Fire preventive facility
A thermally expandable fireproof material with low elution rates and specific compositions addresses the issue of water resistance and fire resistance degradation, maintaining performance and appearance in fire protection equipment.
Patent Information
- Application Number
- JP2024144063
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2040-10-23
AI Technical Summary
Thermally expandable fireproof materials used in fire protection equipment, particularly at openings in buildings, suffer from low water resistance, leading to elution of components and reduced fire resistance when exposed to high humidity or water, causing appearance issues and requiring time-consuming maintenance.
A thermally expandable fireproof material with an elution rate of 3% or less when immersed in water at 60°C for 1000 hours, composed of specific matrix components like chloroprene rubber, styrene-butadiene rubber, and PVC, along with thermally expandable graphite and inorganic fillers, is used to maintain fire resistance and appearance integrity.
The material maintains high fire resistance and prevents component elution, ensuring long-term performance even in humid or water-exposed environments without deteriorating appearance.
Smart Images

Figure 2024161096000002 
Figure 2024161096000003 
Figure 2024161096000004
Abstract
Description
[Technical field]
[0001] The present invention relates to fire protection equipment, such as fittings, equipped with a thermally expandable fire-resistant material. [Background technology]
[0002] Conventionally, fire protection equipment is installed in areas where there is a risk of fire spreading, such as openings in buildings. Fire protection equipment is often equipped with a heat-expandable fire-resistant material containing a heat-expandable material such as heat-expandable graphite. In addition, in order to improve fire resistance, attempts have been made to incorporate relatively large amounts of flame retardants, inorganic fillers, etc. in addition to heat-expandable graphite into the heat-expandable fire-resistant material.
[0003] On the other hand, it is known that drainage holes are provided at the bottom of fittings such as sills and bottom frames to ensure drainage paths so that rainwater, condensation, etc. can be discharged to the outside in fittings installed at openings of buildings. Drainage paths such as drainage holes become fire-resistant defects and can cause a fire to spread. For this reason, drainage paths such as drainage holes are sometimes designed to be blocked by heat-expandable fire-resistant materials in the event of a fire (for example, see Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 6701318 Summary of the Invention [Problem to be solved by the invention]
[0005] However, the flame retardants and inorganic fillers used in thermally expandable fire-resistant materials often have low water resistance, and condensation or moisture can cause the internal materials to dissolve, resulting in problems such as poor appearance and reduced fire resistance. The thermally expandable fireproofing materials used for blocking the lower part of fire protection equipment, especially drainage paths, are placed in high humidity and come into contact with water during use, so they are prone to poor appearance and reduced fire resistance. When these problems occur, measures such as recall and replacement are taken, but in the case of buildings such as buildings and apartments, replacement requires steps such as setting up scaffolding, which is extremely time-consuming.
[0006] Therefore, an object of the present invention is to provide a fire prevention facility in which a thermally expandable fireproof material is unlikely to suffer from poor appearance or reduced fire resistance even when the material is placed in an environment of high humidity or in contact with water. [Means for solving the problem]
[0007] As a result of intensive research to solve the above problems, the present inventors have found that the above problems can be solved by using a thermally expandable fireproof material in a fire protection facility, the elution rate of which is 3% or less when immersed in water at 60°C for 1000 hours, and have completed the present invention. That is, the present invention is as follows: [1] to [9]. [1] Fire protection equipment that is at least partially equipped with a heat-expandable fire-resistant material that has a dissolution rate of 3% or less when immersed in water at 60°C for 1,000 hours. [2] The fire protection equipment according to the above [1], wherein the thermally expandable fireproof material contains a matrix component and thermally expandable graphite. [3] The fire protection equipment according to the above [2], wherein the thermally expandable fireproof material further contains an inorganic filler. [4] The fire protection equipment according to [2] or [3] above, wherein the matrix component contains at least one selected from the group consisting of chloroprene rubber, styrene butadiene rubber, butyl rubber, urethane rubber, and PVC. [5] The fire protection equipment according to any one of the above [1] to [4], wherein the thermally expandable fireproof material is substantially free of phosphorus components. [6] The fire protection equipment according to any one of the above [1] to [5], wherein the thermally expandable fireproof material is mounted on a lower portion of the fire protection equipment. [7] The fire prevention equipment according to any one of the above [1] to [6], which is used in at least one of a building and an apartment building. [8] The fire protection equipment is provided with a drainage path, The fire prevention facility according to any one of the above [1] to [7], wherein the heat-expandable fire-resistant material is arranged so as to block the drainage path when it thermally expands due to heating. [9] The fire protection equipment has a drainage hole, The fire prevention facility according to any one of the above [1] to [8], wherein the heat-expandable fire-resistant material is arranged so as to block the drain hole when it thermally expands due to heating. Effect of the Invention
[0008] According to the present invention, it is possible to provide a fire prevention facility in which the thermally expandable fireproof material is unlikely to suffer from poor appearance or reduced fire resistance even when placed in an environment of high humidity or in contact with water. [Brief description of the drawings]
[0009] [Figure 1] FIG. 2 is a front view showing the fittings that constitute the fire prevention equipment. [Diagram 2] FIG. 2 is a partially enlarged cross-sectional view of the fitting according to the first embodiment. [Diagram 3] FIG. 11 is a partially enlarged cross-sectional view of a fitting according to a second embodiment. [Figure 4] FIG. 11 is a partially enlarged cross-sectional view of a fitting according to a third embodiment. [Diagram 5] FIG. 11 is a partially enlarged cross-sectional view of a fitting according to a fourth embodiment. [Figure 6] FIG. 11 is a partially enlarged cross-sectional view of a fitting according to a fifth embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, the present invention will be described with reference to embodiments. The fire-resistant equipment of the present invention is at least partially equipped with a thermally expandable fire-resistant material. The thermally expandable fire-resistant material used in the present invention will be described in detail below.
[0011] [Thermally expandable fireproof material] The heat-expandable fireproof material used in the present invention has an elution rate of 3% or less when immersed in water for 1000 hours at 60° C. If the elution rate exceeds 3%, when the heat-expandable fireproof material mounted on a fireproof equipment is placed in a high humidity environment or in a position where it comes into contact with water, the components constituting the heat-expandable fireproof material will elute, reducing the fire resistance or the eluted components will contaminate the fireproof equipment, causing poor appearance, etc. From the viewpoint of preventing the appearance of the fire prevention equipment from being deteriorated and further improving the fire resistance, the elution rate is preferably 1% or less, more preferably 0.5% or less, and even more preferably 0.2% or less. The lower the elution rate, the better, and it is sufficient if it is 0% or more. The elution rate can be adjusted by appropriately selecting each component to be blended in the thermally expandable fireproof material. Specifically, it is sufficient to use compounds with low solubility in water for the matrix component, inorganic filler, organic flame retardant, and other additives described below. The specific method for measuring the dissolution rate is as described in the Examples.
[0012] <Matrix components> In the present invention, the thermally expandable fireproof material comprises a matrix component and thermally expandable graphite, the thermally expandable graphite being dispersed in the matrix component. The matrix component is at least one selected from a resin component, a rubber component, and an elastomer component.
[0013] Examples of rubber components include diene rubbers such as isoprene rubber (IR), butadiene rubber (BR), styrene butadiene rubber (SBR), hydrogenated styrene-butadiene copolymer rubber (HSBR), chloroprene rubber (CR), and acrylonitrile-butadiene rubber (NBR); ethylene-propylene rubber (EPM), ethylene-propylene-diene rubber (EPDM), natural rubber, butyl rubber, chlorinated butyl rubber, chlorosulfonated polyethylene, acrylic rubber, epichlorohydrin rubber, multi-vulcanized rubber, non-vulcanized rubber, silicone rubber, fluororubber, and urethane rubber.
[0014] The elastomer component may include a thermoplastic elastomer, specifically, an olefin-based thermoplastic elastomer (TPO), a styrene-based thermoplastic elastomer, an ester-based thermoplastic elastomer, an amide-based thermoplastic elastomer, a vinyl chloride-based thermoplastic elastomer, or a combination thereof. TPO is a thermoplastic elastomer that consists of polyolefins such as polyethylene and polypropylene as hard segments and rubbers such as ethylene-propylene rubber and ethylene-propylene-diene rubber as soft segments. Styrene-based thermoplastic elastomers include block copolymers with polystyrene blocks as the hard segments, such as styrene-butadiene-styrene block copolymer (SBS), styrene-ethylene-styrene block copolymer (SES), styrene-ethylene-butylene-styrene block copolymer (SEBS), and styrene-ethylene-propylene-styrene block copolymer (SEPS).
[0015] The resin component in the matrix component may be a thermoplastic resin or a thermosetting resin, but is preferably a thermoplastic resin. Examples of the thermoplastic resin include polyolefin resins such as polypropylene resin, polyethylene resin, poly(1-)butene resin, and polypentene resin, polyester resins such as polyethylene terephthalate, polystyrene resin, acrylonitrile-butadiene-styrene (ABS) resin, ethylene-vinyl acetate copolymer resin (EVA), polycarbonate resin, polyphenylene ether resin, (meth)acrylic resin, polyamide resin, polyvinyl chloride resin (PVC), novolac resin, polyurethane resin, and polyisobutylene. From the viewpoint of fire resistance, the thermoplastic resin preferably contains at least one of a halogen atom and a structural unit derived from styrene or vinyl acetate. From such a viewpoint, among the thermoplastic resins, polyvinyl chloride resin (PVC) and ethylene-vinyl acetate copolymer resin (EVA) are preferred, and polyvinyl chloride resin (PVC) is more preferred.
[0016] Examples of polyvinyl chloride resins (PVC) include homopolymers of vinyl chloride monomers, copolymers of vinyl chloride monomers and monomers having unsaturated bonds copolymerizable with vinyl chloride monomers, and graft copolymers in which vinyl chloride monomers are graft-copolymerized onto polymers or copolymers other than vinyl chloride monomers. These may be used alone or in combination of two or more. In the present invention, chlorinated polyvinyl chloride resins, which are chlorinated polyvinyl chloride resins, are also included in the polyvinyl chloride resins. The degree of polymerization of the polyvinyl chloride resin is preferably from 500 to 2,000, more preferably from 800 to 1500. Within such a range, the fluidity of the resin component is increased, making it easier to adjust the expansion ratio to a desired range.
[0017] The ethylene-vinyl acetate copolymer resin (EVA) may be a non-crosslinked ethylene-vinyl acetate copolymer resin or a high-temperature crosslinked ethylene-vinyl acetate copolymer resin. In addition, the ethylene-vinyl acetate copolymer resin may be a modified ethylene-vinyl acetate resin such as a saponified ethylene-vinyl acetate copolymer or a hydrolyzed ethylene-vinyl acetate. The ethylene-vinyl acetate copolymer resin preferably has a vinyl acetate content of 5 to 90 mass %, more preferably 8 to 50 mass %, and even more preferably 12 to 35 mass %, as measured in accordance with JIS K 6730 "Testing methods for ethylene-vinyl acetate resins". The melt flow rate (MFR) of the ethylene-vinyl acetate copolymer resin at 190° C. is preferably 0.5 to 15 g / 10 min, and more preferably 1 to 8 g / 10 min. The melt flow rate of the ethylene-vinyl acetate copolymer at 190° C. is a value measured under a load of 2.16 kg in accordance with JIS K7210:1999.
[0018] The thermosetting resin is not particularly limited, but examples thereof include epoxy resins, polyurethane resins, phenolic resins, melamine resins, urea resins, unsaturated polyester resins, alkyd resins, and thermosetting polyimides. Among these, epoxy resins are preferred from the viewpoint of improving fire resistance.
[0019] The epoxy resin may be either an epoxy resin having an aromatic ring or an epoxy resin not having an aromatic ring, but from the viewpoint of enhancing non-flammability, an epoxy resin having an aromatic ring is preferable. The epoxy resin is obtained, for example, by reacting an epoxy compound having an epoxy group with a curing agent. Examples of epoxy compounds used to obtain the above-mentioned epoxy resin having an aromatic ring include bisphenol A type epoxy compounds, bisphenol F type epoxy compounds, biphenyl type epoxy compounds, naphthalene type epoxy compounds, phenol novolac type epoxy compounds, bisphenol A novolac type epoxy compounds, tetraphenolethane type epoxy compounds, tetraglycidyldiaminodiphenylmethane type epoxy compounds, aminophenol type epoxy compounds, aniline type epoxy compounds, xylylenediamine type epoxy compounds, etc. Among these, bisphenol A type epoxy compounds and bisphenol F type epoxy compounds are preferred.
[0020] The curing agent used may be of polyaddition type or catalyst type. Examples of polyaddition type curing agents include polyamines, acid anhydrides, polyphenols, and polymercaptans. Examples of catalyst type curing agents include tertiary amines, imidazoles, and Lewis acid complexes. The method for curing the epoxy compound is not particularly limited, and may be performed by a known method. The content of the curing agent is preferably within a range of 50 to 150 parts by mass relative to 100 parts by mass of the epoxy compound. When the content is 50 parts by mass or more, the epoxy compound is easily cured, and when the content is 150 parts by mass or less, an effect according to the amount of the curing agent is obtained.
[0021] As the matrix component, from the viewpoint of achieving both water resistance and fire resistance, at least one selected from chloroprene rubber, styrene butadiene rubber, butyl rubber, urethane rubber, and PVC is preferred among the above. Among these, from the viewpoint of fire resistance, at least one selected from chloroprene rubber, styrene butadiene rubber, and PVC is more preferred, and in particular, from the viewpoint of increasing the hardness of the expansion residue and increasing the expansion rate, at least one selected from chloroprene rubber and styrene butadiene rubber is even more preferred. The matrix component may be used alone or in combination of two or more kinds. When two or more kinds are used in combination, it is particularly preferable to use chloroprene rubber and styrene-butadiene rubber in combination. When styrene-butadiene rubber (SBR) and chloroprene rubber (CR) are used in combination, the content ratio (SBR / CR) of these is preferably 90 / 10 to 10 / 90 by mass, and more preferably 80 / 20 to 20 / 80.
[0022] The bound styrene content of the styrene butadiene rubber (SBR) used in the present invention is not particularly limited, but is, for example, 10 to 60 mass%, preferably 15 to 55 mass%, and more preferably 20 to 50 mass%. 1 It can be measured by H-NMR. The Mooney viscosity [ML(1+4)100° C.] of the styrene-butadiene rubber is not particularly limited, but is, for example, 30-150, preferably 35-70, and more preferably 40-60. The Mooney viscosity [ML(1+4)100° C.] of the chloroprene rubber (CR) is not particularly limited, but is, for example, 25-150, preferably 30-100, and more preferably 35-75. In this specification, the Mooney viscosity is a value measured in accordance with JIS K6300.
[0023] The content of the matrix component in the thermally expandable fireproof material is preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, even more preferably 45% by mass or more, and also preferably 70% by mass or less, more preferably 65% by mass or less, and even more preferably 60% by mass or less. When the content of the matrix resin is equal to or more than these lower limits, the expandable graphite and inorganic filler blended in the thermally expandable fireproof material are appropriately held by the matrix component, and it is easy to prevent them from falling off or eluting. In addition, the residual hardness after expansion can be increased. When the content of the matrix component is equal to or less than these upper limits, the content of the thermally expandable graphite and inorganic filler described later can be increased, and the fire resistance is easily improved.
[0024] <Plasticizer> The heat-expandable fireproof material of the present invention may contain a plasticizer. When the matrix contains a plasticizer, the matrix component becomes more fluid, and the heat-expandable fireproof material becomes more expandable. In addition, when a polyvinyl chloride resin is used as the matrix component, it is preferable to use a plasticizer in combination. By using a plasticizer in combination, moldability is improved.
[0025] The plasticizer is not particularly limited, but examples thereof include phthalate ester plasticizers such as di-2-ethylhexyl phthalate (DOP), dibutyl phthalate (DBP), diheptyl phthalate (DHP), and diisodecyl phthalate (DIDP), fatty acid ester plasticizers such as di-2-ethylhexyl adipate (DOA), diisobutyl adipate (DIBA), and dibutyl adipate (DBA), epoxidized ester plasticizers such as epoxidized soybean oil, adipic acid ester plasticizers such as adipic acid ester and adipic acid polyester, trimellitic acid ester plasticizers such as tri-2-ethylhexyl trimellitate (TOTM) and triisononyl trimellitate (TINTM), and process oils such as mineral oil. The plasticizers may be used alone or in combination of two or more.
[0026] When the heat-expandable fireproof material of the present invention contains a plasticizer, the content thereof is preferably 10 to 90 parts by mass, more preferably 20 to 80 parts by mass, relative to 100 parts by mass of the matrix component. When the content of the plasticizer is within the above range, the moldability of the heat-expandable fireproof material tends to be improved, and the molded body can be prevented from becoming too soft.
[0027] <Thermal expandable graphite> Thermally expandable graphite expands when heated, and is produced by treating powders of natural scaly graphite, pyrolytic graphite, kish graphite, etc. with an inorganic acid and a strong oxidizing agent to generate a graphite intercalation compound, which is a type of crystalline compound that maintains the layered structure of carbon. Examples of inorganic acids include concentrated sulfuric acid, nitric acid, and selenic acid. Examples of strong oxidizing agents include concentrated nitric acid, perchloric acid, perchlorates, permanganates, dichromates, and hydrogen peroxide. The thermally expandable graphite obtained by the acid treatment as described above may be further neutralized with a neutralizing agent such as ammonia, an aliphatic lower amine, an alkali metal compound, an alkaline earth metal compound, etc. Examples of the aliphatic lower amine include monomethylamine, dimethylamine, trimethylamine, ethylamine, propylamine, butylamine, etc. Examples of the alkali metal compound and the alkaline earth metal compound include hydroxides, oxides, carbonates, sulfates, organic acid salts, etc. of potassium, sodium, calcium, barium, magnesium, etc.
[0028] The content of thermally expandable graphite in the thermally expandable refractory material is preferably 15% by mass or more, more preferably 20% by mass or more, even more preferably 30% by mass or more, and preferably 60% by mass or less, more preferably 50% by mass or less, even more preferably 45% by mass or less, and even more preferably 40% by mass or less. If the content of thermally expandable graphite is equal to or more than these lower limits, it becomes easier to obtain an expansion suitable for preventing the passage of flames, and if it is equal to or less than these upper limits, the strength of the thermally expandable residue of the thermally expandable refractory material tends to be high, and the processability and moldability are also improved.
[0029] <Inorganic filler> The thermally expandable fireproof material of the present invention preferably contains an inorganic filler in addition to the matrix component and the thermally expandable graphite. The inorganic filler is an inorganic filler other than the thermally expandable graphite. When heated to form an expandable insulating layer, the inorganic filler increases the heat capacity and suppresses heat transfer, while acting as an aggregate to improve the strength of the thermally expandable residue and improve the fire resistance.
[0030] From the viewpoint of improving the moldability of the refractory material, it is preferable that the inorganic filler contains an inorganic filler A having a specific gravity of 2.5 or more. By including the inorganic filler A, the amount of matrix components per unit volume can be increased, which improves the brittleness of the refractory material and makes it easier to improve the moldability and the residual hardness after expansion. From this viewpoint, the specific gravity of the inorganic filler A is preferably 3 or more, more preferably 4 or more. For example, metal oxides and metal carbonates described later can be used as the inorganic filler A having a specific gravity of 2.5 or more. The inorganic filler A may be used alone or in combination. The content of the inorganic filler A based on the total amount of the inorganic fillers is preferably 50% by mass or more, more preferably 80% by mass or more, and even more preferably 100% by mass. As the inorganic filler, it is preferable to use the above-mentioned inorganic filler A having a specific gravity of 2.5 or more, but it is also possible to use an inorganic filler having a specific gravity of less than 2.5.
[0031] The inorganic filler that can be used in the present invention is not particularly limited, and examples thereof include metal oxides such as alumina, zinc oxide, titanium oxide, calcium oxide, magnesium oxide, iron oxide, tin oxide, antimony oxide, and ferrite; metal carbonates such as calcium carbonate, zinc carbonate, strontium carbonate, and barium carbonate; metal hydroxides such as calcium hydroxide, magnesium hydroxide, aluminum hydroxide, and hydrotalcite; calcium sulfate, gypsum fiber, calcium salts such as calcium silicate; silica, diatomaceous earth, dawsonite, barium sulfate, talc, clay, mica, montmorillonite, bentonite, activated clay, sepiolite, imogolite, sericite, glass fiber, glass beads, Examples of suitable inorganic fillers include silica-based balloons, aluminum nitride, boron nitride, silicon nitride, carbon black, graphite, carbon fibers, carbon balloons, various metal powders, potassium titanate, magnesium sulfate, lead zirconate titanate, aluminum borate, molybdenum sulfide, silicon carbide, stainless steel fibers, zinc borate, various magnetic powders, slag fibers, fly ash, metal phosphates such as sodium phosphate, potassium phosphate, magnesium phosphate, and aluminum phosphate, metal phosphite such as sodium phosphite, potassium phosphite, magnesium phosphite, and aluminum phosphite, ammonium polyphosphate, metal orthophosphate, metal metaphosphate, and metal tripolyphosphate. The inorganic fillers may be used alone or in combination of two or more.
[0032] Among these, from the viewpoint of improving water resistance, it is preferable to use a water-insoluble substance as the inorganic filler, and from the viewpoints of water resistance and fire resistance, metal oxides, metal carbonates, poorly water-soluble phosphorus compounds, etc. are preferable.
[0033] As a specific inorganic filler, at least one selected from iron oxide, zinc oxide, calcium carbonate, and aluminum phosphite is more preferable, one selected from iron oxide and calcium carbonate is further preferable, and it is also preferable to use iron oxide and calcium carbonate in combination. In addition, an embodiment in which the inorganic filler contains at least iron oxide is also preferred. By using iron oxide, even if the expansion ratio of the thermally expandable fireproof material is relatively large, the strength of the thermally expanded residue is easily maintained and the fire resistance is easily improved. When iron oxide is used, the amount used is preferably 15 mass % or more, more preferably 25 mass % or more, and even more preferably 40 mass % or more, based on the total amount of the inorganic filler. When iron oxide and calcium carbonate are used in combination, the mass ratio thereof (iron oxide / calcium carbonate) is preferably 10 / 90 to 90 / 10, and more preferably 20 / 80 to 80 / 20.
[0034] From the viewpoints of improving residual hardness and fire resistance, the content of the inorganic filler in the thermally expandable fireproof material is preferably 3 mass % or more, more preferably 8 mass % or more, and even more preferably 13 mass % or more, and is preferably 50 mass % or less, and more preferably 30 mass % or less.
[0035] The thermally expandable fireproof material of the present invention preferably contains thermally expandable graphite and an inorganic filler as described above, and the total content of the thermally expandable graphite and the inorganic filler in the thermally expandable fireproof material is preferably 35% by mass or more. When the total content of the thermally expandable graphite and the inorganic filler is 35% by mass or more, the expansion ratio of the thermally expandable fireproof material and the strength of the expansion residue are easily improved, and the fire resistance is improved. From the viewpoint of improving the fire resistance, the total content of the thermally expandable graphite and the inorganic filler is preferably 40% by mass or more, and from the viewpoint of increasing the blending amount of the matrix component to ensure the retention performance by the matrix component, it is preferably 80% by mass or less, more preferably 75% by mass or less, and even more preferably 70% by mass or less.
[0036] <Other ingredients> The thermally expandable fire-resistant material may contain an organic flame retardant. The thermally expandable fire-resistant material may also contain additives other than those mentioned above, such as a colorant and an antioxidant. Examples of organic flame retardants include bromine-containing flame retardants, nitrogen-containing flame retardants, phosphate compounds, etc. In this specification, organic salts consisting of organic and inorganic substances, such as ethylenediamine phosphate, are also considered to be organic flame retardants. Examples of bromine-containing flame retardants include hexabromobenzene, pentabromotoluene, hexabromobiphenyl, decabromobiphenyl, hexabromocyclodecane, decabromodiphenyl ether, octabromodiphenyl ether, hexabromodiphenyl ether, bis(pentabromophenoxy)ethane, ethylene-bis(tetrabromophthalimide), tetrabromobisphenol A, and the like.
[0037] Examples of the nitrogen-containing flame retardant include melamine derivatives such as melamine, butyl melamine, trimethylol melamine, hexamethylol melamine, hexamethoxymethyl melamine, and melamine phosphate; cyanuric acid derivatives such as cyanuric acid, methyl cyanurate, diethyl cyanurate, trimethyl cyanurate, and triethyl cyanurate; isocyanuric acid derivatives such as isocyanuric acid, methyl isocyanurate, N,N'-diethyl isocyanurate, trismethyl isocyanurate, trisethyl isocyanurate, bis(2-carboxyethyl)isocyanurate, 1,3,5-tris(2-carboxyethyl)isocyanurate, and tris(2,3-epoxypropyl)isocyanurate; melamine cyanurate, melamine isocyanurate, and ethylenediamine phosphate.
[0038] Examples of the phosphate ester compound include trimethyl phosphate, triethyl phosphate, tributyl phosphate, trioctyl phosphate, octyl diphenyl phosphate, tributoxyethyl phosphate, trichloroethyl phosphate, tris(2-chloropropyl)phosphate, tris(2,3-dichloropropyl)phosphate, tris(2,3-dibromopropyl)phosphate, tris(bromochloropropyl)phosphate, bis(2,3-dibromopropyl)-2,3-dichloropropyl phosphate, bis(chloropropyl)monoctyl phosphate, tris(2-ethylhexyl)phosphate, triphenyl phosphate, tricresyl phosphate (TCP), trixylenyl phosphate, cresyl diphenyl phosphate, and xylenyl diphenyl phosphate. The organic flame retardant may be used alone or in combination of two or more. Among the above-mentioned organic flame retardants, it is preferable to use melamine cyanurate. The content of the organic flame retardant in the thermally expandable fire-resistant material is, for example, 1 to 35 mass%, preferably 5 to 30 mass%, and more preferably 8 to 20 mass%.
[0039] <Phosphorus component> The heat-expandable fireproof material of the present invention preferably does not substantially contain phosphorus components. By substantially not containing phosphorus components, the water resistance of the heat-expandable fireproof material is easily improved, and the fireproof property is well maintained even when the material is used under high humidity or in an environment where the material comes into contact with water. Furthermore, by substantially not containing phosphorus components, the coloring of the fireproof equipment due to the eluted phosphorus components, which causes poor appearance, is prevented. In addition, the thermally expandable fireproof material being substantially free of phosphorus components means that the thermally expandable fireproof material contains nothing other than phosphorus atoms that are inevitably mixed in, and the phosphorus atom content in the thermally expandable fireproof material is, for example, less than 0.5 mass%, preferably less than 0.1 mass%, and even more preferably 0 mass%.
[0040] Therefore, although inorganic fillers, organic flame retardants, etc. are blended in the thermally expandable fireproof material, it is preferable not to use compounds containing phosphorus atoms in these. In particular, flame retardants containing phosphorus atoms other than poorly water-soluble phosphorus compounds, such as ammonium polyphosphate and ethylenediamine phosphate, are preferably not included in the thermally expandable fireproof material because they lower the water resistance. In addition, even if the thermally expandable fireproof material does not contain a phosphorus component, sufficient fire resistance can be obtained by appropriately adjusting the types of matrix components and inorganic fillers and increasing the amount of inorganic fillers.
[0041] The thermally expandable fireproof material of the present invention is preferably, but not limited to, in a sheet form. The thickness of the thermally expandable fireproof material is not particularly limited, but from the viewpoints of fire resistance and ease of handling, the thickness is preferably 0.2 to 10 mm, and more preferably 0.5 to 3.0 mm.
[0042] The thermally expandable fireproof material of the present invention maintains a high expansion ratio even after immersion in water for a long time. Specifically, the expansion ratio after immersion in water at 60° C. for one week is preferably 5 times or more, more preferably 10 times or more, even more preferably 20 times or more, and even more preferably 30 times or more, from the viewpoint of fire resistance and water resistance. In addition, the expansion ratio after immersion in water at 60° C. for one week is preferably 70 times or less, more preferably 60 times or less, even more preferably 55 times or less, and even more preferably 50 times or less, from the viewpoint of maintaining a certain residual hardness even after expansion and easily ensuring fire resistance. The expansion ratio is measured by the method described in the examples.
[0043] In addition, the thermally expandable fireproof material of the present invention can maintain a certain level of residual hardness when expanded after being immersed in water for a long period of time. Specifically, the residual hardness when expanded after being immersed in water at 60° C. for one week is preferably 0.15 kgf / cm from the viewpoints of fire resistance and water resistance. 2 More preferably, 0.20kgf / cm 2 More preferably, 0.27 kgf / cm 2 More preferably, 0.30 kgf / cm 2In addition, the residual hardness after immersion in water at 60° C. for one week is preferably 0.70 kgf / cm from the viewpoint of maintaining a constant expansion ratio and easily ensuring fire resistance. 2 More preferably, it is 0.60 kgf / cm or less. 2 More preferably, it is 0.55 kgf / cm or less. 2 The above-mentioned expansion ratio and residual hardness can be measured by the method described in the Examples.
[0044] The thermally expandable fireproof material of the present invention can be produced, for example, as follows. First, predetermined amounts of matrix components, thermally expandable graphite, and additives such as inorganic fillers, organic flame retardants, colorants, and antioxidants, which are blended as necessary, are kneaded in a kneading machine such as a kneading roll to obtain a fire-resistant resin composition. Next, the obtained fire-resistant resin composition is molded into a desired shape such as a sheet by a known molding method such as press molding, calendar molding, extrusion molding, etc., to obtain a thermally expandable fire-resistant material.
[0045] The heat-expandable fire-resistant material may be used alone, or may be used with other members attached as appropriate. For example, the heat-expandable fire-resistant material may be laminated with members other than the heat-expandable fire-resistant material, or a base material, a pressure-sensitive adhesive layer, etc. may be laminated on the heat-expandable fire-resistant material. The substrate may be provided on at least one surface of the thermally expandable fireproof material. The substrate may be a combustible material layer, or a quasi-noncombustible material layer or a noncombustible material layer. The thickness of the substrate is not particularly limited, but is, for example, 5 μm to 1 mm. Examples of materials used for the combustible material layer include one or more of cloth materials, paper materials, wood materials, and resin films. When the substrate is a quasi-noncombustible material layer or a noncombustible material layer, examples of the materials used include metals and inorganic materials, and more specifically, woven or nonwoven fabrics made of glass fibers, ceramic fibers, carbon fibers, and graphite fibers. Composite materials of these fibers and metals may also be used, and aluminum glass cloth is preferable. For example, the adhesive layer may be provided on the substrate, or may be formed directly on the surface of the thermally expandable fireproof material. The adhesive layer is a layer made of an adhesive, and examples of the adhesive include an acrylic adhesive, a urethane adhesive, and a rubber adhesive.
[0046] [Fire prevention equipment] The thermally expandable fireproof material of the present invention is used by being mounted in at least a part of a fire prevention facility. The fire prevention facility is installed in an opening of various buildings to prevent a fire from spreading through the opening. The fire prevention facility is a fire prevention facility that complies with Article 2, Paragraph 9-2 of the Building Standards Act. Examples of buildings include detached houses, apartment buildings, high-rise houses, skyscrapers, commercial facilities, and public facilities, with buildings and condominiums being preferred. In buildings such as buildings and condominiums, when replacing each part used in fire protection equipment, complicated steps such as assembling scaffolding are required, but in the present invention, by using a heat-expandable fireproof material with a low elution rate as described above, the heat-expandable fireproof material can be used for a long period of time, so that the frequency of recovery and replacement can be reduced. Furthermore, the low elution rate suppresses contamination due to elution, making it less likely that the fire protection equipment will have poor appearance.
[0047] In the present invention, the thermally expandable fireproof material is preferably mounted on the lower part of the fireproof equipment. Since the thermally expandable fireproof material of the present invention has a low elution rate, it can maintain good fire resistance for a long period of time even when it is mounted on the lower part of the fireproof equipment where moisture such as rainwater and condensation is likely to accumulate and is in contact with water for a long period of time or placed under high humidity.
[0048] In the present invention, the fire prevention equipment is preferably a fixture. The fixture includes a window, a paper screen, a door, a sliding door, a sliding door, and the like. Fig. 1 shows an embodiment in which the fixture is a window. As shown in Fig. 1, the fixture 10 includes a frame 12 that is attached to an opening of a building, for example, a frame-shaped frame 31 that is disposed on the inner periphery of the frame 12 and supported by the frame 12, and a surface material 30 that is attached to the inner periphery of the frame 31. In this embodiment, the bottom frame 13 of the frame body 12 and the bottom frame 33 of the frame body 31 constitute the lower part of the fire prevention equipment (door 10). Therefore, it is preferable that the thermally expandable fireproof material is mounted on the bottom frame 13, the bottom frame 33, or both. The thermally expandable fireproof material may be attached directly to the bottom frame 13 or the bottom frame 33, or may be attached to the bottom frame 13 or the bottom frame 33 via a member (for example, a mounting member, a protruding piece, a reinforcing material, etc., described later) attached to the bottom frame 13 or the bottom frame 33.
[0049] A drainage path is provided in the fire prevention equipment (fitting 10), preferably in the lower part of the fire prevention equipment, specifically in the sill 13, the sill 33, or both. Water adheres to fire prevention equipment such as fitting 10 due to rainwater, condensation, etc., and accumulates in the lower part of fitting 10, so by providing a drainage path, the water adhering to fitting 10 can be drained to the outside. The drainage path may include a drainage hole, preferably provided in the lower part of the fire prevention equipment, specifically in the sill 13, the sill 33, or both. Water tends to accumulate on the upper surfaces of the sill 13 and the sill 33, but providing a drainage hole makes it easier to prevent water from accumulating in the fitting 10.
[0050] In addition, the heat-expandable fireproof material of the present invention is preferably arranged so as to block the drainage path, particularly the drainage hole, provided at the bottom of the fire prevention equipment (fitting 10) when it expands thermally due to heating such as a fire. Therefore, the heat-expandable fireproof material is preferably arranged close to the drainage path, particularly the drainage hole. Note that, before thermal expansion, the heat-expandable fireproof material is arranged close to the drainage path, preferably the drainage hole, but not to block them. The drainage path, especially the drainage hole, is a portion that ventilates the inside and outside of the fire protection equipment, and therefore may become a passageway for flames when a fire occurs, which may cause the fire to spread. Therefore, when the heat-expandable fireproof material blocks the drainage path, especially the drainage hole, by thermal expansion, the fire spread through the drainage path can be prevented. On the other hand, the heat-expandable fireproof material has a leaching rate of a predetermined value or less when immersed in water at 60°C for 1000 hours, and is excellent in water resistance. Therefore, when the heat-expandable fireproof material is placed close to the drainage path, especially the drainage hole, it comes into contact with water and is placed in a high humidity environment, but it can maintain high fire resistance for a long period of time even in such an environment. In addition, because of its excellent water resistance, the components that constitute the heat-expandable fireproof material, such as phosphorus compounds, do not dissolve, and the appearance of the fire protection equipment can be prevented from being deteriorated.
[0051] The position of the thermally expandable fire-resistant material at the bottom of the fitting 10 will be described in more detail below with reference to Figs. 2 to 6. Fig. 2 shows the fitting according to the first embodiment. The fitting according to the first embodiment is a fitting in which a drain hole is provided in the bottom frame 33, and the thermally expandable fire-resistant material is placed in a position close to the drain hole. The first embodiment is an example in which a window is used as the facing material.
[0052] The lower frame 33 is composed of a frame-shaped member and is supported by the lower frame 13. The lower frame 33 has both outdoor side and indoor side walls 33A, 33B, and an upper surface portion 33C and a lower surface portion 33D that connect the both side walls 33A, 33B. The panel 30 is placed on the upper surface portion 33C. The lower surface portion 33D is disposed below the upper surface portion 33C, and together with the both side walls 33A, 33B and the upper surface portion 33C, forms a rectangular hollow portion 33E, which provides the lower frame 33 with a certain level of strength. A block-shaped mounting member 34 is provided on the upper surface portion 33C, and the face material 30 is placed on the mounting member 34. The face material 30 placed on the mounting member 34 is sealed between the lower frame 33 and the lower frame 33 by a sealing member 35 on the mounting member 34. The face material 30 is supported by the lower frame 33 via the sealing member 35.
[0053] The upper surface portion 33C is provided with a drainage hole 36A. The drainage hole 36A constitutes a part of a drainage path that drains water accumulated on the upper surface portion 33C. Similarly, the lower surface portion 33D is provided with a drainage hole 36B. The drainage hole 36B of the lower surface portion 33D is arranged at a position that coincides with the drainage hole 36A of the upper surface portion 33C, and water discharged from the drainage hole 36A can be discharged to the outside of the fixture through the drainage hole 36B. As a result, the drainage hole 36B constitutes a part of the drainage path. The drainage hole 36B of the lower surface portion 33D may also drain water accumulated on the lower surface portion 33D.
[0054] A recess 34A is provided on the lower surface of the mounting member 34 disposed on the upper surface portion 33C, and the recess 34A is disposed so as to cover the drainage hole 36A. A thermally expandable fire-resistant material 40A is disposed inside the recess 34A. The thermally expandable fire-resistant material 40 may be fitted into the recess 34A and disposed inside the recess 34A, or may be attached to the bottom surface of the recess 34A by an adhesive layer or the like. With the above configuration, the heat-expandable fire-resistant material 40A is disposed in the vicinity of the drainage hole 36A. Therefore, when the heat-expandable fire-resistant material 40A is heated and thermally expanded, it is possible to block the drainage hole 36A, and in the event of a fire, it is possible to prevent the flame from passing through the drainage path and spreading. In addition, as described above, the heat-expandable fire-resistant material 40A has a low elution rate when immersed in water and is excellent in water resistance. Therefore, the heat-expandable fire-resistant material 40A is provided in the vicinity of the drainage path, comes into contact with water, and is placed in a high humidity environment, but can maintain high fire resistance for a long period of time even in such an environment. In addition, because of its excellent water resistance, the components constituting the heat-expandable fire-resistant material, such as phosphorus compounds, do not dissolve, and it is possible to prevent the appearance of the fire protection equipment from being deteriorated.
[0055] In the first embodiment, the heat-expandable fireproof material is attached to the mounting member, but the heat-expandable fireproof material does not need to be attached to the mounting member and may be attached to another member. Figure 3 shows one aspect of a fitting in which the heat-expandable fireproof material is attached to a member other than the mounting member as the second embodiment. Hereinafter, only the differences between the first embodiment and the second embodiment will be described, and the parts that will not be described are the same as the first embodiment.
[0056] In the second embodiment, a protrusion 34F is provided around the drainage hole 36B on the lower surface 33D of the lower frame 33, and a thermally expandable fireproof material 40B is attached to the protrusion 34F. The protrusion 34F may be provided integrally with the lower frame 33 or may be provided as a separate member. In this embodiment, the heat-expandable fire-resistant material 40B is also disposed in the vicinity of the drain hole 36B. Therefore, when the heat-expandable fire-resistant material 40B is heated and expands, it can block the drain hole 36B, and in the event of a fire, it is possible to prevent the flame from passing through the drain path and spreading. Furthermore, although the heat-expandable fire-resistant material 40B is placed in a high humidity environment in contact with water, the elution rate is below a predetermined value and the material has excellent water resistance, so that the material can maintain high fire resistance for a long period of time and does not cause poor appearance.
[0057] 4 shows a fitting according to a third embodiment. Hereinafter, only the differences between the first embodiment and the third embodiment will be described. In the third embodiment, the thermally expandable fireproof material 40C is attached to the side wall 33A of the lower frame 33. In this embodiment, the heat-expandable fire-resistant material 40C may be attached to the side wall 33A via an adhesive layer or the like. However, the heat-expandable fire-resistant material 40C does not need to be attached via an adhesive layer, and may be, for example, provided with a locking piece (not shown) on the lower surface portion 33D or the upper surface portion 33C, and the heat-expandable fire-resistant material 40C may be disposed between the locking piece and the side wall 33A and locked by the locking piece.
[0058] In this embodiment, the heat-expandable fire-resistant material 40C is also disposed in the vicinity of the drain hole 36B. Therefore, when the heat-expandable fire-resistant material 40C is heated and thermally expanded, it can block the drain hole 36B, and in the event of a fire, it is possible to prevent the flame from passing through the drain path and spreading. Furthermore, although the heat-expandable fire-resistant material 40C is placed in a high humidity environment in contact with water, the elution rate is below a predetermined value and the material has excellent water resistance, so that the material can maintain high fire resistance for a long period of time and does not cause poor appearance.
[0059] In the case where drainage holes are provided in the bottom frame 33 as in the above-mentioned embodiments, the heat-expandable fire-resistant material can be arranged in various positions without being limited to the configurations of the above-mentioned embodiments, as long as it can block one of the drainage holes in the bottom frame 33 when heated and expanded. For example, the heat-expandable fire-resistant material may be arranged on the upper surface portion 33C, the lower surface portion 33D, etc., or in other positions. Furthermore, in each of the above embodiments, the lower surface portion 33D is provided on the frame 33, but the lower surface portion 33D may be omitted. In that case, the thermally expandable fireproof material may be disposed in a position where it blocks the drainage hole 36A of the upper surface portion 33C when it expands due to heating. Also, the mounting member 34 and the sealing material 35 may be omitted, and the surface material may be attached to the frame by a different configuration. In addition, in each of the above embodiments, a configuration has been shown in which one of the multiple drainage holes is blocked by a heat-expandable fire-resistant material that expands when heated, but the multiple drainage holes that constitute the drainage path may be blocked by one or more heat-expandable fire-resistant materials that expand when heated.
[0060] In each of the above embodiments, the drainage hole is provided in the sill, but the drainage hole may be provided in the sill. Fig. 5 shows a fourth embodiment of the fitting in which the drainage hole is provided in the sill and the heat-expandable fireproof material is disposed in a position close to the drainage hole of the sill. This embodiment is an example in which a sliding window is used as the surface material.
[0061] In this embodiment, the lower frame 13 is provided with a rail 23, and the lower frame 33 is supported by the lower frame 13 via the rail 23. A surface material is attached to the inner periphery of the lower frame 33. The lower frame 13 is provided with a first lower frame member 13A on the outdoor side and a second lower frame member 13B on the indoor side, and each frame member 13A, 13B is provided with a first and a second rail 23A, 23B. The first lower frame 33A and the second lower frame (not shown) constituting the lower frame 33 are supported by the first lower frame member 13A and the second lower frame member 13B via the first and the second rail 23A, 23B, respectively. The first surface material 30A and the second surface material (not shown) are attached to the inner periphery of the first lower frame 33A and the second lower frame (not shown), respectively.
[0062] The first lower frame member 13A is formed in a frame shape by an exterior side wall 14A, an interior side wall 14B, an upper surface portion 14C, and a lower surface portion 14D, and has a hollow portion 14E formed therein. The first lower frame member 13A, specifically, the exterior side wall 14A and the upper surface portion 14C are provided with drainage holes 16A and 16B, respectively. In addition, protrusions 15A and 15B are provided around the drainage holes 16A and 16B, and thermally expandable fireproof materials 40D and 40E are attached to the protrusions 15A and 15B. The protrusions 15A are provided, for example, on the side wall 14A, and the protrusions 15B are provided on the upper surface portion 14C. The protrusions 15A and 15B may be provided integrally with the lower frame material 13A or may be provided as separate members.
[0063] In this embodiment, even if water accumulates on the upper surface of the lower frame 13 (first lower frame material 13A), the water is drained to the outside of the fitting 10 through the drain hole 16B, the inside of the hollow portion 14E, and the drain hole 16A. In addition, in this embodiment, the thermally expandable fire-resistant materials 40D and 40E are arranged in positions close to the drain holes 16A and 16B, respectively. Therefore, when the thermally expandable fire-resistant materials 40D and 40E are heated and thermally expanded, they can block the drain holes 16A and 16B, and when a fire occurs, it is possible to prevent the flame from passing through the drainage path and spreading. Furthermore, although the thermally expandable fire-resistant materials 40D and 40E are in contact with water and placed in a high humidity environment, the elution rate is below a predetermined value and they have excellent water resistance, so they can maintain high fire resistance for a long period of time and do not cause poor appearance.
[0064] 6 illustrates another embodiment in which drainage holes are provided in the lower frame as the fifth embodiment. The fifth embodiment will be described below with a focus on the differences from the fourth embodiment, and the parts that are not described are the same as the fourth embodiment. In the fifth embodiment, drainage holes are provided in the sill and the reinforcing material inserted inside the sill, and the heat-expandable fireproof material is disposed in a position close to the drainage hole of the reinforcing material. Note that the fifth embodiment is an example in which a sliding window is used as the surface material.
[0065] In this embodiment, rails 23 (first and second rails 23A, 23B) are provided on the lower frame 13, and the lower frame 33 (first and second lower frames 33A, 33B) are supported on the lower frame 13 via each rail. Panel materials 30A, 30B that form the window are attached to the inner periphery of each of the lower frames 33A, 33B. In this embodiment, the lower frame 13 is made of a frame material 13X, and the first and second rails 23A, 23B are provided on the frame material 13X.
[0066] The frame material 13X is formed in a frame shape with a hollow portion 14E formed therein, and drainage holes 16A, 16B are provided in the side wall 14A and the top surface portion 14C on the exterior side, respectively. A reinforcing material 18 is inserted into the hollow portion 14E, and drainage holes 16C, 16D are also provided in the reinforcing material 18. In this embodiment, the thermal expansion-compensating fireproof material 40F is attached to the reinforcing material 18, and thus the thermal expansion-compensating fireproof material 40F is disposed in a position close to the drainage hole 16C of the reinforcing material.
[0067] In this embodiment, even if water accumulates on the upper surface of the frame material 13X, the water is drained to the outside of the fitting through the drain holes 16B, 16D, 16C, and 16A (i.e., the drain path). Also in this embodiment, the heat-expandable fire-resistant material 40F is disposed in a position close to the drain hole 16C that constitutes a part of the drain path. Therefore, when the heat-expandable fire-resistant material 40F is heated and thermally expanded, it is possible to block the drain hole 16C, and in the event of a fire, it is possible to prevent the flame from passing through the drain path and spreading. Furthermore, since the heat-expandable fire-resistant material 40F is disposed in a high humidity environment in contact with water, the elution rate is below a predetermined value and the material has excellent water resistance, so that the material can maintain high fire resistance for a long period of time and does not cause poor appearance.
[0068] In the fourth and fifth embodiments described above, the heat-expandable fire-resistant material is shown attached to a protrusion or reinforcing material provided on the bottom frame 13, but it may be arranged in another position as long as it is positioned to block the drainage hole when heated and thermally expanded.For example, it may be attached to the frame material itself that constitutes the bottom frame, or it may be attached to a member other than the reinforcing material or protrusion provided on the bottom frame. In the fourth embodiment, a heat-expandable fire-resistant material is provided adjacent to each of the drainage holes constituting the drainage path, while in the fifth embodiment, one heat-expandable fire-resistant material is provided adjacent to one drainage hole, but in the fourth embodiment, one heat-expandable fire-resistant material may be provided adjacent to one drainage hole. In the fifth embodiment, a heat-expandable fire-resistant material may be provided adjacent to each of the drainage holes.
[0069] In each of the above embodiments, the heat-expandable fireproof material is disposed in the vicinity of the drainage hole and blocks the drainage hole when thermally expanded, but it may block other than the drainage hole as long as it blocks the drainage path when thermally expanded. For example, in the first to third embodiments, the space between both side walls 33A and 33B may form part of the drainage path on the upper surface of the upper surface portion 33C or the lower surface portion 33D of the lower frame 33. In such a case, for example, the heat-expandable fireproof material may be provided on the inner surface of the side wall of the lower frame 33, and the heat-expanded heat-expandable fireproof material may block the space between both side walls on the upper surface of the upper surface portion 33C or the lower surface portion 33D. EXAMPLES
[0070] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these.
[0071] [Evaluation method] (1) Elution rate A sample weight of 10 g (two pieces in this embodiment and comparative example) of the test piece made from the obtained thermally expandable fireproof material was immersed in 200 g of pure water, and after immersion for 1000 hours in a sealed container at 60° C., the sample was taken out, the pure water in which the sample was immersed was evaporated and dried at 60° C. for 96 hours, and the mass of the precipitate that was generated was measured. The elution rate was calculated using the following formula and used as an index of water resistance. Dissolution rate (%) = [(mass of precipitate) / (mass of thermally expandable refractory material before immersion in pure water)] × 100 (2) Expansion ratio A test piece (length: 100 mm, width: 100 mm, thickness: thickness of the thermally expandable fireproof material) made from the obtained thermally expandable fireproof material was immersed in 500 mL of pure water in a sealed container at 60 ° C for one week, and then the sample was taken out. The sample was evaporated and dried at 60 ° C for 96 hours to prepare a test piece, which was placed on the bottom of a stainless steel holder (101 mm square, height 80 mm), fed into an electric furnace, and heated at 600 ° C for 30 minutes. Thereafter, the thickness of the highest part of the test piece was measured, and the expansion ratio was calculated by ((thickness of the test piece after heating) / (thickness of the test piece before heating)).
[0072] (3) Residual hardness The heated test piece after measuring the expansion ratio was fed into a compression tester (Kato Tech Co., Ltd., "Finger Feeling Tester") and compressed at a speed of 0.1 cm / sec with a three-point indenter with a diameter of 1 mm. The maximum stress up to 10 mm compression from the top surface of the residue was measured, and the compressive strength (kgf / cm) of the test piece after combustion was calculated. 2 ) was measured.
[0073] (Examples 1 to 10, Comparative Examples 1 to 3) A matrix component, a plasticizer, a thermally expandable graphite, an inorganic filler, and an organic flame retardant were put into a roll and kneaded at 150°C for 5 minutes according to the composition shown in Table 1 below to obtain a fire-resistant resin composition. The obtained fire-resistant resin composition was press-molded at 150°C for 3 minutes to obtain a heat-expandable fire-resistant material having a thickness of 1.5 mm. The components used in each of the examples and comparative examples are as follows.
[0074] (1) Matrix components CR Tosoh Corporation "Y-20E", chloroprene rubber Mooney viscosity [ML(1+4)100℃]: 43~53 SBR "JSR1500" manufactured by JSR Corporation, styrene butadiene rubber Bound styrene content: 23.5% by mass, Mooney viscosity [ML(1+4)100℃]: 52 PVC Shin-Etsu Chemical Co., Ltd. "TK-1000", average polymerization degree 1030, polyvinyl chloride resin (2) Plasticizers DOP Di-2-ethylhexyl phthalate, "DOP" manufactured by JPlus Corporation (3) Thermally expandable graphite Thermally expandable graphite: Air Water "CA-60N" (4) Inorganic filler Iron oxide: Titanium Industries Co., Ltd. "BL-100", specific gravity 5.1 Zinc oxide: Sakai Chemical Industry Co., Ltd., product name "Zinc oxide type 1", specific gravity 5.7 Calcium carbonate: Bihoku Powder Industry Co., Ltd. "Whiten BF-300", specific gravity 2.93 Aluminum hydroxide: Hayashi Kasei Co., Ltd. "C-305", specific gravity 2.42 Aluminum phosphite: Taihei Chemical Industry Co., Ltd. "APA100" Ammonium polyphosphate: Clariant "AP422" (5) Organic flame retardants Melamine cyanurate: Nissan Chemical Industries, Ltd. "MC-4000" ·EDAP (Ethylenediamine phosphate) Albright & Wilson "Amgard EDAP"
[0075] [Table 1]
[0076] The thermally expandable fireproof materials of the Examples had low elution rates when immersed in water at 60° C. for 1000 hours, and maintained a constant level of expansion ratio and residual hardness even after immersion in water. Therefore, even when installed in fire protection equipment, especially in the lower part of fire protection equipment that is likely to come into contact with water or become highly humid, they can maintain good fire resistance for a long period of time. On the other hand, the thermally expandable fireproof materials of each comparative example have a high elution rate when immersed in water at 60°C for 1000 hours. Therefore, when the materials are installed in a fireproof equipment, especially in the lower part of the fireproof equipment that is likely to come into contact with water or become highly humid, it is difficult to maintain good fireproof performance for a long period of time. Furthermore, because the elution rate is high, phosphorus components and the like may elute and discolor the fireproof equipment, damaging the appearance of the fireproof equipment. [Explanation of symbols]
[0077] 10. Fittings (fire prevention equipment) 12 Frame 13 Bottom frame 18 Reinforcement 23 Rail 30 Surface material 31 Frame 33 Lower stile 34 Mounting member 35 Sealing material 16A~16D, 36A, 36B drainage hole 40A~40F Thermal expandable fireproof material
Claims
1. Contains a matrix component (excluding polyvinyl chloride resin and chlorinated polyvinyl resin), thermally expandable graphite, and an inorganic filler, A thermally expandable fire-resistant material for fire protection equipment that has a dissolution rate of 3% or less when immersed in water at 60°C for 1,000 hours.
2. 2. The thermally expandable fire-resistant material for fire prevention equipment according to claim 1, wherein the matrix component contains at least one selected from the group consisting of chloroprene rubber, styrene-butadiene rubber, butyl rubber, and urethane rubber.
3. 3. The thermally expandable fireproof material for fire prevention equipment according to claim 1 or 2, which is substantially free of phosphorus components.
4. The thermally expandable fireproof material for fire prevention equipment according to any one of claims 1 to 3, wherein the content of the thermally expandable graphite is 15 to 60 mass%.
5. The thermally expandable fireproof material for fire prevention equipment according to any one of claims 1 to 4, wherein the content of the inorganic filler is 3 to 50 mass%.
6. The inorganic filler contains at least one selected from the group consisting of metal oxides, metal carbonates, metal hydroxides, and metal phosphites. The thermally expandable fireproof material for fire prevention equipment according to any one of claims 1 to 5.
Citation Information
Patent Citations
Work execution method of fire-preventive and fire- resistive exterior wall constitutive body
JP2001073480A
Fire-resistant resin composition and fire-resistant resin molding
JP2018100408A
Thermoplastic resin sheet
JP2020125395A
Fire-resistant resin composition and fire-resistant resin molded body
WO2018117075A1
Building materials
JP6701318B2