Pellet and moldings
The composite resin composition with partially defibrated fibrous fillers in general-purpose plastics addresses mechanical weaknesses, achieving high elastic modulus and impact resistance, suitable for industrial applications traditionally requiring engineering plastics or metals.
Patent Information
- Application Number
- JP2024153571
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2037-01-18
AI Technical Summary
General-purpose plastics lack sufficient mechanical strength and have limited application due to their inherent weaknesses, while engineering plastics are expensive and environmentally burdensome.
A composite resin composition is developed, comprising a base resin and fibrous fillers with partially defibrated ends, where the fibrous fillers have specific fiber length, diameter, and aspect ratio, and pores are present at the interface, enhancing mechanical properties.
The composite resin molded article achieves high elastic modulus and impact resistance, making it suitable for mechanical products traditionally requiring engineering plastics or metals, thus reducing manufacturing costs.
Smart Images

Figure 2024161256000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to pellets capable of realizing a molded article having excellent mechanical properties, and to a molded article obtained by molding the pellets. [Background technology]
[0002] So-called "general-purpose plastics" such as polyethylene (PE), polypropylene (PP), polystyrene (PS), and polyvinyl chloride (PVC) are not only very inexpensive, but also easy to mold and are a fraction of the weight of metals or ceramics. For this reason, general-purpose plastics are often used as materials for a variety of everyday items such as bags, various types of packaging, various containers, and sheets, as well as industrial parts such as automobile parts and electrical parts, and as materials for daily necessities and miscellaneous goods.
[0003] However, general-purpose plastics have drawbacks such as insufficient mechanical strength, etc. Therefore, general-purpose plastics do not have sufficient properties required for materials used in various industrial products such as mechanical products such as automobiles, and electrical, electronic, and information products, and the current situation is that the range of applications of general-purpose plastics is limited.
[0004] On the other hand, so-called "engineering plastics" such as polycarbonate, fluororesin, acrylic resin, and polyamide have excellent mechanical properties and are used in various industrial products, including mechanical products such as automobiles, and electrical, electronic, and information products. However, engineering plastics have issues such as being expensive, difficult to recycle as monomers, and a large environmental impact.
[0005] Therefore, there is a demand for a significant improvement in the material properties (mechanical strength, etc.) of general-purpose plastics. A technique is known for improving the mechanical strength of general-purpose plastics by dispersing fibrous fillers such as natural fibers, glass fibers, and carbon fibers in the resin of the general-purpose plastics in order to strengthen the general-purpose plastics. Among these, organic fibrous fillers such as cellulose are attracting attention as reinforcing fibers because they are inexpensive and have excellent environmental friendliness when disposed of.
[0006] Companies are conducting research to improve the mechanical strength of general-purpose plastics. In Patent Document 1, cellulose fibers with a maximum fiber diameter of 100 nm or less and an aspect ratio of 2000 or more are added to increase the elastic modulus and dimensional stability. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Patent No. 5577176 Summary of the Invention [Problem to be solved by the invention]
[0008] However, in Patent Document 1, fibers with an aspect ratio of 2000 or more are added, and as shown in Figures 4 and 5, the fibers 2 tend to be oriented in the flow direction of the molten base resin 1 injected during molding, resulting in a problem that the strength in the direction perpendicular to the flow direction is weak, and in particular the surface impact strength is reduced. The pellets of the present invention solve the above-mentioned problems of the conventional art, and have an object to realize a composite resin molding having a high elastic modulus and high impact resistance. [Means for solving the problem]
[0009] In order to achieve the above object, the pellet of the present invention contains a base resin and a fibrous filler, the end of the fibrous filler in the fiber length direction is defibrated, the defibrated portion of the end of the fibrous filler in the fiber length direction is 5% to 50% of the entire fiber length of the fibrous filler, the fiber diameter in the defibrated portion of the fibrous filler is 1 / 1000 to 1 / 10 of the fiber diameter in the undefibrated portion, the aspect ratio of the undefibrated portion of the fibrous filler is 5 to 1000, the elastic modulus of the fibrous filler is greater than the elastic modulus of the base resin, the difference between the elastic modulus of the fibrous filler and the elastic modulus of the base resin is within 20 GPa, voids are present at the interface between the base resin and the fibrous filler, and the volume of the voids is 10% or less of the volume of the fibrous filler. Effect of the Invention
[0010] The pellets of the present invention can realize a composite resin molding having a high elastic modulus and high impact resistance. [Brief description of the drawings]
[0011] [Figure 1] 1 is a schematic cross-sectional view of a composite resin composition according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram of a fibrous filler according to an embodiment of the present invention. [Diagram 3] FIG. 2 is a schematic diagram of a process for producing pellets made of a composite resin composition according to an embodiment of the present invention. [Figure 4] 1 is a schematic cross-sectional view of a composite resin molded body in Patent Document 1. FIG. [Diagram 5] FIG. 5 is an enlarged view of a portion of FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, a composite resin composition according to an embodiment of the present invention will be described with reference to the drawings. In the following description, the same components are denoted by the same reference numerals, and the description will be omitted as appropriate.
[0013] The composite resin composition according to the embodiment of the present invention is a melt-kneaded product containing a base resin, a fibrous filler, and a dispersant. As shown in the schematic cross-sectional view of Fig. 1, the composite resin composition has a fibrous filler 2 dispersed in a base resin 1. The fibrous filler 2 is carbonized at a specific ratio.
[0014] In this embodiment, the base resin 1 is preferably a thermoplastic resin in order to ensure good moldability. Examples of thermoplastic resins include olefin resins (including cyclic olefin resins), styrene resins, (meth)acrylic resins, organic acid vinyl ester resins or derivatives thereof, vinyl ether resins, halogen-containing resins, polycarbonate resins, polyester resins, polyamide resins, thermoplastic polyurethane resins, polysulfone resins (polyethersulfone, polysulfone, etc.), polyphenylene ether resins (polymers of 2,6-xylenol, etc.), cellulose derivatives (cellulose esters, cellulose carbamates, cellulose ethers, etc.), silicone resins (polydimethylsiloxane, polymethylphenylsiloxane, etc.), rubber or elastomers (diene rubbers such as polybutadiene and polyisoprene, styrene-butadiene copolymers, acrylonitrile-butadiene copolymers, acrylic rubbers, urethane rubbers, silicone rubbers, etc.). The above resins may be used alone or in combination of two or more kinds. The base resin 1 is not limited to the above materials as long as it has thermoplasticity.
[0015] Of these thermoplastic resins, the main resin 1 is preferably an olefin-based resin having a relatively low melting point. The olefin-based resin includes homopolymers of olefin-based monomers, copolymers of olefin-based monomers, and copolymers of olefin-based monomers and other copolymerizable monomers. Examples of the olefin-based monomer include linear olefins (α-C2-20 olefins such as ethylene, propylene, 1-butene, isobutene, 1-pentene, 4-methyl-1-pentene, and 1-octene), and cyclic olefins. These olefin-based monomers may be used alone or in combination of two or more kinds. Of the above olefin-based monomers, linear olefins such as ethylene and propylene are preferred. Examples of other copolymerizable monomers include fatty acid vinyl esters such as vinyl acetate and vinyl propionate; (meth)acrylic monomers such as (meth)acrylic acid, alkyl (meth)acrylates, and glycidyl (meth)acrylates; unsaturated dicarboxylic acids or anhydrides such as maleic acid, fumaric acid, and maleic anhydride; vinyl esters of carboxylic acids (e.g., vinyl acetate and vinyl propionate); cyclic olefins such as norbornene and cyclopentadiene; and dienes such as butadiene and isoprene. These copolymerizable monomers may be used alone or in combination of two or more. Specific examples of olefin resins include copolymers of chain olefins (particularly α-C2-4 olefins) such as polyethylene (low density, medium density, high density, or linear low density polyethylene), polypropylene, ethylene-propylene copolymers, and terpolymers such as ethylene-propylene-butene-1.
[0016] Next, the dispersant will be described. The composite resin composition in this embodiment contains a dispersant for the purpose of improving the adhesion between the fibrous filler 2 and the main resin 1, or the dispersibility of the fibrous filler 2 in the main resin 1. Examples of the dispersant include various titanate-based coupling agents, silane coupling agents, unsaturated carboxylic acids, maleic acid, maleic anhydride, or modified polyolefins grafted with the anhydrides thereof, fatty acids, fatty acid metal salts, and fatty acid esters. The silane coupling agents are preferably unsaturated hydrocarbon-based or epoxy-based. There is no problem even if the surface of the dispersant is treated with a thermosetting or thermoplastic polymer component and modified. The content of the dispersant in the composite resin molded body in this embodiment is preferably 0.01% by mass or more and 20% by mass or less, more preferably 0.1% by mass or more and 10% by mass or less, and even more preferably 0.5% by mass or more and 5% by mass or less. If the content of the dispersant is less than 0.01% by mass, poor dispersion occurs, while if the content of the dispersant exceeds 20% by mass, the strength of the composite resin molded body decreases. The dispersant is appropriately selected depending on the combination of the base material 1 and the fibrous filler 2, and in the case of a combination in which a dispersant is not required, it need not be added.
[0017] Next, the fibrous filler 2 will be described. The fibrous filler 2 (hereinafter, sometimes simply referred to as fiber) contained in the composite resin composition in this embodiment is used mainly for the purpose of improving mechanical properties and improving dimensional stability by reducing the linear expansion coefficient in a resin molded body molded using the composite resin composition. For this purpose, the fibrous filler 2 preferably has a higher elastic modulus than the main resin 1, and specific examples thereof include carbon fiber, carbon nanotube, pulp, cellulose, cellulose nanofiber, lignocellulose, lignocellulose nanofiber, basic magnesium sulfate fiber (magnesium oxysulfate fiber), potassium titanate fiber, aluminum borate fiber, calcium silicate fiber, calcium carbonate fiber, silicon carbide fiber, wollastonite, xonotlite, various metal fibers, natural fibers such as cotton, silk, wool or hemp, regenerated fibers such as jute fiber, rayon or cupra, semi-synthetic fibers such as acetate and promix, synthetic fibers such as polyester, polyacrylonitrile, polyamide, aramid, polyolefin, and further modified fibers chemically modified on the surface and end thereof. Among these, carbon fibers and cellulose fibers are particularly preferred from the viewpoints of availability, high elastic modulus, and low linear expansion coefficient, and natural fibers of cellulose fibers are more preferred from the viewpoint of environmental friendliness.
[0018] Next, the shape of the fibrous filler 2 will be described. FIG. 2 is a schematic diagram of the fibrous filler 2. The symbol L is the length of the fibrous filler 2 (hereinafter, sometimes referred to as the fiber length), and the symbol d is the width of the fibrous filler 2 (hereinafter, sometimes referred to as the fiber diameter). If the aspect ratio (L / d) of the fibrous filler 2 is high, the fibers are likely to be oriented in the flow direction during injection molding, and the strength in the fiber orientation direction is strong but the strength in the direction perpendicular to it is weak, resulting in a decrease in impact strength in a drop test or the like. Therefore, it is preferable that the aspect ratio (L / d) of the fibers as a whole is small, that is, the fiber diameter d is large. On the other hand, from the viewpoint of mechanical properties, it is preferable that the specific surface area of the fibers is high, that is, the fiber diameter d is small, because a larger number of bonding interfaces between the fibers and the resin leads to improved strength.
[0019] To achieve the above two objectives, a structure in which the end in the fiber length direction within a single fiber is partially defibrated, as shown in Figure 2, is most preferable. Reference numeral 3 indicates the defibrated portion. The optimal fiber shape has been calculated as follows from the results of experiments and simulations. The defibrated portion 3 is preferably 5% or more and 50% or less of the entire fiber length L of the fibrous filler 2. If the defibrated portion 3 is less than 5% of the entire fiber length L, the specific surface area is small and no improvement in strength is observed, whereas if it is 50% or more, the defibrated portion 3 with a large aspect ratio becomes dominant, which makes it easier for the fibers to be oriented during injection molding and reduces the impact strength.
[0020] The fiber diameter in the defibrated portion 3 of the fibrous filler 2 is preferably 1 / 1000 or more and 1 / 10 or less of the undefibrated fiber diameter d. If it is less than 1 / 1000, the fiber diameter in the defibrated portion becomes too small and is torn by the shear force during kneading, making it difficult to maintain the shape of the present invention. If it exceeds 1 / 10, the strength improvement effect due to the improvement in the specific surface area is small. In addition, the aspect ratio of the undefibrated portion of the fibrous filler 2 (portion with large fiber diameter) is preferably 5 or more and 1000 or less. If it is less than 5, the reinforcing effect due to the fiber shape is small, and if it is 1000 or more, the fibers are easily oriented during injection molding.
[0021] Next, the characteristics of the fibrous filler 2 will be described. The types of the main resin 1 and the fibrous filler 2 are as described above. However, if the fibrous filler 2 is too soft relative to the main resin 1, i.e., if the elastic modulus is small, the composite resin composition as a whole will have a small elastic modulus, resulting in a decrease in strength. On the other hand, if the fibrous filler 2 is too hard relative to the main resin 1, i.e., if the elastic modulus is large, shock waves generated upon impact will not be propagated but will be absorbed at the interface between the main resin 1 and the fibrous filler 2, making it easier for cracks and crazes to occur near the interface, resulting in a decrease in impact resistance. Therefore, in the relationship between the elastic modulus of the main resin 1 and the fibrous filler 2, it is preferable that the elastic modulus of the fibrous filler 2 is higher, and the difference between them is as small as possible. The optimal relationship is calculated from the results of a simulation, and it is preferable that the difference in elastic modulus between the main resin 1 and the fibrous filler 2 is within 20 GPa.
[0022] Furthermore, for the purpose of improving the adhesiveness to the base resin 1 or the dispersibility in the composite resin composition, the fibrous fillers 2 may be surface-treated with various titanate coupling agents, silane coupling agents, unsaturated carboxylic acids, maleic acid, maleic anhydride, or modified polyolefins grafted with the anhydrides thereof, fatty acids, fatty acid metal salts, fatty acid esters, etc. Alternatively, the fibrous fillers 2 may be surface-treated with a thermosetting or thermoplastic polymer component.
[0023] Next, the manufacturing method will be described. Fig. 3 is a flow diagram illustrating a manufacturing process of pellets made of a composite resin composition in this embodiment. First, a base resin, a fibrous filler, and, if necessary, a dispersant are charged into a melt-kneading processing device, and melt-kneaded in the device. This melts the base resin, and the fibrous filler and dispersant are dispersed in the molten base resin. At the same time, the shearing action of the device promotes defibration of agglomerates of the fibrous filler, allowing the fibrous filler to be finely dispersed in the base resin.
[0024] Conventionally, fibrous fillers have been used in which the fibers have been defibrated in advance by pretreatment such as wet dispersion. However, when the fibrous filler is defibrated in advance in the solvent used in wet dispersion, it is easier to defibrate than in a molten base resin, so it is difficult to defibrate only the ends, and the entire fibrous filler ends up in a defibrated state. In addition, the inclusion of pretreatment increases the number of processes, which reduces productivity.
[0025] In contrast, in the manufacturing process of the composite resin composition in this embodiment, a pretreatment by wet dispersion for the purpose of defibrating and modifying the fibrous filler is not performed, and the fibrous filler is melt-kneaded together with a base resin, a dispersant, etc. (all-dry method). In this method, by not performing a wet dispersion treatment of the fibrous filler, it is possible to partially defibrate only the ends of the fibrous filler as described above, and the number of steps is reduced, thereby improving productivity.
[0026] In the all-dry method, the fibers are not modified in advance, but are mixed with a dispersant in a molten base resin, so that the entire fiber is not modified, and there are some parts that do not blend well with the base resin, and voids are formed at these parts because they do not blend well with the base resin. If voids exist in the composite resin composition, the resin and the fibers do not blend well at those parts even when the composite resin molded body is molded, so the voids remain as they are. The voids slightly reduce the elastic modulus of the composite resin molded body, but improve its impact resistance. In home appliance housings, especially mobile home appliances such as vacuum cleaners, cracking when dropped is a problem, so improvement in impact resistance is desired rather than elastic modulus. Therefore, it is preferable to have a few voids in the composite resin composition to improve impact resistance. The reason why voids improve impact resistance is that the shock waves propagated at the interface between the base resin and the fibrous filler during impact load are mitigated by the voids. The volume of the voids is calculated from the simulation results, and it is preferable that it is 10% or less of the volume of the fibrous filler.
[0027] The composite resin composition extruded from the melt kneader is cut into pellets using a pelletizer, etc. Pelletization methods include air hot cutting, underwater hot cutting, and strand cutting, which are performed immediately after the resin is melted, and also include a crushing method in which a molded body or sheet is molded and then crushed and cut.
[0028] Next, the shape of the composite resin composition (hereinafter, sometimes simply referred to as pellets) produced by this pelletization will be described. The pellets are made into various composite resin molded bodies through the following molding process. During the molding process, the composite resin composition enters a kneading machine such as a screw or roll, but depending on the shape of the screw or roll, the pellets are difficult to bite into. Therefore, in order to improve the intrusion into the molding device, it is preferable that the pellets have an uneven shape that makes it difficult to roll. In this embodiment, a method of cutting without cooling to below room temperature is adopted in the pelletization process. As a result, the cut surface is stretched as if it is torn off, and the shape of the pellet is not cylindrical but is an uneven shape with at least one side being elliptical. As a result, the intrusion of the pellets into the kneading machine of the molding device is improved.
[0029] In addition, when the pellets are torn off, the fibers inside the pellets partially protrude to the surface, forming irregularities on the surface. This also makes it possible to suppress the pellets from rolling compared to a smooth spherical or cylindrical shape, improving the ease of entry into the kneader of the molding device.
[0030] By injection molding these pellets, an injection molded article can be produced as a composite resin molding. As described above, the pellets have a structure in which only the ends are partially defibrated, so that the fibers are less likely to be oriented in the injection direction, and an injection molded article with both improved impact resistance and elastic modulus can be obtained. Below, each example and each comparative example in the experiments conducted by the inventors will be described.
[0031] Example 1 Pulp-dispersed polypropylene pellets were produced by the following production method.
[0032] Polypropylene (manufactured by Prime Polymer Co., Ltd., product name: J108M) as the base resin, cotton-like softwood pulp (manufactured by Mitsubishi Paper Mills Co., Ltd., product name: NBKP Celgar) as the fibrous filler, and maleic anhydride (manufactured by Sanyo Chemical Industries Co., Ltd., product name: Umex) as the dispersant were weighed out in a weight ratio of 85:15:5 and dry-blended. The softwood pulp had an elastic modulus of about 6 GPa, and the polypropylene had an elastic modulus of 1.5 GPa. The mixture was then melted, kneaded, and dispersed in a twin-screw kneader (KRC Kneader, manufactured by Kurimoto Iron Works Co., Ltd.). The shear force can be changed by changing the screw configuration of the twin-screw kneader, and in Example 1, a medium shear type was used. The resin melt was hot-cut to prepare pulp-dispersed polypropylene pellets.
[0033] The prepared pulp-dispersed polypropylene pellets were used to prepare test pieces of composite resin moldings using an injection molding machine (180AD manufactured by Japan Steel Works, Ltd.). The conditions for preparing the test pieces were resin temperature 190°C, mold temperature 60°C, injection speed 60mm / s, and holding pressure 80Pa. The pellets were fed into the screw of the molding machine through a hopper, and the penetration at that time was measured by the pellet loss per hour, and it was confirmed that it was constant. The shape of the test piece was changed depending on the evaluation items described below. A dumbbell of size 1 was prepared for the elastic modulus measurement, and a flat plate of 100 mm square and 5 mm thick was prepared for the drop impact test. The obtained pulp-dispersed polypropylene pellets and test pieces were evaluated by the following methods.
[0034] (Aspect ratio of undefibrated area, length ratio and diameter ratio of defibrated area) The obtained pulp-dispersed polypropylene pellets were immersed in a xylene solvent to dissolve the polypropylene, and the shape of the remaining pulp fibers was observed by SEM. Measurements of about 10 representative fibers showed that the fiber diameter was 2-10 μm, the fiber length was 200-1000 μm, and the aspect ratio of the non-defibrated portion (hereinafter sometimes simply referred to as the aspect ratio) was 100-200. Defibrated portions were observed at the ends in the fiber length direction, and the defibrated portions accounted for about 20-30% of the entire fiber length, and the fiber diameter in the defibrated portions was 100-1000 nm, about 1 / 20 of the entire fiber diameter.
[0035] (Pellet shape) In addition, because the shape of the obtained pulp-dispersed polypropylene pellets was produced by hot cutting, the cut part was cut while being stretched, and the shape had an elliptical bottom. In addition, the fibers tended to protrude from the surface, and it was confirmed under a microscope that the fibers were present on the surface. In addition, by observing the interface between the fibers and the base resin by SEM observation of the pellets, it was confirmed that there were voids with a volume of less than 10% of the volume of the fibers.
[0036] (Elastic modulus of composite resin molding) A tensile test was carried out using the No. 1 dumbbell-shaped test piece obtained. The elastic modulus was evaluated as follows: less than 1.8 GPa was x, 1.8 GPa or more but less than 2.0 GPa was △, and 2.0 GPa or more was ◯. The elastic modulus of the test piece was 2.2 GPa, and the evaluation was ◯.
[0037] (Drop test results for composite resin molded body) A drop impact test was carried out using the obtained flat plate-shaped test piece. Specifically, an iron ball weighing 300g was dropped from a height of 100cm onto the plate surface of the test piece to check whether cracks were formed. In this evaluation method, a test piece with no confirmed cracks was rated as ◯, a test piece with cracks only on the surface and less than 10mm long was rated as △, and a test piece with cracks that penetrated the plate or were 10mm or longer long was rated as ×. No cracks were confirmed in the test piece, and it was rated as ◯.
[0038] (Moldability) If the penetration of the pellets into the molding device (stability of penetration) is poor, the amount of resin supplied during molding will vary and moldability will also deteriorate, so the moldability of the composite resin molding was evaluated based on the penetration. Specifically, when the pellets were supplied to the molding device, the variation in the amount of pellet loss per unit time was less than 10%, and the variation was rated as △ when the variation was 10% or more. In Example 1, the variation in the amount of pellet loss was less than 10%, and the evaluation was ◯.
[0039] Example 2 In Example 2, the screw configuration was changed to a low shear type, and the conditions other than the screw configuration were the same as in Example 1 to produce pulp-dispersed polypropylene pellets and a molded body. The same evaluations as in Example 1 were also carried out.
[0040] Example 3 In Example 3, the screw configuration was changed to a high shear type, and the other conditions were the same as in Example 1 to produce pulp-dispersed polypropylene pellets and a molded body. The same evaluations as in Example 1 were also carried out.
[0041] Example 4 In Example 4, the fiber was changed to jute fiber obtained from hemp raw material, and pulp-dispersed polypropylene pellets and a molded body were produced in the same manner as in Example 1. The evaluation was also performed in the same manner as in Example 1.
[0042] Example 5 In Example 5, the method used for pellet preparation was changed to an underwater hot cutting method, and the other conditions were the same as in Example 1 to prepare pulp-dispersed polypropylene pellets and a molded body. The same evaluations as in Example 1 were also carried out.
[0043] Example 6 In Example 6, the pellet production method was changed to a method in which the resin melt was formed into a strand shape, which was then cooled with water and cut by a pelletizer, and the other conditions were the same as in Example 1 to produce pulp-dispersed polypropylene pellets and molded bodies. Evaluations were also performed in the same manner as in Example 1.
[0044] Example 7 In Example 7, the softwood pulp was changed to pulp fibers that were completely hydrophobically modified with a silane coupling agent in advance and were compatible with PP, and the other conditions were the same as in Example 1 to produce pulp-dispersed polypropylene pellets and molded bodies. Evaluations were also performed in the same manner as in Example 1.
[0045] Example 8 In Example 8, pulp-dispersed polypropylene pellets and a molded body were produced in the same manner as in Example 1, without adding maleic anhydride.
[0046] Comparative Example 1 In Comparative Example 1, the screw configuration was changed to only a conveying screw that was hardly subjected to shear, and the conditions other than the screw configuration were the same as in Example 1 to produce pulp-dispersed polypropylene pellets and a molded body. Evaluations were also performed in the same manner as in Example 1.
[0047] Comparative Example 2 In Comparative Example 2, the screw configuration was changed to a high shear type, and pulp-dispersed polypropylene pellets were produced in the same manner as in Example 1 except for the screw configuration. The obtained pellets were again put into the kneader to produce pulp-dispersed polypropylene pellets, and this was repeated to produce pulp-dispersed polypropylene pellets through the kneader a total of 10 times. Using these pellets, a molded body was produced in the same manner as in Example 1. Evaluations were also performed in the same manner as in Example 1.
[0048] Comparative Example 3 In Comparative Example 3, the coniferous pulp was changed to hardwood pulp, and the conditions other than the type of pulp were the same as in Example 1 to prepare pulp-dispersed polypropylene pellets and a molded body. The same evaluations as in Example 1 were also carried out.
[0049] Comparative Example 4 In Comparative Example 4, softwood pulp was crushed into powder in advance, and pulp-dispersed polypropylene pellets and a molded body were produced under the same conditions as in Example 1. Evaluations were also performed in the same manner as in Example 1.
[0050] Comparative Example 5 In Comparative Example 5, pulp-dispersed polypropylene pellets and a molded body were produced in the same manner as in Example 1, except that softwood pulp was used in which pulp fibers had been defibrated in advance by a wet defibration treatment. Evaluations were also performed in the same manner as in Example 1.
[0051] Comparative Example 6 In Comparative Example 6, the fibrous filler was changed to rubber fiber, and the other conditions were the same as in Example 1 to prepare pulp-dispersed polypropylene pellets and a molded body. The same evaluations as in Example 1 were also carried out.
[0052] Comparative Example 7 In Comparative Example 7, the fibrous filler was changed to glass fiber, and the other conditions were the same as in Example 1 to prepare pulp-dispersed polypropylene pellets and a molded body. The same evaluations as in Example 1 were also carried out. The measurement results for each of Examples 1 to 8 and Comparative Examples 1 to 7 are shown in Table 1.
[0053] [Table 1]
[0054] As is clear from Table 1, in Example 2 in which the screw configuration was changed to a low shear type, the fibers were not defibrated much in the molten resin, the aspect ratio was 5 to 20, the length ratio of the defibrated part was 5 to 10%, and the diameter of the defibrated part was about 1 / 10 of the whole. On the other hand, in Example 3 in which the screw configuration was changed to a high shear type, the fibers were well defibrated in the molten resin, the aspect ratio was 900 to 1000, the length ratio of the defibrated part was 40 to 50%, and the diameter of the defibrated part was about 1 / 50 of the whole. In both Examples 2 and 3, there were no problems with the modulus of elasticity, impact test, and moldability, as in Example 1, and it was confirmed that a high-strength resin can be obtained if the aspect ratio was 5 to 1000, the ratio of the defibrated part was 5 to 50%, and the diameter of the defibrated part was 1 / 10 or less of the whole diameter. In Example 4 in which the fibers were jute fibers obtained from hemp raw materials, there were no problems with the modulus of elasticity, impact test, and moldability, as in Example 1. Since the difference in elastic modulus between the resin and the fiber is within 20 GPa, impact resistance is not an issue, and it was confirmed that a high-strength resin could be obtained.
[0055] In Comparative Example 1, in which the screw configuration was changed to only a conveying screw that was hardly subjected to shear, the pulp was not defibrated in parts, with the proportion of defibrated areas being 0 to 4%. This resulted in a decrease in the elastic modulus of the composite resin molding, with the strength decreasing to 1.7 GPa.
[0056] In Comparative Example 2, in which the screw configuration was changed to a high shear type and the mixture was passed through the kneader 10 times, pulp defibration was significantly promoted and the length ratio of the defibrated area was 80-100%. This resulted in the fibers being more likely to be oriented during injection molding, which resulted in cracks occurring in the drop impact test and reduced impact resistance.
[0057] In Comparative Example 3, where softwood pulp was replaced with hardwood pulp, the defibration performance changed when the same shear force was applied, and the diameter of the defibrated area became about 1 / 5 of the total diameter. This resulted in a decrease in the elastic modulus and a decrease in strength to 1.7 GPa.
[0058] In Comparative Example 4, in which the softwood pulp was crushed into powder in advance, the aspect ratio was 1 to 2. This resulted in a decrease in the elastic modulus and a decrease in strength to 1.7 GPa.
[0059] In Comparative Example 5, which used pulp fibers in which softwood pulp had been previously wet-type defibration treated to further defibrate the fibers, the aspect ratio was large, ranging from 1000 to 2000. This made it easier for the fibers to be oriented during injection molding, resulting in cracks occurring in the drop impact test and reduced impact resistance.
[0060] In Comparative Example 6, where the fibrous filler was changed to rubber fiber, the elastic modulus of the rubber was 0.001 GPa, which was lower than that of the base resin PP. This resulted in a decrease in the elastic modulus and a decrease in strength to 1.4 GPa.
[0061] In Comparative Example 7, where the fibrous filler was changed to glass fiber, the elastic modulus of the glass was 68 GPa, which was more than 20 GPa higher than that of the main resin, PP. This resulted in stress being more likely to concentrate at the interface between the resin and the fiber upon impact, causing cracks in the drop impact test and reducing impact resistance.
[0062] In Example 5, in which the method used for pellet production was changed to the underwater hot cutting method, the molten resin was quenched, so a viscosity gradient occurred within the pellet, and the fibers were likely to move toward the inside where the viscosity was low, resulting in a state in which there were no fibers on the pellet surface. As a result, the pellets were less likely to interfere with each other during molding, the penetration ability was deteriorated, the productivity was unstable, and the moldability was somewhat inferior. On the other hand, there were no problems in the elastic modulus and impact tests.
[0063] In Example 6, the pellet production method was changed to a method in which the resin melt was made into a strand, which was then cooled with water and cut by a pelletizer. Since cylindrical strands were produced and then cut after cooling, the pellets were cylindrical. This caused the pellets to roll on the screw during molding, which resulted in poor penetration, unstable productivity, and slightly inferior moldability. However, there were no problems in the elastic modulus and impact tests.
[0064] In Example 7, in which the softwood pulp was changed to pulp fibers that were completely hydrophobically modified with a silane coupling agent in advance and were compatible with PP, the affinity between the fiber and PP increased, and there were no voids around the fiber. This resulted in stress being more likely to concentrate at the resin / fiber interface upon impact, resulting in slightly inferior impact resistance compared to other Examples. However, compared to Comparative Examples 1 to 7, it can be said that the elastic modulus and impact test results were superior.
[0065] In Example 8, where maleic anhydride was not added, the fibers and PP did not have an affinity with each other, and the volume of the voids around the fibers was about 70% of the volume of the fibers. This resulted in a slightly inferior elastic modulus compared to other Examples. However, compared to Comparative Examples 1 to 7, it can be said that the elastic modulus and impact test were superior.
[0066] From the above evaluation, it was found that by producing a molded body using resin pellets in which only the ends of the fibers added to the composite resin composition are defibrated, a high elastic modulus can be achieved even if the aspect ratio is not so high, and because the aspect ratio is not high, the fibers are less likely to be oriented during injection molding, and a composite resin molded body with high diametral impact strength can be provided. It was also found that the presence of fibers on the surface of the composite resin pellet and the elliptical shape of the bottom surface of the pellet improves the pellet penetration during molding and improves moldability. [Industrial Applicability]
[0067] The composite resin composition according to the present invention can provide a molded product having superior mechanical strength to conventional general-purpose resins. Since the properties of the base resin can be improved by the present invention, the composite resin composition can be used as a substitute for engineering plastics or metal materials. Therefore, the manufacturing cost of various industrial products or daily necessities made of engineering plastics or metals can be significantly reduced. Furthermore, the composite resin composition can be used for housings of home appliances, building materials, and automobile parts. [Explanation of symbols]
[0068] 1. Base resin 2. Fibrous filler 3 Defibration site
Claims
1. The material contains a thermoplastic resin as a base resin and cellulose as a fibrous filler, The end of the fibrous filler in the fiber length direction is defibrated, The defibrated portion at the end of the fibrous filler in the fiber length direction is 5% or more and 50% or less of the entire fiber length of the fibrous filler, The fiber diameter in the defibrated portion of the fibrous filler is 1 / 1000 or more and 1 / 10 or less of the fiber diameter in the non-defibrated portion, The aspect ratio of the fibrous filler in an undefibrated portion is 5 or more and 1000 or less, The elastic modulus of the fibrous filler is greater than the elastic modulus of the base resin. A composite resin molding comprising:
2. 2. The composite resin molding according to claim 1, wherein the base resin is an olefin resin.
3. 3. The composite resin molding according to claim 2, wherein the base resin is polypropylene.
4. A composite resin molding described in any one of claims 1 to 3, characterized in that voids exist at the interface between the base resin and the fibrous filler, and the volume of the voids is 10% or less of the volume of the fibrous filler.
5. 5. The composite resin molding according to claim 1, wherein a difference between a modulus of elasticity of the fibrous filler and a modulus of elasticity of the base resin is within 20 GPa.
Citation Information
Patent Citations
Method for producing high performance lignocellulosic fiber composites
JP2009516032A
Gas barrier film, fluid dispersion of cellulosic material and manufacturing method of gas barrier film
JP2016160406A
Method and apparatus for the manufacturing of composite material
US20160186382A1
Composition containing microfibrillated plant fibers
WO2011049162A1
Preparation of semiconductor integrated circuit
JP1980077176A