Fiber sheet for reinforcing concrete structures
The fiber sheet with a multiaxial mesh and matrix resin integration addresses the issue of opaque reinforcement layers by ensuring high tensile strength and visibility, allowing transparent inspection and maintaining structural integrity.
Patent Information
- Application Number
- JP2024141106
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-08-27
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-15
AI Technical Summary
Existing methods for reinforcing concrete structures using fiber sheets result in opaque layers that obscure the condition of the concrete base, making visual inspection difficult and potentially weakening the structure, while also failing to achieve high tensile strength.
A fiber sheet composed of a multiaxial mesh sheet integrated with a matrix resin, ensuring high tensile strength and visibility by maintaining a refractive index difference of 0.04 or less, with a basis weight of 500-1000 g/m² and mesh openings of 1-25 mm, allowing for transparent observation.
The solution provides sufficient reinforcing performance with high base visibility, maintaining structural integrity and enabling effective visual inspection without reducing strength.
Smart Images

Figure 2024161057000001 
Figure 2024161057000002 
Figure 2024161057000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a fiber sheet for reinforcing a concrete structure. [Background technology]
[0002] Reinforcing existing concrete structures generally involves removing deteriorated concrete, injecting crack reinforcement agents, and pouring covering concrete, but as this involves heavy work at height, a simpler method is needed.
[0003] In response to this, a reinforcement method has been proposed in which synthetic fiber woven fabric, knitted fabric, nonwoven fabric, etc. is attached to the area to be reinforced, and then a resin is applied and cured from above, forming a so-called FRP (fiber reinforced plastic).
[0004] When the reinforcement is performed with a fiber sheet, aramid fiber or carbon fiber has been used as the fiber sheet.
[0005] However, the surface of a concrete structure reinforced by such conventional methods is covered with a reinforcing layer such as an opaque resin or sheet member, making it difficult to visually observe the condition of the concrete structure's base material from the outside. In recent years, there have been many cases where it has become necessary to monitor the changes over time of a concrete structure after the surface has been reinforced, but there has been a problem in that it is not easy to meet this requirement.
[0006] In the past, when it became necessary to visually observe the condition of the base material from the outside, it was necessary to remove part of the existing reinforcing layer applied to the surface and create an inspection window to expose the base material.
[0007] However, forming an inspection window in this manner raised concerns that the strength of that area would be reduced and that the inspection window area could become a starting point for deterioration of the reinforcing layer.
[0008] As a construction method that uses an adhesive and a fiber mesh sheet to enable observation of the base material of a concrete structure after construction, Patent Document 1 describes a repair method characterized by applying an acrylic resin with a parallel light transmittance of 75% or more at a thickness of 1 mm to the surface of a concrete structure, and then attaching nylon fibers or vinylon fibers. Patent Document 2 proposes a reinforced coating method for the surface of a concrete structure in which a transparent polyurethane resin solution is applied, a glass fiber sheet is attached after that, the transparent polyurethane resin solution is applied on top of that to impregnate the glass fiber sheet, and this is dried and solidified to form a transparent or translucent coating layer. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2006-342538 A [Patent Document 2] JP 2010-001707 A Summary of the Invention [Problem to be solved by the invention]
[0010] However, the methods described in the above Patent Documents 1 and 2 are intended to merely suppress the peeling off of deteriorated structural pieces on the surface of a concrete structure, and therefore it has not been possible to obtain an FRP structure with the high tensile strength required for reinforcing a concrete structure. [Means for solving the problem]
[0011] In view of the above problems, an object of the present invention is to provide a reinforcing method that provides high substrate visibility and sufficient reinforcing performance.
[0012] As a result of extensive investigation, the inventors of the present invention have determined that the basis weight is 500 g / m 2 ~1000g / m 2The inventors have found that by using a fiber sheet made of the above multiaxial mesh sheet and a matrix resin, it is possible to ensure not only excellent reinforcing performance such as high tensile strength but also visibility of the underlying surface, thereby completing the present invention.
[0013] That is, the present invention provides the following (1) to (18).
[0014] (1) A fiber sheet for reinforcing a concrete structure, which is used in a method for reinforcing a concrete structure, The multiaxial mesh sheet (A) is made of filaments and the matrix resin (B) is integrated into one structure. The weight of the multiaxial mesh sheet (A) is 500 g / m 2 ~1000g / m 2 A fiber sheet for reinforcing concrete structures.
[0015] (2) The fiber sheet for reinforcing a concrete structure according to (1), wherein the multiaxial mesh sheet (A) has an opening size of 1 to 25 mm.
[0016] (3) The fiber sheet for reinforcing a concrete structure according to (1) or (2), wherein the multiaxial mesh sheet (A) contains a thermoplastic resin in at least one axial direction.
[0017] (4) The content of the thermoplastic resin contained in the multiaxial mesh sheet (A) is 50 g / m 2 A fiber sheet for reinforcing a concrete structure according to (3) below.
[0018] (5) The multiaxial mesh sheet (A) is a glass fiber sheet having at least two axes, and the glass fiber sheet has at least ZrO 2 12% by mass or more, and R 2 The fiber sheet for reinforcing a concrete structure according to any one of (1) to (4), containing 10 mass % or more of O (R is at least one selected from the group consisting of Li, Na, and K).
[0019] (6) The fiber sheet for reinforcing a concrete structure according to any one of (1) to (5), wherein the matrix resin (B) contains at least one component selected from the group consisting of (meth)acrylic resins, vinyl ester resins, unsaturated polyester resins, urethane resins, urea resins, epoxy resins, and silicone resins in an amount of at least 50 mass%.
[0020] (7) The content of the matrix resin (B) is 20 g / m 2 ~400g / m 2 The fiber sheet for reinforcing a concrete structure according to any one of (1) to (6), wherein
[0021] (8) A fiber sheet for reinforcing a concrete structure according to any one of (1) to (7), wherein the difference in refractive index between the multiaxial mesh sheet (A) and the matrix resin (B) is 0.04 or less when measured using a light source with a wavelength of 589 nm according to Method A in Section 4.1 of JIS K 7142:2014.
[0022] (9) The fiber sheet for reinforcing a concrete structure according to any one of (1) to (8), having an opening size of 1 to 25 mm.
[0023] (10) The combined weight of the filaments is 500g / m 2 ~1000g / m 2 A step of impregnating a multiaxial mesh sheet (A) with a matrix resin (B); the impregnated matrix resin (B) is cured and / or non-fluidized by a heat treatment and / or an active energy ray irradiation treatment to integrally mold the multiaxial mesh sheet (A) and the matrix resin (B) to obtain a fiber sheet; A method for producing a fiber sheet for reinforcing a concrete structure, comprising the steps of:
[0024] (11) The matrix resin (B) is a non-polymerizable high molecular weight material, a step of diluting the matrix resin (B), which is a high molecular weight resin, with an organic solvent (C) capable of dissolving the matrix resin (B); a step of impregnating the multiaxial mesh sheet (A) with the matrix resin (B) and then volatilizing the organic solvent (C) by heat treatment; The method for producing according to (10), further comprising:
[0025] (12) the matrix resin (B) is a radical polymerizable resin, adding a thermal polymerization initiator (D-1) that generates radicals upon heating to the matrix resin (B); a step of impregnating the multiaxial mesh sheet (A) with the matrix resin (B) and then radically polymerizing the matrix resin (B) by heat treatment; The method according to (10), further comprising:
[0026] (13) the matrix resin (B) is a radical polymerizable resin, adding a photopolymerization initiator (D-2) that generates radicals upon irradiation with active energy rays to the matrix resin (B); a step of impregnating the multiaxial mesh sheet (A) with the matrix resin (B) and then radically polymerizing the matrix resin (B) by an active energy ray irradiation treatment; The method according to (10), further comprising:
[0027] (14) Winding the fiber sheet into a roll. The method according to any one of (10) to (13), further comprising:
[0028] (15) A step of applying a concrete structure adhesive (E) to the fiber sheet according to any one of (1) to (9) or the fiber sheet obtained by the manufacturing method according to any one of (10) to (14); placing the fiber sheet on a surface of a concrete structure, curing the adhesive for concrete structures (E), and forming a reinforcing layer on the surface of the concrete structure; Including, A method for reinforcing a concrete structure, wherein the tensile strength of the reinforcing layer is at least 150 kN / m per unit length when measured using a B-type test piece prepared in accordance with JIS A 1191:2004.
[0029] (16) The reinforcing method according to (15), wherein the reinforcing layer has a total light transmittance of at least 5% as measured by the method described in JIS K 7375:2008.
[0030] (17) The reinforcement method according to (15) or (16), wherein the difference in refractive index between the multiaxial mesh sheet (A) and the concrete structure adhesive (E) is 0.04 or less when measured using a light source having a wavelength of 589 nm according to Method A in Section 4.1 of JIS K 7142:2014.
[0031] (18) The reinforcement method according to any one of (15) to (17), wherein the adhesive for concrete structures (E) contains at least one component selected from the group consisting of (meth)acrylic resins, vinyl ester resins, unsaturated polyester resins, urethane resins, urea resins, epoxy resins, and silicone resins in an amount of at least 50 mass%. Effect of the Invention
[0032] By using the fiber sheet provided in the embodiment of the present invention for reinforcing a concrete structure, sufficient reinforcing performance can be obtained while maintaining high visibility of the substrate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0033] In this specification, the amounts (parts) and ratios (%) are by mass unless otherwise specified. Numerical ranges in this specification include the upper and lower limits unless otherwise specified. Unless otherwise specified, concrete in this specification collectively refers to cement paste, mortar, and concrete.
[0034] <Fiber sheet for reinforcing concrete structures> A fiber sheet for reinforcing concrete structures (hereinafter also simply referred to as "fiber sheet") according to an embodiment of the present invention has a structure in which a multiaxial mesh sheet (A) made of combined filaments and a matrix resin (B) are integrated together. In manufacturing the fiber sheet, the multiaxial mesh sheet (A) is impregnated with matrix resin (B) in a fluid state (fluid state), and the matrix resin (B) is hardened and / or non-fluidized by heat treatment and / or activation energy irradiation, thereby forming an integrated structure. By combining the fiber sheet with an adhesive for concrete structures (E) described below, an FRP structure can be created as a reinforcing layer.
[0035] <Multiaxial mesh sheet (A)> The weight of the multiaxial mesh sheet (A) is 500 to 1000 g / m 2 500~800g / m 2 It is preferable that the weight per unit area is 500 g / m 2 If the thickness is less than 1000g / m, the tensile load-bearing performance required for the reinforcement method of concrete structures cannot be exhibited. 2 If it exceeds this value, impregnation of the matrix resin (B) is hindered, and the visibility of the concrete structure substrate decreases.
[0036] The opening of the multiaxial mesh sheet (A) is preferably 1 to 25 mm, and more preferably 2 to 10 mm. By using a mesh sheet with an opening within this range, excellent adhesion to the concrete structure can be obtained, and the tensile strength of the FRP can be improved, and thus the fire spread can be suppressed.
[0037] The multiaxial mesh sheet (A) preferably contains a thermoplastic resin at least in one axial direction. The thermoplastic resin is used, for example, as a heat-sealing thread. By containing a thermoplastic resin, crossing filaments can be bonded to each other, and the multiaxial mesh sheet can be prevented from unraveling. The type of thermoplastic resin is not particularly limited, and examples thereof include polyvinyl chloride (PVC), polyethylene, polypropylene, polystyrene, (meth)acrylonitrile-butadiene-styrene, (meth)acrylonitrile-styrene, polymethyl (meth)acrylic, polyvinyl alcohol, polyvinylidene chloride, polyethylene terephthalate, polyamide (nylon, etc.), polyacetal, polycarbonate, polyphenylene ether, polybutylene terephthalate, ultra-high molecular weight polyethylene, polyvinylidene fluoride, polysulfone, polyethersulfone, polyphenylene sulfide, polyarylate, polyamideimide, polyetherimide, polyetheretherketone, polyimide, liquid crystal polymer, polytetrafluoroethylene (Teflon (registered trademark)), etc.
[0038] The content of thermoplastic resin contained in the multiaxial mesh sheet (A) is 50 g / m 2 Less than 20 g / m is preferable. 2 More preferably, the thermoplastic resin content is 50 g / m 2 When the thickness is less than or equal to this, the visibility of the concrete structure base is improved.
[0039] The multiaxial mesh sheet (A) is preferably at least biaxial, more preferably a biaxial or more glass fiber sheet, and most preferably a biaxial glass fiber sheet. When the multiaxial mesh sheet (A) is a biaxial glass fiber sheet, it is possible to improve both the strength required for reinforcing a concrete structure and the visibility of the concrete structure base.
[0040] The method for producing the glass fiber sheet is not limited. For example, a method for producing a biaxial glass fiber sheet may be used in which a certain number of long fibers such as glass yarns or glass rovings are bundled together to form a fiber bundle, the fiber bundles are arranged in the warp and weft directions, and the intersecting fiber bundles are woven or bonded together.
[0041] Glass fiber is at least ZrO 2 12% by mass or more, and R 2 It is preferable that the alloy contains 10 mass % or more of ZrO (R is at least one selected from the group consisting of Li, Na, and K). 2 and R 2 If the amount of O is within the above range, the effect of the glass fiber sheet being less susceptible to deterioration by alkaline components derived from concrete structures can be obtained. 2 30% by mass or less, and R 2 It is preferable that the O content is 25 mass % or less.
[0042] The multiaxial mesh sheet (A) may contain other components. The other components refer to components other than fibers and components other than thermoplastic resins. Examples of the other components include long fibers made of components other than glass, thermosetting resins, inorganic compounds, metals, etc., and these may be used in combination. Among these, sizing materials and binders that are aqueous dispersions of urethane resins and acrylic resins are particularly suitable. The content of the other components is 50 g / m 2 Less than 50 g / m is preferable. 2 The content of other components is preferably less than 50 g / m 2 The visibility of the substrate can be improved by the following.
[0043] <Matrix resin (B)> By impregnating the multiaxial mesh sheet (A) with matrix resin (B) to form a fiber sheet, the visibility of the concrete structure base can be improved after the reinforcing layer is formed.
[0044] The matrix resin (B) may be any resin that can be impregnated into the multiaxial mesh sheet (A). The matrix resin (B) preferably contains at least one component selected from the group consisting of (meth)acrylic resin, vinyl ester resin, unsaturated polyester resin, urethane resin, urea resin, epoxy resin, and silicone resin in an amount of at least 50% by mass. The matrix resin (B) is preferably at least one component selected from the group consisting of radical polymerizable resin and epoxy resin. These components are easily integrated with the multiaxial mesh sheet (A), and when used in a method for reinforcing a concrete structure (hereinafter also simply referred to as a "reinforcing method"), high visibility of the substrate is achieved.
[0045] The resin(s) contained in the matrix resin (B) may be selected from among monomers, oligomers, and polymers, and these may be used in combination.
[0046] To the matrix resin (B), inorganic fillers, oils, rubbers, viscosity modifiers, pigments, dyes, plasticizers, polymerization initiators, sensitizers, catalysts, polymerization inhibitors, waxes, tackifiers, silane coupling agents, antioxidants, flame retardants, organic solvents, and the like may be added as long as the addition does not impair the performance.
[0047] The content (impregnation amount) of the matrix resin (B) contained in the fiber sheet is 20 g / m 2 ~400g / m 2 is preferred, and 50 g / m 2 ~200g / m 2 It is more preferable that the mass of the matrix resin (B) is 20 g / m 2 When the mass of the matrix resin (B) is 400 g / m or more, sufficient resin is impregnated between the fibers of the multiaxial mesh sheet (A), and when the multiaxial mesh sheet (A) is used in a reinforcement method, the visibility of the substrate is improved. 2 When it is equal to or less than this, the mass of the multiaxial mesh sheet (A) can be reduced, the sheet does not fall off when used in a reinforcement method, and workability is improved.
[0048] <Fiber sheet for reinforcing concrete structures> The difference in refractive index between the multiaxial mesh sheet (A) and the matrix resin (B) is preferably 0.04 or less, more preferably 0.025 or less, when measured using a light source with a wavelength of 589 nm according to Method A in Section 4.1 of JIS K 7142: 2014. When the difference in refractive index is 0.04 or less, the visibility of the substrate is improved when used in a reinforcement method.
[0049] The opening of the fiber sheet is preferably 1 to 25 mm, more preferably 3 to 10 mm. When the opening is within this range, excellent adhesion to a concrete structure can be obtained, and high reinforcing performance can be exhibited when used in a reinforcing method.
[0050] <Method of manufacturing fiber sheet> As described above, in this production method, the matrix resin (B) in a fluid state is impregnated into the multiaxial mesh sheet (A), which is then cured and / or non-fluidized.
[0051] In one example of the case where heat treatment is employed, a solution may be obtained by diluting the matrix resin (B), which is a non-polymerizable high molecular weight material, with an organic solvent (C) capable of dissolving the matrix resin (B). The solution is then impregnated into the multiaxial mesh sheet (A), and the organic solvent (C) is then volatilized by heat treatment to integrate the matrix resin (B) with the multiaxial mesh sheet (A).
[0052] The viscosity of the solution obtained by diluting the matrix resin (B) with the organic solvent (C), measured using a Brookfield type rotational viscometer, is preferably 2,000 mPa·s or less at 23°C and 20 rpm, and more preferably 500 mPa·s or less. If the viscosity is 2,000 mPa·s or less, the impregnation into the multiaxial mesh sheet (A) is sufficient, and the visibility of the substrate is improved when used in a reinforcement method. The viscosity is more preferably 1 mPa·s or more at 23°C and 20 rpm.
[0053] The organic solvent (C) capable of dissolving the matrix resin (B), which is a high molecular weight substance, can be used without limitation as long as it is an organic solvent that can be volatilized by heating, and two or more types may be used in combination. Examples of organic solvents that can be volatilized by heating include acetone, isobutyl alcohol, isopropyl alcohol (2-propanol), isopentyl alcohol (isoamyl alcohol), ethyl ether, ethylene glycol monoethyl ether (cellosolve), ethylene glycol monoethyl ether acetate (cellosolve acetate), ethylene glycol mono-normal-butyl ether (butyl cellosolve), ethylene glycol monomethyl ether (methyl cellosolve), ortho-dichlorobenzene, xylene, cresol, chlorobenzene, isobutyl acetate, isopropyl acetate, and isopentyl acetate. (isoamyl acetate), ethyl acetate, n-butyl acetate, n-propyl acetate, n-pentyl acetate (n-amyl acetate), methyl acetate, cyclohexanol, cyclohexanone, N,N-dimethylformamide, tetrahydrofuran, 1,1,1-trichloroethane, toluene, n-hexane, 1-butanol, 2-butanol, methanol, methyl ethyl ketone, methylcyclohexanol, methylcyclohexanone, methyl-n-butyl ketone, gasoline, coal tar naphtha, petroleum ether, petroleum naphtha, petroleum benzine, turpentine, and mineral spirits.
[0054] The compounding ratio of the matrix resin (B) and the organic solvent (C) capable of dissolving the matrix resin (B) is not limited, and they may be mixed at any ratio. However, the amount of the organic solvent (C) used is preferably 200 parts by mass or less, more preferably 10 to 150 parts by mass, per 100 parts by mass of the radical polymerizable resin.
[0055] As another example of the case where heat treatment is employed, a radical polymerizable resin (fluid) may be used as the matrix resin (B), and a step of adding a thermal polymerization initiator (D-1) that generates radicals by heating to the matrix resin (B) may be carried out. The obtained solution is then impregnated into the multiaxial mesh sheet (A), and the matrix resin (B) is then radically polymerized and cured by heat treatment, so that the matrix resin (B) and the multiaxial mesh sheet (A) can be integrated together. The amount of the thermal polymerization initiator (D-1) used is preferably 0.1 to 10 parts by mass relative to 100 parts by mass of the radical polymerizable resin.
[0056] The viscosity of the solution containing the matrix resin (B), which is a radical polymerizable resin in a fluid state, and the thermal polymerization initiator (D-1), measured with a Brookfield rotational viscometer, is preferably 2,000 mPa·s or less, more preferably 500 mPa·s or less, at 23°C and 20 rpm. If the viscosity is 2,000 mPa·s or less, the impregnation into the multiaxial mesh sheet (A) is sufficient, and when used in a reinforcement method, the visibility of the base is improved. The viscosity is more preferably 1 mPa·s or more at 23°C and 20 rpm.
[0057] The matrix resin (B) may contain a non-radically polymerizable resin.
[0058] There is no limitation on the thermal polymerization initiator (D-1) that generates radicals by heating, and for example, dihalogen-based, azo compound-based, organic peroxide-based, etc. can be used alone or in combination. Among these, organic peroxides are preferred. Among the organic peroxides, one or more of cumene hydroperoxide and benzoyl peroxide are preferred.
[0059] The matrix resin (B) may contain a reducing agent. When the reducing agent is used in combination with a thermal polymerization initiator (D-1) such as an organic peroxide, the thermal polymerization initiator (D-1) is reduced, improving the reaction rate of the radical polymerization and the physical properties of the polymerized product, the matrix resin (B). Among reducing agents, cobalt octylate is preferred.
[0060] The method of heat treatment is not limited. For example, a method of applying hot air to one or both sides of a multiaxial mesh sheet (A) impregnated with a matrix resin (B) in a fluid state to apply heat by convection may be adopted. Alternatively, a method of applying heat by radiating electromagnetic waves such as an infrared heater or a microwave irradiator is also common.
[0061] As an example of the case where active energy ray irradiation is used, a radical polymerizable resin (fluid) may be used as the matrix resin (B), and a step of adding a photopolymerization initiator (D-2) that generates radicals by active energy ray irradiation to the matrix resin (B) may be carried out. Then, the multiaxial mesh sheet (A) is impregnated with the obtained solution, and the matrix resin (B) is radically polymerized and cured by active energy ray irradiation, and the matrix resin (B) and the multiaxial mesh sheet (A) can be integrated.
[0062] The viscosity of the solution containing the matrix resin (B), which is a radical polymerizable resin in a fluid state, and the photopolymerization initiator (D-2), measured with a Brookfield rotational viscometer, is preferably 2,000 mPa·s or less, more preferably 500 mPa·s or less, at 23°C and 20 rpm. If the viscosity is 2,000 mPa·s or less, the impregnation into the multiaxial mesh sheet (A) is sufficient, and when used in a reinforcement method, the visibility of the base is improved. The viscosity is more preferably 1 mPa·s or more at 23°C and 20 rpm.
[0063] The photopolymerization initiator (D-2) that generates radicals by irradiation with active energy rays is not limited, and for example, alkylphenone derivatives, dihalogens, and azo compounds can be used alone or in combination. Among these, alkylphenone derivatives are preferred. Among alkylphenone derivatives, 1-hydroxycyclohexyl phenyl ketone is preferred.
[0064] The matrix resin (B) may contain a reducing agent. When the reducing agent is used in combination with the photopolymerization initiator (D-2), the photopolymerization initiator (D-2) is reduced, and the reaction rate of the radical polymerization and the physical properties of the polymerized product, the matrix resin (B), are improved. The amount of the photopolymerization initiator (D-2) used is preferably 0.1 to 10 parts by mass relative to 100 parts by mass of the radical polymerizable resin.
[0065] The type of active energy ray is not limited, and any energy source including active energy ray or an irradiator that selectively emits ultraviolet ray (UV), electron beam (EB), etc. can be used. Examples of irradiators that include active energy ray include black light and UV-LED light that preferably emit ultraviolet ray (UV) with a wavelength of 365 nm. The matrix resin (B) may contain a non-radical polymerizable resin.
[0066] The manufacturing process of the fiber sheet preferably includes a step of winding the fiber sheet into a roll, which not only ensures high portability but also makes it easy to manufacture a long fiber sheet, making it suitable for use at the site where the reinforcement method is carried out.
[0067] In the process of winding the fiber sheet into a roll, a release paper may be laminated on the fiber sheet and wound at the same time. By laminating the release paper, blocking between the sheets can be suppressed.
[0068] In the manufacturing process of the fiber sheet, the equipment for impregnating the multiaxial mesh sheet (A) with the matrix resin (B) in a fluid state is not particularly limited and any equipment can be used. Examples of the equipment for impregnation include a gravure coater, a dip coater, a comma coater, a top feed coater, a bar coater, a knife coater, a die coater, a reverse coater, an impregnation coater, a slot die coater, and a vacuum die coater. Among these, an impregnation coater is preferred because it has good impregnation properties of the matrix resin (B) into the multiaxial mesh sheet (A).
[0069] In the process of producing the fiber sheet, the method and equipment for impregnating the multiaxial mesh sheet (A) with the matrix resin (B) to integrate them may be a combination of two or more different methods.
[0070] <Adhesive for concrete structures (E)> A reinforcing layer can be formed on the surface of a concrete structure by applying and integrating the above-mentioned fiber sheet with an adhesive for concrete structures (E) (hereinafter also simply referred to as "adhesive (E)").
[0071] The tensile strength of the FRP sheet as a reinforcing layer obtained by using the fiber sheet and adhesive (E) is preferably at least 150 kN / m or more, more preferably 175 kN / m or more per unit length, when measured using a B-type test piece prepared according to a method conforming to JIS A 1191: 2004. A tensile strength of 150 kN / m or more can exhibit reinforcing performance comparable to that of conventional reinforcing methods for concrete structures using carbon fiber sheets or aramid fiber sheets.
[0072] The difference in refractive index between the multiaxial mesh sheet (A) contained in the fiber sheet and the adhesive (E) is preferably 0.04 or less, more preferably less than 0.025, when measured using a light source with a wavelength of 589 nm according to Method A in Section 4.1 of JIS K 7142: 2014. If the difference in refractive index is 0.04 or less, the visibility of the substrate is improved when used in a reinforcement method.
[0073] The adhesive (E) preferably contains at least one component selected from the group consisting of (meth)acrylic resin, vinyl ester resin, unsaturated polyester resin, urethane resin, urea resin, epoxy resin, and silicone resin, at least 50% by mass. The adhesive (E) is preferably at least one component selected from the group consisting of (meth)acrylic resin and epoxy resin. These resins can exhibit high tensile strength when integrated with a fiber sheet to form FRP. The (meth)acrylic resin may be the same component as the matrix resin (B), which is a radical polymerizable (meth)acrylic resin. The epoxy resin may be, for example, a mixture of 100 parts by mass of an epoxy compound and 10 to 100 parts by mass of a curing agent. The epoxy compound may be bisphenol A diglycidyl ether, etc. The curing agent may be an amine-based curing agent such as modified amine, etc.
[0074] The adhesive (E) may contain inorganic fillers, oils, rubbers, viscosity modifiers, pigments, dyes, plasticizers, polymerization initiators, sensitizers, catalysts, polymerization inhibitors, waxes, tackifiers, silane coupling agents, antioxidants, flame retardants, organic solvents, and the like, as long as the additives do not impair the performance of the adhesive.
[0075] The curing method of the adhesive (E) is not limited. The curing method of the adhesive (E) may be a method in which a coating film is formed by volatilizing a volatile component, a method in which a resin component reacts with moisture in the air to cure, a method in which two agents (or more) of a base agent and a curing agent are mixed and cured by a chemical reaction, or a method in which external energy such as heat or light is applied to cure. Among these, the method in which two agents are mixed and cured by a chemical reaction is preferred in terms of strength after application and applicability to concrete surfaces.
[0076] Two or more types of adhesives (E) can be used in combination. When two or more types are used in combination, two or more types of adhesives may be mixed and used, or one type of adhesive may be applied first, followed by application of a second or subsequent type of adhesive.
[0077] The viscosity of the adhesive (E) is not particularly limited, but if the viscosity measured using a Brookfield rotational viscometer is 20,000 mPa s or more at 23°C and 20 rpm, it is suitable because this allows the adhesive (E) to be applied to the ceiling or wall surfaces of a concrete structure in the required thickness and allows the formation of a reinforcing layer.
[0078] <Reinforcing layer> In the reinforcing method according to the embodiment of the present invention, a reinforcing layer can be formed on the surface of a concrete structure using the above-mentioned fiber sheet.
[0079] The reinforcing layer preferably has a total light transmittance of 5% or more, more preferably 15% or more, measured by the method described in JIS K 7375: 2008. When the reinforcing layer has a total light transmittance of 5% or more, sufficient visibility of the substrate can be obtained when used in the reinforcing method.
[0080] When forming the reinforcing layer, it is preferable to perform a surface treatment of the concrete in advance as necessary. By performing the surface treatment, the adhesiveness of the reinforcing layer can be ensured for a long period of time. The surface treatment is performed to remove laitance, surface dirt, and deteriorated base material, and may be performed using known techniques such as water jet treatment, sandblasting, sander scraping, and wire brushing.
[0081] When forming the reinforcing layer, it is preferable to repair the cross section of the structure beforehand as necessary. By repairing the cross section, the adhesiveness of the reinforcing layer can be ensured. As the cross section repair material, known materials such as concrete, mortar, cement paste, grout material, polymer cement mortar, and resin mortar can be used, and these may be used in combination.
[0082] When forming the reinforcing layer, it is preferable to coat the structure with a primer in advance, if necessary. Coating the primer not only improves the adhesion between the concrete structure and the reinforcing layer, but also impregnates the concrete structure deteriorated with cracks, etc., and restores the structure. It inhibits moisture, alkali metals, gases, etc. that seep out of the concrete structure, and ensures the performance of the reinforcing layer over a long period of time. As the primer, known materials such as acrylic resin-based primers, epoxy resin-based primers, vinyl ester resin-based primers, silicone resin-based primers, and inorganic primers can be used, and these may be used in combination. Among these, materials with a Gardner color scale of 8 or less are preferable. The amount of primer applied varies depending on the condition of the concrete structure, but is generally 0.05 to 1.0 kg / m 2 The application can be appropriately carried out using a known method such as application with a roller, a brush, a trowel, a spatula, or the like, or spray coating.
[0083] When forming the reinforcing layer, it is preferable to adjust the unevenness of the structure beforehand, if necessary. By adjusting the unevenness, the reinforcing layer can be applied uniformly to the concrete structure, and the reinforcing performance can be stably demonstrated over a large area. As the unevenness adjustment agent that can be used for unevenness adjustment, known materials such as resin mortar and polymer cement mortar that combine resin and aggregate can be used, and these may be used in combination. Of these, materials with a Gardner color number of 8 or less are preferable. The amount of unevenness adjustment agent to be applied varies depending on the unevenness of the primer surface, but generally, it is 1.8 kg / m. 2 The unevenness control agent can be appropriately applied using a known method such as application with a trowel or spatula, or spray application.
[0084] The reinforcing layer can be formed by hardening the liquid adhesive (E) and fixing the fiber sheet for reinforcing concrete structures. The liquid adhesive (E) can be applied by known methods such as application with a roller, trowel, or spatula, or spray coating. After the liquid adhesive (E) is applied, a fiber sheet is continuously laminated before hardening, and the fiber sheet is impregnated with the adhesive (E) and hardened to form FRP, thereby exhibiting reinforcing performance. The adhesive (E) may be applied for the entire process at once or may be applied in two or more steps, but it is preferable to apply it in two or more steps. By applying it in two or more steps, it is possible to apply the resin in the amount necessary to form the fiber sheet into FRP while preventing dripping. The amount of adhesive (E) to be applied is 0.2 to 2.0 kg / m per fiber sheet. 2 is preferable, and 0.5 to 1.4 kg / m 2 More preferably, the coating amount is 0.2 kg / m 2 If the amount is more than 2.0 kg / m, the fiber sheet can be fixed properly. 2 When the thickness is less than or equal to this, the visibility of the substrate is improved when the film is used in a reinforcement method.
[0085] Although the method for laminating the fiber sheets is not limited, it is preferable to use a defoaming roller. By using a defoaming roller, air bubbles in the adhesive (E) and the fiber sheets are removed, making it easier for the adhesive (E) to penetrate, and sufficient visibility of the substrate can be obtained when used in a reinforcement method.
[0086] In preparing the reinforcing layer, two or more fiber sheets may be laminated, and it is more preferable to laminate two fiber sheets. By laminating two or more fiber sheets, it is possible to achieve the same reinforcing performance as existing reinforcing methods using carbon fiber sheets or aramid fiber sheets. Two or more fiber sheets may be attached at once, or may be attached one by one in two or more steps, but it is preferable to attach one by one in two or more steps. By attaching one by one in two or more steps, it is possible to prevent the fiber sheets from falling due to their own weight.
[0087] The reinforcing layer may be provided with measures to prevent the fiber sheet from falling using known techniques such as anchor pins and anchor bolts. There is no limit to the number of anchor pins and anchor bolts used, but in consideration of the visibility of the base of the concrete structure, the area of the reinforcing layer covered by the anchor pins and anchor bolts is preferably less than 20% of the total area of the reinforcing layer, and more preferably less than 10%.
[0088] A protective layer may be further formed on the outer side of the reinforcing layer by applying a protective coating.
[0089] The method for curing the protective coating is not limited. For example, a method in which a coating film is formed by volatilizing a volatile component, a method in which a resin component reacts with moisture in the air to cure, a method in which two or more components are mixed and cured by a chemical reaction, a method in which external energy such as heat or light is applied to cure, etc. may be used.
[0090] The amount of protective coating applied is 0.01 to 1.0 kg / m2 in terms of solid content. 2 The range is preferably 0.02 to 0.2 kg / m 2 The protective coating can be appropriately applied using a known method such as application with a roller, brush, trowel or spatula, or spray coating.
[0091] In some embodiments, in addition to the reinforcing layer, layers of materials such as paint, adhesive, fiber sheet, film, resin molding, and layers of combinations of these materials may be laminated.
[0092] In a preferred embodiment, the reinforcing layer obtained by the above-mentioned reinforcing method can be made to have an average mouse behavior suspension time of 6.8 minutes or more when subjected to a gas toxicity test (using multiple mice) specified in the Fire Resistance Performance Testing and Evaluation Service Manual based on the Building Standards Act of Japan. The average mouse behavior suspension time refers to the average time from the start of the test until the mice stop behavior, and is sometimes called the average time. If the average mouse behavior suspension time is within the above range, in the event of a tunnel fire, there is little risk that evacuees will be engulfed in harmful combustion gases and put their lives at risk, and the effect of being suitable for use in tunnels can be obtained.
[0093] In a preferred embodiment, the reinforcing layer obtained by the above-mentioned reinforcing method can be made to have a flame-extinguishing time of 30 seconds or less and a tip of a fire caused by combustion that is less than 600 mm from the ignition point when subjected to a fire spread test in accordance with NEXCO Test Method 738. In that case, in the event of a tunnel fire, there is little risk of evacuees being caught in a flame caused by the spread of the fire and putting their lives at risk, making it suitable for use in tunnels. EXAMPLES
[0094] Examples of the present invention will be described below, but the present invention is not limited to these examples.
[0095] <Multiaxial mesh sheet> The raw material (yarn) and glue (and nylon fiber as a heat-sealed thread, if included) shown in Table 1 below were bound together, and an emulsion containing a vinylsilane-based silane coupling agent was used as a bundling agent (corresponding to "other" in the table) to obtain a beam. The beam was cut one by one and sewn into either a uniaxial, biaxial, or triaxial shape. After that, the beam was deoiled and surface-treated, and wound into a roll to obtain multiaxial mesh sheets No. 1-1 to 1-13. The mesh size of the obtained multiaxial mesh sheet was measured with a vernier caliper and shown in the table below. The refractive index of the obtained multiaxial mesh sheet was also measured using a light source with a wavelength of 589 nm according to Method A in Section 4.1 of JIS K 7142:2014. The results are shown in the table below.
[0096] [Table 1]
[0097] <Glass fiber> Of the multiaxial mesh sheets described above, glass fiber yarn was used as the raw material. The yarn was obtained by melting and spinning glass fibers having one of the compositions shown in Table 2 below. The other components in the table are impurities, mainly Al. 2 O 3 It was.
[0098] [Table 2]
[0099] <Matrix resin> Matrix resins No. 3-1 to 3-9 were obtained using commercially available monomer or polymer-based designs shown in Table 3 below. These were integrated with the multiaxial mesh sheet (A) by the manufacturing method shown in the table to form a fiber sheet. The viscosity of the impregnation solution was measured at 23°C and 20 rpm using a Brookfield type rotational viscometer. The results are shown in the table below.
[0100] <Acrylic resin polymer A> A polymer formed by heating a mixture of 100 parts by mass of Viscoat #160 (product name, benzyl acrylate, manufactured by Osaka Organic Chemical Industry Co., Ltd.) and 2 parts by mass of Niper NS (product name, benzoyl peroxide suspension solution, manufactured by NOF Corporation) at 120°C for 10 minutes.
[0101] <Acrylic resin polymer B> A polymer formed by heating a mixture of 100 parts by mass of Viscoat #155 (product name, Osaka Organic Chemical Industry Co., Ltd., cyclohexyl acrylate) and 2 parts by mass of Niper NS (product name, NOF Corporation, benzoyl peroxide suspension solution) at 120°C for 10 minutes.
[0102] <Acrylic resin monomer> Viscoat #160 (product name, Osaka Organic Chemical Industry Co., Ltd., benzyl acrylate)
[0103] <Vinyl acetate resin> A one-component curing adhesive CH18 (product name, manufactured by Konishi Co., Ltd., vinyl acetate resin emulsion type adhesive), which cures by the evaporation of water, was used as packaged. [Table 3]
[0104] The manufacturing method shown in Table 3 above is as follows. The fiber sheet for reinforcing a concrete structure was produced by the following method. After forming the fiber sheet for reinforcing a concrete structure, the mesh size was measured with a vernier caliper and is shown in Table 5 below.
[0105] (※3-1) Method of dilution with organic solvent (C) and evaporation The matrix resin (B) was diluted with acetone (manufactured by Taishin Chemical Co., Ltd.) in the amount shown in Table 3 as the organic solvent (C) to obtain an impregnation solution. The diluted matrix resin was put into a dip coater, and a multiaxial mesh sheet (A) with a width of 1 m and a length of 30 m wound on a roll was sequentially unwound, dipped so that the solid content of the matrix resin (B) reached the target mass, and then squeezed out with a roll. It was then heated for 5 minutes in a thermal drying oven (infrared heater) at 120 ° C to volatilize the organic solvent (C). After that, the sheet was wound again into a roll while wrapping a release-treated PET film around it so that the sheet surface did not come into contact with it, and a fiber sheet was obtained.
[0106] (※3-2) Method using the addition of a thermal polymerization initiator (D-1) and thermal polymerization Niper NS (trade name, NOF Corp., benzoyl peroxide suspension solution) was added to the matrix resin (B) as a thermal polymerization initiator (D-1) in the amount shown in Table 3 to obtain an impregnation solution. The matrix resin to which the initiator was added was placed in a dip coater, and a 1 m wide x 30 m long multiaxial mesh sheet (A) wound on a roll was sequentially unwound and dipped to the target mass, and then squeezed with a roll. The sheet was then heated for 5 minutes in a thermal drying oven (infrared heater) at 120°C to radically polymerize the matrix resin (B). The sheet was then wound up again into a roll while wrapping a release-treated PET film around it so that the sheet surface did not come into contact with the sheet, to produce a fiber sheet.
[0107] (※3-3) Method using the addition of a photopolymerization initiator (D-2) and exposure to active energy rays Irgacure 184 (trade name, IGM Resins BV, 1-hydroxycyclohexyl phenyl ketone) was added as a photopolymerization initiator (D-2) to the matrix resin (B) in the amount shown in Table 3 to obtain an impregnation solution. The matrix resin to which the initiator was added was placed in a dip coater, and a multiaxial mesh sheet (A) 1 m wide x 30 m long wound on a roll was successively unwound and dipped to the target mass, and then squeezed out with a roll. Next, in order to prevent polymerization inhibition by oxygen, both sides of the sheet were sandwiched between release-treated PET films, and then the sheet was immersed in a 100-m thick PET film with a peak emission wavelength of 355 nm and an illuminance of 1.1 mW / cm on the sheet surface. 2 The matrix resin (B) was radically polymerized by irradiating it with ultraviolet light for 5 minutes using a UV-LED light. After that, the fiber was wound up again into a roll to obtain a fiber sheet.
[0108] (※3-4) Combination system A fiber sheet was similarly obtained by combining the above methods (※3-1) and (※3-2).
[0109] <Adhesive for concrete structures> Nos. 4-1 to 4-7 were obtained as adhesives (E) using commercially available adhesives or monomer-based designed products shown in Table 4 below. The refractive indexes of the adhesives were measured using a light source with a wavelength of 589 nm according to Method A in Section 4.1 of JIS K 7142:2014. The results are also shown in the table below.
[0110] [Table 4]
[0111] <Acrylic adhesive A> A resin composition was used in which Viscoat #160 (product name, benzyl acrylate, manufactured by Osaka Organic Chemical Industry Co., Ltd.) / Percumyl H (product name, cumene hydroperoxide, manufactured by NOF Corporation) / cobalt octylate (manufactured by Osaki Kogyo Co., Ltd.) were mixed in a ratio of 100 / 2 / 2 parts by mass and cured by redox polymerization.
[0112] <Acrylic adhesive B> A resin composition was used in which Viscoat #155 (product name, Osaka Organic Chemical Industry Co., Ltd., cyclohexyl acrylate) / Percumyl H (product name, NOF Corporation, cumene hydroperoxide) / cobalt octylate (Osaki Kogyo Co., Ltd.) were mixed in a ratio of 100 / 2 / 2 parts by mass and cured by redox polymerization.
[0113] <Epoxy adhesive> A resin composition prepared by mixing jER828 (product name, manufactured by Mitsubishi Chemical Corporation, bisphenol A diglycidyl ether) / ST11 (product name, manufactured by Mitsubishi Chemical Corporation, modified amine) in a ratio of 100 / 60 parts by mass, and curing the composition through a polyaddition reaction between the glycidyl group and the amino group.
[0114] <Vinyl acetate adhesive> A one-component curing adhesive CH18 (product name, manufactured by Konishi Co., Ltd., vinyl acetate resin emulsion type adhesive), which cures by the evaporation of water, was used as packaged.
[0115] <Water glass> No. 3 water glass (manufactured by Fuji Chemical Co., Ltd.) specified in JIS K 1408:1966, which dries and hardens by volatilization of water, was used.
[0116] <Reinforcement method> The test substrates shown below were prepared as objects to which a reinforcing layer was applied.
[0117] Test Substrate (1) Mortar test plate for evaluating substrate visibility (compliant with JIS R 5201:2015) The mortar test plate was prepared in accordance with the method of preparing specimens according to Section 11.5 of JIS R 5201:2015. The adherend surface (150mm x 70mm surface) of the 150mm x 70mm x 10mm mortar piece was scraped with a #150 paper sander to remove laitance, and dust was removed with an air blower. Three crack patterns of 0.2mm width, 0.5mm width, and 1.0mm width were drawn in the longitudinal direction of the adherend surface with a black HB pencil. Hereinafter, this test plate is referred to as the "mortar piece for visibility evaluation."
[0118] (2) Mortar test plate for evaluating alkali resistance (compliant with JIS R 5201:2015) The mortar test plate was prepared in accordance with the method of preparing specimens according to Section 11.5 of JIS R 5201:2015. The surface of the 150mm x 70mm x 10mm mortar piece (150mm x 70mm surface) was scraped with a #150 paper sander to remove laitance, and dust was removed with an air blower. Hereinafter, this test plate is referred to as the "mortar piece for evaluating alkali resistance."
[0119] (3) Concrete slab for workability evaluation / concrete adhesion evaluation (compliant with JIS A 5371:2016) The concrete slab was made in accordance with JIS A 5371:2016, Appendix B (regulations) for slabs of paving and boundary blocks. The surface of the 300mm x 300mm x 60mm concrete slab (300mm x 300mm surface) was scraped with a #150 paper sander to remove laitance, and dust was removed with an air blower. The slab obtained in this way is hereafter referred to as the "concrete slab".
[0120] (4) FRP strength evaluation test pieces Compliant with JIS A 1191:2004 (see below).
[0121] (5) Calcium silicate board for gas toxicity assessment (compliant with JIS A 5430:2018) The calcium silicate board is a calcium silicate board (type 2) according to JIS A 5430: 2018. It was obtained by removing dust from the surface of the adherend (220 mm x 220 mm surface) of a calcium silicate board of 220 mm x 220 mm x 10 mm with an air blower.
[0122] (6) Calcium silicate board for evaluating fire spread (compliant with JIS A 5430:2018) The calcium silicate board is a calcium silicate board (type 2) according to JIS A 5430: 2018. It was obtained by removing dust from the surface of the adherend (900 mm x 600 mm surface) of a calcium silicate board of 900 mm x 600 mm x 12 mm with an air blower.
[0123] Using the combinations of multiaxial mesh sheets, matrix resins, and adhesives shown in Table 5 below, reinforcing layers according to Examples 1 to 39 and Comparative Examples 1 to 4 were each produced on any of the test substrates described above.
[0124] First, a fiber sheet was prepared using the combination of multiaxial mesh sheet and matrix resin shown in Table 5 (see also Tables 1 to 3). The number of multiaxial mesh sheets stacked is also shown in Table 5.
[0125] Of the reinforcement performance properties shown in Table 5, the test specimens for which "visibility of base," "alkali resistance," "workability," "adhesion to concrete," "gas hazards," and "fire spread" were evaluated were prepared using the following procedure.
[0126] As a primer, Denka DK550-003R, an acrylic crack injection repair material manufactured by Denka Co., Ltd., was applied to the corresponding test substrate with a roller (application amount 0.15 kg / m 2 ).
[0127] After applying the primer, the test substrate was left for 15 minutes to form a reinforcing layer. The reinforcing layer was first prepared by applying the adhesives shown in Tables 4 and 5 as an undercoat to the test substrate with a rubber spatula or metal trowel (application amount 0.6 kg / m2). 2 ), the above-mentioned fiber sheet was immediately adhered thereto, and the fiber sheet was rubbed with a defoaming roller to allow the adhesive to be impregnated into the fiber sheet.
[0128] Next, immediately afterwards, the adhesives shown in Tables 4 and 5 were applied as topcoat resins onto the fiber sheet using a rubber spatula or metal trowel (application amount 0.6 kg / m 2 ) and then cured at 20°C for 24 hours to form a reinforcing layer.
[0129] Test pieces for evaluating the "FRP strength" of the reinforcement method were prepared using the following procedure.
[0130] According to the method for preparing B-type test specimens in JIS A 1191:2004, the adhesives for concrete structures shown in Tables 4 and 5 were poured to a thickness of 2 mm, and the fiber sheets shown in Tables 1, 2 and 5 were placed in the center of the thickness direction and left to stand. After hardening and curing at 20°C for 7 days, a metal tab for tensile testing (SPCC test specimen) was attached with an acrylic adhesive for steel plates (DKP63, manufactured by Denka) to prepare an FRP test specimen.
[0131] <Evaluation of reinforcement performance> To evaluate the reinforcement performance, evaluations were carried out on "visibility of base," "alkali resistance," "workability," "concrete adhesion," "FRP strength," "gas toxicity," and "fire spread," as shown in Table 5. The evaluation results are all shown in Table 5.
[0132] <Evaluation method for "Base visibility"> After forming the reinforcing layer, the cracks were visually observed and evaluated according to the following criteria. ○ Cracks of 0.2mm and 0.5mm were visible throughout the entire area. △: 0.5 mm cracks were visible over the entire area, but some or all of the 0.2 mm cracks were not visible. × None of the 0.2 mm or 0.5 mm cracks were visible, either partially or entirely.
[0133] <Evaluation method for "alkali resistance"> The mortar pieces for evaluating alkali resistance with the reinforcing layer formed were submerged in a saturated calcium hydroxide solution for 28 days, and after being removed, any changes that occurred on the surface were immediately visually observed and evaluated according to the following criteria. ○ No discoloration, cracks, peeling, swelling, fissures, leakage, or other abnormalities were observed in the reinforcing layer. △: Any abnormality such as discoloration, cracking, peeling, swelling, fissures, or leakage was observed in the reinforcing layer.
[0134] <Evaluation method for "workability"> The 300mm x 60mm surface of the concrete slab on which the reinforcing layer was formed was placed in contact with the ground, and the adherend surface (the surface on which the reinforcing layer was applied) was placed perpendicular to the ground. The condition of the surface was visually observed from the formation of the reinforcing layer until the hardening was completed, and was evaluated according to the following criteria. ○ There was no peeling, sliding or falling of the sheet, and no dripping of the resin. △: Slight slippage of the sheet, dripping of the resin, etc. were observed. x: Peeling or falling of the sheet, or serious slippage of the sheet, dripping of resin, or the like was observed.
[0135] <Evaluation method for "concrete adhesion"> A 40 mm x 40 mm steel jig was attached to the outermost surface of the reinforcing layer using an acrylic resin mortar adhesive (Denka Dyna N, manufactured by Denka Co., Ltd.), and a cut was made along the jig until it reached the concrete plate. The jig was then pulled perpendicularly to the attachment surface using a Construction Research Institute tensile adhesion tester, and the adhesion strength (N / mm 2 ) was measured and evaluated according to the following criteria. ○ 2.0N / mm 2 (Surface protection work (medium corrosion protection type C) conformity standard according to the Hanshin Expressway Co., Ltd. repair guidelines) △ 1.5N / mm 2 More than 2.0N / mm 2 Less than (NEXCO Bridge Structure Collapsing Prevention Method Compliance Standard) × 1.5N / mm 2 less than
[0136] <Evaluation method for "FRP strength"> The FRP strength test was carried out in accordance with JIS A 1191:2004, and the FRP tensile load (kN) was calculated. Then, the FRP tensile strength per unit length (kN / m) was calculated according to the following formula 1. [Formula 1] FRP tensile strength per unit length (kN / m) = FRP tensile load (kN) × number of fiber bundles in the test piece (pieces) ÷ Number of fiber bundles aligned in the tensile direction per 1m width of fiber sheet (bundles / m)
[0137] Furthermore, to roughly calculate the FRP strength in the reinforcing layer, we also calculated the converted FRP tensile strength (kN / m) by multiplying the FRP tensile strength per unit length (kN / (m·sheet)) in Equation 1 by the number of fiber sheets bonded together in the reinforcing layer (sheets), as shown in Equation 2 below. [Formula 2] Converted FRP tensile strength (kN / m) = FRP tensile load per unit length calculated using [Equation 1] (kN / (m sheet)) × Number of fiber sheets bonded together (sheets)
[0138] The FRP tensile strength was evaluated according to the following criteria. ○ Converted FRP tensile strength (kN / m) is 350kN / m or more △ Converted FRP tensile strength (kN / m) is 300kN / m or more and less than 350kN / m × Converted FRP tensile strength (kN / m) is less than 300kN / m
[0139] <Evaluation method for "gas hazard"> The gas toxicity test is based on the fire resistance performance test and evaluation procedure manual based on the Building Standards Act of Japan, and is conducted using mice to measure the average behavioral pause time (X s ) was calculated and evaluated according to the following criteria. The above fire resistance performance test and evaluation procedure manual is, for example, that published by the General Incorporated Foundation, Construction Materials Testing Center. ○ X s 7.2 minutes or more △ X s Between 6.8 and 7.2 minutes × X s Less than 6.8 minutes
[0140] <How to evaluate "fire spread"> Using the flame spread test specified in NEXCO Test Method 738, the flame extinguishing time and the ignition point at the tip of the flame due to combustion were recorded and evaluated according to the following criteria. The flame extinguishment time was 10 seconds or less, and the tip of the fire was less than 500 mm from the ignition point. △ The flame was extinguished in 30 seconds or less, and the tip of the fire was less than 600 mm from the ignition point. × The flame extinguishing time exceeds 30 seconds or the tip of the fire caused by combustion is 600 mm or more from the ignition point.
[0141] [Table 5] (※1): FRP could not be formed.
[0142] As can be seen from Table 5, all of the Examples showed good to excellent reinforcement performance. On the other hand, Comparative Examples 1 and 3 had defects in the visibility of the substrate. Comparative Example 2 had insufficient FRP strength. Comparative Example 4 was unable to form an FRP. In other words, all of the Comparative Examples were not practically usable as reinforcement methods.
[0143] The present invention can be used to reinforce concrete structures, for example, to reinforce existing concrete structures.
Claims
1. A fiber sheet for reinforcing a concrete structure, which is used in a method for reinforcing a concrete structure, A multiaxial mesh sheet (A) made of a combination of filaments and a matrix resin (B) are integrated together, and The weight of the multiaxial mesh sheet (A) is 500 g / m 2 ~1000g / m 2 is Fiber sheet for reinforcing concrete structures.
2. 2. The fiber sheet for reinforcing a concrete structure according to claim 1, wherein the opening of the multiaxial mesh sheet (A) is 1 to 25 mm.
3. The fiber sheet for reinforcing a concrete structure according to claim 1 or 2, wherein the multiaxial mesh sheet (A) contains a thermoplastic resin in at least one axial direction.
4. The content of the thermoplastic resin contained in the multiaxial mesh sheet (A) is 50 g / m 2 4. The fiber sheet for reinforcing a concrete structure according to claim 3, wherein:
5. The multiaxial mesh sheet (A) is a glass fiber sheet having at least two axes, and the glass fiber sheet has at least ZrO 2 12% by mass or more, and R 2 5. The fiber sheet for reinforcing a concrete structure according to claim 1, containing 10 mass% or more of O (R is at least one selected from the group consisting of Li, Na and K).
6. 6. The fiber sheet for reinforcing a concrete structure according to any one of claims 1 to 5, wherein the matrix resin (B) contains at least one component selected from the group consisting of (meth)acrylic resins, vinyl ester resins, unsaturated polyester resins, urethane resins, urea resins, epoxy resins, and silicone resins in an amount of at least 50 mass%.
7. The content of the matrix resin (B) is 20 g / m 2 Up to 400 g / m 2 The fiber sheet for reinforcing a concrete structure according to any one of claims 1 to 6,
8. The fiber sheet for reinforcing a concrete structure according to any one of claims 1 to 7, wherein the difference in refractive index between the multiaxial mesh sheet (A) and the matrix resin (B) is 0.04 or less when measured using a light source having a wavelength of 589 nm according to Method A in Section 4.1 of JIS K 7142:2014.
9. The fiber sheet for reinforcing a concrete structure according to any one of claims 1 to 8, wherein the mesh size is 1 to 25 mm.
10. The combined weight of the filaments is 500 g / m 2 ~1000g / m 2 A step of impregnating a multiaxial mesh sheet (A) with a matrix resin (B); the impregnated matrix resin (B) is cured and / or non-fluidized by a heat treatment and / or an active energy ray irradiation treatment to integrally mold the multiaxial mesh sheet (A) and the matrix resin (B) to obtain a fiber sheet; A method for producing a fiber sheet for reinforcing a concrete structure comprising the steps of:
11. the matrix resin (B) is a non-polymerizable high molecular weight material, a step of diluting the matrix resin (B), which is a high molecular weight resin, with an organic solvent (C) capable of dissolving the matrix resin (B); a step of impregnating the multiaxial mesh sheet (A) with the matrix resin (B) and then volatilizing the organic solvent (C) by heat treatment; The method of claim 10 further comprising:
12. the matrix resin (B) is a radical polymerizable resin, adding a thermal polymerization initiator (D-1) that generates radicals upon heating to the matrix resin (B); a step of impregnating the multiaxial mesh sheet (A) with the matrix resin (B) and then radically polymerizing the matrix resin (B) by heat treatment; The method of claim 10 further comprising:
13. the matrix resin (B) is a radical polymerizable resin, adding a photopolymerization initiator (D-2) that generates radicals upon irradiation with active energy rays to the matrix resin (B); a step of impregnating the multiaxial mesh sheet (A) with the matrix resin (B) and then radically polymerizing the matrix resin (B) by an active energy ray irradiation treatment; The method of claim 10 further comprising:
14. The method according to any one of claims 10 to 13, further comprising a step of winding the fiber sheet into a roll.
15. A step of applying a concrete structure adhesive (E) to the fiber sheet according to any one of claims 1 to 9 or the fiber sheet obtained by the manufacturing method according to any one of claims 10 to 14; placing the fiber sheet on a surface of a concrete structure, curing the adhesive for concrete structures (E), and forming a reinforcing layer on the surface of the concrete structure; Including, A method for reinforcing a concrete structure, wherein the tensile strength of the reinforcing layer is at least 150 kN / m per unit length when measured using a B-type test piece prepared in accordance with JIS A 1191:2004.
16. The reinforcing method according to claim 15, wherein the reinforcing layer has a total light transmittance of at least 5% as measured by the method specified in JIS K 7375:2008.
17. The reinforcing method according to claim 15 or 16, wherein the difference in refractive index between the multiaxial mesh sheet (A) and the concrete structure adhesive (E) is 0.04 or less when measured using a light source having a wavelength of 589 nm according to Method A in Section 4.1 of JIS K 7142:2014.
18. The reinforcing method according to any one of claims 15 to 17, wherein the concrete structure adhesive (E) contains at least one component selected from the group consisting of (meth)acrylic resins, vinyl ester resins, unsaturated polyester resins, urethane resins, urea resins, epoxy resins, and silicone resins in an amount of at least 50 mass%.
Citation Information
Patent Citations
Concrete structure repairing method and concrete structure
JP2006342538A
Reinforced coating method of concrete structure surface
JP2010001707A