Resin composition

A resin composition with thermally expandable graphite having a lower expansion start temperature than resin decomposition ensures high expandability and residual hardness, addressing the challenge of achieving both properties in thermally expandable resins, suitable for fire-resistant applications.

JP2024161143AInactive Publication Date: 2024-11-15SEKISUI CHEMICAL CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2024146052
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2014-08-27
Filing Date
2024-08-27
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing thermally expandable resin compositions face challenges in achieving both high expansibility and high residual hardness, as high expandability often compromises the hardness of the residue after combustion.

Method used

The resin composition is formulated with thermally expandable graphite having an expansion start temperature lower than the decomposition start temperature of the resin component, ensuring high expandability and residual hardness by forming a hard heat-insulating layer that delays resin decomposition.

Benefits of technology

The composition allows for stable extrusion to form complex shapes and maintains high residual hardness and fire resistance, even after combustion, making it suitable for applications like door and window sashes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024161143000001_ABST
    Figure 2024161143000001_ABST
Patent Text Reader

Abstract

To provide a resin composition for extrusion molding that allows extrusion molding, and has both high expansibility and high residual hardness.SOLUTION: A resin composition contains resin component 100 pts.wt, thermally-expandable graphite 3-300 pts.wt, and inorganic filler 2-200 pts.wt. An expansion initiation temperature of the thermally-expandable graphite is lower than a decomposition initiation temperature of the resin component.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] (Cross-references to related fields) This application claims the benefit of priority from Japanese Patent Application No. 2014-172997, filed on August 27, 2014, the entirety of which is incorporated herein by reference. (Technical field) The present invention relates to a resin composition from which a fire-resistant molded article can be produced. [Background technology]

[0002] Synthetic resins are widely used as building materials because they have good moldability and can be mass-produced as uniform products, but because they melt or burn easily and generate gas and smoke, materials with low smoke emission and excellent fire resistance are required for fire safety. In particular, for door and window sashes, materials are required that are not only flame-resistant but also able to maintain their shape even if they do burn and prevent the flames from spreading to the outside (back side) of the door or window.

[0003] As a material that meets such requirements, Patent Documents 1 and 2 describe a chlorinated polyvinyl chloride resin composition that exhibits fire resistance and low smoke generation during combustion. This chlorinated polyvinyl chloride resin composition contains a chlorinated polyvinyl chloride resin, a phosphorus compound, neutralized thermally expandable graphite, and an inorganic filler, and relative to 100 parts by weight of the chlorinated polyvinyl chloride resin, the total amount of the phosphorus compound and neutralized thermally expandable graphite is 20 to 200 parts by weight, the inorganic filler is 30 to 500 parts by weight, and the weight ratio of neutralized thermally expandable graphite:phosphorus compound is 9:1 to 1:9.

[0004] Furthermore, Patent Document 3 describes a chlorinated polyvinyl chloride resin composition that can be stably extrusion molded for a long period of time into irregular molded articles with complex cross-sectional shapes, such as sashes. This chlorinated polyvinyl chloride resin composition contains 100 parts by weight of chlorinated polyvinyl chloride resin, 3 to 300 parts by weight of thermally expandable graphite, 3 to 300 parts by weight of an inorganic filler, and 20 to 200 parts by weight of a plasticizer, and does not contain any phosphorus compounds (except for phosphate ester plasticizers). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 9-227747 [Patent Document 2] Japanese Patent Application Publication No. 10-95887 [Patent Document 3] Patent No. 53522017 Summary of the Invention [Problem to be solved by the invention]

[0006] In general, in the case of a thermally expandable resin composition, if the expandability is high, the hardness of the residue after combustion of the resin composition is significantly reduced, and it has been thought to be difficult to achieve both, but the above-mentioned literature did not address this issue.

[0007] An object of the present invention is to provide a resin composition having both high expandability and high residual hardness. [Means for solving the problem]

[0008] As a result of intensive research by the present inventors to solve the above problems, it was unexpectedly discovered that when the expansion start temperature of the thermally expandable graphite is lower than the decomposition start temperature of the resin component, and further when the difference between the two is large, high expansion properties and high residue hardness after combustion can be obtained, and this led to the completion of the present invention. .

[0009] The present invention is as follows.

[0010] Item 1. A resin composition comprising 100 parts by weight of a resin component, 3 to 300 parts by weight of thermally expandable graphite, and 2 to 200 parts by weight of an inorganic filler, wherein the expansion start temperature of the thermally expandable graphite is lower than the decomposition start temperature of the resin component. Item 2. The resin composition according to item 1, wherein the expansion start temperature of the thermally expandable graphite is 15° C. or more lower than the decomposition start temperature of the resin component. Item 3. The resin composition according to item 1 or 2, wherein the thermally expandable graphite has an expansion start temperature of 200° C. or lower, and the resin component has a decomposition start temperature of higher than 200° C. Item 4. The resin composition according to any one of Items 1 to 3, wherein the resin component is a chlorinated polyvinyl chloride resin or a polyvinyl chloride resin, and the expansion onset temperature of the thermally expandable graphite is 215°C or lower, or the resin component is at least one selected from the group consisting of EVA (ethylene-vinyl acetate copolymer resin), EPDM, polybutene, and polybutadiene, and the expansion onset temperature of the thermally expandable graphite is 300°C or lower. Item 5. The resin composition according to any one of Items 1 to 4, which does not contain a phosphorus compound (excluding phosphate ester plasticizers). Item 6. A fire-resistant member comprising the resin composition according to any one of items 1 to 5. Item 7. A fixture equipped with the fire-resistant material described in item 6. Effect of the Invention

[0011] The resin composition of the present invention can be extrusion molded stably for a long period of time, and in particular can be extrusion molded into irregular molded articles having complex cross-sectional shapes such as sashes stably for a long period of time. The obtained molded articles have high expansibility and high residual hardness, and therefore have excellent fire resistance. [Brief description of the drawings]

[0012] [Figure 1] 1 is a schematic front view showing a fire-resistant window having a sash frame provided with an article molded from the resin composition of the present invention. [Diagram 2] 1 is a graph showing the relationship between the expansion ratio and residual hardness of each sample. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] As used herein, the singular forms (a, an, the) are intended to include both the singular and the plural unless otherwise expressly stated in the specification or clearly contradictory in context.

[0014] The resin composition of the present invention contains 100 parts by weight of a resin component, 3 to 300 parts by weight of thermally expandable graphite, and 2 to 200 parts by weight of an inorganic filler, and is characterized in that the expansion start temperature of the thermally expandable graphite is lower than the decomposition start temperature of the resin component.

[0015] The resin component used in the present invention may be a synthetic resin such as a thermoplastic resin or a thermosetting resin, or rubber.

[0016] Examples of thermoplastic resins include polyolefin resins such as polypropylene resin, polyethylene resin, poly(1-)butene resin, and polypentene resin, polystyrene resins, acrylonitrile-butadiene-styrene (ABS) resins, polycarbonate resins, polyphenylene ether resins, acrylic resins, polyamide resins, polyvinyl chloride resins, and polyisobutylene resin.

[0017] Examples of thermosetting resins include urethane resins, isocyanurate resins, epoxy resins, phenolic resins, urea resins, unsaturated polyester resins, alkyd resins, melamine resins, Examples of the resin include diallyl phthalate resin and silicone resin.

[0018] Examples of rubber include natural rubber, butyl rubber, silicone rubber, polychloroprene rubber, polybutadiene rubber, polyisoprene rubber, polyisobutylene rubber, styrene-butadiene rubber, butadiene-acrylonitrile rubber, nitrile rubber, and rubber resins such as ethylene-α-olefin copolymer rubbers, such as ethylene-propylene-diene copolymers.

[0019] These synthetic resins and / or rubbers can be used alone or in combination. In order to adjust the melt viscosity, flexibility, adhesion, etc. of the resin, a blend of two or more resins may be used as the base resin.

[0020] The resin component may be crosslinked or modified to the extent that the fire resistance is not impaired. When crosslinking or modifying the resin component, the resin component may be crosslinked or modified in advance, or may be crosslinked or modified during or after the blending of other components such as a phosphorus compound or an inorganic filler described below.

[0021] The crosslinking method is not particularly limited, and includes crosslinking methods that are commonly used for the above resin components, such as crosslinking methods using various crosslinking agents, peroxides, and crosslinking methods using electron beam irradiation.

[0022] In one embodiment, the resin component comprises a chlorinated vinyl chloride resin, and in another embodiment, the resin component comprises at least one selected from the group consisting of EPDM, polybutene, and polybutadiene.

[0023] Chlorinated polyvinyl chloride resin is a chlorinated vinyl chloride resin. If the chlorine content is low, heat resistance decreases, and if the chlorine content is high, melt extrusion molding becomes difficult, so the range of 60 to 72% by weight is preferable.

[0024] The vinyl chloride resin is not particularly limited and may be any conventionally known vinyl chloride resin, such as a vinyl chloride homopolymer; a copolymer of a vinyl chloride monomer and a monomer having an unsaturated bond copolymerizable with the vinyl chloride monomer; a graft copolymer in which vinyl chloride is graft-copolymerized onto a (co)polymer other than vinyl chloride, and the like. These may be used alone or in combination of two or more kinds.

[0025] The monomer having an unsaturated bond copolymerizable with vinyl chloride monomer is not particularly limited as long as it is copolymerizable with vinyl chloride monomer, and examples thereof include α-olefins such as ethylene, propylene, butylene, etc.; vinyl esters such as vinyl acetate, vinyl propionate, etc.; vinyl ethers such as butyl vinyl ether, cetyl vinyl ether, etc.; (meth)acrylic acid esters such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl acrylate, etc.; aromatic vinyls such as styrene, α-methylstyrene, etc.; N-substituted maleimides such as N-phenylmaleimide, N-cyclohexylmaleimide, etc., and the like. These may be used alone or in combination of two or more kinds.

[0026] The (co)polymer to be graft-copolymerized with vinyl chloride is not particularly limited as long as it is a polymer to be graft-copolymerized with vinyl chloride, and examples thereof include ethylene-vinyl acetate copolymer, ethylene-vinyl acetate-carbon monoxide copolymer, ethylene-ethyl acrylate copolymer, ethylene-butyl acrylate-carbon monoxide copolymer, ethylene-methyl methacrylate copolymer, ethylene-propylene copolymer, acrylonitrile-butadiene copolymer, polyurethane, chlorinated polyethylene, chlorinated polypropylene, and the like. These may be used alone or in combination of two or more kinds.

[0027] The average polymerization degree of the vinyl chloride resin is not particularly limited, but a smaller average polymerization degree leads to a decrease in the mechanical properties of the molded article, while a larger average polymerization degree leads to an increase in melt viscosity, making melt extrusion molding difficult. Therefore, a polymerization degree of 600 to 1,500 is preferable.

[0028] The EPDM used in the present invention includes, for example, a terpolymer of ethylene, propylene and a crosslinking diene monomer.

[0029] The crosslinking diene monomer used in EPDM is not particularly limited, and examples thereof include cyclic dienes such as 5-ethylidene-2-norbornene, 5-propylidene-5-norbornene, dicyclopentadiene, 5-vinyl-2-norbornene, 5-methylene-2-norbornene, 5-isopropylidene-2-norbornene, and norbornadiene; and linear non-conjugated dienes such as 1,4-hexadiene, 4-methyl-1,4-hexadiene, 5-methyl-1,4-hexadiene, 5-methyl-1,5-heptadiene, 6-methyl-1,5-heptadiene, and 6-methyl-1,7-octadiene.

[0030] EPDM has a Mooney viscosity (ML 1+4 100° C.) is preferably in the range of 4 to 100, and more preferably in the range of 20 to 75.

[0031] When the Mooney viscosity is 4 or more, the flexibility is excellent. When the Mooney viscosity is 100 or less, the composition can be prevented from becoming too hard.

[0032] The Mooney viscosity is a measure of the viscosity of EPDM measured using a Mooney viscometer.

[0033] The content of the crosslinking diene monomer in the EPDM is preferably in the range of 2.0% by weight to 20% by weight, and more preferably in the range of 5.0% by weight to 15% by weight.

[0034] If it is 2.0% by weight or more, cross-linking between molecules proceeds, resulting in excellent flexibility, while if it is 20% by weight or less, the weather resistance is excellent.

[0035] As the polybutadiene, a commercially available product can be appropriately selected and used. Examples of such polybutadiene include homopolymer type such as Kuraray LBR-305 (manufactured by Kuraray Co., Ltd.) and 1,2-bond type butadiene and 1,2-bond type butadiene such as Poly bd (manufactured by Idemitsu Kosan Co., Ltd.). copolymers of ethylene, 1,4-bonded butadiene, and 1,2-bonded butadiene, such as Kuraray L-SBR-820 (manufactured by Kuraray Co., Ltd.);

[0036] The polybutene preferably has a weight average molecular weight of 300 to 2,000 as measured by a method in accordance with ASTM D 2503.

[0037] If the weight average molecular weight is less than 300, the viscosity is low, so that the polybutene tends to bleed onto the surface of the molded article after molding, whereas if it exceeds 2000, the viscosity is high, so that extrusion molding tends to become difficult.

[0038] Examples of polybutenes used in the present invention include "100R" (weight average molecular weight: 940) and "300R" (weight average molecular weight: 1450) manufactured by Idemitsu Petrochemical Co., Ltd., "HV-100" (weight average molecular weight: 970) manufactured by Nippon Petrochemical Co., Ltd., and "H-100" (weight average molecular weight: 940) manufactured by AMOCO Corporation.

[0039] The resin component used in the present invention is a mixture of polybutene and polybutadiene with EPDM. Addition of at least one of them is preferred from the viewpoint of improving moldability.

[0040] The amount of at least one of the polybutene and polybutadiene added per 100 parts by weight of the resin component is preferably in the range of 1 to 30 parts by weight, and more preferably in the range of 3 to 25 parts by weight.

[0041] Thermally expandable graphite is a conventionally known substance, and is produced by treating powder of natural flaky graphite, pyrolytic graphite, kish graphite, or the like with an inorganic acid, such as concentrated sulfuric acid, nitric acid, or selenic acid, and a strong oxidizing agent, such as concentrated nitric acid, perchloric acid, a perchlorate, a permanganate, a dichromate, or hydrogen peroxide, to produce a graphite intercalation compound, which is a crystalline compound that maintains the layered structure of carbon.

[0042] The thermally expandable graphite may be obtained by treating the thermally expandable graphite with an acid and then neutralizing the same with ammonia, an aliphatic lower amine, an alkali metal compound, an alkaline earth metal compound, or the like.

[0043] Examples of the aliphatic lower amine include monomethylamine, dimethylamine, trimethylamine, ethylamine, propylamine, and butylamine. Examples of the alkali metal compounds and alkaline earth metal compounds include hydroxides, oxides, carbonates, sulfates, and organic acid salts of potassium, sodium, calcium, barium, magnesium, and the like. A specific example of such thermally expandable graphite is "CA-60S" manufactured by Nippon Kasei Kasei Co., Ltd.

[0044] If the particle size of the thermally expandable graphite is too fine, the degree of expansion of the graphite will be small and the foaming properties will decrease, while if it is too large, although there is an effect of increasing the degree of expansion, the dispersibility will be poor when kneaded with a resin, decreasing moldability, and the mechanical properties of the obtained extrusion molded article will decrease, so a particle size of 20 to 200 mesh is preferable.

[0045] The amount of thermally expandable graphite added is 3 to 300 parts by weight per 100 parts by weight of the resin component, because a smaller amount results in decreased fire resistance and foaming properties, while a larger amount makes extrusion molding difficult, deteriorates the surface properties of the obtained molded body, and decreases the mechanical properties.

[0046] The amount of thermally expandable graphite added is preferably within the range of 10 to 200 parts by weight per 100 parts by weight of the resin component.

[0047] The resin composition of the present invention has high expandability and high residual hardness after combustion because the expansion start temperature of the thermally expandable graphite is lower than the decomposition start temperature of the resin component. The decomposition start temperature of the resin component refers to the temperature at which the solid resin component decomposes and weight loss begins to be confirmed. Although it is not desired to be bound by theory as to the reason for this, when the resin composition is heated, if the expansion start temperature of the thermally expandable graphite is lower than the decomposition start temperature of the resin component, the expandable graphite starts to expand before the resin component decomposes, so that a hard insulating layer of the expandable graphite is formed, the decomposition of the resin component is delayed, and the resin component is arranged so as to fill the gaps in the insulating layer, so that it is considered that high expandability is ensured while maintaining high residual hardness.

[0048] For example, when the resin component is a chlorinated polyvinyl chloride resin or a polyvinyl chloride resin, the expansion onset temperature of the thermally expandable graphite is usually 215°C or lower, and when the resin component is at least one selected from the group consisting of EVA, EPDM, polybutene, and polybutadiene, the expansion onset temperature of the thermally expandable graphite is 300°C or lower.

[0049] In one embodiment, the expansion start temperature of the thermally expandable graphite is lower than the decomposition start temperature of the resin component by 15° C. or more. In another embodiment, the expansion start temperature of the thermally expandable graphite is lower than the decomposition start temperature of the resin component by 15° C. or more. In another embodiment, the expansion start temperature of the thermally expandable graphite is 200° C. or lower, and the decomposition start temperature of the resin component is higher than 200° C. In another embodiment, when the resin composition is heated at a temperature higher than the expansion start temperature of the thermally expandable graphite and the decomposition start temperature of the resin component for a period of time sufficient for the thermally expandable graphite to expand and the resin component to decompose, the expansion ratio of the resin composition after heating exceeds 10 and the residual hardness is 0.25 kgf / cm 2 More than When heated at 600°C for 30 minutes, the expansion ratio of the resin composition after heating exceeds 10 and the residual hardness is 0.25 kgf / cm 2 In a more preferred embodiment, the residual hardness is greater than is 0.3kgf / cm 2 More than 2kgf / cm 2In a more preferred embodiment, the residual hardness is 0.5 kgf / cm 2 More than 2kgf / cm 2 The expansion ratio is calculated as (thickness of test piece after heating) / (thickness of test piece before heating) of the test piece of the resin composition. The residual hardness is calculated by compressing the test piece after heating with a known compression tester and measuring the breaking stress. In this application, the test piece is compressed to 0.25 cm using a compression tester. 2 with an indenter of 0.1 cm / sec This refers to the material compressed at a given speed and the breaking stress measured.

[0050] The inorganic filler is not particularly limited as long as it is an inorganic filler that is generally used in producing polyvinyl chloride resin molded articles, and examples thereof include silica, diatomaceous earth, alumina, zinc oxide, titanium oxide, calcium oxide, magnesium oxide, iron oxide, tin oxide, antimony oxide, ferrites, calcium hydroxide, magnesium hydroxide, aluminum hydroxide, basic magnesium carbonate, calcium carbonate, magnesium carbonate, zinc carbonate, barium carbonate, dawnnite, hydrotalcite, calcium sulfate, barium sulfate, gypsum fiber, calcium silicate, talc, clay, myca, montmorillonite, bentonite, activated Examples of inorganic fillers include white clay, sepiolite, imogolite, sericite, glass fiber, glass beads, silica balloon, aluminum nitride, boron nitride, silicon nitride, carbon black, graphite, carbon fiber, carbon balloon, charcoal powder, various metal powders, potassium titanate, magnesium sulfate, lead zirconium titanate, aluminum borate, molybdenum sulfide, silicon carbide, stainless steel fiber, zinc borate, various magnetic powders, slag fiber, fly ash, dehydrated sludge, etc., and calcium carbonate and hydrated inorganic substances such as calcium hydroxide, magnesium hydroxide, and aluminum hydroxide, which dehydrate when heated and have a heat absorbing effect, are preferred. Antimony oxide is also preferred because it has the effect of improving flame retardancy. These inorganic fillers may be used alone or in combination of two or more.

[0051] The amount of inorganic filler added is 3 to 200 parts by weight per 100 parts by weight of the resin component, because a smaller amount results in a decrease in fire resistance, while a larger amount makes extrusion molding difficult, deteriorates the surface properties of the resulting molded body, and decreases the mechanical properties.

[0052] The amount of the inorganic filler added is preferably within a range of 10 to 150 parts by weight per 100 parts by weight of the resin component.

[0053] As described above, the resin composition of the present invention contains a resin component, thermally expandable graphite, and an inorganic filler, but since the inclusion of a phosphorus compound (excluding phosphate ester plasticizers) reduces extrusion moldability, it is preferable that the resin composition does not contain a phosphorus compound (excluding phosphate ester plasticizers). Note that the resin composition may contain a phosphate ester plasticizer, which is a plasticizer described later.

[0054] The phosphorus compounds which inhibit extrusion moldability are as follows:

[0055] Red phosphorus, various phosphoric acid esters such as triphenyl phosphate, tricresyl phosphate, trixylenyl phosphate, cresyl diphenyl phosphate, and xylenyl diphenyl phosphate; Metal phosphates such as sodium phosphate, potassium phosphate, and magnesium phosphate; Ammonium polyphosphates, Examples include a compound represented by the following chemical formula (1).

[0056] [ka]

[0057] In the formula, R1 and R3 each represent a hydrogen atom, a linear or branched alkyl group having 1 to 16 carbon atoms, or an aryl group having 6 to 16 carbon atoms. R 2 is a hydroxyl group, a linear or branched alkyl group having 1 to 16 carbon atoms, 6 linear or branched alkoxy group, aryl group having 6 to 16 carbon atoms, or aryloxy group having 6 to 16 carbon atoms.

[0058] Examples of the compound represented by the chemical formula (1) include methylphosphonic acid, dimethyl methylphosphonate, diethyl methylphosphonate, ethylphosphonic acid, propylphosphonic acid, butylphosphonic acid, 2-methylpropylphosphonic acid, t-butylphosphonic acid, 2,3-dimethyl-butylphosphonic acid, octylphosphonic acid, phenylphosphonic acid, dioctylphenylphosphonate, dimethylphosphinic acid, methylethylphosphinic acid, methylpropylphosphinic acid, diethylphosphinic acid, dioctylphosphinic acid, phenylphosphinic acid, diethylphenylphosphinic acid, diphenylphosphinic acid, and bis(4-methoxyphenyl)phosphinic acid.

[0059] The ammonium polyphosphates are not particularly limited, and examples thereof include ammonium polyphosphate, melamine-modified ammonium polyphosphate, and the like.

[0060] In the present invention, no phosphorus compounds that inhibit extrusion moldability are used.

[0061] The resin composition of the present invention may further include a plasticizer. In one embodiment, when the resin component is a vinyl chloride resin, the resin composition of the present invention includes a plasticizer.

[0062] The plasticizer is not particularly limited as long as it is a plasticizer generally used in producing polyvinyl chloride resin molded bodies, and examples thereof include phthalate ester plasticizers such as di-2-ethylhexyl phthalate (DOP), dibutyl phthalate (DBP), diheptyl phthalate (DHP), and diisodecyl phthalate (DIDP); fatty acid ester plasticizers such as di-2-ethylhexyl adipate (DOA), diisobutyl adipate (DIBA), and dibutyl adipate (DBA); epoxidized ester plasticizers such as epoxidized soybean oil; polyester plasticizers such as adipic acid esters and adipic acid polyesters; trimellitic acid ester plasticizers such as tri-2-ethylhexyl trimellitate (TOTM) and triisononyl trimellitate (TINTM); and phosphate ester plasticizers such as trimethyl phosphate (TMP) and triethyl phosphate (TEP). These may be used alone or in combination of two or more.

[0063] The amount of plasticizer added is 20 to 200 parts by weight per 100 parts by weight of the resin component, since a smaller amount results in a decrease in extrusion moldability, and a larger amount results in the obtained molded body being too soft.

[0064] To the resin composition of the present invention, as necessary, heat stabilizers other than phosphorus compounds, lubricants, processing aids, pyrolysis type foaming agents, antioxidants, antistatic agents, pigments, and the like that are generally used in thermoforming of vinyl chloride resin compositions may be added, provided that the physical properties of the resin composition are not impaired.

[0065] Examples of the heat stabilizer include lead heat stabilizers such as tribasic lead sulfate, tribasic lead sulfite, dibasic lead phosphite, lead stearate, and dibasic lead stearate; organotin heat stabilizers such as organotin mercapto, organotin malate, organotin laurate, and dibutyltin malate; and metal soap heat stabilizers such as zinc stearate and calcium stearate. These may be used alone or in combination of two or more.

[0066] Examples of lubricants include waxes such as polyethylene, paraffin, and montanic acid; various ester waxes; organic acids such as stearic acid and ricinoleic acid; organic alcohols such as stearyl alcohol; and amide compounds such as dimethylbisamide. These may be used alone or in combination of two or more.

[0067] Examples of processing aids include chlorinated polyethylene, methyl methacrylate-ethyl acrylate copolymers, and high molecular weight polymethyl methacrylate.

[0068] Examples of the thermal decomposition type foaming agent include azodicarbonamide (ADCA), dinitrosopentamethylenetetramine (DPT), p,p-oxybisbenzenesulfonylhydrazide (OBSH), azobisisobutyronitrile (AIBN), and the like.

[0069] The resin composition of the present invention can be melt-extruded at 130 to 170° C. in a single-screw extruder, twin-screw extruder, or other extruder according to a conventional method to obtain a long molded product. The resin composition of the present invention is used to impart fire resistance to building materials such as windows, paper screens, doors (i.e., doors), doors, sliding doors, and transoms; ships; and elevators. In particular, the resin composition of the present invention has excellent moldability, so that a long, irregular molded product having a complex cross-sectional shape can be easily obtained.

[0070] Therefore, the present invention also includes fireproof members, such as molded bodies, that are provided with the above-mentioned resin composition of the present invention, as well as fittings that are provided with such fireproof members. For example, Fig. 1 is a schematic diagram showing a sash frame of a window 1 as a fitting, to which a molded body 4 formed from the resin composition of the present invention is attached. In this example, the sash frame has two inner frames 2 and one outer frame 3 that surrounds the inner frame 2, and the molded body 4 is attached inside the inner frame 2 and the outer frame 3 along each side of the frame body of the inner frame 2 and the outer frame 3. In this way, by providing the molded body 4, fire resistance can be imparted to the window 1. EXAMPLES

[0071] The present invention will be described in detail below by way of examples with reference to the drawings, although the present invention is not limited to these examples in any way.

[0072] (Examples 1-2, Comparative Examples 1-2) The samples were prepared by mixing the specified amounts of chlorinated polyvinyl chloride resin ("HA-53F" manufactured by Tokuyama Sekisui Co., Ltd., polymerization degree 1000, chlorine content 64.0% by weight, decomposition temperature 230°C, hereinafter referred to as "CPVC") shown in Table 1, neutralized thermally expandable graphite, calcium carbonate ("Whiten BF300" manufactured by Shiraishi Calcium Co., Ltd.), antimony trioxide ("Patox C" manufactured by Nippon Seiko Co., Ltd.), diisodecyl phthalate ("DIDP" manufactured by J-Plus Co., Ltd., hereinafter referred to as "DIDP"), Ca-Zn composite stabilizer ("NT-231" manufactured by Mizusawa Chemical Co., Ltd.), calcium stearate ("SC-100" manufactured by Sakai Chemical Co., Ltd.), chlorinated polyethylene ("135A" manufactured by Weihai Jinhong Co., Ltd.), and polymethylmethacrylate (hereinafter referred to as "PTMC"), which were then mixed with the mixture. A compound consisting of acrylate (Mitsubishi Rayon Co., Ltd., "P-530A") was fed into a single-screw extruder (Ikegai Kihan Co., Ltd., 65 mm extruder) and extruded at 150°C for 2 hours at a speed of 1 m / hr to produce a long irregularly shaped molded product with an E-shaped cross-section (base width 100 mm, three side walls of 50 mm each hanging down from both ends and the center of the base, base thickness 3.0 mm, side wall thickness 2.0 mm).

[0073] Example 1 was the case where ADT Corporation's "ADT501" (expansion starting temperature 160°C) was used as the thermally expandable graphite, Example 2 was ADT Corporation's "ADT351" (expansion starting temperature 200°C), Comparative Example 1 was Tosoh Corporation's "GREP-EG" (expansion starting temperature 220°C), and Comparative Example 2 was Air Water Corporation's "MZ160" (expansion starting temperature 260°C).

[0074] (Moldability) In both Examples 1 and 2 and Comparative Examples 1 and 2, long irregular molded articles with beautiful surfaces could be extruded for 2 hours, and there was no adhesion of the compound to the screw or mold after 2 hours of extrusion molding, showing good moldability.

[0075] (Expansion ratio) A test piece (length 100 mm, width 100 mm, thickness 2.0 mm) made from the obtained molded body was fed into an electric furnace and heated at 600°C for 30 minutes. The thickness of the test piece was then measured and the expansion ratio was calculated as (thickness of test piece after heating) / (thickness of test piece before heating).

[0076] (residue hardness) The test piece after heating for measuring the expansion ratio was fed into a compression tester (Kato Tech Co., Ltd., "Finger Feeling Tester") and compressed to 0.25 cm 2 The specimen was compressed at a speed of 0.1 cm / sec with an indenter of , and the stress at break was measured.

[0077] The measurement results of the expansion ratio and residual hardness of the obtained molded body are shown in Figure 2. In Examples 1 and 2, in which the expansion start temperature of the thermally expandable graphite was lower than the decomposition start temperature of the resin component, a relatively high expansion ratio and high residual hardness were maintained, but in Comparative Examples 1 and 2, in which the expansion start temperature of the thermally expandable graphite was higher than the decomposition start temperature of the resin component, the residual hardness dropped sharply.

[0078] (Residue shape retention) The above residue hardness is an index of the hardness of the residue after expansion, but since the measurement is limited to the surface portion of the residue, it may not be an index of the hardness of the entire residue, so shape retention was measured as an index of the hardness of the entire residue. The shape retention of the residue was measured by lifting both ends of the test piece for which the expansion ratio was measured by hand and visually observing how easily the residue crumbled at that time. If the test piece could be lifted without crumbling, it was evaluated as PASS, and if the test piece collapsed and could not be lifted, it was evaluated as FAIL.

[0079] [Table 1]

[0080] (Examples 3 to 22) A mixture containing the components shown in Table 2 was fed to a single-screw extruder in the same manner as described above for Examples 1-2 and Comparative Examples 1-2, and extrusion molding was performed at 150°C for 2 hours at a speed of 1 m / hr to produce a long irregularly shaped product having an E-shaped cross-section.

[0081] As the resin component, CPVC was used in Examples 3 to 6, polyvinyl chloride resin (degree of polymerization 1000, decomposition onset temperature 215°C, referred to as "PVC") in Examples 7 to 10, ethylene-vinyl acetate copolymer resin (decomposition onset temperature 225°C, referred to as "EVA") in Examples 11 to 15, ethylene-propylene-diene rubber (decomposition onset temperature 230°C, referred to as "EPDM") in Examples 16 to 20, and epoxy resin (decomposition onset temperature 275°C, referred to as "epoxy") in Examples 21 and 22.

[0082] The ammonium polyphosphate was Clariant's "AP422," and the softener was Idemitsu Kosan's "Diana Process Oil PW-90."

[0083] (Moldability) In all of Examples 3 to 22, long irregular molded articles with beautiful surfaces could be extruded for 2 hours, and there was no adhesion of the blend to the screw or die after 2 hours of extrusion molding, showing good moldability.

[0084] (Expansion ratio) A test piece (length 100 mm, width 100 mm, thickness 2.0 mm) made from the obtained molded body was fed into an electric furnace and heated at 600°C for 30 minutes. The thickness of the test piece was then measured and the expansion ratio was calculated as (thickness of test piece after heating) / (thickness of test piece before heating).

[0085] (residue hardness) The test piece after heating for measuring the expansion ratio was fed into a compression tester (Kato Tech Co., Ltd., "Finger Feeling Tester") and compressed to 0.25 cm 2 The specimen was compressed at a speed of 0.1 cm / sec with an indenter of , and the stress at break was measured.

[0086] All of the molded articles of Examples 3 to 22 maintained a relatively high expansion ratio and high residual hardness, similar to Examples 1 and 2 (data not shown).

[0087] (Residue shape retention) The above residue hardness is an index of the hardness of the residue after expansion, but since the measurement is limited to the surface portion of the residue, it may not be an index of the hardness of the entire residue, so shape retention was measured as an index of the hardness of the entire residue. The shape retention of the residue was measured by lifting both ends of the test piece for which the expansion ratio was measured by hand and visually observing how easily the residue crumbled at that time. If the test piece could be lifted without crumbling, it was evaluated as PASS, and if the test piece collapsed and could not be lifted, it was evaluated as FAIL.

[0088] [Table 2]

Claims

1. A resin composition comprising 100 parts by weight of a resin component, 3 to 300 parts by weight of thermally expandable graphite, and 2 to 200 parts by weight of an inorganic filler, wherein the expansion initiation temperature of the thermally expandable graphite is lower than the decomposition initiation temperature of the resin component.

2. 2. The resin composition according to claim 1, wherein the expansion start temperature of the thermally expandable graphite is lower by 15° C. or more than the decomposition start temperature of the resin component.

3. 3. The resin composition according to claim 1, wherein the thermally expandable graphite has an expansion initiation temperature of 200°C or lower, and the resin component has a decomposition initiation temperature of higher than 200°C.

4. The resin component is a chlorinated polyvinyl chloride resin or a polyvinyl chloride resin, and the expansion start temperature of the thermally expandable graphite is 215° C. or less, or The resin composition according to any one of claims 1 to 3, wherein the resin component is at least one selected from the group consisting of EVA (ethylene-vinyl acetate copolymer resin), EPDM, polybutene, and polybutadiene, and the expansion initiation temperature of the thermally expandable graphite is 300°C or lower.

5. 5. The resin composition according to claim 1, which does not contain a phosphorus compound (excluding phosphate ester plasticizers).

6. A fire-resistant member comprising the resin composition according to any one of claims 1 to 5.

7. A fitting comprising the fire-resistant member according to claim 6.

Citation Information

Patent Citations

  • Piping materials for building, and its molding method

    JP2008180068A

  • Fire-preventive construction of resin sash

    JP2015098773A

  • Fire-resistant sheet-shaped molded article and sheet laminate

    JP3838780B2

  • Resin composition

    JP6243925B2

  • resin composition

    JP6375040B2