

[0065] (Method of manufacturing packaging articles) Next, a method for producing a packaged article 500 using the laminate 100 will be described.

[0066] First, a pair of laminates 100 is prepared. Then, the sealant layers 30 of the pair of laminates 100 are placed opposite each other, and the sealant layers 30 are bonded together. At this time, a part of the peripheral portion of the laminate is bonded to form a U-shape to form a bonded portion, and a non-bonded portion (unbonded portion) is also formed. In this manner, a packaging bag having an opening formed by the unbonded portion is obtained.

[0067] Next, the contents C are filled in through the opening of the packaging bag. Thereafter, the sealant layers 30 of the laminate 100 are bonded together at the unbonded portions, so that the unbonded portions also become bonded portions. In this manner, a packaged article 500 including the packaging bag 400 and the contents C contained therein can be manufactured.

[0068] Although the preferred embodiments of the present disclosure have been described above, the present disclosure is not limited to the above embodiments. For example, in the packaged article 500 shown in Fig. 2, the packaging bag 400 is formed using a pair of laminates 100, but the laminates 200 may be used instead of the laminates 100. The packaging bag may also be manufactured by folding one of the laminates 100, 200 with the sealant layer 30 on the inside and bonding the overlapping peripheral portions together.

[0069] 2, the shape of the packaging bag 400 may be a standing pouch-shaped packaging bag, a two-sided bag, a three-sided bag, a four-sided bag, a palm-shaped bag, or a gusset bag. The packaging bag 400 may be provided with a spout or a synthetic resin fastener that can be repeatedly sealed by fitting a strip-shaped protrusion and a strip-shaped groove.

[0070] The embodiments of the present disclosure have been described above, and the outline of the present disclosure is as follows. [1] A laminate for packaging materials comprising an outer layer base material and a sealant layer, the outer layer base material and the sealant layer are polyolefin resin films, The content of recycled resin in the laminate for packaging material is 20% by volume or more, The laminate for packaging materials, wherein the recycled resin is a chemically recycled resin. [2] The laminate for packaging materials according to [1], further comprising an intermediate substrate between the outer layer substrate and the sealant layer. [3] The laminate for packaging materials according to [1] or [2], wherein the recycled resin is a post-consumer recycled resin. [4] The laminate for packaging materials according to any one of [1] and [3], wherein the content of polyolefin resin in the laminate for packaging materials is 80 volume % or more. [5] The laminate for packaging materials according to any one of [1] to [3], wherein the outer layer base material and the sealant layer are made of the same material. [6] The laminate for packaging materials according to any one of [1] to [5], wherein the sealant layer is a non-recycled polyolefin resin film. [7] The laminate according to any one of [1] to [5], wherein the sealant layer is composed of a plurality of layers, and the layer located farthest from the outer layer base material is a non-recycled polyolefin resin film. [8] The laminate for packaging materials according to any one of [1] to [7], further comprising a gas barrier layer between the outer layer base material and the sealant layer. [9] A packaging bag obtained by using the laminate for packaging material according to any one of [1] to [8].

[10] A packaging article comprising the packaging bag described in [9] and contents contained in the packaging bag. EXAMPLES

[0071] The present disclosure will be described more specifically with reference to the following examples, but the present disclosure is not limited to these examples.

[0072] Example 1 As the outer layer substrate, a chemically recycled low-density polyethylene (PCR ChemiR 100%-LDPE) film (thickness 35 μm) was prepared using used packaging materials, and as the sealant layer, a petroleum-derived low-density polyethylene (petroleum-derived LDPE) film (thickness 60 μm) was prepared. Note that "PCR ChemiR 100%-LDPE" means that the content of post-consumer chemically recycled resin (PCR ChemiR) in the outer layer substrate is 100% by volume (100% by mass). Then, a printing layer was formed on one surface of the outer layer substrate using aqueous flexographic ink, and then a dry lamination adhesive (urethane-based adhesive) was applied to the surface of the printing layer to form an adhesive layer with a thickness of 3 μm (dry film thickness). The adhesive layer was then bonded to the sealant layer to produce a packaging laminate (outer layer substrate / printing layer / adhesive layer / sealant layer).

[0073] Example 2 A packaging laminate (outer layer substrate / printed layer / adhesive layer / sealant layer) was produced in the same manner as in Example 1, except that the outer layer substrate was changed from a PCR ChemiR 100%-LDPE film (thickness 35 μm) to a PCR ChemiR 100%-LDPE film (thickness 25 μm) and the sealant layer was changed from a petroleum-derived LDPE film (thickness 60 μm) to a biomass-derived low-density polyethylene (biomass-derived LDPE) film (thickness 60 μm).

[0074] Example 3 A PCR ChemiR 100%-LDPE film (thickness 25 μm) was prepared as the outer layer substrate, a PCR ChemiR 100%-LDPE film (thickness 25 μm) was prepared as the intermediate substrate, and a petroleum-derived LDPE film (thickness 60 μm) was prepared as the sealant layer. Then, a printed layer was formed on one surface of the outer layer substrate using water-based flexographic ink, and then a dry lamination adhesive (urethane-based adhesive) was applied to the surface of the printed layer to form a first adhesive layer with a thickness of 3 μm (dry film thickness), and the intermediate substrate was bonded to the first adhesive layer. Next, a dry lamination adhesive (urethane-based adhesive) was applied to the surface of the intermediate substrate to form a second adhesive layer with a thickness of 3 μm (dry film thickness), and the second adhesive layer was bonded to the sealant layer to produce a packaging laminate (outer layer substrate / printed layer / first adhesive layer / intermediate substrate / second adhesive layer / sealant layer).

[0075] Example 4 A packaging laminate (outer layer substrate / printed layer / first adhesive layer / intermediate substrate / second adhesive layer / sealant layer) was produced in the same manner as in Example 3, except that the outer layer substrate was changed from a PCR ChemiR 100%-LDPE film (thickness 25 μm) to a biomass-derived LDPE film (thickness 25 μm) and the sealant layer was changed from a petroleum-derived LDPE film (thickness 60 μm) to a biomass-derived LDPE film (thickness 60 μm).

[0076] Example 5 A laminate for packaging material (outer layer substrate / printed layer / first adhesive layer / intermediate substrate / second adhesive layer / sealant layer) was prepared in the same manner as in Example 4, except that the sealant layer was changed from a biomass-derived LDPE film (thickness 60 μm) to a sealant layer prepared by co-extruding three layers: a biomass-derived LDPE film (thickness 20 μm), a PCR Chemi R 100%-LDPE film (thickness 20 μm), and a biomass-derived LDPE film (thickness 20 μm).

[0077] Example 6 A petroleum-derived LDPE film (thickness 20 μm) was prepared as the outer layer substrate, a film made by co-extrusion of three layers of a petroleum-derived LDPE film (thickness 5 μm), a PCR ChemiR 100%-LDPE film (thickness 30 μm), and a petroleum-derived LDPE film (thickness 5 μm) was prepared as the intermediate substrate, and a petroleum-derived LDPE film (thickness 5 μm) was prepared as the sealant layer. Then, a printing layer was formed on one surface of the outer layer substrate using an aqueous flexographic ink, a dry lamination adhesive (urethane adhesive) was applied to the surface of the printing layer to form a first adhesive layer having a thickness of 3 μm (dry film thickness), and the intermediate substrate was bonded to the first adhesive layer. Next, a dry lamination adhesive (urethane adhesive) was applied to the surface of the intermediate substrate to form a second adhesive layer having a thickness of 3 μm (dry film thickness), and the intermediate substrate was bonded to the sealant layer using the second adhesive layer to produce a packaging laminate (outer layer substrate / printing layer / first adhesive layer / intermediate substrate / second adhesive layer / sealant layer).

[0078] Comparative Example 1 The outer layer substrate was a low-density polyethylene (PCRMR100%-LDPE) film (thickness 25μm) made from recycled materials using used polyethylene bags, and the sealant layer was a petroleum-derived LDPE film (thickness 60μm). Note that "PCR ChemiR100%-LDPE" means that the content of post-consumer mechanically recycled resin (PCRMR) in the outer layer substrate is 100% by volume (100% by mass). Then, a printing layer was formed on one surface of the outer layer substrate using water-based flexographic ink, and a dry laminating adhesive (urethane-based adhesive) was applied to the surface of the printing layer to form an adhesive layer 3 μm thick (dry film thickness). The adhesive layer was then bonded to the sealant layer to produce a packaging laminate.

[0079] Comparative Example 2 A packaging laminate was produced in the same manner as in Comparative Example 1, except that the outer layer substrate was changed from a PCRMR100%-LDPE film (thickness 20 μm) to a low-density polyethylene (PCRMR40%-LDPE) film (thickness 60 μm) obtained by cleaning used polyethylene bags and mixing low-density polyethylene (PCRMR-LDPE) pellets obtained by mechanically recycling them with petroleum-derived LDPE pellets in a ratio of 40:60 (mass ratio), and the sealant layer was changed from a petroleum-derived LDPE film (thickness 60 μm) to a petroleum-derived LDPE film (thickness 50 μm). "PCRMR40%-LDPE" means that the content of post-consumer mechanically recycled resin (PCRMR) in the outer layer substrate is 40% by mass. In this case, the volume of the layer made of recycled material can be calculated by taking into account the density of the mixed resin, and this can be used to calculate the film thickness ratio. If the density of the mixed resins is the same, mass% = volume% can be used. In addition, the density of the PCRMR-LDPE40% film used for the outer layer substrate is low (0.920 g / cm 3 ) was decided.

[0080] Comparative Example 3 A PCRMR100%-LDPE film (thickness 25 μm) was prepared as the outer layer substrate, a PCRMR100%-LDPE film (thickness 25 μm) was prepared as the intermediate substrate, and a petroleum-derived LDPE film (thickness 60 μm) was prepared as the sealant layer. A printed layer was formed on one surface of the outer layer substrate using water-based flexographic ink, a laminating adhesive (urethane adhesive) was applied to the surface of the printed layer to form a first adhesive layer with a thickness of 3 μm (dry film thickness), and the intermediate substrate was bonded to the first adhesive layer. Next, a dry laminating adhesive (urethane adhesive) was applied to the surface of the intermediate substrate to form a second adhesive layer with a thickness of 3 μm (dry film thickness), and the intermediate substrate was bonded to the sealant layer using the second adhesive layer to produce a packaging laminate (outer layer substrate / printed layer / first adhesive layer / intermediate substrate / second adhesive layer / sealant layer).

[0081] Comparative Example 4 The outer layer substrate was a low-density polyethylene (PCRMR-LLDPE 100%) film (thickness 35 μm) that had been material-cycled using used packaging material (nylon / printed layer / PET layer / aluminum vapor deposition layer / linear low-density polyethylene (LLDPE) sealant layer), and a petroleum-derived LDPE film (thickness 60 μm) was prepared as the sealant layer. Then, a printed layer was formed on one surface of the outer layer substrate using water-based flexographic ink, and a laminating adhesive (urethane-based adhesive) was applied to the surface of the printed surface to form an adhesive layer with a thickness of 3 μm (dry film thickness). The adhesive layer was then bonded to the sealant layer to produce a laminate for packaging material.

[0082] Comparative Example 5 As the outer layer substrate, a low-density polyethylene film (PCRMR-HDPE-LLDPE100%) (thickness 25 μm) that was material-cycled using used packaging materials (high-density polyethylene (HDPE) layer / printed layer / HDPE layer / LLDPE sealant layer) was prepared, and as the sealant layer, a petroleum-derived LDPE film (thickness 60 μm) was prepared. Note that "PCRMR-HDPE-LLDPE100%" means that the total content of mechanically recycled high-density polyethylene (HDPE) and linear low-density polyethylene (LLDPE) in the outer layer substrate is 100% by volume (100% by mass). Then, a printed layer was formed on one surface of the outer layer substrate using water-based flexographic ink, and a laminating adhesive (urethane-based adhesive) was applied to the surface of the printed surface to form an adhesive layer with a thickness of 3 μm (dry film thickness). The adhesive layer was then bonded to the sealant layer to produce a laminate for packaging material.

[0083] (Reference example 1) A petroleum-derived LDPE film (thickness 25 μm) was prepared as the outer layer substrate, and a petroleum-derived LDPE film (thickness 60 μm) was prepared as the sealant layer. Then, a printed layer was formed on one surface of the outer layer substrate using water-based flexographic ink, and a laminating adhesive (urethane-based adhesive) was applied to the surface of the printed surface to form an adhesive layer with a thickness of 3 μm (dry film thickness). The adhesive layer was then bonded to the sealant layer to produce a laminate for packaging material.

[0084] <Recycled resin content> For the laminates for packaging materials of the Examples, Comparative Examples and Reference Examples prepared as described above, the content of recycled resin in the laminates for packaging materials was calculated based on the following formula. Recycled resin content = 100 x total thickness of layers containing recycled resins / total thickness of laminate for packaging material However, when the layer containing the recycled resin is a layer containing a recycled resin and a resin derived from petroleum or biomass, the value obtained by multiplying the thickness of this layer by the content (mass%) of the recycled resin in the layer was used as the thickness value of the layer containing the recycled resin.

[0085] <Evaluation> The laminates for packaging materials of the Examples, Comparative Examples and Reference Examples prepared as described above were subjected to the following evaluations: Evaluation 1 (generation of odorous components), Evaluation 2 (fish eyes), Evaluation 3 (impurities) and Evaluation 4 (variation in dynamic friction force). Here, Evaluation 1 is an evaluation on quality, and Evaluations 2 and 3 are evaluations on hygiene.

[0086] (1) Rating 1 (Odor component generation) First, the laminate for packaging materials was analyzed using purge-and-trap gas chromatography mass spectrometry. Specifically, a 1.0 gram sample was cut out from the laminate for packaging materials, and this sample was placed in a 20 mL vial together with a collector for odor components, and heated at 60°C for 1 hour to adsorb the volatile components from the sample onto the collector. The volatile components in the collector were then analyzed using a purge-and-trap gas chromatography mass spectrometry device, and a total ion chromatogram was obtained. Next, in the total ion chromatogram obtained as described above, the ratio R1 of the peak area of ​​nonanal to the sum of the peak area values ​​of all the aliphatic hydrocarbon components, and the ratio R2 of the peak area of ​​decanal to the sum of the peak area values ​​of all the aliphatic hydrocarbon components, as indicators of odor components, were calculated. The evaluation was carried out based on the following evaluation criteria. The results are shown in Table 1. (Evaluation Criteria) ◎ R1 is less than 1.5% and R2 is less than 0.35% ○ R1 is less than 1.5% and R2 is 0.35% or more, or R1 is 1.5% or more and R2 is less than 0.35% × R1 is 1.5% or more and R2 is 0.35% or more

[0087] (2) Rating 2 (Fisheye) A sample measuring 1m x 1m was cut from the packaging laminate, and placed on a black table. Protrusions (protruding foreign objects) with a diameter of 0.5mm or more and less than 1mm were visually counted as fisheye 1 (N1), and protrusions (protruding foreign objects) with a diameter of 1mm or more were visually counted as fisheye 2 (N2), and evaluation was performed based on the following evaluation criteria. The results are shown in Table 1. (Evaluation Criteria) ◎ N1 is 10 or less and N2 is 0 ○ N1 is 11 to 99 and N2 is 0 × N1 is 100 or more or N2 is 1 or more

[0088] (3) Rating 3 (impurities) The laminate for packaging material was analyzed by Fourier transform infrared spectroscopy (FT-IR) using attenuated total reflection (ATR) to obtain an ATR spectrum. At this time, a diamond prism was used as the prism to be attached to the laminate for packaging material, and the incident angle to the surface of the laminate for packaging material was set to 45°. In addition, the 2915 cm spectrum of polyethylene is -1 Absorption coefficients of CH inverse symmetric stretching of methylene groups near 1720 cm from polyesters and polyurethanes -1 The ratio R3 of the absorption coefficients of the C=O stretching near the nucleus was calculated and evaluated based on the following criteria. The results are shown in Table 1. (Evaluation Criteria) ◎ R3 is less than 0.05 ○ R3 is 0.05 or more and less than 0.1 × R3 is 0.1 or more

[0089] (4) Rating 4 (variation in dynamic friction force) The kinetic friction force of the laminate for packaging materials was measured using a multi-function static and kinetic friction tester TL201Tt (manufactured by Trinity Lab Co., Ltd.) and a tactile tester. Specifically, the packaging laminate was placed on a test table with the sealant layer facing down, and a tactile probe was moved at a sliding speed of 10 mm / sec while being in contact with the packaging laminate (on the outer layer substrate side) with a load of 50 grams, and the standard deviation of the dynamic frictional force was obtained, and this standard deviation σ of the dynamic frictional force was taken as the variation in the dynamic frictional force. Evaluation was then performed based on the following evaluation criteria. The results are shown in Table 1. (Evaluation Criteria) A σ is less than 0.35 B σ is 0.35 or more and less than 0.45 C σ is 0.45 or more

[0090] [Table 1]

[0091] As can be seen from the results shown in Table 1, in all of the packaging laminates of Examples 1 to 6 which used chemically recycled resin, even when the recycled resin content was increased to 20% by volume or more, almost no odorous components were generated and the amount of foreign matter and impurities was small. In contrast, in the laminates for packaging materials of Comparative Examples 1 to 5, which used material recycled resin, when the recycled resin content was increased to 20 volume % or more, at least one of the following occurred: an increase in the amount of odorous components, an increase in the number of fish eyes, and an increase in the amount of impurities.

[0092] In the above examples and comparative examples, the polyolefin resin is polyethylene. However, even if polypropylene is used as the polyolefin resin, the results are similar in terms of odor components, fish eyes, impurities, and dynamic friction coefficient due to the similarity of the resin structure.

[0093] From the above, it was confirmed that according to the laminate for packaging material of the present disclosure, hygiene and quality can be improved even if the content of recycled resin is sufficiently increased. [Explanation of symbols]

[0094] 10...outer layer substrate, 20...intermediate substrate, 30...sealant layer, 100...laminate, 400...packaging bag, 500...packaged article, C...contents.

Claims

1. A packaging laminate comprising an outer layer base material and a sealant layer, the outer layer base material and the sealant layer are polyolefin resin films, The content of recycled resin in the laminate for packaging material is 20% by volume or more, The laminate for packaging materials, wherein the recycled resin is a chemically recycled resin.

2. The laminate for packaging materials according to claim 1 , further comprising an intermediate substrate between the outer layer substrate and the sealant layer.

3. 2. The laminate for packaging materials according to claim 1, wherein the recycled resin is a post-consumer recycled resin.

4. 2. The packaging laminate according to claim 1, wherein the content of the polyolefin resin in the packaging laminate is 80 volume % or more.

5. 2. The packaging laminate according to claim 1, wherein the outer layer base material and the sealant layer are made of the same material.

6. The laminate for packaging materials according to claim 1 , wherein the sealant layer is a polyolefin resin film derived from petroleum or biomass.

7. The laminate according to claim 1 , wherein the sealant layer is composed of a plurality of layers, and the layer located furthest from the outer layer substrate is a non-recycled polyolefin resin film.

8. The packaging material laminate according to claim 1 , further comprising a gas barrier layer between the outer layer base material and the sealant layer.

9. A packaging bag obtained by using the laminate for packaging material according to any one of claims 1 to 8.

10. The packaging bag according to claim 9 , and contents contained within the packaging bag.

Citation Information

Patent Citations

  • Polyolefin resin-based cross-linked foam and adhesive tape

    JP2023001768A

  • Laminate, packaging material, and packaging container

    JP2023048894A

  • Flexible pouches using post-consumer resins

    JP2022552096A

Cited By

  • Film package, in particular for wet wipes