Solid cross-linked polyolefin composition for coating wire and cable

A crosslinked polymer blend of thermoplastic and moisture-curable polyolefins addresses the limitations of traditional insulation materials by improving processability and temperature resistance, suitable for high-speed extrusion and PoE applications.

JP2024161214AInactive Publication Date: 2024-11-15DOW GLOBAL TECHNOLOGIES LLC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024152221
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2018-12-27
Filing Date
2024-09-04
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing polyolefin compositions for wire and cable insulation face challenges in high-speed extrusion processes due to narrow molecular weight distribution, leading to melt fracture and reduced surface smoothness, while traditional thermoplastic materials struggle with high temperature limitations and compressive stress, limiting their use in Power over Ethernet (PoE) applications.

Method used

A crosslinked polymer composition comprising 4% to 45% thermoplastic polymer, 52% to 95% moisture-curable polyolefin, and 0.05% to 7% moisture condensation catalyst, which enhances melt strength, flexibility, and high-speed extrusion performance.

Benefits of technology

The composition achieves improved processability, surface smoothness, and high temperature resistance, enabling effective insulation for PoE category data cables with enhanced tensile strength and reduced creep properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024161214000001
    Figure 2024161214000001
  • Figure 2024161214000002
    Figure 2024161214000002
  • Figure 2024161214000003
    Figure 2024161214000003
Patent Text Reader

Abstract

To provide an excellent composition.SOLUTION: The disclosure provides a composition. In one embodiment, provided is a cross-linked polymer composition containing (A) 4-45 wt.% thermoplastic polymer, (B) 52-95 wt.% moisture curable polyolefin, and (C) 0.05-7 wt.% moisture condensation catalyst. The disclosure provides an article. In one embodiment, a coated conductor is provided which includes a conductor and a coating on the conductor. The coating includes the cross-linked polymer composition containing (A) 4-45 wt.% the thermoplastic polymer, (B) 52-95 wt.% the moisture curable polyolefin, and (C) 0.05-7 wt.% the moisture condensation catalyst.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] Improving the rheological or melt flow properties of polyolefin resins is important for wire and cable applications to meet the growing demand for improved processability for various cable constructions. The continuing trend for twisted pair category data cables requires increased use of low voltage signals to power devices over data cables (Power over Ethernet or PoE), resulting in higher cable operating temperatures. High temperatures can soften cable insulation, raising concerns about whether thermoplastic solid or foamed insulation can withstand compressive stresses over the decades-long life of a cable. For example, the temperature limitations of traditional thermoplastic materials limit PoE category data cable use to approximately 100 watts. Cross-linked solid (non-foamed) or foamed insulation may offer a better alternative for PoE category data cable applications.

[0002] Moisture-curable polyolefins provide the flexibility required for wire and cable insulation materials, but may have narrow molecular weight distributions (MWDs). Many moisture-curable polyolefins exhibit viscosity profiles that limit processability (e.g., onset of melt fracture) and exhibit reduced surface smoothness at extrusion line speeds above 300 meters per minute.

[0003] A need exists for moisture curable polyolefin compositions that have good processability (ie, little or no melt fracture) and suitable tensile strength, elongation, high temperature resistance, and high temperature creep properties suitable for wire and cable applications. Summary of the Invention

[0004] The inventors have discovered that higher melting point solid polymers (e.g., broad MWD high density polyethylene) can be blended with moisture curable polyolefins to produce crosslinked compositions that have high melt strength and high flexibility, and also exhibit good processability and surface smoothness in high speed extrusion applications.

[0005] The present disclosure provides a crosslinked polymer composition comprising: (A) 4% to 45% by weight of a thermoplastic polymer; (B) 52% to 95% by weight of a moisture-curable polyolefin; and (C) 0.05% to 7% by weight of a moisture condensation catalyst.

[0006] The present disclosure also provides a coated conductor comprising a conductor and a coating on the conductor, the coating comprising a crosslinked polymer composition comprising: (A) 4% to 45% by weight of a thermoplastic polymer, (B) 52% to 95% by weight of a moisture-curable polyolefin, and (C) 0.05% to 7% by weight of a moisture condensation catalyst.

[0007] definition For purposes of United States patent practice, the contents of any referenced patent, patent application, or publication are incorporated by reference in their entirety (or the equivalent United States version thereof is so incorporated by reference), particularly with respect to the disclosure of definitions (to the extent not inconsistent with any definitions specifically provided in this disclosure) and general knowledge in the art.

[0008] Numerical ranges disclosed herein include all values ​​from the lower limit to the upper limit, inclusive. For ranges including explicit values ​​(e.g., 1-7), any subrange between any two explicit values ​​is included (e.g., 1-2, 2-6, 5-7, 3-7, 5-6, etc.).

[0009] The terms "comprising," "including," "having," and their derivatives are not intended to exclude the presence of any additional components, steps, or procedures, whether specifically disclosed or not. For the avoidance of doubt, all compositions claimed through the use of the term "comprising" may include any additional additives, adjuvants, or compounds, whether polymeric or non-polymeric, unless stated to the contrary. In contrast, the term "consisting essentially of" excludes from the scope of any succeeding recitation any other component, step, or procedure, except those that are not essential to operability. The term "consisting of" excludes any component, step, or procedure not expressly delineated or listed. The term "or" refers to the recited members individually as well as in any combination, unless otherwise stated. The use of the singular includes the use of the plural, and vice versa.

[0010] Any references to the Periodic Table of the Elements are to that published in 1990-1991 by CRC Press, Inc. References to the Groups of the Elements in this Periodic Table are to the new notation for numbering the Groups.

[0011] Unless stated to the contrary, implicit from the context, or customary in the art, all parts and percentages are by weight and all testing methods are current as of the filing date of this disclosure.

[0012] "Ambient conditions" and like terms mean the temperature, pressure, and humidity of the area or environment surrounding an article. Ambient conditions in a typical office building or laboratory include a temperature of 23° C. and atmospheric pressure.

[0013] A "blend," "polymer blend," and similar terms, is a combination of two or more polymers. Such blends may or may not be miscible. Such combinations may or may not be phase separated. Such combinations may or may not contain one or more domain configurations as determined from transmission electron spectroscopy, light scattering, x-ray scattering, and any other method known in the art.

[0014] By "catalytic amount" is meant the amount of catalyst required to promote a reaction, such as, for example, the grafting of a silane compound to a polyolefin or the crosslinking of an ethylene-vinylsilane polymer, at a detectable level, preferably at a commercially acceptable level.

[0015] "Coating" and like terms mean applying one material (i.e., the material to be applied) to another material (i.e., the substrate) in any manner, such as by contacting, depositing, "salting out," precipitating, etc., such that the applied material and the substrate adhere to one another. "Coating" also refers to an applied material that has been contacted or deposited, etc., on a substrate. In the context of wire and cable, a coating is typically a polymer that is extruded over and in contact with a wire or previously coated wire or cable, such as a semiconducting layer, or an insulating layer, or an outer protective jacket.

[0016] "Composition" and like terms mean a mixture or blend of two or more components. For example, in the context of preparing a silane-grafted ethylene polymer, the composition would include at least one ethylene polymer, at least one vinyl silane, and at least one free radical initiator. In the context of preparing a cable sheath or other article of manufacture, the composition would include an ethylene-vinyl silane copolymer, a catalytic cure system, and any desired additives such as lubricants, fillers, antioxidants, and the like.

[0017] "Conductor" refers to one or more wires or fibers for simultaneously conducting power (electricity) and data (light). Conductors can be single-wire, single-fiber, multi-wire, or multi-fiber and can be in stranded or tubular form. Non-limiting examples of suitable conductors include optical fibers made from metals (e.g., silver, gold, copper, aluminum) and glass or plastic. Conductors can be used in local area networks (LAN) / data or fiber optic cables.

[0018] As used herein, "crosslink" refers to a covalent bond between two or more polymers that are otherwise structurally distinct chemical entities.

[0019] "Crosslinkable," "curable," and like terms refer to a polymer that contains additive(s) or functionality that causes or promotes substantial crosslinking when the polymer is subjected to or exposed to a treatment that induces substantial crosslinking (e.g., exposure to water), but that has not been cured or crosslinked and has not been subjected to or exposed to a treatment that induces substantial crosslinking. The polymer can be crosslinked either before or after it is formed into an article.

[0020] "Crosslinked," "cured," and like terms mean that the polymer has been subjected to or exposed to a process which induced crosslinking and has 90 weight percent or less extractable xylene or decalene (i.e., a gel content of 10 weight percent or more). The polymer can be crosslinked either before or after it is formed into an article. The phase of the process during which the crosslinks are being created is called the "curing phase," and the process of creating the crosslinks is called "curing."

[0021] An "ethylene-based polymer" is a polymer that contains greater than 50 weight percent polymerized ethylene monomer (based on the total amount of polymerizable monomers) and may optionally contain at least one comonomer. Ethylene-based polymers include ethylene homopolymers and ethylene copolymers (meaning units derived from ethylene and one or more comonomers). The terms "ethylene-based polymer" and "polyethylene" may be used interchangeably. Non-limiting examples of ethylene-based polymers (polyethylenes) include low density polyethylene (LDPE) and linear polyethylene. Non-limiting examples of linear polyethylenes include linear low density polyethylene (LLDPE), ultra low density polyethylene (ULDPE), very low density polyethylene (VLDPE), multicomponent ethylene-based copolymers (EPE), ethylene / α-olefin multiblock copolymers (also known as olefin block copolymers (OBC)), single-site catalyzed linear low density polyethylene (m-LLDPE), substantially linear or linear plastomers / elastomers, and high density polyethylene (HDPE). In general, polyethylene can be produced in gas phase, fluidized bed reactors, liquid phase slurry process reactors, or liquid phase solution process reactors using heterogeneous catalyst systems such as Ziegler-Natta catalysts, homogeneous catalyst systems including group 4 transition metals and ligand structures such as metallocenes, nonmetallocene metal centers, heteroaryls, heterovalent aryloxy ethers, phosphinimines, and others. A combination of heterogeneous and / or homogeneous catalysts can also be used in either a single reactor or dual reactor configuration. In one embodiment, the ethylene-based polymer does not contain an aromatic comonomer polymerized therein.

[0022] "Ethylenic" and like terms mean (i) containing ethylene or an ethylene derivative, or (ii) relating to or characteristic of ethylene (e.g., the ethylenic double bond).

[0023] "Foamed" and like terms refer to a solid or liquid that has many trapped gas bubbles. The trapped gas bubbles in the solid or liquid are typically produced through the use of a blowing agent.

[0024] "Grafting conditions" and like terms refer to the temperature, pressure, humidity, residence time, agitation, etc., under which the hydrolyzably unsaturated silane grafts, i.e., is added to or combined with, the polyolefin when the two are in contact with one another. Grafting conditions can vary depending on the nature of the silane and polyolefin, and the presence or absence of a catalyst.

[0025] "Interpolymer" and "copolymer" refer to polymers prepared by the polymerization of at least two different types of monomers. These collective terms include classical copolymers, i.e., polymers prepared from two different types of monomers, and polymers prepared from three or more different types of monomers, e.g., terpolymers, tetrapolymers, etc.

[0026] A "masterbatch" is a concentrated mixture of a polyolefin resin (e.g., low density polyethylene), compounds with different functional groups, and optionally additives. A masterbatch can be formed by melt blending the components of the mixture, followed by cooling and processing into granules.

[0027] "Melt blending" is a process in which at least two components are combined or otherwise mixed together, with at least one of the components being in a molten state. Melt blending may be accomplished by one or more of a variety of known processes, such as, for example, batch mixing, extrusion blending, extrusion molding, etc. A "melt blend" composition is a composition formed through the process of melt blending.

[0028] "Moisture-curable polymer" and similar terms refer to a polymer that can be crosslinked upon exposure to moisture. The amount or extent of crosslinking will depend, among other things, on (1) the curing conditions, such as temperature, amount and form of water (bath, mist, etc.), residence time, presence or absence of catalyst, and if present, type and amount of catalyst, etc., and (2) the moisture-curable polymer itself. In the context of polyolefin polymers that contain hydrolyzable silane groups, the silane groups are first hydrolyzed upon exposure to water, the hydrolyzable silane groups are converted to silanol groups, and alcohol is formed as a by-product. The silanol groups are then crosslinked by a condensation reaction. Typically, both the first and second steps are catalyzed with a condensation catalyst.

[0029] "Non-foamed" and similar terms refer to a solid or liquid that does not have a significant amount of trapped air bubbles. The non-foamed compositions of the present disclosure can be made in the absence of a blowing agent. If a blowing agent is present, the non-foamed compositions are made under conditions that render the blowing agent inactive. For purposes of this disclosure, the terms "non-foaming" and "solid" are used interchangeably.

[0030] An "olefin-based polymer" or "polyolefin" is a polymer that contains more than 50 weight percent polymerized olefin monomer (based on the total amount of polymerizable monomers) and may optionally contain at least one comonomer. Non-limiting examples of olefin-based polymers include ethylene-based polymers and propylene-based polymers. "Olefin" and similar terms refer to a hydrocarbon composed of hydrogen and carbon, whose molecules contain a pair of carbon atoms joined together by a double bond.

[0031] "Pellets" and similar terms refer to small particles typically formed by compressing powder or granular material or by chopping off strands formed during extrusion of a melt through a die. Pellets can vary widely in shape and size.

[0032] "Polymer" refers to a compound prepared by reacting (i.e., polymerizing) a set of monomers, the set being a homogeneous (i.e., only one type) set of monomers or a heterogeneous (i.e., multiple types) set of monomers. As used herein, the term polymer includes the term "homopolymer," which refers to a polymer prepared from a homogeneous set of monomers, and the term "interpolymer," as defined below.

[0033] "Silane-functionalized polyolefin" and like terms mean an olefin polymer that contains silane functional groups.

[0034] "Thermoplastic polymer" and like terms refer to a linear or branched polymer that can be repeatedly softened and flowable when heated and then returned to a hardened state when cooled to room temperature. Thermoplastic polymers of the present disclosure generally have a modulus of elasticity greater than 10,000 psi (68.95 MPa) as measured according to ASTM D638-72. Furthermore, when heated to a softened state, the thermoplastic polymer can be molded or extruded into an article of any given shape.

[0035] "Thermoset polymer", "thermosetting polymers" and similar terms indicate that once cured, the polymer cannot be softened or even shaped by heat. Thermosetting polymers, once cured, are spatial network polymers that are highly cross-linked to form a rigid three-dimensional molecular structure.

[0036] "Wire" and similar terms refer to a single strand of conductive metal or a single strand of optical fiber.

[0037] Test Method Density is measured according to ASTM D792, Method B, and the results are reported in grams per cubic centimeter (g) (g / cc or g / cm 3 )

[0038] Gel Content The gel content test is a measure of the degree of crosslinking within a polymer composition. Gel content is usually proportional to the degree of crosslinking. The degree of crosslinking is measured by dissolving the composition in a solvent for a specified time and measuring the amount of unextractable material. The amount of unextractable material is used to calculate the gel content as a percentage. Gel content is measured by extraction with boiling decalin at 180°C for 5 hours according to ASTM D2765.

[0039] High temperature creep test High temperature creep test was performed according to ASTM D412 Type D using a 20 N / cm 2 The test is carried out at 200°C using a weight of 1.5 kgf / cm2. The elongation of the specimen from its initial value is recorded after 15 minutes of exposure to the oven without removing the specimen from the oven. High temperature creep is tested according to ICEA T-28-562.

[0040] Heat Deformation Heat deformation tests are performed according to ASTM D4565. Two duplicate samples of the polymer composition are obtained and preheated in an oven at 150°C for 60 minutes. The preheated samples are pressed with a 2 kg weight at 150°C for 1 hour. The weight remains in place and the pressed samples are placed in a climate controlled room at 23°C for an additional hour. The change in thickness of the samples is recorded and the Heat Deformation Percentage (HD%) is HD%=(D0-D1) / D0*100% where D0 represents the original sample thickness and D1 represents the sample thickness after deformation treatment. The average deformation ratio of two duplicate samples is reported.

[0041] Melt index (MI) measurements for polyethylene are performed according to ASTM D1238, condition 190°C / 2.16 kilogram (kg) weight, formerly known as "Condition E", also known as I2 or I2, and are reported in grams dissolved per 10 minutes (g / 10 min). Melt index is inversely proportional to the molecular weight of the polymer. Thus, the higher the molecular weight, the lower the melt index, although the relationship is not linear.

[0042] Surface Smoothness Test The surface smoothness of wire specimens is measured according to ANSI 1995 using a SURFTEST™ SJ-400 surface texture measuring instrument. The wire specimen is placed on a V-block and the stylus (10urn) is lowered to a specific starting position (applying approximately 1 gram of force to the wire). The stylus is moved laterally at a fixed speed of 2 millimeters per second to make the measurement. Four readings per wire specimen and four specimens are tested, which are then averaged to a value reported in microinches. A lower value indicates a higher smoothness. Surface smoothness testing complies with JIS'82, JIS'94, JIS'01, ISO, ANSI, VDA standards.

[0043] Tensile strength and elongation are measured in accordance with ASTM D638. Tensile strength is reported in units of "psig" and elongation is reported as a percentage of the difference between the final and initial lengths of the specimen. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0044] The present disclosure provides a crosslinked polymer composition, the crosslinked polymer composition (interchangeably referred to as "composition") comprising 4% to 45% by weight of a thermoplastic polymer, 52% to 95% by weight of a moisture curable polyolefin, and 0.05% to 7% by weight of a moisture condensation catalyst.

[0045] Thermoplastic Polymers The composition includes a thermoplastic polymer, such as, for example, a polyolefin. In one embodiment, the thermoplastic polymer is an ethylene-based polymer. Non-limiting examples of suitable ethylene-based polymers include high density polyethylene (HDPE), medium density polyethylene (MDPE), low density polyethylene (LDPE), linear low density polyethylene (LLDPE), and ethylene / α-olefin copolymers.

[0046] In one embodiment, the thermoplastic polymer is HDPE. "High density polyethylene" or "HDPE" refers to a polyethylene having a molecular weight of from 0.940, or 0.950, or 0.960 to 0.970, or 0.980 grams per cubic centimeter (g / cm 3 HDPE is an ethylene-based polymer with a density ranging from C3 to C 20 or a C4 to C8 α-olefin comonomer. The HDPE has a melt index of from 0.5, or 1.0, or 3.0 to 5.0, or 8.0, or 10.0 grams per 10 minutes (g / 10 min).

[0047] In an embodiment, the thermoplastic polymer has the following characteristics:

[0048] (i) 0.945 g / cm 3 ~0.970g / cm 3 density, and / or

[0049] (ii) HDPE of ethylene / C4-C8 alpha-olefin copolymers having one, some, or all of the following melt indexes: from 0.5 g / 10 min, alternatively from 1.0 g / 10 min, alternatively from 3.0 g / 10 min to 8.0 g / 10 min, alternatively from 10.0 g / 10 min.

[0050] The composition comprises the thermoplastic polymer in an amount of from 4, or 5, or 8, or 10, or 15-20, or 25, or 30, or 35, or 40, or 45 weight percent. In further embodiments, the composition comprises the thermoplastic polymer in an amount of 4-45 weight percent, or 5-45 weight percent, or 10-35 weight percent, or 15-20 weight percent. The weight percent of the thermoplastic polymer is based on the total weight of the composition.

[0051] The present disclosure contemplates the use of blends of two or more thermoplastic polymers disclosed herein. The blends can be two or more of the thermoplastic polymers HDPE, MDPE, LDPE and / or LLDPE. The blends can be, for example, two different HDPEs.

[0052] The thermoplastic polymer can comprise two or more embodiments disclosed herein.

[0053] Moisture-curable polyolefin The composition comprises a moisture-curable polyolefin. The moisture-curable polyolefin is a silyl polyolefin. The silyl polyolefin is a polyolefin that contains silane groups. The silane groups can be introduced by copolymerization reaction between olefin and silane, or by grafting silane to polyolefin, as described, for example, in U.S. Pat. Nos. 3,646,155 and 6,048,935.

[0054] The grafting of silanes to polyolefins can be carried out in the presence of a free radical initiator or alternatively using ionizing radiation. Non-limiting examples of free radical initiators include peroxides and azo compounds. Peroxides suitable for use include dicumyl peroxide, di-tert-butyl peroxide, t-butyl benzoyl peroxide, benzoyl peroxide, cumene hydroperoxide, t-butyl peroctoate, methyl ethyl ketone peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, lauryl peroxide, and tert-butyl peracetate. A suitable azo compound is 2,2-azobisisobutyronitrile. In one embodiment, the amount of free radical initiator is from 0.001, or 0.005, or 0.01, or 0.03, or 0.05, or 0.07-0.08, or 0.1, or 0.15, or 0.3, or 0.5, or 1, or 1.5, or 2, or 3, or 5 percent resin (phr). In further embodiments, the amount of free radical initiator is from 0.001-5 phr, or 0.005-1 phr, or 0.01-0.15, or 0.03-0.1 phr. The term "resin" in "percent resin" refers to the moisture curable polyolefins described herein. In one embodiment, the weight ratio of silane to initiator is from 10:1, or 18:1 to 250:1, or 500:1. In further embodiments, the weight ratio of silane to initiator is from 10:1 to 500:1, or from 18:1 to 250:1. Grafting of silane to polyolefin can be carried out by blending the free radical initiator in the first stage of a reactor extruder, such as a BUSS™ kneader. The melt temperature used during the grafting process can be from 160°C to 260°C, or from 190°C to 230°C, depending on the residence time and half-life of the free radical initiator.

[0055] Silanes suitable for use include unsaturated silanes that contain (i) an ethylenically unsaturated hydrocarbyl group (e.g., a vinyl, allyl, isopropenyl, butenyl, cyclohexenyl, or γ-(meth)acryloylallyl group) and (ii) a hydrolyzable group (e.g., a hydrocarbyloxy group, a hydrocarbonyloxy group, or a hydrocarbylamino group). Non-limiting examples of hydrolyzable groups include methoxy, ethoxy, formyloxy, acetoxy, propionyloxy, and alkyl or arylamino groups.

[0056] In one embodiment, the silane is an unsaturated alkoxysilane (e.g., vinyltrimethoxysilane, vinyltriethoxysilane, vinyltriacetoxysilane, and gamma-(meth)acryloxypropyltrimethoxysilane), as disclosed along with methods of preparation in U.S. Pat. No. 5,266,627, which is incorporated herein by reference in its entirety.

[0057] Non-limiting examples of silyl polyolefins suitable for use include those having the formula: [ka] (wherein R1 is a hydrogen atom or a methyl group, x and y are 0 or 1 (with the proviso that when x is 1, y is 1), m and n are independently integers of 0 to 12 (inclusive), preferably 0 to 4, and each R″ independently represents a hydrolyzable organic group such as an alkoxy group having 1 to 12 carbon atoms (e.g., methoxy, ethoxy, butoxy), an aryloxy group (e.g., phenoxy), an aroxy group (e.g., benzyloxy), an aliphatic acyloxy group having 1 to 12 carbon atoms (e.g., formyloxy, acetyloxy, propanoyloxy), an amino or substituted amino group (e.g., alkylamino, arylamino), or a lower alkyl group having 1 to 6 carbon atoms (inclusive), provided that not more than one of the three R groups is alkyl).

[0058] The silyl polyolefin may further include heat stabilizers, light stabilizers, and pigments.

[0059] Silyl polyolefins suitable for use include SI-LINK™ DFDA-5451 and DFDB-5451, which are copolymers of ethylene and vinyltrimethoxysilane, available from The Dow Chemical Company.

[0060] In one embodiment, the amount of silicon in the moisture curable polyolefin is from 0.1, or 0.3, or 0.5, or 0.7, or 1, or 1.5, or 2-2.5, or 3, or 3.5, or 5, or 7, or 10, or 20% by weight. In further embodiments, the amount of silicon in the moisture curable polyolefin is 0.1-20% by weight, or 0.3-10% by weight, or 0.7-5% by weight, or 0.5-3% by weight. The amount of silicon is based on the total weight of the moisture curable polyolefin.

[0061] In one embodiment, the moisture curable polyolefin has a viscosity of from 0.870, or 0.900, or 0.920 to 0.930, or 0.950, or 0.970 g / cm 3 In a further embodiment, the moisture curable polyolefin has a density of from 0.870 to 0.970 g / cm 3 , or 0.900 to 0.950 g / cm 3 , or 0.920~0.930g / cm 3 In a particular embodiment, the moisture curable polyolefin has a density of 0.922 g / cm 3 has a density of

[0062] In one embodiment, the moisture curable polyolefin has a melt index of from 0.3, or 0.5, or 1, or 1.2, or 1.4 to 1.6, or 1.8, or 2, or 4, or 8, or 10, or 50 grams per 10 minutes (g / 10 min). In further embodiments, the moisture curable polyolefin has a melt index of from 0.3 to 50 g / 10 min, or from 1.2 to 1.8 g / 10 min, or from 1.4 to 1.6 g / 10 min. In a particular embodiment, the moisture curable polyolefin has a melt index of 1.5 g / 10 min.

[0063] In one embodiment, the moisture curable polyolefin has the following properties:

[0064] (I) 0.920-0.930 g / cm 3 density, and / or

[0065] (ii) silyl polyolefins, which are copolymers of ethylene and vinyltrimethoxysilane having one, some, or all of the following melt indexes: 0.5 g / 10 min to 2.5 g / 10 min.

[0066] In one embodiment, the composition comprises the moisture curable polyolefin in an amount of from 52, or 53, or 55, or 60-70, or 75, or 85, or 90, or 95 weight percent. In one embodiment, the composition comprises the moisture curable polyolefin in an amount of 52-95 weight percent, or 55-95 weight percent, or 55-75 weight percent, or 60-70 weight percent. The weight percent of the moisture curable polyolefin is based on the total weight of the composition.

[0067] The moisture curable polyolefin can comprise two or more embodiments disclosed herein.

[0068] Water Condensation Catalyst Moisture condensation catalysts (also known as crosslinking catalysts) suitable for use include Lewis acids, Lewis bases, Bronsted acids, Bronsted bases, and combinations thereof. Lewis acids are chemical species that can accept electrons from another chemical species. Lewis bases are chemical species that can donate electrons to another chemical species. Non-limiting examples of water condensation catalysts suitable for use include: (i) tin carboxylates such as dibutyltin dilaurate (DBTDL), dimethyl hydroxytin oleate, dioctyl tin maleate, di-n-butyl tin maleate, dibutyltin diacetate, dibutyltin dioctoate, stannous acetate, stannous octoate, (ii) organometallic compounds such as lead naphthenate, zinc caprylate, cobalt naphthenate, (iii) mineral acids such as hydrofluoric acid, hydrochloric acid, hydrobromic acid, hydroiodic acid, nitric acid, phosphoric acid, sulfuric acid, sulfonic acid, boric acid, and perchloric acid, (iv) amines such as primary amines, secondary amines, and tertiary amines. In one embodiment, the water condensation catalyst is DBTDL or a sulfonic acid.

[0069] The moisture condensation catalyst is present during the process of melt blending the thermoplastic polymer and the moisture-curable polyolefin. In one embodiment, the moisture condensation catalyst can be added to the thermoplastic polymer and / or the moisture-curable polyolefin in the form of a masterbatch.

[0070] In one embodiment, the moisture condensation catalyst has a concentration of from 0.88, or 0.90, or 0.91, or 0.93, or 0.95 to 0.97, or 0.99, or 1.0, or 1.2, or 1.45, or 1.6 g / cm 3 In a further embodiment, the moisture condensation catalyst has a density of from 0.88 to 1.6 g / cm 3 or 0.93~1.45g / cm 3 has a density of

[0071] In one embodiment, the moisture condensation catalyst has a melt index of from 0.3, or 0.5, or 0.7, or 0.9, or 0.91, or 0.92-0.93, or 0.94, or 1, or 2, or 4, or 8, or 10 grams / 10 minutes (g / 10 min.). In further embodiments, the moisture condensation catalyst has a melt index of from 0.3 to 10 g / 10 min., or from 0.9 to 4 g / 10 min., or from 0.92 to 0.93 g / 10 min.

[0072] Suitable water condensation catalysts for use include 、 Included are SI-LINK™ DFDA-5481, DFDB-5480, and DFDA-5488, which are masterbatch copolymers available from The Dow Chemical Company.

[0073] In one embodiment, the composition comprises a moisture condensation catalyst in an amount from 0.05, or 0.1, or 0.5, or 1, or 3, or 4-6, or 7 weight percent. In further embodiments, the composition comprises a moisture condensation catalyst in an amount from 0.05-7 weight percent, or 3-7 weight percent, or 4-6 weight percent. In certain embodiments, the composition comprises 5 weight percent moisture condensation catalyst. The weight percentage of the moisture condensation catalyst is based on the total weight of the composition.

[0074] The moisture condensation catalyst may comprise two or more embodiments disclosed herein.

[0075] Fillers and Additives The composition of the present disclosure may include an optional filler. In one embodiment, the filler has flame retardant properties. The filler may or may not interact with the moisture condensation catalyst and / or may or may not react with the moisture condensation catalyst. In a further embodiment, the filler is coated with a material (e.g., stearic acid) that prevents or retards the filler from interfering with the silane / polyolefin crosslinking reaction. Non-limiting examples of fillers suitable for use include kaolin clay, magnesium hydroxide, silica, calcium carbonate and carbon black, stearic acid, and combinations thereof.

[0076] The amount of filler in the composition is less than that which would cause an unacceptably large deterioration of the mechanical and / or chemical properties of the composition. In one embodiment, the composition comprises a filler in an amount of from 0.1, or 0.5, or 1, or 2, or 5-8, or 10, or 20, or 35 wt. %. In a further embodiment, the composition comprises a filler in an amount of from 0.1-35 wt. %, or 0.5-8 wt. %. The weight percentage of the filler is based on the total weight of the composition.

[0077] The filler may comprise two or more embodiments disclosed herein.

[0078] The composition of the present disclosure may include optional additives. Non-limiting examples of fillers suitable for use may include antioxidants (e.g., hindered phenols such as IRGANOX™ 1010 available from Ciba Specialty Chemicals), phosphites (e.g., IRGAFOS™ 168 available from Ciba Specialty Chemicals), UV stabilizers, adhesion additives, light stabilizers (such as hindered amines), plasticizers (such as dioctyl phthalate or epoxidized soybean oil), metal deactivators, char inhibitors, mold release agents, tackifiers (such as hydrocarbon tackifiers), waxes (such as polyethylene wax), nucleating agents, processing aids (oils, organic acids such as stearic acid, metal salts of organic acids, etc.), oil extenders (such as paraffin oil and mineral oil), colorants or pigments. Moisture generating agents can accelerate the curing stage of the process where crosslinks are generated.

[0079] The compositions of the present disclosure exclude the use of blowing agents, in other words, they are non-foaming compositions.

[0080] The amount of additive in the composition is less than the amount that would interfere with the desired physical or mechanical properties of the composition, as determined by one of ordinary skill in the art. In one embodiment, the composition comprises an additive in an amount of from 0.1, or 0.5, or 1, or 2, or 5-8, or 10, or 20, or 35 wt. %. In a further embodiment, the composition comprises an additive in an amount of from 0.1-35 wt. %, or 0.5-8 wt. %. The weight percentage of the additive is based on the total weight of the composition.

[0081] The additive may comprise two or more embodiments disclosed herein.

[0082] composition In one embodiment, the composition has a combined weight of thermoplastic polymer (TP) and moisture curable polyolefin (MCP) of 80, or 85, or 90, or 91, or 92, or 93, or 94-95, or 96, or 97, or 98% by weight. In further embodiments, the composition has a combined weight of TP and MCP of 80-98%, or 90-97%, or 94-96% by weight. In certain embodiments, the composition has a combined weight of TP and MCP of 95% by weight.

[0083] In one embodiment, the composition has a combined weight of moisture curable polyolefin (MCP) and moisture condensation catalyst (MCC) of 50, or 60, or 70, or 75, or 80, or 85, or 90-95, or 97, or 98% by weight. In further embodiments, the composition has a combined weight of MCP and MCC of 50-98%, or 60-95%, or 85-95% by weight.

[0084] In one embodiment, the composition comprises a weight ratio of MCP to TP of 1, or 1.4, or 2, or 3, or 3.8, or 5, or 5.3, or 7-8, or 8.5, or 9, or 15, or 18, or 20. In further embodiments, the composition comprises a weight ratio of MCP to TP of 1-20, or 3-18, or 5-9.

[0085] In one embodiment, the composition comprises a weight ratio of MCP to MCC from 5, or 10, or 11, or 13, or 15, or 16-17, or 18, or 19, or 20, or 30. In further embodiments, the composition comprises a weight ratio of MCP to MCC from 5-30, or 10-20, or 15-18.

[0086] In one embodiment, the composition comprises a weight ratio of TP to MCC from 0.5, or 1, or 2, or 3, or 4-5, or 6, or 7, or 8, or 10, or 20, or 30. In further embodiments, the composition comprises a weight ratio of TP to MCC from 0.5-30, or 1-10, or 3-8.

[0087] The weight percentages of the additives are based on the total weight of the composition.

[0088] The composition of the present disclosure comprises a polymer component comprising a thermoplastic polymer and a moisture curable polyolefin. In one embodiment, the polymer component is a crosslinked form of the thermoplastic polymer and the moisture curable polyolefin. Without wishing to be limited by theory, the crosslinks within the polymer component can provide heat resistance to the polymer component and the composition comprising the polymer component. Heat resistance is quantified by measuring the high temperature creep and high temperature deformation properties of the composition.

[0089] The degree of crosslinking within the polymeric component correlates with the gel content of the composition, i.e., the degree of crosslinking is proportional to the gel content. Alternatively, the degree of crosslinking within the polymeric component can be correlated with the high temperature creep value of the composition, the high temperature deformation value of the composition, or a combination thereof. In one embodiment, the polymeric component is crosslinked as indicated by a gel content of 60%, or 65% to 70%, or 75%, or 80%, as disclosed herein. In a further embodiment, the polymeric component is crosslinked as indicated by a high temperature creep value of 10%, or 20% to 30%, or 45%, as disclosed herein. In yet another embodiment, the polymeric component is crosslinked as indicated by a heat deformation value of 7% to 36%, as disclosed herein.

[0090] In one embodiment, the polymeric components are crosslinked when the thermoplastic polymer is present in an amount of 5 to 40 weight percent, the moisture curable polyolefin is present in an amount of 55 to 90 weight percent, and the moisture condensation catalyst is present in an amount of 3 to 7 weight percent (weight percentages are based on the total weight of the composition).

[0091] In one embodiment, the composition of the present disclosure is a non-foaming composition.

[0092] In one embodiment, the composition of the present disclosure is a thermosetting composition.

[0093] In one embodiment, the compositions of the present disclosure are devoid of monomer units derived from propylene.

[0094] In one embodiment, the composition has a surface smoothness of from 3, or 13, or 25, or 51, or 89, or 102, or 114 to 127, or 140, or 149, or 152, or 162, or 178, or 184, or 191, or 203, or 216, or 229, or 254 μ·inch. In further embodiments, the composition has a surface smoothness of 3 to 254 μ·cm (1 to 100 μ·in), or 51 to 229 μ·cm (20 to 90 μ·in), or 89 to 216 μ·cm (35 to 85 μ·in), or 89 to 191 μ·cm (35 to 75 μ·in), or 102 to 184 μ·cm (40 to 72 μ·in), or 102 to 162 μ·cm (40 to 64 μ·in), or 102 to 127 μ·cm (40 to 50 μ·in).

[0095] In one embodiment, the composition has a high temperature creep value of from 1%, or 5%, or 10%, or 15%, or 20%-25%, or 30%, or 35%, or 40%, or 45%. In further embodiments, the composition has a high temperature creep value of from 1%-45%, or 5%-43%, or 10%-41%, or 10%-35%, or 10%-30%, or 10%-25%.

[0096] In one embodiment, the composition has a high temperature distortion value of from 1%, or 5%, or 7%, or 10%, or 15%, or 20% to 25%, or 30%, or up to 36%. In further embodiments, the composition has a high temperature distortion creep value of from 1% to 55%, or 5% to 40%, or 7% to 36%, or 10% to 25%.

[0097] In one embodiment, the composition has a gel content of from 60%, or from 65% to 70%, or from 75%, or from 80%. In further embodiments, the composition has a gel content of from 60% to 80%, or from 65% to 75%.

[0098] Formulation and Manufacturing The melt mixing of the thermoplastic polymer, the moisture curable polyolefin, the moisture condensation catalyst, and the optional fillers and additives is carried out by standard methods known to those skilled in the art. Examples of compounding equipment include BRABENDER™, BANBURY™ and BOLLING™ internal batch mixers. Continuous single or twin screw mixers or extruders suitable for use include DAVIS STANDARD™ extruders, FARREL™ continuous mixes, WERNER AND PFLEIDERER™ twin screw mixers, and BUSS™ kneading continuous extruders. The type of mixer used and the operating conditions of the mixer affect the properties of the composition, such as viscosity, volume resistivity, extrusion surface smoothness, etc.

[0099] The components of the composition are typically mixed at a temperature and for a length of time sufficient to completely homogenize the mixture, but insufficient to gel the material. The moisture condensation catalyst can be added directly to the moisture curable polyolefin, or alternatively, before, with, or after optional fillers and additives are added to the moisture curable polyolefin. Typically, the components are mixed together in a melt mixing device. The mixture is then molded into the final article. The temperature of compounding and article manufacture is above the melting point of the moisture curable polyolefin, but preferably below 250°C.

[0100] In one embodiment, the moisture curable polyolefin, the moisture condensation catalyst, the fillers, the additives, and combinations thereof are added in the form of a masterbatch.

[0101] In one embodiment, to reduce or eliminate possible scorching that may result from moisture present in or associated with the ingredients, such as the filler, one or more of the ingredients are dried prior to blending, or the mixture of ingredients is dried after blending.

[0102] In one embodiment, the polymer composition is non-foamable; (A) 5% by weight to 40% by weight of HDPE, (B) 55% to 90% by weight of an ethylene and vinyltrimethoxysilane copolymer, and (C) 0.05% by weight to 7% by weight of a dibutyltin dilaurate moisture condensation catalyst. The polymer composition has the following characteristics: (i) a gel content of 60% to 80%; and / or (ii) a high temperature creep value between 10% and 45%, and / or (ii) having one, some, or all of the following heat distortion values ​​between 7% and 36% (hereafter referred to as Polymer Composition 1).

[0103] manufactured goods In one embodiment, the composition of the present invention can be applied to the conductor as a coating in known amounts and by known methods (e.g., using the equipment and methods described in USP 5,246,783 and 4,144,202). Typically, the composition is prepared in a reactor-extruder equipped with a conductor coating die, and after the components of the composition are blended, the composition is extruded onto the conductor as the conductor is drawn through the die. The composition can be extruded onto the conductor at a linear speed of 800 to 2000 feet per minute (243 to 610 meters per minute, m / min). The curing stage of the process, in which crosslinks are produced, can begin in the reactor-extruder. The molded article may be exposed to either or both elevated temperatures and external humidity, and if elevated, is typically at or above ambient temperature but below the melting point of the composition for a period of time such that the article reaches the desired degree of crosslinking. The temperature of any post-molding cure should be above 0°C.

[0104] In one embodiment, the coating is an insulating layer in direct contact with the conductor. As used herein, the term "in direct contact" indicates that the conductor and the insulating layer are in adhesive relationship with one another, with the conductor disposed directly adjacent the insulating layer, with no intervening structure therebetween.

[0105] In certain embodiments, the insulation layer is used in twisted pair category data cables. The insulation layer is suitable for all category data cable ratings including Cat2, Cat3, Cat4, Cat5, Cat5e, Cat6, Cat6a, and Cat7. Category data cables are capable of transmitting low voltage power that serves as a power source for electronic devices. The combined use of power and data cables is referred to as "Power over Ethernet" or "PoE".

[0106] In one embodiment, the insulating layer has a thickness of 127 μm (5 mils), or 178 μm (7 mils), or 229 μm (9 mils), or 254 μm (10 mils), or 305 μm (12 mils) to 381 μm (15 mils), or 451 μm (18 mils), or 508 μm (205 mils). In further embodiments, the insulating layer has a thickness of 127 μm (5 mils) to 508 μm (205 mils), or 178 μm (7 mils) to 381 μm (15 mils), or 229 μm (9 mils) to 305 μm (12 mils).

[0107] In one embodiment, the insulating layer is a non-foamed insulating layer.

[0108] In one embodiment, a coated conductor is provided, comprising a conductor and a coating on the conductor. (A) 5% by weight to 40% by weight of HDPE, (B) 55% to 90% by weight of ethylene and vinyltrimethoxysilane, and (C) a non-foamed polymer composition comprising a polymer composition 1 comprising 0.5% by weight to 7% by weight of a dibutyltin dilaurate moisture condensation catalyst; The coating has the following properties: (i) a surface smoothness between 102 μ·cm and 184 μ·cm; and / or (ii) a tensile strength of 1905 psig to 2410 psig; and / or (iii) having one, some, or all of the following elongations from 215% to 265%.

[0109] Other articles of manufacture that can be made from the polymer compositions of the present disclosure include fibers, ribbons, sheets, tapes, tubes, pipes, weatherstripping, seals, gaskets, hoses, footwear, and bellows. These articles can be manufactured using known equipment and techniques.

[0110] The invention is more fully illustrated by the following examples in which all parts and percentages are by weight unless otherwise stated. EXAMPLES

[0111] The raw materials used in the invention examples ("IE") and comparative examples ("CS") are detailed in Table 1 below. [Table 1]

[0112] The polymer compositions of the invention examples IE-1, IE-2, IE-3, IE-4, IE-5 and the comparative samples CS-1 and CS-2 are prepared for the coated conductor samples using the raw materials listed in Table 1 according to the formulations listed in Table 2.

[0113] Coated conductor samples are prepared from tin-plated 7 strand, 24 American Wire Gauge (AWG) core. The component compositions are first dry blended. The compositions are then melt blended by extrusion blending using a 2.5 inch DAVIS STANDARD extruder with a 22:1 L / D and fitted with a PE screw with a double flight mixing section. The melt blended composition is extruded onto the conductor as it is drawn through the extruder die at a linear speed of 548 meters per minute. The extruder temperature profile is 150°C to 182°C across four zones. The extruded coated strands are time cured in a 90°C water bath for 14 to 18 hours and then dried overnight at 80°C in a convection oven or cured in a humidity chamber at 50°C and 75% relative humidity for 14 days and then dried overnight at 80°C.

[0114] The coated conductor thickness is 254 μm (10 mils).

[0115] The polymer compositions of the invention examples IE-7, IE-8, IE-9, IE-10, IE-11 and the comparative samples CS-3, CS-4, CS-5 and CS-6 are prepared for tape samples according to the formulations listed in Table 2 and the raw materials listed in Table 1.

[0116] Tape samples are prepared by first dry blending the components of the composition. The composition is then melt blended by extrusion blending into a 2 inch tape using a 3 / 4 inch single screw BRABENDER™ batch mixer having a 25:1 L / D and fitted with a Maddox mixing screw. The melt mixed composition is extruded at 50 revolutions per minute (rpm) and a take up speed of 38 feet per minute. The extruder temperature profile is 150°C to 182°C across all five zones. The extruded tape is cured in a 90°C water bath for 14 to 18 hours and then dried overnight at 80°C in a convection oven or cured in a humidity chamber at 50°C and 75% relative humidity for 14 days and then dried overnight at 80°C.

[0117] The formulations of the test results for the inventive and comparative samples are reported in Table 2 below. [Table 2]

[0118] Results and Discussion CS-1 and CS-2 are coated conductors. CS-1 is a wire coated with HDPE without crosslinking that failed the high temperature creep test. CS-2 is a wire coated with a crosslinked polymer with no thermoplastic components. CS-2 has the least favorable results in terms of surface smoothness and tensile properties of all the coated conductors investigated.

[0119] CS-3 through CS-6 are tape samples. CS-3 and CS-4 are HDPE thermoplastic compounds with no crosslinking. CS-3 and CS-4 each exhibit poor tensile properties, 100% high temperature creep values, and failure of the high temperature deformation test. The CS-5 tape sample contains no thermoplastic components and exhibits the lowest degree of crosslinking (51% gel content) of all tape samples investigated. CS-6 is an acid catalyzed crosslinked composition with no thermoplastic compounds. The CS-6 tape sample swells during the heat deformation test as indicated by the negative results presented. CS-6 has extensive crosslinking as indicated by the 82% gel content.

[0120] Applicants have discovered a non-foamable insulating composition of a thermoplastic polymer and a moisture curable polyolefin that is crosslinked as indicated by a percent gel content of 60-82.

[0121] The compositions of the present invention (IE-1 to IE-5) unexpectedly provide insulating coated conductor articles having (i) a surface smoothness of 102 to 184 μ·cm (40 to 72 μ·in), which is 44% to 80% improved over crosslinked compositions without a thermoplastic polymer, (ii) a high temperature creep percentage of 26.5 to 33.0, which is 8% to 30% improved over crosslinked compositions without a thermoplastic polymer, and (iii) a tensile strength of 1905 to 2410 psig, which is 5% to 132% improved over crosslinked compositions without a thermoplastic polymer.

[0122] The compositions of the present invention (IE-7 to IE-11) unexpectedly provide tape articles having (i) high temperature creep rates of 11.1 to 40.4, which are 12% to 308% improved over crosslinked compositions that do not contain a thermoplastic polymer, and (ii) heat deformation rates of 9.2 to 35.7, which are 26% to 390% improved over crosslinked compositions that do not contain a thermoplastic polymer.

[0123] The present disclosure is not limited to the embodiments and figures contained herein, but is specifically intended to include modifications of these embodiments, including portions of the embodiments, and combinations of elements of different embodiments that fall within the scope of the following claims.

Claims

1. (A) 4% to 45% by weight of a thermoplastic polymer; (B) 52% to 95% by weight of a moisture-curable polyolefin; and (C) a crosslinked polymer composition comprising 0.05% to 7% by weight of a moisture condensation catalyst.

2. The composition of claim 1 , wherein the thermoplastic polymer comprises high density polyethylene.

3. The high density polyethylene has a viscosity of 0.945 g / cm 3 ~0.970g / cm 3 and a melt index from 0.5 g / 10 min to 10 g / 10 min.

4. The moisture-curable polyolefin has a viscosity of 0.920 g / cm 3 ~0.930g / cm 3 and a melt index from 0.5 g / 10 min to 2.5 g / 10 min.

5. The composition of claim 1, wherein the polymer composition has a gel content of from 60% to 80%.

6. The composition of claim 5, wherein the polymer composition has a high temperature creep value of from 10% to 45%.

7. The composition of claim 1, wherein the polymer composition has a high temperature distortion value at 150°C of 7% to 36%.

8. The composition of claim 1 , wherein the polymer composition comprises a polymer component, the polymer component consisting of (A) and (B).

9. 5% to 40% by weight of high density polyethylene; 55% to 90% by weight of said moisture-curable polyolefin; 3% to 7% by weight of said moisture condensation catalyst; 60% to 80% gel content; High temperature creep values ​​of 10% to 40%, and The composition of claim 3 having a high temperature deformation value of from 7% to 36%.

10. The composition of claim 1 , wherein the polymer composition is non-foamed.

11. The composition of claim 1 , wherein the polymer composition is free of monomer units derived from propylene.

12. The composition of claim 1 , wherein the polymeric composition is a thermosetting composition.

13. A coated conductor, Conductors, and a coating on the conductor, the coating comprising: (A) 4% to 45% by weight of a thermoplastic polymer; (B) 52% to 95% by weight of a moisture-curable polyolefin; and (C) a coated conductor comprising a crosslinked polymer composition comprising 0.05% to 7% by weight of a moisture condensation catalyst.

14. The coated conductor of claim 13 , wherein the thermoplastic polymer comprises high density polyethylene and the coating is in direct contact with the conductor.

15. Surface smoothness of 102μ cm to 184μ cm; High temperature creep values ​​of 10% to 40%, and 15. The coated conductor of claim 14, comprising a high temperature deformation value at 150°C of 7% to 36%.