Laminate, packaging bag and packaging container

A laminate with polypropylene base and sealant layers, enhanced by an electron beam cured resin layer, addresses heat resistance issues, ensuring stable heat sealing and recyclability.

JP2024160806APending Publication Date: 2024-11-15DAI NIPPON PRINTING CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023076195
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-02
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Conventional laminates with polypropylene as a main component for both the base material and sealant layer lack sufficient heat resistance, leading to damage during heat-sealing, impairing their functionality as packaging materials.

Method used

A laminate structure comprising a base material and a sealant layer, both primarily made of polypropylene, with an electron beam cured resin layer on the base material to enhance heat resistance, allowing for improved heat sealing without deformation.

Benefits of technology

The laminate exhibits excellent heat resistance, enabling stable heat sealing and maintaining structural integrity during processing, facilitating recyclability and suitability for retort and boiling treatments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024160806000002
    Figure 2024160806000002
  • Figure 2024160806000003
    Figure 2024160806000003
  • Figure 2024160806000004
    Figure 2024160806000004
Patent Text Reader

Abstract

To provide a laminate that has excellent heat resistance, wherein a base material and a sealant layer each contain polypropylene as the main component.SOLUTION: A laminate includes: a substrate having a first surface and a second surface; an electron beam curable resin layer provided on a first surface of the substrate; and a sealant layer provided on a second surface of the substrate, wherein the substrate contains polypropylene as a main component and the sealant layer contains polypropylene as a main component.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a laminate, a packaging bag, and a packaging container. [Background technology]

[0002] Conventionally, a laminate having a substrate and a sealant layer has been used as a packaging material (see, for example, Patent Document 1). For example, a polyolefin film is used as the sealant layer because it has flexibility, transparency, and excellent heat sealability. A stretched polyester film or a stretched polyamide film is used as the substrate because it has excellent strength and heat resistance. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2009-202519 A Summary of the Invention [Problem to be solved by the invention]

[0004] In recent years, there has been a demand for recycling packaging materials in order to reduce the environmental load. From the viewpoint of recycling, it is preferable that the substrate and the sealant layer are each made of the same type of resin material (mono-materialization). The present inventors have investigated a laminate in which the substrate and the sealant layer each contain polypropylene as a main component. However, the present inventors have found that in this case, it is not possible to provide a sufficient difference in heat resistance between the substrate and the sealant layer, and the laminate may be significantly damaged by heat during, for example, a heat sealing process, and may lose its function as a packaging material.

[0005] One of the problems to be solved by the present disclosure is to provide a laminate in which a substrate and a sealant layer each contain polypropylene as a main component, and which has excellent heat resistance. [Means for solving the problem]

[0006] The laminate of the present disclosure comprises a substrate having a first surface and a second surface, an electron beam cured resin layer provided on the first surface of the substrate, and a sealant layer provided on the second surface of the substrate, wherein the substrate contains polypropylene as a primary component, and the sealant layer contains polypropylene as a primary component. Effect of the Invention

[0007] According to the present disclosure, it is possible to provide a laminate having excellent heat resistance, in which the substrate and the sealant layer each contain polypropylene as a main component. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a schematic cross-sectional view showing one embodiment of a laminate. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing one embodiment of a laminate. [Diagram 3] FIG. 3 is a perspective view showing one embodiment of a packaging container. [Figure 4] FIG. 4 is a schematic cross-sectional view showing one embodiment of a packaging container. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] In this specification, when multiple upper limit candidates and multiple lower limit candidates are given for a certain parameter, the numerical range of the parameter may be configured by combining any one of the upper limit candidates and any one of the lower limit candidates. As an example, the description "parameter B is preferably A1 or more, more preferably A2 or more, even more preferably A3 or more, and also preferably A4 or less, more preferably A5 or less, and even more preferably A6 or less." will be explained. In this example, the numerical range of parameter B may be A1 or more and A4 or less, A1 or more and A5 or less, A1 or more and A6 or less, A2 or more and A4 or less, A2 or more and A5 or less, A2 or more and A6 or less, A3 or more and A4 or less, A3 or more and A5 or less, or A3 or more and A6 or less.

[0010] Hereinafter, the embodiments of the present disclosure will be described in detail. The present disclosure can be implemented in many different forms, and is not to be interpreted as being limited to the description of the embodiments exemplified below. In the drawings, the width, thickness, shape, etc. of each layer may be shown diagrammatically in order to make the explanation clearer, but these are merely examples and do not limit the interpretation of the present disclosure. In this specification and each figure, elements similar to those already explained with respect to the previous figures are given the same reference numerals, and detailed explanations may be omitted as appropriate.

[0011] Each of the components (for example, polyolefins such as polypropylene, α-olefins, resin materials, additives, metals, and inorganic oxides) appearing in the following description may be used alone or in combination of two or more kinds.

[0012] In this specification, the "main component" of a certain layer refers to a component whose content in the layer is preferably more than 50% by mass, more preferably 60% by mass or more, even more preferably 70% by mass or more, and particularly preferably 80% by mass or more.

[0013] [Laminate] The laminate of the present disclosure comprises: a substrate having a first surface and a second surface; an electron beam cured resin layer provided on a first surface of a substrate; a sealant layer disposed on the second surface of the substrate; Equipped with.

[0014] The substrate contains polypropylene as a main component. The sealant layer contains polypropylene as a main component. The polypropylene of the substrate and the polypropylene of the sealant layer may be the same or different. In one embodiment, the laminate of the present disclosure is a packaging material. A packaging bag at least partially produced using a laminate including a substrate containing polypropylene as a main component and a sealant layer containing polypropylene as a main component, and a lid material made of the laminate are excellent in recyclability, and it is not necessary to separate the substrate and the sealant layer after collecting the used packaging bag or lid material. In addition, such a packaging bag or lid material is excellent in retort processing suitability and boiling processing suitability, for example.

[0015] The laminate 1 shown in Fig. 1 comprises an electron beam cured resin layer 20, a substrate 10 having a first surface and a second surface, an adhesive layer A, and a sealant layer 40 in this order in the thickness direction (hereinafter, also simply referred to as "arranged in this order"). The electron beam cured resin layer 20 is provided on the first surface of the substrate 10. The sealant layer 40 is provided on the second surface of the substrate 10 via the adhesive layer A. The adhesive layer A is provided as desired. The laminate 1 may further comprise a printed layer (not shown) on the second surface of the substrate 10.

[0016] 2 includes, in this order, an electron beam cured resin layer 20, a substrate 10 having a first surface and a second surface, an adhesive layer A1, a vapor-deposited film layer 30, an adhesive layer A2, and a sealant layer 40. The vapor-deposited film layer 30 includes a stretched polypropylene film 32 and a vapor-deposited film 34. The laminate 1 may further include a printed layer (not shown) on the second surface of the substrate 10.

[0017] <Base material> The base material contains polypropylene as a main component, that is, preferably in a range of more than 50 mass %. The polypropylene may be any of propylene homopolymer (homopolypropylene), propylene random copolymer (random polypropylene) such as propylene-α-olefin random copolymer, and propylene block copolymer (block polypropylene) such as propylene-α-olefin block copolymer, or a mixture of two or more selected from these. From the viewpoint of reducing the environmental load, the polypropylene may be biomass-derived polypropylene or mechanically or chemically recycled polypropylene.

[0018] In the present disclosure, polypropylene refers to a propylene homopolymer or a polymer in which the content of propylene-derived structural units in all repeating structural units is greater than the content of structural units derived from any comonomer. In this polymer, the content of propylene-derived structural units may be, for example, 50 mol% or more, 60 mol% or more, 70 mol% or more, or 80 mol% or more. The content is measured by NMR.

[0019] A propylene homopolymer is a polymer of propylene only. A propylene random copolymer is a random copolymer of propylene and an α-olefin other than propylene. A propylene block copolymer is a copolymer having a polymer block of propylene and a polymer block of an α-olefin other than propylene. Examples of α-olefins other than propylene include α-olefins having 2 to 20 carbon atoms, specifically ethylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, 1-eicosene, 3-methyl-1-butene, 4-methyl-1-pentene, and 6-methyl-1-heptene. Examples of propylene random copolymers include propylene-ethylene random copolymers. Examples of propylene block copolymers include propylene-ethylene block copolymers.

[0020] The polypropylene may be isotactic polypropylene, syndiotactic polypropylene, or atactic polypropylene. From the viewpoint of the heat resistance of the substrate, the polypropylene contained in the substrate is preferably isotactic polypropylene or syndiotactic polypropylene, and more preferably isotactic polypropylene.

[0021] Among polypropylenes, propylene random copolymers are preferred from the viewpoint of the transparency of the packaging material, propylene homopolymers are preferred when the rigidity and heat resistance of the packaging material are important, and propylene block copolymers are preferred when the impact resistance of the packaging material is important.

[0022] The density of polypropylene is, for example, 0.88 g / cm 3 More than 0.92g / cm 3 In the present disclosure, the density is measured in accordance with JIS K7112:1999 D method (density gradient tube method, 23°C). The melting point (Tm) of polypropylene is preferably 120°C or higher, more preferably 125°C or higher, and preferably 170°C or lower, more preferably 165°C or lower, for example, 120°C or higher and 170°C or lower, from the viewpoints of strength, heat resistance, and the like. In the present disclosure, Tm is the melting peak temperature obtained by differential scanning calorimetry (DSC) in accordance with JIS K7121:2012.

[0023] From the viewpoint of film-forming and processability, the melt flow rate (MFR) of polypropylene is preferably 0.1 g / 10 min or more, more preferably 0.2 g / 10 min or more, even more preferably 0.5 g / 10 min or more, and preferably 50 g / 10 min or less, more preferably 30 g / 10 min or less, even more preferably 10 g / 10 min or less, for example, 0.1 g / 10 min or more and 50 g / 10 min or less. The MFR of polypropylene is measured by the A method at a temperature of 230° C. and a load of 2.16 kg in accordance with JIS K7210-1:2014.

[0024] The polypropylene content in the base material is preferably more than 50% by mass, more preferably 60% by mass or more, even more preferably 70% by mass or more, still more preferably 80% by mass or more, particularly preferably 85% by mass or more or 90% by mass or more.

[0025] The substrate may contain a resin material other than polypropylene, such as polyolefin other than polypropylene, (meth)acrylic resin, vinyl resin, cellulose resin, polyamide, polyester, and ionomer resin.

[0026] The substrate may contain additives, such as crosslinkers, antioxidants, antiblocking agents, lubricants, UV absorbers, light stabilizers, fillers, reinforcing agents, antistatic agents, compatibilizers, pigments, and modifying resins.

[0027] The substrate may be surface-treated. This can improve the adhesion between the substrate and other layers, for example. Examples of surface treatment methods include physical treatments such as corona discharge treatment, ozone treatment, low-temperature plasma treatment using oxygen gas and / or nitrogen gas, and glow discharge treatment; and chemical treatments such as oxidation treatment using chemicals. An easy-adhesion layer may be provided on the surface of the substrate.

[0028] The substrate may be a substrate that has been subjected to a stretching treatment, i.e., a stretched substrate, or a substrate that has not been subjected to a stretching treatment, i.e., an unstretched substrate. An unstretched substrate means a substrate that has not been subjected to an intentional stretching treatment (a substrate whose molecules have not been oriented by stretching). Films that are inevitably stretched during extrusion molding or film winding are also included in the unstretched substrate.

[0029] The stretched substrate is excellent in, for example, strength, heat resistance, and transparency. The stretching process may be uniaxial stretching or biaxial stretching. The stretching ratio in the machine direction (flow direction of the substrate, MD direction) is preferably 2 times or more, more preferably 3 times or more, preferably 10 times or less, more preferably 7 times or less, for example, 2 times or more and 10 times or less. The stretching ratio in the width direction (direction perpendicular to the MD direction, TD direction) is preferably 2 times or more, more preferably 3 times or more, preferably 10 times or less, more preferably 7 times or less, for example, 2 times or more and 10 times or less. By setting the stretching ratio at 2 times or more, for example, the strength, heat resistance, and transparency of the substrate can be improved, and the printability of the substrate can be improved. From the viewpoint of the breaking limit of the substrate, the stretching ratio is preferably 10 times or less.

[0030] In one embodiment, the substrate is an unoriented polypropylene film, a uniaxially oriented polypropylene film, or a biaxially oriented polypropylene film.

[0031] The haze value of the substrate is preferably 25% or less, more preferably 20% or less, further preferably 15% or less, and particularly preferably 10% or less. The smaller the haze value of the substrate, the more preferable it is, but for example, the lower limit may be 0.1% or 1%. The haze value of the substrate is measured in accordance with JIS K7136:2000.

[0032] The thickness of the substrate is preferably 5 μm or more, more preferably 10 μm or more, and preferably 100 μm or less, more preferably 50 μm or less, for example, 5 μm or more and 50 μm or less. Substrates having a thickness equal to or greater than the lower limit are, for example, excellent in strength, heat resistance, and recyclability. Substrates having a thickness equal to or less than the upper limit are, for example, excellent in processability. In this specification, the thickness of the substrate and each layer is the average value of the thicknesses of 10 points measured based on a scanning electron microscope (SEM) image obtained by observing a cross section perpendicular to the surface of the laminate.

[0033] The substrate may have a single layer structure or a multi-layer structure. The substrate may have two or more polypropylene layers containing polypropylene as a main component. The number of polypropylene layers is preferably two or more, more preferably three or more, and preferably seven or less, more preferably five or less, for example, two or more and seven or less.

[0034] The substrate includes, for example, a first resin layer containing a propylene homopolymer as a main component, a second resin layer containing a propylene homopolymer as a main component, and a third resin layer containing a propylene homopolymer as a main component, in this order. Such a substrate has excellent heat resistance.

[0035] The substrate includes, for example, a first resin layer containing a propylene homopolymer as a main component, a second resin layer containing a propylene homopolymer as a main component, and a third resin layer containing a propylene random copolymer as a main component, in this order. Such a substrate has excellent printability on the second surface and excellent adhesion of the printed layer.

[0036] The substrate includes, in this order, a first resin layer containing a propylene homopolymer as a main component, a second resin layer containing a propylene homopolymer as a main component, and a third resin layer containing a mixture of a propylene homopolymer and a propylene random copolymer as a main component. Such a substrate has excellent heat resistance, and is excellent in printability and adhesion of a printed layer to the second surface. The content of the propylene random copolymer in the mixture may be, for example, 1% by mass or more, 5% by mass or more, 10% by mass or more, 15% by mass or more, 20% by mass or more, 25% by mass or more, 30% by mass or more, 99% by mass or less, 95% by mass or less, 90% by mass or less, 85% by mass or less, 80% by mass or less, 75% by mass or less, or 70% by mass or less, for example, 1% by mass or more and 99% by mass or less. The first resin layer constitutes a first surface of the substrate. The third resin layer constitutes the second surface of the substrate.

[0037] In one embodiment, the laminate of the present disclosure includes an electron beam cured resin layer on the first surface of the substrate having the above-mentioned multi-layer structure. Therefore, such a laminate has better heat resistance, and a large difference in heat resistance can be provided between one surface layer (electron beam cured resin layer) and the other surface layer (sealant layer) of the laminate, and deformation of the laminate during heat sealing can be effectively suppressed.

[0038] The substrate can be prepared, for example, by forming polypropylene or a resin composition thereof into a film by a T-die method, an inflation method or the like, and then stretching the film as desired.

[0039] The laminate of the present disclosure may have a deposition film, which will be described later, on the second surface of the substrate, or may have a deposition film and a barrier coat layer, which will be described later, on the second surface of the substrate. Thus, the laminate of the present disclosure may have an electron beam cured resin layer, a substrate, and a deposition film in this order as a part of the laminate configuration, or may have an electron beam cured resin layer, a substrate, a deposition film, and a barrier coat layer in this order. Details of the deposition film and the barrier coat layer are described below, and will not be described here.

[0040] <Electron beam cured resin layer> The electron beam cured resin layer is a layer formed by irradiating a layer containing an electron beam curable compound with an electron beam (EB) to cure the compound. The electron beam curable compound is a compound that cures when irradiated with an electron beam. The electron beam cured resin layer is a layer containing a cured product obtained by curing the electron beam curable compound by irradiation with an electron beam.

[0041] In one embodiment, the laminate of the present disclosure comprises an electron beam cured resin layer as one surface layer. The electron beam cured resin layer has a high melting temperature and is excellent in heat resistance. A substrate containing polypropylene as a main component does not have sufficient heat resistance, and for example, deformation such as warping and wrinkles may occur in the substrate during heat sealing treatment. By providing an electron beam cured resin layer on the first surface of the substrate, heat resistance can be improved. Therefore, a laminate having an electron beam cured resin layer as one surface layer and a sealant layer as the other surface layer has a larger difference in heat resistance (e.g., melting temperature) between the two surface layers than a laminate having a substrate as one surface layer and a sealant layer as the other surface layer. For example, the above-mentioned deformation during heat sealing treatment can be suppressed. As a result, for example, when the laminate of the present disclosure is used as a lid material, leakage of the contents can be suppressed well after the lid material is heat-sealed to a hard adherend such as a cup by heat sealing treatment. The laminate of the present disclosure can increase the heat sealing temperature in so-called mono-material packaging materials. Furthermore, the laminate of the present disclosure has suitability for filling and processing contents and resistance to heat sterilization, and can greatly contribute to the spread of environmentally friendly packaging materials.

[0042] The layer containing the electron beam curable compound can be formed, for example, by applying a coating agent containing the electron beam curable compound and, if desired, a solvent to the first surface of the substrate. In the case of the electron beam curable resin layer, unlike the curing of the ultraviolet curable compound that requires a photopolymerization initiator, no photopolymerization initiator is required when curing the electron beam curable compound. The photopolymerization initiator may affect food hygiene. The laminate of the present disclosure can avoid the problem of bleeding out of the photopolymerization initiator, and is therefore safer.

[0043] The electron beam curable compound is preferably a (meth)acrylate, for example, a polyfunctional (meth)acrylate having two or more (meth)acryloyl groups in the molecule, such as a polyfunctional (meth)acrylate monomer, a polyfunctional (meth)acrylate oligomer, and a polyfunctional (meth)acrylate prepolymer. The number of (meth)acryloyl groups in the polyfunctional (meth)acrylate is preferably 2 to 15, more preferably 2 to 8, and even more preferably 2 to 6, from the viewpoint of improving heat resistance and preventing shrinkage during curing.

[0044] The hardness of the electron beam cured resin layer can be adjusted by changing the amount ratio and type of the monomer, oligomer and prepolymer in the multifunctional (meth)acrylate. For example, the hardness of the electron beam cured resin layer tends to be reduced by using a large amount of oligomer and prepolymer. For example, the migration of low molecular weight components from the electron beam cured resin layer tends to be suppressed by reducing the amount of monomer used.

[0045] Examples of the polyfunctional (meth)acrylate oligomer and polyfunctional (meth)acrylate prepolymer include urethane (meth)acrylate, epoxy (meth)acrylate, polyester (meth)acrylate, polyether (meth)acrylate, acrylic (meth)acrylate, and polybutadiene (meth)acrylate. In the present disclosure, "(meth)acrylate" includes both "acrylate" and "methacrylate", and "(meth)acryloyl group" includes both "acryloyl group" and "methacryloyl group".

[0046] The urethane (meth)acrylate can be obtained, for example, by reacting an isocyanate group-containing urethane prepolymer obtained by reacting a polyol with a polyisocyanate under conditions of excess isocyanate groups, with a (meth)acrylate having a hydroxyl group. Alternatively, the urethane (meth)acrylate can be obtained by reacting a hydroxyl group-containing urethane prepolymer obtained by reacting a polyol with a polyisocyanate under conditions of excess hydroxyl groups, with a (meth)acrylate having an isocyanate group. Examples of the urethane (meth)acrylate include polyether-based urethane (meth)acrylate, polycarbonate-based urethane (meth)acrylate, polyester-based urethane (meth)acrylate, and caprolactone-based urethane (meth)acrylate.

[0047] Examples of the polyol include ethylene glycol, propylene glycol, diethylene glycol, dipropylene glycol, butylene glycol, 1,6-hexanediol, 3-methyl-1,5-pentane glycol, neopentyl glycol, hexanetriol, trimellitolpropane, polytetramethylene glycol, and a condensation polymer of adipic acid and ethylene glycol. Examples of the polyisocyanate include tolylene diisocyanate, isophorone diisocyanate, and hexamethylene diisocyanate.

[0048] Examples of (meth)acrylates having a hydroxyl group include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, pentaerythritol tri(meth)acrylate, and dipentaerythritol penta(meth)acrylate. Examples of (meth)acrylates having an isocyanate group include 2-(meth)acryloyloxyethyl isocyanate, and (meth)acryloyl isocyanate.

[0049] Epoxy (meth)acrylates are compounds in which the epoxy group of an epoxy resin is esterified with (meth)acrylic acid to make the functional group a (meth)acryloyl group. Examples of such compounds include a (meth)acrylic acid adduct to a bisphenol A type (or F type) epoxy resin, and a (meth)acrylic acid adduct to a novolac type epoxy resin.

[0050] Examples of the polyfunctional (meth)acrylate monomer include aliphatic monomers such as trimethylolpropane tri(meth)acrylate, ditrimethylolpropane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol tri(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate and dipentaerythritol hexa(meth)acrylate; monomers having an isocyanurate skeleton such as tris(2-(meth)acryloxyethyl)isocyanurate; and modified products thereof. Examples of the modified products include ethylene oxide (EO) modified products, propylene oxide (PO) modified products and caprolactone (CL) modified products. Specific examples of the modified products include EO-modified trimethylolpropane tri(meth)acrylate, PO-modified trimethylolpropane tri(meth)acrylate, EO-modified dipentaerythritol hexa(meth)acrylate, PO-modified dipentaerythritol hexa(meth)acrylate, CL-modified dipentaerythritol hexa(meth)acrylate, and CL-modified tris(2-(meth)acryloxyethyl)isocyanurate.

[0051] For the purpose of adjusting the viscosity of the coating agent, a monofunctional (meth)acrylate monomer such as methyl (meth)acrylate may be used as a diluent. In addition to the monofunctional (meth)acrylate monomer, a normal solvent may be used as the diluent. The coating agent may contain a solvent, for example, from the viewpoint of improving its applicability. Examples of the solvent include hydrocarbon solvents such as toluene, xylene, hexane, and octane; alcohol solvents such as ethanol, propanol, butanol, pentanol, hexanol, octanol, and decanol; ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, diisobutyl ketone, and cyclohexanone; ester solvents such as ethyl acetate, butyl acetate, amyl acetate, ethyl butyrate, butyl butyrate, butyl stearate, methyl benzoate, methyl lactate, ethyl lactate, and butyl lactate; and water. The solvent may be a mixture of two or more of these.

[0052] The electron beam cured resin layer is formed, for example, as follows. A coating agent is applied to a first surface of a substrate in a desired thickness, and if a solvent is used, the coating agent is dried to remove the solvent to form a coating film (uncured resin layer). The drying conditions are, for example, 40°C to 120°C for 10 seconds to 10 minutes. Next, the coating film is irradiated with an electron beam to cure the electron beam curable compound. The electron beam can be irradiated from either surface of the substrate as long as it can cure the electron beam curable compound. In this manner, an electron beam cured resin layer can be formed.

[0053] Methods for applying the coating agent to the first surface of the substrate include, for example, gravure printing, offset printing, flexographic printing, screen printing, spraying, spin coating, die coating, roll coating, reverse roll coating, comma coating, blade coating, and air knife coating.

[0054] The acceleration voltage of the electron beam can be appropriately selected according to the type of the electron beam curable compound and the thickness of the layer. The acceleration voltage of the electron beam is preferably 70 kV or more and 300 kV or less. The exposure dose of the electron beam is preferably 1 kGy or more and 300 kGy or less, more preferably 5 kGy or more and 200 kGy or less, and even more preferably 10 kGy or more and 100 kGy or less. As the electron beam source, for example, various electron beam accelerators such as Cockroft-Walton type, Van de Graff type, resonant transformer type, insulating core transformer type, linear type, dynamitron type, and high frequency type can be used.

[0055] The content of the cured product of the electron beam curable compound in the electron beam cured resin layer is preferably more than 50% by mass, more preferably 60% by mass or more, even more preferably 70% by mass or more, even more preferably 80% by mass or more, and particularly preferably 90% by mass or more. A laminate having such an electron beam cured resin layer is, for example, excellent in heat resistance. The electron beam cured resin layer contains, for example, a cured product of (meth)acrylate.

[0056] The electron beam cured resin layer may contain the above-mentioned additives.

[0057] The thickness of the electron beam cured resin layer is preferably 0.1 μm or more, more preferably 0.3 μm or more, even more preferably 0.5 μm or more, still more preferably 0.7 μm or more, particularly preferably 1 μm or more, and is preferably 10 μm or less, more preferably 7 μm or less, even more preferably 5 μm or less, still more preferably 3 μm or less, particularly preferably 2 μm or less, for example, 0.1 μm or more and 10 μm or less. A laminate having such an electron beam cured resin layer has, for example, excellent heat resistance.

[0058] <Deposition film layer> The laminate of the present disclosure may further include a deposition film layer between the above-mentioned substrate and the sealant layer. The deposition film layer includes a stretched polypropylene film and a deposition film provided on one side of the stretched polypropylene film. The laminate including the deposition film layer has, for example, excellent gas barrier properties, specifically, excellent oxygen barrier properties and water vapor barrier properties. In addition, the laminate including the deposition film, which is a metal deposition film, has, for example, excellent brightness.

[0059] The vapor-deposited film layer is preferably arranged so that the vapor-deposited film faces the substrate and the stretched polypropylene film faces the sealant layer, thereby making it possible to suppress the effect of heat on the vapor-deposited film during heat sealing treatment and to suppress the effect of the contents on the vapor-deposited film.

[0060] (oriented polypropylene film) The stretched polypropylene film contains polypropylene as the main component, i.e., preferably in the range of more than 50% by mass. The polypropylene may be any of propylene homopolymer, propylene random copolymer, and propylene block copolymer, and may be a mixture of two or more selected from these. From the viewpoint of reducing the environmental load, the polypropylene may be biomass-derived polypropylene or mechanically recycled or chemically recycled polypropylene. The details of polypropylene are as described above, and will not be described here.

[0061] The content of polypropylene in the stretched polypropylene film is preferably more than 50% by mass, more preferably 60% by mass or more, even more preferably 70% by mass or more, still more preferably 80% by mass or more, particularly preferably 85% by mass or more or 90% by mass or more. A laminate including such a stretched polypropylene film has, for example, excellent recyclability.

[0062] The stretched polypropylene film may contain the above-mentioned resin materials other than polypropylene. The stretched polypropylene film may contain the above-mentioned additives.

[0063] The stretched polypropylene film may be subjected to the above-mentioned surface treatment. An easy-adhesion layer may be provided on the surface of the stretched polypropylene film.

[0064] The stretched polypropylene film is a polypropylene film that has been subjected to a stretching process. The stretching process may be uniaxial stretching or biaxial stretching. The details of the stretching process are as described above, and will not be described in this section. In one embodiment, the stretched polypropylene film is a uniaxially stretched polypropylene film or a biaxially stretched polypropylene film.

[0065] The haze value of the stretched polypropylene film is preferably 25% or less, more preferably 20% or less, further preferably 15% or less, and particularly preferably 10% or less. The smaller the haze value of the stretched polypropylene film, the more preferable it is, but for example, the lower limit may be 0.1% or 1%.

[0066] The stretched polypropylene film may have a single layer structure or a multilayer structure. The stretched polypropylene film may have two or more polypropylene layers containing polypropylene as a main component. The number of polypropylene layers is preferably two or more, more preferably three or more, and preferably seven or less, more preferably five or less, for example, two or more and seven or less.

[0067] The thickness of the stretched polypropylene film is preferably 5 μm or more, more preferably 10 μm or more, and preferably 100 μm or less, more preferably 50 μm or less, for example, 5 μm or more and 100 μm or less. Films having a thickness equal to or greater than the lower limit are excellent in, for example, strength, heat resistance, and recyclability. Films having a thickness equal to or less than the upper limit are excellent in, for example, processability.

[0068] The stretched polypropylene film can be produced, for example, by forming polypropylene or a resin composition thereof into a film by a T-die method, an inflation method or the like, and then stretching the film.

[0069] (evaporated film) Examples of the vapor deposition film include a vapor deposition film containing one or more metals, a vapor deposition film containing one or more inorganic oxides, and a vapor deposition film containing one or more metals and one or more inorganic oxides. Examples of metals include aluminum, chromium, tin, nickel, copper, silver, gold, and platinum. Examples of inorganic oxides include aluminum oxide, silicon oxide, magnesium oxide, calcium oxide, zirconium oxide, titanium oxide, boron oxide, hafnium oxide, barium oxide, and silicon carbide oxide (carbon-containing silicon oxide). Among these, aluminum vapor deposition film, aluminum oxide (alumina) vapor deposition film, silicon oxide (silica) vapor deposition film, and silicon carbide vapor deposition film are preferred.

[0070] The thickness of the vapor-deposited film is preferably 1 nm or more, more preferably 5 nm or more, even more preferably 10 nm or more, and is preferably 150 nm or less, more preferably 100 nm or less, even more preferably 80 nm or less, for example, 1 nm or more and 150 nm or less. A laminate having a vapor-deposited film with a thickness equal to or greater than the lower limit has, for example, excellent gas barrier properties. A laminate having a vapor-deposited film with a thickness equal to or less than the upper limit can, for example, suppress the occurrence of cracks in the vapor-deposited film and has excellent recyclability.

[0071] When the vapor-deposited film is an aluminum vapor-deposited film, the optical density (OD value) of the aluminum vapor-deposited film is preferably 2.0 or more and 3.5 or less. A laminate having such a vapor-deposited film has, for example, excellent gas barrier properties while maintaining productivity. The OD value is measured in accordance with JIS K7361-1:1997.

[0072] The vapor-deposited film may be subjected to the above-mentioned surface treatment.

[0073] Examples of methods for forming the vapor-deposited film include physical vapor deposition (PVD) methods such as vacuum deposition, sputtering, and ion plating, and chemical vapor deposition (CVD) methods such as plasma chemical vapor deposition, thermal chemical vapor deposition, and photochemical vapor deposition. The vapor-deposited film may be a composite film containing two or more layers of different vapor-deposited films formed by combining both physical vapor deposition and chemical vapor deposition. The vapor-deposited film may be a single layer formed by one vapor deposition process, or a multilayer formed by multiple vapor deposition processes. When the vapor-deposited film is multilayered, each layer may be composed of the same component or different components. Each layer may be formed by the same method or different methods.

[0074] (Barrier coat layer) The vapor-deposited film layer may further include a barrier coat layer on the vapor-deposited film. That is, the vapor-deposited film layer may include a stretched polypropylene film, a vapor-deposited film, and a barrier coat layer in this order. Such a vapor-deposited film layer has, for example, excellent gas barrier properties, and can effectively suppress the occurrence of cracks in the vapor-deposited film, for example, when the vapor-deposited film contains an inorganic oxide such as aluminum oxide or silicon oxide.

[0075] In one embodiment, the barrier coat layer contains a gas barrier resin, such as an ethylene-vinyl alcohol copolymer, polyvinyl alcohol, polyacrylonitrile, polyester, polyamide such as nylon 6, nylon 6,6, and polymetaxylylene adipamide, polyurethane, or (meth)acrylic resin.

[0076] The content of the gas barrier resin in the barrier coat layer is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more. A laminate including such a barrier coat layer has, for example, excellent gas barrier properties. The barrier coat layer may contain the above-mentioned additives.

[0077] The thickness of the barrier coat layer containing the gas barrier resin is preferably 0.01 μm or more, more preferably 0.1 μm or more, and preferably 10 μm or less, more preferably 5 μm or less, for example, 0.01 μm or more and 10 μm or less. A laminate having a barrier coat layer whose thickness is equal to or greater than the lower limit has, for example, excellent gas barrier properties. A laminate having a barrier coat layer whose thickness is equal to or less than the upper limit has, for example, excellent processability and recyclability.

[0078] The barrier coat layer can be formed, for example, by applying a coating liquid obtained by dissolving or dispersing a material such as a gas barrier resin in water or an appropriate organic solvent onto the surface of the vapor-deposited film and drying it.

[0079] In another embodiment, the barrier coat layer is a gas barrier coating film formed by mixing a metal alkoxide, a water-soluble polymer, and optionally a silane coupling agent, and adding water, an organic solvent, and a sol-gel catalyst as required to obtain a gas barrier composition, which is then applied to the surface of the deposition film and dried. The gas barrier coating film contains a hydrolysis polycondensate obtained by hydrolyzing and polycondensing the above-mentioned metal alkoxide by the sol-gel method. A laminate having such a barrier coat layer on a deposition film can effectively suppress the occurrence of cracks in the deposition film, for example, when the deposition film contains an inorganic oxide.

[0080] Examples of metal alkoxides include alkoxysilanes such as tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, and tetrabutoxysilane. Examples of water-soluble polymers include hydroxyl-containing polymers such as polyvinyl alcohol and ethylene-vinyl alcohol copolymers. Examples of organic solvents include methyl alcohol, ethyl alcohol, n-propyl alcohol, isopropyl alcohol, and n-butyl alcohol. Examples of sol-gel catalysts include acids or amine-based compounds.

[0081] The thickness of the gas barrier coating film is preferably 0.01 μm or more, more preferably 0.1 μm or more, and preferably 10 μm or less, more preferably 5 μm or less, and even more preferably 3 μm or less, for example, 0.01 μm or more and 10 μm or less. A laminate including such a gas barrier coating film has, for example, excellent gas barrier properties, can suppress the occurrence of cracks in a vapor deposition film containing an inorganic oxide, and is also excellent in recyclability and processability.

[0082] <Print layer> The laminate of the present disclosure may have a printed layer on the surface of the substrate and the vapor deposition film layer. Examples of images formed in the printed layer include characters, patterns, symbols, and combinations thereof. The printed layer may be formed using, for example, ink derived from biomass. This can, for example, further reduce the environmental load.

[0083] Examples of methods for forming the printed layer include conventionally known printing methods such as gravure printing, offset printing, and flexographic printing. Among these, flexographic printing is preferred from the viewpoint of reducing the environmental load.

[0084] The printed layer may be formed on either side of the substrate. The printed layer is preferably formed on the surface of the substrate facing the sealant layer, since this can prevent the printed layer from coming into contact with the outside air and can prevent the printed layer from deteriorating over time. The printed layer may be formed on either side of the vapor-deposited film layer.

[0085] <Adhesive layer> The laminate of the present disclosure may include an adhesive layer between any layers, such as between the substrate and the sealant layer, between the substrate and the vapor-deposited film layer, between the vapor-deposited film layer and the sealant layer, etc. Such a laminate has, for example, excellent adhesion between layers.

[0086] The adhesive layer is, for example, made of an adhesive, and the adhesive may be any of a one-component curing adhesive, a two-component curing adhesive, and a non-curing adhesive. The adhesive may be a solventless adhesive or a solvent-based adhesive. Examples of the adhesive include polyether adhesives, polyester adhesives, polyurethane adhesives, silicone adhesives, epoxy adhesives, rubber adhesives, vinyl adhesives, olefin adhesives, and phenol adhesives. Among these, polyurethane adhesives are preferred, and two-component curing polyurethane adhesives are more preferred.

[0087] The thickness of the adhesive layer is preferably 0.1 μm or more, more preferably 0.2 μm or more, even more preferably 0.5 μm or more, particularly preferably 0.8 μm or more, and is preferably 10 μm or less, more preferably 8 μm or less, even more preferably 6 μm or less, particularly preferably 5 μm or less, for example, 0.1 μm or more and 10 μm or less.

[0088] The adhesive layer can be formed by applying an adhesive to the surface of the object by a conventionally known method such as a direct gravure roll coating method, a gravure roll coating method, a kiss coating method, a reverse roll coating method, a Fontaine method, or a transfer roll coating method, and drying it as desired. The laminate of the present disclosure may be produced by, for example, laminating a substrate and a sealant film, or a substrate, a vapor deposition film, and a sealant film, by a non-solvent lamination method using a solvent-free adhesive, or by a dry lamination method using a solvent-based adhesive. The vapor deposition film corresponds to the vapor deposition film layer. The sealant film corresponds to the sealant layer.

[0089] <Sealant layer> The sealant layer contains polypropylene as a main component, i.e., preferably in a range of more than 50 mass %. The polypropylene may be any of propylene homopolymer, propylene random copolymer, and propylene block copolymer, and may be a mixture of two or more selected from these. From the viewpoint of reducing the environmental load, the polypropylene may be biomass-derived polypropylene or mechanically recycled or chemically recycled polypropylene. The details of polypropylene are as described above, and the explanation will be omitted in this section.

[0090] The content of polypropylene in the sealant layer is preferably more than 50% by mass, more preferably 60% by mass or more, even more preferably 70% by mass or more, still more preferably 80% by mass or more, particularly preferably 85% by mass or more or 90% by mass or more. A laminate having such a sealant layer has, for example, excellent recyclability.

[0091] The sealant layer may contain the above-mentioned resin materials other than polypropylene. The sealant layer may contain the above-mentioned additives.

[0092] From the viewpoint of heat sealability, the sealant layer is preferably an unstretched resin film, more preferably an unstretched coextruded resin film, and each layer constituting the sealant layer is a coextruded resin layer. The above resin film can be produced, for example, by using a T-die method or an inflation method.

[0093] The sealant layer may have a single-layer structure or a multi-layer structure. The sealant layer may have two or more polypropylene layers containing polypropylene as a main component. The number of polypropylene layers is preferably two or more, more preferably three or more, and preferably seven or less, more preferably five or less, for example, two or more and seven or less.

[0094] The thickness of the sealant layer is preferably 5 μm or more, more preferably 10 μm or more, even more preferably 20 μm or more, still more preferably 30 μm or more, and is preferably 200 μm or less, more preferably 150 μm or less, even more preferably 100 μm or less, still more preferably 80 μm or less, for example, 5 μm or more and 200 μm or less. When the sealant layer has a multi-layer structure, it is preferable that the total thickness is in the above range.

[0095] The sealant layer may contain a heat seal modifier from the viewpoint of improving low-temperature heat sealability. The heat seal modifier is not particularly limited as long as it is a component that has excellent compatibility with the polypropylene that constitutes the sealant layer, and examples of the heat seal modifier include olefin-based polymers with low melting points, specifically olefin-based copolymers. Ultra-low density polyethylene may also be used.

[0096] The olefin copolymer is not particularly limited as long as it is compatible with polypropylene and has a low melting point, and examples thereof include olefin elastomers and olefin plastomers.

[0097] Examples of the olefin-based elastomer include polyethylene-based elastomers such as ethylene-α-olefin copolymers, and polypropylene-based elastomers such as propylene-α-olefin copolymers. Examples of the α-olefins include α-olefins having 2 to 8 carbon atoms, such as ethylene, propylene, 1-butene, 1-hexene, 1-octene, and 4-methyl-1-pentene.

[0098] From the viewpoint of improving heat sealability, the melting point (Tm) of the polypropylene-based elastomer is preferably 140° C. or less, more preferably 135° C. or less. The lower limit of Tm is not particularly limited, but is, for example, 70° C., 80° C., or 90° C.

[0099] A plastomer is a polymer that does not exhibit elastic deformation like an elastomer, but easily undergoes plastic deformation, in contrast to an elastomer (a polymer that deforms in response to the application of an external force and returns to its original shape in a short time when the external force is removed).

[0100] Examples of olefin-based plastomers include polyethylene-based plastomers. Polyethylene-based plastomers are polyethylenes obtained by copolymerizing ethylene and α-olefins using a single-site catalyst such as a metallocene catalyst. Examples of α-olefins are preferably α-olefins having 4 to 8 carbon atoms, such as 1-butene, 1-hexene, 1-octene, and 4-methyl-1-pentene. Specific examples of polyethylene-based plastomers include ethylene-1-butene copolymers, ethylene-1-hexene copolymers, and ethylene-1-octene copolymers.

[0101] From the viewpoint of improving heat sealability, the melting point (Tm) of the polyethylene plastomer is preferably 115° C. or less, more preferably 110° C. or less, and even more preferably 105° C. or less. The lower limit of Tm is not particularly limited, and is, for example, 50° C., 60° C., or 70° C.

[0102] The density of the olefin copolymer is preferably 0.850 g / cm 3 More preferably, 0.860 g / cm 3 More preferably, 0.870 g / cm 3 or more, preferably 0.920 g / cm 3 Less than or equal to 0.915 g / cm 3 or less, more preferably 0.910 g / cm 3 For example, 0.850 g / cm 3 More than 0.920g / cm 3 The following is the result.

[0103] From the viewpoint of film-forming property and processability, the MFR of the olefin copolymer is preferably 0.2 g / 10 min or more, more preferably 0.3 g / 10 min or more, even more preferably 0.5 g / 10 min or more, and preferably 20 g / 10 min or less, more preferably 15 g / 10 min or less, even more preferably 10 g / 10 min or less, particularly preferably 5 g / 10 min or less, for example, 0.2 g / 10 min or more and 20 g / 10 min or less. The MFR of the olefin copolymer is measured by the A method at a temperature of 190 ° C. and a load of 2.16 kg in accordance with JIS K7210-1:2014.

[0104] The content of the heat seal modifier in the entire sealant layer is preferably 1% by mass or more, more preferably 2% by mass or more, even more preferably 3% by mass or more, and is preferably 30% by mass or less, more preferably 20% by mass or less, even more preferably 15% by mass or less, for example, 1% by mass or more and 30% by mass or less. Such a sealant layer has, for example, excellent heat sealability.

[0105] The sealant layer may have a single-layer structure or a multi-layer structure. In one embodiment, the surface layer of the sealant layer having a multi-layer structure opposite to the substrate contains polypropylene and a heat seal modifier. The content of the heat seal modifier in the surface layer is preferably 10% by mass or more, more preferably 20% by mass or more, preferably 55% by mass or less, more preferably less than 50% by mass, for example 10% by mass or more and 55% by mass or less. The content of polyolefin in the surface layer is preferably 45% by mass or more, more preferably more than 50% by mass, preferably 90% by mass or less, more preferably 80% by mass or less, for example 45% by mass or more and 90% by mass or less. The sealant layer having such a surface layer has, for example, excellent heat sealability and recyclability.

[0106] The thickness of the surface layer is preferably 1 μm or more, more preferably 2 μm or more, and is preferably 20 μm or less, more preferably 15 μm or less, and even more preferably 10 μm or less, for example, 1 μm or more and 20 μm or less. A sealant layer having such a surface layer has, for example, excellent heat sealability and recyclability.

[0107] In one embodiment, the sealant layer may have easy peel properties. A laminate having a sealant layer with easy peel properties is suitable, for example, as a lid material constituting a packaging container. Easy peel properties refer to, for example, the ease of peeling the lid material from the container body after the lid material is heat-sealed and fused to the container body. Mechanisms that impart easy peel properties include, for example, an interface peeling mechanism, an interlayer peeling mechanism, and a cohesive peeling mechanism, and any of these mechanisms can be adopted. Among these, the cohesive peeling mechanism is preferred from the viewpoint of enabling thermal sterilization treatments such as retort treatment and boiling treatment when used as a lid material. Specifically, the easy peel property can be imparted by forming a sealant layer from a mixture of polypropylene and a resin that is incompatible or partially incompatible with polypropylene.

[0108] As the polypropylene, from the viewpoint of suitability for retort treatment and boiling treatment, a block copolymer having a propylene block and an ethylene block or a propylene-ethylene random copolymer is preferred, and from the viewpoint of easy peelability, a propylene-ethylene random copolymer is preferred.

[0109] Examples of resins that are incompatible or partially incompatible with polypropylene (hereinafter also referred to as "incompatible resins") include polyethylene, polybutene, and polystyrene. Among these, polyethylene is preferred, and high-density polyethylene is more preferred. By forming the sealant layer from a mixture of polypropylene and an incompatible resin, a sea-island structure can be developed in the sealant layer, thereby imparting easy peelability. In one embodiment, the sea-island structure includes a sea portion made of polypropylene and an island portion made of an incompatible resin.

[0110] The sea-island structure can be realized, for example, by adjusting the ratio of the amounts of polypropylene and the incompatible resin. The sea-island structure can be well realized if the amount of polypropylene is preferably 40 parts by mass or more and 90 parts by mass or less, more preferably 60 parts by mass or more and 80 parts by mass or less, and the amount of the incompatible resin is preferably 10 parts by mass or more and 60 parts by mass or less, more preferably 20 parts by mass or more and 40 parts by mass or less, relative to 100 parts by mass of the total of the polypropylene and the incompatible resin. From the viewpoints of recyclability, and furthermore suitability for retort treatment and boiling treatment, a higher proportion of polypropylene is preferable.

[0111] The sealant layer may have a single layer structure or a multi-layer structure. For example, in the case of a lid material made of a laminate, the easy peel property may be imparted only to the layer in the sealant layer having a multi-layer structure that contacts the container body. The sealant layer may include a layer having easy peel property and another layer containing polypropylene as a main component. The layer having easy peel property is called layer A, and the other layer is called layer B.

[0112] Layer A contains polypropylene as a main component, and further contains an incompatible resin. When Layer A contains such an incompatible resin, the retort processability and boil processability of the laminate can be improved. The content ratio of polypropylene in Layer A is preferably more than 50% by mass, more preferably 60% by mass or more, and preferably 90% by mass or less, more preferably 80% by mass or less, for example, more than 50% by mass and 90% by mass or less. This can further improve the retort processability and boil processability of the laminate. The content ratio of the incompatible resin in Layer A is preferably 10% by mass or more, more preferably 20% by mass or more, preferably less than 50% by mass, more preferably 40% by mass or less, for example, 10% by mass or more and less than 50% by mass. This can obtain an appropriate easy peel property.

[0113] The MFR of the polypropylene which is the main component of Layer A is preferably 5 g / 10 min or more and 30 g / 10 min or less. From the viewpoint of obtaining an appropriate seal strength, the polypropylene which is the main component of Layer A is preferably a propylene-ethylene random copolymer. The MFR of the incompatible resin is preferably 0.1 g / 10 min or more, more preferably 0.5 g / 10 min or more, and preferably 4 g / 10 min or less, more preferably 3 g / 10 min or less, for example, 0.1 g / 10 min or more and 4 g / 10 min or less. The incompatible resin is preferably a resin having a density of 0.940 g / cm 3 Polyethylene having a density of 0.940 g / cm or more is preferred. 3 More than 0.965g / cm 3 The following polyethylene is more preferred. The MFR of polyethylene is measured by Method A under conditions of a temperature of 190° C. and a load of 2.16 kg in accordance with JIS K7210-1:2014.

[0114] The polypropylene content in Layer B is preferably more than 50% by mass, more preferably 60% by mass or more, even more preferably 70% by mass or more, still more preferably 80% by mass or more, particularly preferably 85% by mass or more or 90% by mass or more.

[0115] The thickness of layer A is preferably 3 μm or more, more preferably 4 μm or more, even more preferably 5 μm or more, and preferably 30 μm or less, more preferably 20 μm or less, even more preferably 10 μm or less, for example, 3 μm or more and 30 μm or less. The thickness of layer A relative to the thickness of the entire sealant layer (thickness of layer A / thickness of sealant layer) is preferably 1 / 11 or more, more preferably 1 / 6 or more, and preferably 1 / 2 or less, more preferably 1 / 3 or less, for example, 1 / 11 or more and 1 / 2 or less.

[0116] <Layer structure of laminate> Specific examples of the layer structure of the laminate of the present disclosure are shown below. (1) A laminate having, in this order, an electron beam cured resin layer, a substrate, and optionally a printed layer, an adhesive layer, and a sealant layer. (2) A laminate comprising, in this order, an electron beam cured resin layer, a substrate, a vapor deposition film, and optionally a printed layer, an adhesive layer, and a sealant layer. (3) A laminate comprising, in this order, an electron beam cured resin layer, a substrate, a vapor deposition film, a barrier coat layer, and optionally a printed layer, an adhesive layer, and a sealant layer. (4) A laminate comprising, in this order, an electron beam cured resin layer, a substrate, and optionally a printed layer, an adhesive layer, a vapor deposition film layer, an adhesive layer, and a sealant layer. (5) A laminate comprising, in this order, an electron beam cured resin layer, a substrate, a vapor deposition film, and optionally a printed layer, an adhesive layer, a vapor deposition film layer, an adhesive layer, and a sealant layer. (6) A laminate comprising, in this order, an electron beam cured resin layer, a substrate, a vapor deposition film, a barrier coat layer, and optionally a printed layer, an adhesive layer, a vapor deposition film layer, an adhesive layer, and a sealant layer.

[0117] In the laminates (1) to (6) above, the substrate is, for example, a biaxially oriented polypropylene film, and the deposited film layer comprises a biaxially oriented polypropylene film and a deposited film. In the laminates (1) to (6) above, the sealant layer comprises, for example, a layer having easy peel properties.

[0118] The polypropylene content in the entire laminate of the present disclosure is preferably 80% by mass or more, more preferably 85% by mass or more, even more preferably 88% by mass or more, and particularly preferably 90% by mass or more. For example, such a laminate can be used to produce a mono-material packaging bag or lid material, and the recyclability of these can be improved. The upper limit of the polypropylene content is not particularly limited, but may be, for example, 99% by mass.

[0119] [Packaging materials] The laminate of the present disclosure can be suitably used as a packaging material. The packaging material can be used, for example, to prepare a packaging bag or as a lid material. The packaging container includes a container body having a storage section and a lid material joined (heat sealed) to the container body so as to seal the storage section. As described above, these packaging bags and lid materials are also excellent in retort treatment suitability and boiling treatment suitability.

[0120] The packaging bag and the packaging container have a heat-sealed portion. Examples of the heat-sealing method include bar sealing, rotary roll sealing, belt sealing, impulse sealing, high frequency sealing, and ultrasonic sealing.

[0121] Examples of packaging bags include packaging bags of various shapes such as standing pouch type, side seal type, two-sided seal type, three-sided seal type, four-sided seal type, envelope seal type, hem seal type (pillow seal type), pleated seal type, flat bottom seal type, square bottom seal type, and gusset type. Specific examples of packaging bags include small bags and standing pouches. The packaging bag may have an easy-to-open part. Examples of the easy-to-open part include a notch part that serves as a starting point for tearing the packaging bag, and a half-cut line formed by laser processing or a cutter as a path for tearing the packaging bag. After the contents are placed in the packaging bag, the opening of the packaging bag is heat-sealed to seal the packaging bag.

[0122] The contents contained in the packaging bag or packaging container include, for example, liquids, solids, powders, and gels. The contents may be food or beverages, or non-food or beverages such as chemicals, cosmetics, medicines, metal parts, and electronic parts. Specific examples of the contents include sauces, soy sauce, dressings, ketchup, syrups, cooking alcohol, edible oils, mayonnaise, and other liquid or viscous seasonings; liquid soups, powdered soups, fruit juices; spices; liquid beverages, jelly-like beverages, instant foods, other food and beverages; shampoos, rinses, conditioners, hand soaps, body soaps, air fresheners, deodorants, insect repellents, detergents; creams; metal parts, and electronic parts.

[0123] In one embodiment, a packaging bag can be produced by folding the laminate of the present disclosure in half and stacking them so that the base material is on the outside and the sealant layer is on the inside, and then heat-sealing the ends, etc. In another embodiment, a packaging bag can be produced by stacking multiple laminates of the present disclosure so that the sealant layers face each other, and then heat-sealing the ends, etc. The entire packaging bag may be made of the above-mentioned laminate, or only a part of the packaging bag may be made of the above-mentioned laminate.

[0124] In one embodiment, the laminate of the present disclosure is used as a lid material in a packaging container. The packaging container includes a container body having a storage section, and a lid material joined to the container body so as to seal the storage section. The lid material is made of the laminate of the present disclosure. A sealant layer of the lid material is joined to, for example, a flange portion of the container body. Examples of the shape of the container body include a cup shape and a bottomed cylindrical shape. As described above, the lid material has excellent retort processing suitability and boiling processing suitability.

[0125] The container body is made of, for example, polypropylene, polyethylene, polystyrene, polyethylene terephthalate or paper, and is preferably made of polypropylene from the viewpoint of improving the recyclability of the container body together with the lid material.

[0126] 3 and 4 show a packaging container 62 including a lid 60 and a container body 61. The container body 61 includes a body portion 63 and a flange portion 64. In one embodiment, the body portion 63 has a bottomed cylindrical shape with a circular opening 65 on the upper surface, and contents 66 are accommodated in a space defined by the body portion 63. The flange portion 64 is formed as a substantially flat surface extending from the outer periphery of the opening 65 in the outer periphery direction. The laminate constituting the lid 60 is stacked so that the sealant layer contacts the flange portion 64 of the container body 61, and is in close contact with at least a part of the flange portion 64 to form a seal portion. As a result, the opening 65 is sealed by the lid 60. In one embodiment, the lid 60 may have a gripping portion 67 protruding from the flange portion 64 to the outer periphery.

[0127] In one embodiment, the standing pouch includes a body (side sheet) and a bottom (bottom sheet). The side sheet and the bottom sheet may be made of the same material or different materials. The bottom sheet retains the shape of the side sheet, which gives the pouch self-supporting properties and allows it to be a standing pouch. A storage space for storing contents is formed within the area surrounded by the side sheet and the bottom sheet. In the standing pouch, only the body may be made of the laminate of the present disclosure, only the bottom may be made of the laminate of the present disclosure, or both the body and the bottom may be made of the laminate of the present disclosure.

[0128] In one embodiment, the side sheet can be formed by making a bag so that the sealant layer of the laminate of the present disclosure is the innermost layer. In one embodiment, the side sheet can be formed by preparing two sheets of the laminate of the present disclosure, overlapping them so that the sealant layers face each other, and heat-sealing the side edges on both sides to make a bag.

[0129] In another embodiment, the side sheet can be formed by preparing two laminates of the present disclosure, overlapping them with the sealant layers facing each other, inserting two laminates folded in a V-shape with the sealant layers facing outward between the laminates at the side edges on both sides of the overlapped laminates, and heat sealing them. According to this production method, a standing pouch having a body with side gussets can be obtained.

[0130] In one embodiment, the bottom sheet can be formed by inserting the laminate of the present disclosure between the lower parts of the side sheets that have been made into a bag, and heat sealing the laminate. More specifically, the bottom sheet can be formed by inserting the laminate folded in a V-shape with the sealant layer facing outward between the lower parts of the side sheets that have been made into a bag, and heat sealing the laminate.

[0131] In one embodiment, two sheets of the laminate are prepared, and these are stacked so that the sealant layers face each other, and then another sheet of the laminate is folded in a V shape so that the sealant layer faces outward, and this is sandwiched under the laminate that faces each other, and heat-sealed to form a bottom. Next, two sides adjacent to the bottom are heat-sealed to form a body. In this way, a standing pouch of one embodiment can be formed.

[0132] The present disclosure relates to, for example, the following [1] to

[12] . [1] A laminate comprising a substrate having a first surface and a second surface, an electron beam cured resin layer provided on the first surface of the substrate, and a sealant layer provided on the second surface of the substrate, wherein the substrate contains polypropylene as a main component, and the sealant layer contains polypropylene as a main component. [2] The laminate according to [1] above, wherein the thickness of the electron beam cured resin layer is 0.1 μm or more and 10 μm or less. [3] The laminate according to [1] or [2] above, wherein the electron beam cured resin layer contains a cured product of a (meth)acrylate. [4] The laminate according to any one of the above [1] to [3], wherein the substrate is a biaxially oriented polypropylene film. [5] The laminate according to any one of [1] to [4], further comprising a vapor-deposited film layer between the substrate and the sealant layer, the vapor-deposited film layer comprising a stretched polypropylene film and a vapor-deposited film provided on one surface of the stretched polypropylene film. [6] The laminate according to any one of [1] to [5], wherein the content of polypropylene in the entire laminate is 80 mass % or more. [7] The laminate according to any one of the above [1] to [6], which is a packaging material. [8] The laminate according to any one of the above [1] to [7], which is a lid material. [9] The laminate according to [8], wherein the sealant layer has easy peel properties.

[10] A packaging bag comprising the laminate described in any one of [1] to [7] above.

[11] The packaging bag according to

[10] above, which is a packaging bag that has been boiled or retorted.

[12] A packaging container comprising a polypropylene container body having a storage section, and a lid material made of the laminate described in any one of [1] to [9] above. EXAMPLES

[0133] Hereinafter, the laminate of the present disclosure will be specifically described based on examples, but the laminate of the present disclosure is not limited to the examples. Hereinafter, "parts by mass" may also be simply referred to as "parts".

[0134] The materials used in the following examples will be described. Coating agent: Elex-one (registered trademark) Gloss Varnish (manufactured by Toyo Ink) Coating agent containing an electron beam curable compound ·Base material: OPP-PFR double-treated product (Argha Karya, 18μm thick, biaxially oriented polypropylene film with three layers: propylene homopolymer layer, propylene homopolymer layer and propylene homopolymer layer, both sides corona-treated OPP with 38dyne or higher) Metallized film: IB-OPP (manufactured by Dai Nippon Printing Co., Ltd.; a vapor deposition film comprising a 20 μm-thick biaxially oriented polypropylene film and a silica vapor deposition film and a barrier coat layer provided on the film) Easy-peel sealant film: Polypropylene film (easy-peel sealant film with a cohesive peeling mechanism (island-sea structure made of a mixture of polypropylene and polyethylene), thickness 50 μm) ·glue: Solvent-based adhesive (Rock Paint, RU76 Glymo Free)

[0135] [Example 1] A coating agent (Elex-one (registered trademark) Gloss Varnish) was applied to the first surface of a biaxially oriented polypropylene film (OPP-PFR double-treated product) to form a coating layer with a thickness of 1.5 μm. Using an electron beam irradiation device (manufactured by Iwasaki Electric Co., Ltd. ESI), the coating layer was irradiated with electron beams under conditions of an acceleration voltage of 110 kV and an exposure dose of 30 kGy to form an electron beam cured resin layer.

[0136] A biaxially oriented polypropylene film with an electron beam cured resin layer formed on the first side was coated with an adhesive (RU76) at a coat weight of 3 g / m under dry lamination conditions on the second side. 2 The adhesive (RU76) was applied to the biaxially oriented polypropylene film side of the vapor deposition film under dry lamination conditions at a coating amount of 3 g / m. 2 The adhesive was applied so as to form a sealant layer, and the adhesive was then laminated to an easy-peel sealant film which would serve as a sealant layer. In this manner, a covering film was produced.

[0137] A polypropylene cup container with a flange (outer diameter: 80 mm, inner diameter: 70 mm, flange width: 5 mm) was prepared. The lid material film was cut to a size of 100 mm x 100 mm. The cut-out lid material film was placed on the flange of the cup container under free tension so that the sealant layer of the lid material film was in contact with the upper surface of the flange, and the sealing temperature was 170°C, the sealing time was 1.0 second, and the sealing pressure was 1 kgf / cm using a heat sealer with a ring-shaped seal head. 2 The heat sealing treatment was carried out twice under the above conditions to prepare a packaging container.

[0138] After cooling, in order to check the state and damage level of the covering material film on the polypropylene cup container, the degree of warping of the covering material film and the level of damage were visually checked.

[0139] [Example 2] The same procedure as in Example 1 was repeated except that the heat sealing temperature was changed from 170°C to 180°C.

[0140] [Example 3] A coating agent (Elex-one (registered trademark) Gloss Varnish) was applied to the first surface of the vapor deposition film (IB-OPP), which was the surface opposite to the barrier coating layer, to form a coating layer having a thickness of 1.5 μm. Using an electron beam irradiation device (manufactured by Iwasaki Electric Co., Ltd. ESI), the coating layer was irradiated with electron beams under conditions of an acceleration voltage of 110 kV and an exposure dose of 30 kGy, to form an electron beam cured resin layer.

[0141] The barrier coat layer of the vapor-deposited film (IB-OPP) on which an electron beam cured resin layer was formed on the first surface was coated with an adhesive (RU76) at a coat amount of 3 g / m under dry lamination conditions. 2 The adhesive was applied so as to form a sealant layer, and the adhesive was then laminated to an easy-peel sealant film which would serve as a sealant layer. In this manner, a covering film was produced.

[0142] A polypropylene cup container with a flange was prepared. A lid material film was cut to a size of 100 mm x 100 mm. The cut lid material film was placed on the flange of the cup container under free tension so that the sealant layer of the lid material film was in contact with the upper surface of the flange, and the sealing temperature was 170°C, the sealing time was 1.0 second, and the sealing pressure was 1 kgf / cm using a heat sealer with a ring-shaped seal head. 2 The heat sealing treatment was carried out twice under the above conditions to prepare a packaging container.

[0143] [Comparative Example 1] The second surface of the biaxially oriented polypropylene film (OPP-PFR treated product) is coated with adhesive (RU76) under dry lamination conditions at a coating amount of 3g / m 2 The adhesive (RU76) was applied to the biaxially oriented polypropylene film side of the vapor deposition film under dry lamination conditions at a coating amount of 3 g / m. 2The coating was applied so that the adhesive layer was coated with the adhesive layer, and the adhesive layer was laminated with an easy-peel sealant film that would serve as a sealant layer. In this manner, a covering film was produced. Using this covering film, a packaging container was produced in the same manner as in Example 1.

[0144] [Comparative Example 2] The same procedure as in Comparative Example 1 was repeated except that the heat sealing temperature was changed from 170°C to 180°C.

[0145] [Quantitative evaluation method for warping of covering film] After cooling, the extent to which the covering film had warped from the upper surface of the flange of the polypropylene cup container was measured with a vernier caliper.

[0146] [Visual evaluation method for heat damage to covering film] After carrying out the quantitative evaluation method for warpage of the covering material film, the damage level of the covering material film in the heat sealing treatment was visually confirmed.

[0147] [Table 1]

[0148] The covering material film made of the laminate of the Example could be stably and neatly heat-sealed to the upper surface of the flange of the cup container at both sealing temperatures of 170° C. and 180° C. When the covering material film made of the laminate of the Comparative Example was heat-sealed to the upper surface of the flange of the cup container at both sealing temperatures of 170° C. and 180° C., the surface of the covering material film was damaged by heat during the heat sealing process and was significantly warped upward on the cup container. [Explanation of symbols]

[0149] 1: Laminate 10: Base material 20: Electron beam curing resin layer 30: Deposition film layer 32: Stretched polypropylene film 34: Evaporation film 40: Sealant layer A, A1, A2: Adhesive layer 60: Lid material 61: Container body 62: Packaging container 63: Main body 64: Flange part 65: Opening 66:Contents 67: Holding part

Claims

1. a substrate having a first surface and a second surface; an electron beam cured resin layer provided on a first surface of the substrate; a sealant layer disposed on a second surface of the substrate; Equipped with The substrate contains polypropylene as a main component, The sealant layer contains polypropylene as a main component. Laminate.

2. The laminate according to claim 1 , wherein the electron beam cured resin layer has a thickness of 0.1 μm or more and 10 μm or less.

3. The laminate according to claim 1 , wherein the electron beam cured resin layer contains a cured product of a (meth)acrylate.

4. The laminate of claim 1 , wherein the substrate is a biaxially oriented polypropylene film.

5. 2. The laminate according to claim 1, further comprising a vapor-deposited film layer between the substrate and the sealant layer, the vapor-deposited film layer comprising a stretched polypropylene film and a vapor-deposited film provided on one surface of the stretched polypropylene film.

6. The laminate according to any one of claims 1 to 5, wherein the content of polypropylene in the entire laminate is 80 mass% or more.

7. The laminate according to any one of claims 1 to 5, which is a packaging material.

8. The laminate according to any one of claims 1 to 5, which is a lid material.

9. The laminate of claim 8 , wherein the sealant layer has easy peel properties.

10. A packaging bag comprising the laminate according to any one of claims 1 to 5.

11. The packaging bag according to claim 10, which is a boiled or retorted packaging bag.

12. A polypropylene container body having a storage portion; A lid material comprising the laminate according to any one of claims 1 to 5; A packaging container comprising:

Citation Information

Patent Citations

  • Gas barrier film, packaging material, package

    JP2009202519A