Fiber composite resin composition

JP2024161266AActive Publication Date: 2024-11-15PANASONIC HOLDINGS CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024153946
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-15
Estimated Expiration
2038-03-16

AI Technical Summary

Benefits of technology

【0013】 本発明の繊維複合樹脂組成物によると、繊維長方向の端部に疎水性の高い解繊された解繊部が形成された繊維状フィラーを主剤樹脂に複合できるため、繊維状フィラーを多く添加した場合でも、成型部品の強度を低下させることなく成形時の溶融粘度を低下させることができる。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024161266000001_ABST
    Figure 2024161266000001_ABST
Patent Text Reader

Abstract

To provide a fiber composite resin composition capable of realizing lowering of melt viscosity during melt molding, without deteriorating the strength of a molded product.SOLUTION: In the fiber composite resin composition, the melt kneading treatment is carried out together with the main resin 1, the dispersant, etc. without pretreatment by the wet dispersion for the purpose of defibering treatment and denaturation of the fibrous filler 2. As a result, the fibrous filler 2 is subjected to defibering from the end of the fibrous filler 2 in the direction of the fiber length, and, at the same time, the dispersing agent component for improving hydrophobicity which is charged simultaneously is selectively adsorbed to a defibered fiber 3 at the end that is defibered and has an expanded surface area. As a result, compared with a non-defibered part 4 having a median diameter of 5 μm or larger and 30 μm or smaller, hydrophobicization of the defibered part 3 having a median fiber diameter of 0.1 μm or larger and 2 μm or smaller is promoted, and a difference of the hydrophobic property in the fiber length direction of the fibrous filler 2 can be formed. Thus, even when the fibrous filler 2 is added in a large amount, without deteriorating the strength of the molded product, the melt viscosity during the melt molding can be decreased.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a fiber composite resin composition containing a fibrous filler. [Background technology]

[0002] So-called "general-purpose plastics" such as polyethylene (PE), polypropylene (PP), polystyrene (PS), and polyvinyl chloride (PVC) are not only very inexpensive, but also easy to mold and light in weight, a fraction of the weight of metals or ceramics. For this reason, general-purpose plastics are widely used as materials for a variety of everyday items such as bags, various types of packaging, various containers, and sheets, as industrial parts such as automobile parts and electrical parts, and as materials for daily necessities and miscellaneous goods.

[0003] However, general-purpose plastics have drawbacks such as insufficient mechanical strength, etc. Therefore, general-purpose plastics do not have sufficient properties required for materials used in mechanical products such as automobiles, and various industrial products including electrical, electronic, and information products, and the current situation is that the range of applications of general-purpose plastics is limited.

[0004] On the other hand, "engineering plastics" have excellent mechanical properties and are used in various industrial products, including mechanical products such as automobiles, and electrical, electronic and information products. However, engineering plastics have issues such as being expensive, the difficulty of monomer recycling, and a high environmental impact.

[0005] Therefore, there is a demand for a significant improvement in the material properties (mechanical strength, etc.) of general-purpose plastics. A technique is known for improving the mechanical strength of general-purpose plastics by dispersing fibrous fillers such as natural fibers, glass fibers, and carbon fibers in the resin of the general-purpose plastics. Among them, organic fibrous fillers such as cellulose are attracting attention as reinforcing fibers because they are inexpensive and have excellent environmental friendliness when disposed of.

[0006] However, when fibrous fillers are added to general-purpose plastics to improve their mechanical strength, the melt viscosity during molding increases, making precise molding impossible. For this reason, various companies are investigating ways to lower the melt viscosity. For example, in Patent Document 1, the melt viscosity of a fiber composite resin composition is lowered by adding a resin material with a low melting point. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2000-103915 A Summary of the Invention [Problem to be solved by the invention]

[0008] However, in Patent Document 1, a resin material having a lower molecular weight than the main resin is compounded, which reduces the melt viscosity during molding, but there is an issue that the strength of the molded product is reduced due to the influence of the low molecular weight resin material. The present invention is intended to solve the above-mentioned problems in the conventional art, and has an object to realize a reduction in the melt viscosity of a resin composition during molding without reducing the strength of the molded article. [Means for solving the problem]

[0009] In order to achieve the above object, the fiber composite resin composition of the present invention is composed of a fiber composite resin containing a fibrous filler in a main resin, and is characterized in that, at the end of each fibrous filler in the fiber length direction in the fiber composite resin, a defibrated portion having a median fiber diameter of 0.1 μm or more and 2 μm or less is formed which has higher hydrophobicity than a non-defibrated portion in the center of the fibrous filler having a median fiber diameter of 5 μm or more and 30 μm or less.

[0010] According to the fiber composite resin composition of the present invention, when the total amount of the base resin and the fibrous filler is taken as 100 mass%, it is preferable that the melt mass-flow rate (MFR) value of the resin composition defined in JIS K 7210 is 50% or more and less than 100% of the MFR value of the base resin, and the content of the fibrous filler is in the range of 10 mass% or more and 80 mass% or less.

[0011] According to the fiber composite resin composition of the present invention, it is preferable that the fibrous filler is a natural fiber of a cellulose family.

[0012] According to the fiber composite resin composition of the present invention, it is preferable that the base resin is an olefin-based resin. Effect of the Invention

[0013] According to the fiber composite resin composition of the present invention, a fibrous filler having a highly hydrophobic defibrated portion formed at the end in the fiber length direction can be compounded with a base resin, so that even when a large amount of fibrous filler is added, the melt viscosity during molding can be reduced without reducing the strength of the molded part. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 is a diagram showing the structure of a fiber composite resin composition according to an embodiment of the present invention. [Diagram 2] FIG. 1 is a flow diagram illustrating a manufacturing process for a fiber composite resin composition according to an embodiment of the present invention. [Diagram 3] FIG. 1 is a schematic diagram showing a molten flow state during molding using a fiber composite resin composition according to an embodiment of the present invention. [Figure 4] Schematic diagram showing other melt flow conditions during molding [Diagram 5] Schematic diagram showing still another melt flow state during molding [Figure 6] FIG. 1 is a graph showing the correlation between the amount of fibrous filler added and the MFR for Examples 1 to 2 and Comparative Examples 1 to 5. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS A fiber composite resin composition and a method for producing the same according to embodiments of the present invention will be described below with reference to the drawings.

[0016] The fiber composite resin composition according to the embodiment of the present invention is obtained from a melt-kneaded product containing a base resin, a fibrous filler, and a dispersant. In this fiber composite resin composition, as shown in FIG. 1, a fibrous filler 2 is dispersed in a base resin 1.

[0017] The main resin 1 must be a thermoplastic resin in order to ensure good moldability. Examples of thermoplastic resins include olefin resins (including cyclic olefin resins), styrene resins, (meth)acrylic resins, organic acid vinyl ester resins or derivatives thereof, vinyl ether resins, halogen-containing resins, polycarbonate resins, polyester resins, polyamide resins, thermoplastic polyurethane resins, polysulfone resins (polyethersulfone, polysulfone, etc.), polyphenylene ether resins (polymers of 2,6-xylenol, etc.), cellulose derivatives (cellulose esters, cellulose carbamates, cellulose ethers, etc.), silicone resins (polydimethylsiloxane, polymethylphenylsiloxane, etc.), rubber or elastomers (diene rubbers such as polybutadiene and polyisoprene, styrene-butadiene copolymers, acrylonitrile-butadiene copolymers, acrylic rubbers, urethane rubbers, silicone rubbers, etc.). The above resins may be used alone or in combination of two or more. The main resin 1 is not limited to the above materials as long as it has thermoplasticity.

[0018] Of these thermoplastic resins, the base resin 1 is preferably an olefin-based resin having a relatively low melting point. Examples of the olefin-based resin include homopolymers of olefin-based monomers, copolymers of olefin-based monomers, and copolymers of olefin-based monomers with other copolymerizable monomers. Examples of the olefin-based monomer include linear olefins (α-C2-20 olefins such as ethylene, propylene, 1-butene, isobutene, 1-pentene, 4-methyl-1-pentene, and 1-octene) and cyclic olefins. These olefin-based monomers may be used alone or in combination of two or more. Of the above olefin-based monomers, linear olefins such as ethylene and propylene are preferred. Examples of other copolymerizable monomers include fatty acid vinyl esters such as vinyl acetate and vinyl propionate; (meth)acrylic monomers such as (meth)acrylic acid, alkyl (meth)acrylate, and glycidyl (meth)acrylate; unsaturated dicarboxylic acids or their anhydrides such as maleic acid, fumaric acid, and maleic anhydride; vinyl esters of carboxylic acids (e.g., vinyl acetate and vinyl propionate); cyclic olefins such as norbornene and cyclopentadiene; and dienes such as butadiene and isoprene. These copolymerizable monomers may be used alone or in combination of two or more. Specific examples of olefin resins include copolymers of chain olefins (particularly α-C2-4 olefins) such as polyethylene (low density, medium density, high density, or linear low density polyethylene), polypropylene, ethylene-propylene copolymers, and terpolymers such as ethylene-propylene-butene-1.

[0019] Next, a description will be given of the fibrous filler 2. Each fibrous filler 2 has defibrated parts 3 formed at both ends in the length direction, and the remaining parts that are not defibrated, that is, non-defibrated parts 4.

[0020] The fibrous filler 2 is used in the resin composition of the present invention mainly for the purpose of improving mechanical properties and improving dimensional stability by reducing the linear expansion coefficient. For this purpose, the fibrous filler 2 preferably has a higher elastic modulus than the main resin 1. Specific examples of the fibrous filler 2 include natural fibers such as pulp, cellulose nanofiber, lignocellulose, lignocellulose nanofiber, cotton, silk, wool, or hemp; regenerated fibers such as jute fiber, rayon, or cupra; semi-synthetic fibers such as acetate and promix; synthetic fibers such as polyester, polyacrylonitrile, polyamide, aramid, and polyolefin; carbon fiber; carbon nanotubes; and modified fibers chemically modified on the surface and end thereof. Furthermore, among these, natural fibers of cellulose are particularly preferred from the viewpoints of availability, high elastic modulus, low linear expansion coefficient, and environmental friendliness.

[0021] The content of the fibrous filler 2 is preferably 10% by mass or more and 80% by mass or less, when the total amount of the base resin and the fibrous filler is taken as 100% by mass. By adding the fibrous filler 2, it is possible to expect an improvement in mechanical strength, but if the amount is less than this range, the mechanical strength cannot be sufficiently increased, and conversely, if the amount is more than this range, the dispersibility of the fibrous filler is drastically reduced.

[0022] Next, the dispersant will be described.

[0023] A dispersant is added to the fibrous filler 2 for the purpose of improving dispersibility in the base resin 1, adhesion to the base resin 1, and hydrophobicity in the fiber composite resin composition. Furthermore, in the present invention, the dispersant imparts higher hydrophobicity to the defibrated parts 3 of the fibrous filler 2 than to the non-defibrated parts 4.

[0024] Examples of dispersants for this purpose include various titanate coupling agents, silane coupling agents, modified polyolefins grafted with unsaturated carboxylic acids, maleic acid, and maleic anhydride, and dispersants surface-treated with fatty acids, fatty acid metal salts, fatty acid esters, etc. The dispersant may be one surface-treated with a thermosetting or thermoplastic polymer component.

[0025] The content of the dispersant in the fiber composite resin composition is preferably 0.01% by mass or more and 20% by mass or less, more preferably 0.1% by mass or more and 10% by mass or less, and even more preferably 0.5% by mass or more and 5% by mass or less, based on the amount of the main resin 1. If the content of the dispersant is less than 0.01% by mass, poor dispersion occurs. On the other hand, if the content of the dispersant exceeds 20% by mass, the strength of the molded product produced using the fiber composite resin composition decreases. The type and amount of the dispersant to be used are appropriately selected depending on the combination of the main resin 1 and the fibrous filler 2.

[0026] Next, a method for producing the fiber composite resin composition will be described.

[0027] FIG. 2 is a flow diagram illustrating a production process of a fiber composite resin composition according to an embodiment of the present invention.

[0028] First, the base resin 1, the fibrous filler 2, and the dispersant for improving hydrophobicity are put into the melt-kneading processing device, and are melt-kneaded in the melt-kneading processing device. This melts the base resin 1, and the fibrous filler 2 and the dispersant are dispersed in the molten base resin 1. At the same time, the shearing action of the device promotes defibration of agglomerates of the fibrous filler 2, allowing the fibrous filler 2 to be finely dispersed in the base resin 1.

[0029] Conventionally, the fibrous filler 2 used is one in which the fibers have been defibrated in advance by a pretreatment such as wet dispersion. However, if the fibrous filler 2 is defibrated in advance in a solvent used in wet dispersion, it is easier to defibrate than in the molten base resin 1, so it is difficult to defibrate only the ends, and the entire fibrous filler 2 ends up in a defibrated state. For this reason, it is not possible to form a difference in hydrophobicity along the fiber length direction of the fibrous filler 2 as in the present invention described below. In addition, there is a problem that the number of steps increases by incorporating a pretreatment, which reduces productivity.

[0030] In contrast, in the manufacturing process of the fiber composite resin composition in this embodiment, the fibrous filler 2 is subjected to a melt kneading process together with the base resin 1 and a dispersant, without performing a pretreatment by wet dispersion for the purpose of defibrating and modifying the fibrous filler 2. In this method, since the wet dispersion treatment of the fibrous filler 2 is not performed in the pretreatment stage, defibration proceeds from the end of the fibrous filler 2 in the fiber length direction, and at that time, the component of the dispersant for improving hydrophobicity, which is simultaneously added, is more selectively adsorbed to the defibrated part 3 at the fiber end whose surface area has been increased by defibration. This promotes hydrophobicity of the defibrated part 3 compared to the non-defibrated part 4, and a difference in hydrophobicity can be formed along the fiber length direction of the fibrous filler 2. In addition, the number of steps is small, and productivity can be improved.

[0031] The hydrophobic state of the fibrous filler 2 has been confirmed as follows: That is, from the results of experiments conducted by the present inventors, it has been confirmed that in a dispersed state in the base resin 1, in the non-defibrated portion 4, gaps are generated between the non-defibrated portion 4 and the hydrophobic base resin 1, whereas in the defibrated portion 3, no gaps are observed between the non-defibrated portion 4 and the hydrophobic base resin 1, improving adhesion, and the hydrophobicity of the defibrated portion 3 relative to the non-defibrated portion 4 is promoted.

[0032] 3, 4 and 5 are schematic cross-sectional views showing the difference in melt flow state during molding due to the difference in fiber shape and hydrophobicity of the fibrous filler 2.

[0033] 3 shows the melt flow state when a resin composition according to an embodiment of the present invention is used. Here, the fibrous filler 2 has a highly hydrophobic defibrated portion 3 formed at its end, and the other portion has a non-defibrated portion 4 having a lower hydrophobicity than the defibrated portion 3. In other words, the fibrous filler 2 has a difference in hydrophobicity in the fiber length direction, so that the flow of the hydrophobic main resin 1 is easily rectified. This effect makes it possible to reduce the melt viscosity during molding even when a large amount of fibrous filler 2 is added.

[0034] In Fig. 4, the fibrous filler 2 is strongly, i.e. excessively, defibrated, and only the defibrated parts 3 are dispersed in the form of short fibers, with no clear non-defibrated parts, and therefore it is not possible to form a difference in hydrophobicity in the fiber length direction of the fibrous filler 2. Furthermore, the total surface area of ​​the fibrous filler 2 is very large. For this reason, when a large amount of fibrous filler 2 is added, the melt viscosity during molding increases, making it impossible to perform precise molding.

[0035] In FIG. 5, the fibrous filler 2 is not fully defibrated, the fiber diameter of the non-defibrated parts 4 is large, and the fibrous filler 2 is dispersed with almost no defibrated parts 3. Therefore, the difference in hydrophobicity in the fiber length direction of the fibrous filler 2 is not fully formed. As a result, the flow of the hydrophobic main resin 1 is not easily rectified in the flow direction, and the fibers are easily entangled and form agglomerates, which impedes flowability. As a result, when a large amount of fibrous filler 2 is added, the melt viscosity during molding increases, making it impossible to perform precise molding.

[0036] Regarding the optimal form of the fibrous filler 2, the results of experiments and simulations conducted by the inventors have confirmed that the median fiber diameter of the defibrated portion 3 is 0.1 μm or more and 2 μm or less, and the median fiber diameter of the non-defibrated portion 4 is 5 μm or more and 30 μm or less.

[0037] The fiber composite resin extruded from the melt kneader is cut into pellets using a pelletizer or similar device. Pelletization methods include air hot cutting, underwater hot cutting, and strand cutting, which are performed immediately after the resin is melted. Alternatively, a crushing method is used in which a molded product or sheet is first formed, and then the molded product is crushed and cut.

[0038] According to the present invention, as described above, defibration proceeds from the end in the fiber length direction of the composite fibrous filler 2, and at that time, the dispersant component for improving hydrophobicity, which is added at the same time, is more selectively adsorbed to the defibrated part 3 at the fiber end that has been defibrated and has an expanded surface area. This promotes hydrophobicity of the defibrated part 3 compared to the non-defibrated part 4, resulting in a structure in which a difference in hydrophobicity is formed in the fiber length direction of the fibrous filler 2. For this reason, even when a large amount of fibrous filler 2 is added, the melt viscosity during molding can be reduced, and a fiber composite resin composition can be obtained that has both high rigidity due to the addition of fibrous filler 2 and improved flowability in a mold or the like during melt molding.

[0039] Regarding the flowability, specifically, when the total amount of the base resin and the fibrous filler is taken as 100 mass%, the content of the fibrous filler is in the range of 10 mass% to 80 mass%, and the melt mass flow rate of the resin composition as defined by JIS K 7210 can be set to a value of 50% or more and less than 100% of the melt mass flow rate of the base resin. In other words, when the melt mass flow rate value is small, it means that the viscosity is high and the flowability is poor, but according to the present invention, as described above, a value of 50% or more of the melt mass flow rate of the base resin can be achieved. In other words, the decrease in flowability can be suppressed within a sufficiently tolerable range. EXAMPLES

[0040] Examples and comparative examples based on experiments conducted by the present inventors will be described below.

[0041] Example 1 Pulp-dispersed polypropylene pellets were produced by the following production method, and various evaluations were carried out using the pellets.

[0042] That is, the content of cotton-like softwood pulp (manufactured by Mitsubishi Paper Mills, product name: NBKP Celgar) as a fibrous filler was weighed out under each condition where the content of the cotton-like softwood pulp (manufactured by Prime Polymer, product name: J108M) as a base resin was 0, 10, 15, 20, 50, 80, 85, and 90% by mass when the total amount of the base resin and the fibrous filler was 100% by mass. Then, under each of these conditions, maleic anhydride (manufactured by Sanyo Chemical Industries, product name: Umex) as a dispersant for improving hydrophobicity was weighed out so that it was 5 parts by mass with respect to 100 parts by mass of polypropylene as the base resin, and dry blended. For example, under the condition where the cotton-like softwood pulp was 15% by mass, 85% by mass of polypropylene and 4.25% by mass of maleic anhydride were weighed out. Thereafter, the mixture was melt-kneaded and dispersed using a twin-screw kneader (S-1KRC kneader manufactured by Kurimoto Iron Works, Ltd.: screw diameter φ25 mm, L / D=10.2).

[0043] At this time, the shear force can be changed by changing the screw configuration of the twin-screw kneader. In Example 1, a medium shear type was used, and the kneading section temperature was set to 180°C and the extrusion speed was set to 0.5 kg / h. Furthermore, the melt kneading dispersion treatment under these conditions was repeated 10 times for a long time treatment. The resin melt was then hot-cut to prepare pulp-dispersed polypropylene pellets. The obtained pulp-dispersed polypropylene pellets were evaluated by the following method.

[0044] (Median fiber diameter of the non-defibrated part, Median fiber diameter of the defibrated part) The pulp-dispersed polypropylene pellets prepared under each of the above conditions were immersed in a xylene solvent to dissolve the polypropylene, and the remaining pulp fibers were observed using an SEM. Specifically, approximately 100 representative fibers were measured using an SEM (Phenom G2pro scanning electron microscope, manufactured by PHENOM-World). The median fiber diameter was calculated from the fiber diameter measurement results, and the median fiber diameter of the non-defibrated portion was 5.2 μm to 9.8 μm, and a defibrated portion was observed at the end in the fiber length direction, with the median fiber diameter of the defibrated portion being 0.3 μm to 0.7 μm.

[0045] (Melt Mass Flow Rate) Using the pulp-dispersed polypropylene pellets prepared under each of the above conditions, the melt mass-flow rate (MFR) was measured in accordance with JIS K 7210. Since the main resin was polypropylene, the measurement was performed under the conditions of test temperature = 230°C and test load = 2.16 kg (JIS K 6921-1).

[0046] Example 2 The change from Example 1 was that the melt kneading dispersion treatment was repeated three times. The other conditions were the same as in Example 1 to prepare pulp-dispersed polypropylene pellets. The evaluation was also performed in the same manner as in Example 1.

[0047] Comparative Example 1 The difference from Example 1 was that pulp fibers in which the fibers had been defibrated by previously subjecting cotton-like softwood pulp to a wet defibration treatment were used. Other than that, pulp-dispersed polypropylene pellets were produced in the same manner as in Example 1. Evaluation was also performed in the same manner as in Example 1.

[0048] Comparative Example 2 The screw configuration was changed to a high shear type compared to Example 1. Pulp-dispersed polypropylene pellets were produced under the same conditions as in Example 1. Evaluations were also performed in the same manner as in Example 1.

[0049] Comparative Example 3 The screw configuration was a high shear type similar to that of Comparative Example 2, and the melt kneading dispersion with this screw configuration was shortened to three treatments. The other conditions were the same as in Example 1, and pulp-dispersed polypropylene pellets were produced. Evaluation was also performed in the same manner as in Example 1.

[0050] Comparative Example 4 The screw configuration was a high shear type similar to that of Comparative Example 2, and the melt kneading dispersion with this screw configuration was shortened to one treatment. The other conditions were the same as in Example 1, and pulp-dispersed polypropylene pellets were produced. Evaluation was also performed in the same manner as in Example 1.

[0051] Comparative Example 5 The screw configuration was changed to a low shear type compared to Example 1. Pulp-dispersed polypropylene pellets were produced under the same conditions as in Example 1. Evaluations were also performed in the same manner as in Example 1.

[0052] The evaluation results for Examples 1 and 2 and Comparative Examples 1 to 5 are shown in Table 1. Moreover, the correlation of MFR with the amount of fibrous filler added for Examples 1 and 2 and Comparative Examples 1 to 5 based on those measurement results is shown in FIG.

[0053] [Table 1]

[0054] As is clear from Table 1 and Fig. 6, in Examples 1 and 2 in which a fibrous filler was added to achieve a defibrated state in which the median fiber diameter of the non-defibrated portion was 5 μm or more and 30 μm or less, and the median fiber diameter of the defibrated portion was 0.1 μm or more and 2 μm or less, defibration proceeded from the end of the fiber length direction of the fibrous filler, and the dispersant component for improving hydrophobicity, which was added at the same time, was more selectively adsorbed to the defibrated portion at the end whose surface area was expanded by defibration, promoting hydrophobicity compared to the non-defibrated portion, and forming a difference in hydrophobicity in the fiber length direction of the fibrous filler. Therefore, due to the effect of easily rectifying the flow direction of the hydrophobic base resin, it was confirmed that the MFR value of the fiber composite resin composition was 50% or more and less than 100% of the MFR value of the base resin when the content of the fibrous filler was 10% by mass or more and 80% by mass or less with respect to the amount of the base resin. In other words, it was confirmed that flowability under normal molding conditions was ensured.

[0055] In contrast, in Comparative Example 1, in which pulp fibers in which pulp fibers had been defibrated in advance by wet defibration treatment of cotton-like softwood pulp as a fibrous filler were used, the fibrous filler was extremely susceptible to defibration in the molten resin, making it difficult to defibrate only the ends, and the entire fibrous filler ended up in a defibrated state. As a result, it was not possible to form a difference in hydrophobicity in the fiber length direction of the fibrous filler, and furthermore, because the surface area of ​​the fibrous filler was large, the MFR dropped significantly when the fibrous filler content was in the range of 15 mass% or more relative to the amount of the base resin, resulting in failure to ensure flowability under normal molding conditions.

[0056] In Comparative Example 2, in which the screw configuration was changed to a high shear type, the median fiber diameter of the defibrated portion was thinned to less than 0.1 μm due to excessive shear, and the median fiber diameter of the non-defibrated portion was also too thin, at 0.9 μm or more and 1.3 μm or less, so that the difference in hydrophobicity of the fibrous filler in the fiber length direction was too small to achieve the effects of the present invention. In other words, the large surface area of ​​the fibrous filler also caused a large decrease in MFR when the fibrous filler content was in the range of 10 mass% or more relative to the amount of the main resin, resulting in failure to ensure flowability under normal molding conditions.

[0057] In Comparative Example 3, in which the screw configuration was changed to a high shear type as in Comparative Example 2, and the number of melt kneading dispersion treatments was reduced to three times to a short-time treatment, the median fiber diameter of the defibrated portion was defibrated to a fine state of 0.5 μm to 0.8 μm, and although a difference in hydrophobicity in the fiber length direction of the fibrous filler was formed to a certain extent, it was not to a degree that could exert the effects of the present invention. Moreover, the surface area of ​​the fibrous filler became too large, also due to the fact that the median fiber diameter of the non-defibrated portion was defibrated too finely to 2.2 μm to 4.1 μm, and as a result, the MFR significantly decreased when the content of the fibrous filler was in the range of 15 mass% or more relative to the amount of the main resin, and as a result, flowability under normal molding conditions could not be ensured.

[0058] In Comparative Example 4, which was changed from Comparative Example 3 by reducing the number of melt kneading dispersion treatments to one and changing to a short-time treatment, the median fiber diameter of the defibrated part was 1.0 μm or more and 1.5 μm or less, and was sufficiently defibrated, but the median fiber diameter of the non-defibrated part (including insufficiently loosened parts) was 35.2 μm or more and 38.4 μm or less, so that although a difference in hydrophobicity in the fiber length direction of the fibrous filler was formed to some extent, it was not to the extent that the effect of the present invention could be exerted. Furthermore, since the fibers were easily entangled with each other and tended to form agglomerates, the MFR was greatly reduced when the content of the fibrous filler was in the range of 20 mass% or more of the main resin amount due to the influence of impeding flowability, and as a result, flowability under normal molding conditions could not be ensured.

[0059] In Comparative Example 5, in which the screw configuration was changed to a low shear type, the median fiber diameter of the non-defibrated portion was thinned to 20.5 μm or more and 25.2 μm or less, but due to the low shear, the median fiber diameter of the defibrated portion was 2.2 μm or more and 3.0 μm or less, resulting in insufficient defibration, and therefore the difference in hydrophobicity in the fiber length direction of the fibrous filler was not sufficiently formed, and the effects of the present invention could not be achieved. Furthermore, the flow was not easily rectified in the flow direction of the hydrophobic base resin, and the fibers were easily entangled and easily formed into agglomerates, which also had the effect of impeding flowability, and the MFR significantly decreased when the content of the fibrous filler was in the range of 50 mass% or more of the base resin amount, resulting in the flowability not being ensured under normal molding conditions.

[0060] From the above evaluation results, according to the present invention, the median fiber diameter of the non-defibrated portion in the fiber length direction of the fibrous filler is 5 μm or more and 30 μm or less, and the median fiber diameter of the defibrated portion is 0.1 μm or more and 2 μm or less, the hydrophobicity of the defibrated portion is promoted compared to the non-defibrated portion, and the difference in hydrophobicity in the fiber length direction of the fibrous filler can be made large, which has the effect of making the fibrous filler more likely to be rectified in the flow direction of the hydrophobic main resin. As a result, it was found that when the content of the fibrous filler is in the range of 10 mass% or more and 80 mass% or less of the main resin amount, the MFR value is 50% or more and less than 100% of the MFR value of the main resin, and therefore a fiber composite resin composition that can ensure flowability under normal molding conditions can be provided. [Industrial Applicability]

[0061] The present invention can provide a fiber composite resin composition that has both high rigidity and improved flowability into a mold or the like during melt molding due to the addition of a fibrous filler. This resin composition can be used as a substitute for engineering plastics or metal materials. Therefore, the manufacturing costs of various industrial products or daily necessities made of engineering plastics or metals can be significantly reduced. Furthermore, it can be used in home appliance housings, building materials, and automobile parts. [Explanation of symbols]

[0062] 1. Base resin 2. Fibrous filler 3. Fiber Defibration Section 4 Non-fibrillated section

Claims

[Claim 1] A fiber composite resin composition comprising a base resin containing a fibrous filler, and at the ends in the fiber length direction of the fibrous filler, defibrated parts having a median fiber diameter of 0.1 μm or more and 2 μm or less are formed, which have higher hydrophobicity than a non-defibrated part in a central part in the fiber length direction of the fibrous filler, which has a median fiber diameter of 5 μm or more and 30 μm or less.

Citation Information

Patent Citations

  • High strength aramide fiber reinforcing composite material having fibrilated terminal

    JP1986143440A

  • Method for producing cellulose-containing thermoplastic resin, the cellulose-containing thermoplastic resin, and molded body of the same

    JP2011219571A

  • Fiber-reinforced plastic

    JP2012246459A

  • Composite material and production of its molded product

    JP2000103915A