By employing a second metal halide gas to react with and remove adhered titanium from the side walls of recesses in semiconductor manufacturing, the method addresses the resistance issue, enhancing the conductivity of semiconductor devices.
Patent Information
- Application Number
- JP2023076830
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-08
- Publication Date
- 2024-11-20
AI Technical Summary
The challenge in semiconductor manufacturing is the adherence of first metals, such as titanium, to the side walls of recesses, which increases resistance due to their higher resistance values, especially as semiconductor devices become more integrated, reducing the opening area and increasing interconnect resistance.
A method using a second metal halide gas, such as tungsten tetrachloride (WCl5), to react with the first metal, like titanium, forming a metal silicide layer and removing the adhered titanium from the side walls of recesses within a substrate processing apparatus.
This approach effectively reduces the increase in wiring resistance by removing the adhered titanium, maintaining the integrity of the conductive layer and ensuring efficient conductivity within the semiconductor devices.
Smart Images

Figure 2024161798000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for processing a substrate and an apparatus for processing a substrate. [Background technology]
[0002] In the manufacturing process of a semiconductor device, a process is performed in which a recess such as a via hole or a trench is formed in an insulator layer formed on a semiconductor wafer (hereinafter also referred to as a "wafer"), which is a substrate, and a conductor, which is a wiring material, is embedded in the recess. At this time, in order to electrically connect the member on the lower layer side of the insulator layer and the conductor embedded in the recess, a metal layer for contact (e.g., a titanium (Ti) layer) may be formed before embedding the conductor.
[0003] Patent Document 1 describes a technique for removing a TiN film formed on the sidewall of a contact hole by wet etching when forming a TiN film used as a barrier metal on the bottom surface of the contact hole. Patent Document 2 describes a technique for forming titanium silicide, which serves as a first contact material, on the bottom surface of the contact hole. Titanium silicide is formed by forming a titanium film on a silicon oxide film stacked on a transfer electrode film made of polysilicon at the bottom surface of the contact hole, and silicidizing the titanium film by annealing. At this time, unreacted titanium that has not been silicided is selectively etched away with a mixed solution of ammonia and hydrogen peroxide. Thus, Cited Documents 1 and 2 disclose techniques for removing TiN or titanium by wet etching. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2009-26864 A [Patent Document 2] JP 2011-238751 A Summary of the Invention [Problem to be solved by the invention]
[0005] The present disclosure provides a technique for removing a first metal attached to a sidewall surface of a recess by using a second metal halide gas that reacts with the first metal. [Means for solving the problem]
[0006] The present disclosure provides a method for processing a substrate, comprising: supplying a first metal halide gas to the substrate, the substrate having an insulating layer stacked on silicon and a recess formed in the insulating layer, to form a metal layer of a first metal contained in the first metal halide on a surface of the silicon exposed in the recess; Next, a second metal halide gas containing a second metal different from the first metal and reacting with the first metal is supplied to the substrate on which a metal silicide layer has been formed by diffusing the silicon into the metal layer, and the first metal adhering to the sidewall surface of the recess is removed. Effect of the Invention
[0007] According to the present disclosure, the first metal attached to the sidewall surface of the recess can be removed by the second metal halide gas that reacts with the first metal. [Brief description of the drawings]
[0008] [Figure 1A] FIG. 11 is a first enlarged vertical cross-sectional side view of a wafer according to a comparative embodiment. [Figure 1B] FIG. 11 is a second enlarged vertical cross-sectional side view of the wafer according to the comparative embodiment. [Figure 1C] FIG. 11 is a third enlarged vertical sectional side view of the wafer according to the comparative embodiment. [Figure 1D] FIG. 11 is a fourth enlarged vertical cross-sectional side view of the wafer according to the comparative embodiment. [Diagram 2] 1 is a plan view showing a configuration example of a substrate processing apparatus according to an embodiment; [Diagram 3]2 is a vertical sectional side view showing a configuration example of a Ti film formation module provided in the substrate processing apparatus. FIG. [Figure 4] 1 is an explanatory diagram showing an example of a flow of a wafer process according to an embodiment; [Figure 5A] 2 is a first enlarged vertical cross-sectional side view of a wafer according to an embodiment. FIG. [Figure 5B] FIG. 4 is a second enlarged vertical cross-sectional side view of the wafer according to the embodiment. [Figure 5C] FIG. 4 is a third enlarged vertical cross-sectional side view of the wafer according to the embodiment. [Figure 6] FIG. 13 is a plan view showing a modified example of the substrate processing apparatus. [Figure 7] FIG. 11 is a plan view showing an example of the configuration of a substrate processing apparatus according to a second embodiment. [Figure 8] FIG. 11 is an explanatory diagram showing an example of a flow of a wafer processing according to the second embodiment. [Figure 9] 4 is an electron microscope photograph of a vertical cross section of a wafer according to a reference example and an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] <Comparative form> Before describing the processing of a substrate (substrate treatment) according to an embodiment of the present disclosure, the contents of substrate treatment according to a comparative embodiment will be described with reference to FIGS. 1A to 1D, and problems associated with the substrate treatment will be discussed. The enlarged vertical cross-sectional view of FIG. 1A shows a configuration in the vicinity of the surface of a wafer W that is the subject of substrate processing according to a comparative embodiment.
[0010] A wafer W on which the substrate processing according to the comparative embodiment is performed has a silicon (Si) layer 61 and a SiO layer 62, which is an insulating layer, laminated thereon, and a recess 60 is formed in the SiO layer 62. A SiN layer 63 used for patterning the recess 60 is formed on the side wall of the recess 60.
[0011] In the wafer W having the above configuration, before a conductor is embedded in the recess 60, a Ti layer 64a, which is a metal layer for contact, is formed on the bottom of the recess 60 (FIG. 1A). Silicon (Si) atoms are diffused from the Si layer 61 into the Ti layer 64a, forming a TiSi layer 64 as shown in FIG. 1B. Thereafter, a conductor such as a Ru film 66 is formed on the wafer W, and Ru is embedded in the recess 60 (FIG. 1C). After that, the upper surface side of the wafer W is removed by CMP (Chemical Mechanical Polishing), and a wafer W having Ru wiring 66a embedded in the recess 60 can be obtained as shown in FIG. 1D.
[0012] 1A, when forming the Ti layer 64a on the bottom of the recess 60, Ti may adhere in a spotty manner to the sidewall surface of the recess 60. Hereinafter, the Ti adhered to the sidewall surface of the recess 60 is also referred to as adhered Ti 65.
[0013] Ti has a higher resistance value than Ru. Meanwhile, with the increase in the integration density of semiconductor devices, the opening area of the recess 60 is becoming smaller and smaller. For example, when the deposited Ti 65 is formed on both side walls of the recess 60 with an opening diameter of 10 nm, the opening diameter of the recess 60 is reduced by about 10 to 20% even if the thickness of the deposited Ti 65 is about 0.5 to 1.0 nm. As a result, the buried area of the Ru wiring 66a is reduced, and the wiring resistance may increase.
[0014] Therefore, in the substrate processing of this embodiment described below, after the Ti layer 64a (TiSi layer 64) is formed, a process is performed to remove the attached Ti 65 attached to the side wall of the recess 60. Specific contents of the substrate processing according to this embodiment will be described below with reference to Figs. 2 to 5C.
[0015] <Substrate processing device 1> 2 and 3, an embodiment of an apparatus (hereinafter referred to as "substrate processing apparatus 1") for forming a contact TiSi layer 64 in a recess 60 formed in a wafer W and then forming a Ru film 66 will be described. Fig. 1 is a schematic plan view showing an example of the configuration of the substrate processing apparatus 1. The substrate processing apparatus 1 includes an atmospheric transfer chamber 11, a load lock chamber 12, a first substrate transfer chamber 13, a second substrate transfer chamber 14, and a plurality of processing modules 151-154.
[0016] The first substrate transfer chamber 13 and the second substrate transfer chamber 14 are each configured to have a rectangular shape in a plan view, and are connected via, for example, two transfer units 17. The insides of the first and second substrate transfer chambers 13, 14 and the transfer unit 17 are set to a vacuum pressure atmosphere, and the pressures are configured to be the same. In addition, first and second transfer mechanisms 131, 141 are disposed inside the first and second substrate transfer chambers 13, 14, respectively.
[0017] The transfer unit 17 is configured to transfer the wafer between the first transfer mechanism 131 provided in the first substrate transfer chamber 13 and the second transfer mechanism 141 provided in the second substrate transfer chamber 14. The first substrate transfer chamber 13, the second substrate transfer chamber 14 and the transfer unit 17 correspond to the vacuum transfer chamber in this embodiment. The first transfer mechanism 131 and the second transfer mechanism 141 correspond to the substrate transfer mechanism in this embodiment.
[0018] The direction in which these substrate transfer chambers 13, 14 are lined up is the length direction, with the first substrate transfer chamber 13 at the front side and the second substrate transfer chamber 14 at the rear side. In this case, an atmospheric transfer chamber 11 set to an atmospheric pressure atmosphere is connected to the front side of the first substrate transfer chamber 13 via, for example, three load lock chambers 12. Between the first and second substrate transfer chambers 13, 14 and the transfer section 17, between the load lock chamber 12 and the first substrate transfer chamber 13, and between the load lock chamber 12 and the atmospheric transfer chamber 11, there are wafer transfer ports and gate valves for opening and closing the transfer ports, respectively, but these are omitted from the drawing.
[0019] For example, four load ports 101 are connected to the atmospheric transfer chamber 11, and a carrier C accommodating a plurality of wafers W is placed on each load port 101. An atmospheric transfer mechanism 111 is provided in the atmospheric transfer chamber 11, and can transfer the wafers W between the carrier C connected to the atmospheric transfer chamber 11 and the load lock chamber 12.
[0020] As viewed from the front side, one COR (Chemical Oxide Removal) module 151, one PHT (Post Heat Treatment) module 152, and two Ti film formation modules 153 are connected to each of the two left and right walls of the first substrate transfer chamber 13. A first transfer mechanism 131 provided in the first substrate transfer chamber 13 is configured to transfer wafers W between these four modules 151 to 153, the transfer section 17, and the load lock chamber 12. In FIG. 2, symbol GV1 indicates a gate valve.
[0021] The COR process performed in the COR module 151 and the PHT process performed in the PHT module 152 are pre-cleaning processes for removing the native oxide film (SiOx) on the surface of the Si layer 61 exposed in the recess 60. Specifically, the COR module 151 uses hydrogen fluoride (HF) gas and ammonia (NH 3 The PHT module 152 is configured to perform an etching process (COR process) of the native oxide film by using a fluorine-containing oxide (HFO) gas. The PHT module 152 is also configured to perform a PHT process in which the reaction products generated in the COR process are sublimated and removed by heating the wafer W.
[0022] In addition, the Ti film forming module 153 is configured to form a Ti layer 64a, which serves as a contact metal layer provided between the Si layer 61 and the Ru wiring 66a. Further, the Ti film forming module 153 also has a function of removing the adhered Ti 65 attached to the side wall surface of the recess 60 by forming the Ti layer 64a. From the perspective of forming the Ti layer 64a, the Ti film forming module 153 corresponds to the first processing module of the present embodiment. Also, from the perspective of removing the adhered Ti 65 attached to the side wall surface of the recess 60, the Ti film forming module 153 also corresponds to the second processing module of the present embodiment. A specific configuration example of the Ti film forming module 153 will be described in detail later with reference to FIG. 3.
[0023] Also, when viewed from the front side, a total of four Ru film forming modules 154, two on each of the left and right wall portions of the second substrate transfer chamber 14, are connected. And the second transfer mechanism 141 is configured to transfer the wafer W between these four Ru film forming modules 154 and the transfer portion 17. In FIG. 2, the reference numeral GV2 indicates a gate valve.
[0024] Each Ru film forming module 154 is configured to form a Ru film 66, for example, by CVD (Chemical Vapor Deposition) method using a raw material gas of Ru which is a conductor. The Ru film forming module 154 corresponds to the fourth processing module of the present embodiment.
[0025] <Ti film forming module 153> Next, a specific configuration example of the Ti film forming module 153 will be described with reference to FIG. 3. The Ti film forming module 153 is configured to supply a film forming gas containing a first metal halide gas, which will be described later, to the wafer W and form the Ti layer 64a by plasma CVD method. Also, the Ti film forming module 153 has a function of supplying a second metal halide gas, which will be described later, to the wafer W after the Ti layer 64a is formed to remove the adhered Ti 65 on the side wall surface of the recess 60.
[0026] 3 is a vertical cross-sectional side view of the Ti film forming module 153 of this embodiment. The Ti film forming module 153 includes a substantially cylindrical processing vessel 210 made of a metal that is resistant to corrosion by chlorine and is grounded. A cylindrical exhaust chamber 211, for example, protruding downward is formed in the center of the bottom surface of the processing vessel 210, and an exhaust path 212 is connected to the side of the exhaust chamber 211. A vacuum exhaust unit 213 including a pressure adjustment valve, for example, a butterfly valve, and a vacuum pump is connected to the exhaust path 212. The vacuum exhaust unit 213 serves to evacuate the processing vessel 210 to a preset vacuum pressure. The processing of the wafer W is performed in the space inside the processing vessel 210.
[0027] A loading / unloading port 214 is formed on the side of the processing vessel 210 for loading / unloading the wafer W between the processing vessel 210 and the first substrate transfer chamber 13. The loading / unloading port 214 is configured to be freely opened and closed by a gate valve 215 (GV1 in FIG. 2). Furthermore, a heater 216 for adjusting the temperature inside the processing vessel 210 is embedded in a wall portion constituting the processing vessel 210.
[0028] A mounting table 22 for holding the wafer W substantially horizontally is provided in the processing vessel 210. The mounting table 22 is supported by a support portion 221 extending from the bottom of the exhaust chamber 211. A heater 220 serving as a heating portion is embedded in the mounting table 22, and the wafer W can be heated to a set temperature. In this example, the heating temperature of the wafer W is set to, for example, 450°C within a range of 350 to 800°C.
[0029] Further, a high frequency power supply 223 that supplies high frequency power for attracting ions is connected to the mounting table 22 via a matching box 222. Furthermore, the mounting table 22 is provided with lift pins (not shown) for holding and lifting the wafer W on the mounting table 22. The wafer W can be transferred between the mounting table 22 and the first transfer mechanism 131 on the first substrate transfer chamber 13 side by lifting and lowering the lift pins.
[0030] A flat, disk-shaped shower head 23 is provided on the ceiling surface of the processing vessel 210 to supply a substrate processing gas toward the wafer W. The shower head 23 is attached to the processing vessel 210 via an insulating member 217. A diffusion chamber 231 for diffusing gas is formed inside the shower head 23. A large number of discharge holes 232 for discharging gas toward the wafer W are provided in a distributed manner on the bottom surface of the shower head 23. A heater 235 is embedded in the upper surface side of the shower head 23.
[0031] A high frequency power supply 234 that supplies high frequency power for plasma generation is connected to the shower head 23 through a matching box 233. That is, the substrate processing apparatus 1 of the present disclosure is configured as a parallel plate type plasma processing apparatus by the shower head 23 that constitutes an upper electrode and the mounting table 22 that constitutes a lower electrode. The wafer W is placed in the space between the shower head 23 and the mounting table 22, and a film forming gas is supplied and high frequency power is applied, so that the gas is ionized to form plasma. The high frequency power supply 234 may be configured to supply high frequency power of any of the following frequencies: 450 KHz, 13.56 MHz, 27 MHz, 40 MHz, 60 MHz, 100 MHz, or 2.45 GHz. For example, the high frequency power supply 234 supplies high frequency power in a range of more than 0 W and less than or equal to 2000 W.
[0032] The downstream end of the gas supply line 40 is connected to the diffusion chamber 231 of the shower head 23. The upstream side of the gas supply line 40 is provided with a first metal halide gas, TiCl2, which contains Ti, the first metal constituting the Ti layer 64a. 4 Gas supply channel: TiCl 4 A gas supply pipe 41, an Ar gas supply pipe 42 which is a flow path for supplying Ar gas added for plasma generation, and a reaction gas H 2 Gas supply channel H 2 A gas supply pipe 43 joins.
[0033] TiCl 4 The upstream end of the gas supply pipe 41 is filled with TiCl4 A gas supply source 410 is connected to the upstream end of the Ar gas supply pipe 42, and a flow rate regulator M41 and a valve V41 are disposed therein (first gas supply unit). An Ar gas supply source 420 is connected to the upstream end of the Ar gas supply pipe 42, and a flow rate regulator M42 and a valve V42 are disposed therein (first gas supply unit). 2 At the upstream end of the gas supply pipe 43, H 2 A gas supply source 430 is connected, and a flow rate regulator M43 and a valve V43 are provided in this order from the upstream side. These TiCl 4 Gas, H 2 A mixed gas (film forming gas) of the H 2 O gas and Ar gas flows into the diffusion chamber 231 of the shower head 23 via the gas supply path 40 and is supplied into the processing vessel 210 through the outlet holes 232 .
[0034] Furthermore, on the upstream side of the gas supply path 40, WCl 5 Gas supply pipe 51 joins. 5 The gas contains a second metal (W) different from the first metal (Ti) and corresponds to a second metal halide gas that reacts with the first metal. 5 At the upstream end of the gas supply pipe 51, WCl 5 A gas supply source 510 is connected, and a flow rate regulator M51 and a valve V51 are provided in this order from the upstream side (second gas supply unit). 5 The gas also flows into the diffusion chamber 231 of the shower head 23 through the gas supply path 40 and is supplied into the processing vessel 210 through the outlet holes 232 .
[0035] According to the above-mentioned configuration, in the example shown in FIG. 3, the Ti film formation module 153 is configured such that the first processing module that forms the Ti layer 64a and the second processing module that removes the adhered Ti 65 share the mounting table 22 and the processing container 210.
[0036] <Other processing modules 151, 152, 153> Although not shown in the figures, the COR module 151, the PHT module 152, and the Ru film-forming module 154 are similar to the Ti film-forming module 153 described above in that they each include a processing vessel 210 and a mounting table 22. The COR module 151 contains HF gas and NH 3 Gas is supplied to the process vessel 210 via the gas supply line 40. In addition, in the PHT module 152, N 2 Gas is supplied to the process vessel 210 via a gas supply line 40 .
[0037] Furthermore, in the Ru film forming module 154, Ru, which is a raw material gas for the Ru film 66, is 3 (CO) 12 The gas and CO gas, which is a carrier gas, are supplied to the processing chamber 210 via the gas supply line 40. 3 (CO) 12 The gas supply source and the flow rate regulator for supplying the gas and the CO gas correspond to the fourth gas supply unit of this embodiment. The Ru film formation module 154 is configured to form the Ru film 66 by, for example, a thermal CVD method. Therefore, unlike the Ti film formation module 153 described with reference to FIG. 3, it does not include the matcher 233 and the high frequency power supply 234 connected to the shower head 23, and the matcher 222 and the high frequency power supply 223 connected to the mounting table 22.
[0038] <Control unit 100> The substrate processing apparatus 1 having the above-mentioned configuration includes a control unit 100 as shown in Fig. 2 and Fig. 3. The control unit 100 is configured with a computer including a storage unit, a memory, and a CPU that stores a program. The program includes instructions (steps) for outputting control signals from the control unit 100 to each unit of the substrate processing apparatus 1 and controlling the supply and cut-off of each gas and the supply of high-frequency power to execute substrate processing using the various modules 151 to 154. The program is stored in a storage unit of the computer, such as a flexible disk, a compact disk, a hard disk, an MO (magneto-optical disk), a non-volatile memory, etc., and is read out from the storage unit and installed in the control unit 100.
[0039] <Substrate processing> The substrate processing carried out by the substrate processing apparatus 1 having the above-described configuration will be described with reference to FIG. 4 and FIGS. 5A to 5C. In the substrate processing apparatus 1, first, the atmospheric transfer mechanism 111 takes out the wafer W accommodated in the carrier C and transfers it to the load lock chamber 12 at atmospheric pressure, and adjusts the inside of the load lock chamber 12 to a vacuum pressure atmosphere. Next, the first transfer mechanism 131 transfers the wafer W in the load lock chamber 12 to the COR module 151 and the PHT module 152 in that order, and the native oxide film formed on the Si layer 61 is removed in these modules 151 and 152 (process P11 in FIG. 4).
[0040] Next, the wafer W is transferred by the first transfer mechanism 131 to the Ti film formation module 153, where a Ti layer 64a is formed (process P12 in FIG. 4; a process for forming a metal layer of a first metal). In this process, after the wafer W is placed on the mounting table 22, the vacuum exhaust unit 213 performs evacuation so that a preset pressure is reached within the processing container 210. In addition, the heater 220 heats the wafer W to the above-mentioned 450° C.
[0041] Thereafter, TiCl is supplied from each of the gas supply sources 410, 420, and 430 at a preset flow rate. 4 Gas, H 2Gas and Ar gas are supplied, and a film-forming gas, which is a mixture of these gases, is introduced into the processing chamber 210. Further, high frequency power is applied from the high frequency power supplies 234 and 223 to convert the film-forming gas into plasma, and a Ti film is formed on the wafer W.
[0042] After the Ti film is formed for a preset time, the supply of the film formation gas and the application of high frequency power are stopped. As a result, as described with reference to FIG. 1A, a Ti layer 64a is formed on the bottom surface of the recess 60. Silicon diffuses into this Ti layer 64a from the Si layer 61 side, and it becomes a TiSi layer 64 in a short time. Furthermore, due to the formation of the Ti film, Ti deposits 65 may adhere to the sidewall surface of the recess 60 (FIG. 5A).
[0043] Therefore, in the Ti film forming module 153 of the present embodiment, after the Ti layer 64a is formed, the gas supplied to the processing chamber 210 is changed to WCl while continuing to heat the wafer W. 5 This results in a switch to WCl 5 Gas supply source 510 supplies WCl at a preset flow rate. 5 Gases are supplied and introduced into the process vessel 210. As shown in FIG. 5A, WCl 5 When the gas reaches the wafer W, the reaction shown in the following formula (1) proceeds. 4WCl 5 (g)+5Ti(s)→5TiCl 4 (g) + 4W(s) …(1)
[0044] By proceeding with the above formula (1), the Ti 65 adhering to the sidewall surface of the recess 60 can be removed as shown in FIG. 5B (step P13 in FIG. 4, a step for removing the first metal). 5 The supply of gas may also remove a part of the surface of the TiSi layer 64 formed on the bottom surface of the recess 60. However, TiSi has a higher solubility in WCl than Ti. 5 Furthermore, by forming the TiSi layer 64 (Ti layer 64a) with a sufficient thickness, the TiSi layer 64 can be left without losing its function as a metal layer for contact.
[0045] Furthermore, according to formula (1), solid tungsten (W) remains as the attached Ti 65 is removed. In this regard, since the resistance value of W is smaller than that of Ti, this can contribute to suppressing the increase in the wiring resistance after embedding the Ru wiring 66a, compared to the state in which the attached Ti 65 is left as is. WCl 5 After removing the attached Ti65 by supplying gas, WCl remaining in the processing vessel 210 is 5 or TiCl 4 To promote the excretion of H 2 A purging process may be performed by supplying a gas.
[0046] Next, the wafer W is transferred to the Ru film formation module 154 via the first transfer mechanism 131, the transfer section 17, and the second transfer mechanism 141. An inert gas is supplied to the first substrate transfer chamber 13, the transfer section 17, and the second substrate transfer chamber 14 to prevent gas diffusion from the film formation module. The pressure is controlled to, for example, 100 Pa within a range of 20 to 200 Pa. In addition, in order to prevent oxidation of the surfaces during transfer, the ultimate vacuum of a vacuum exhaust mechanism (not shown) that evacuates these spaces (the first substrate transfer chamber 13, the transfer section 17, and the second substrate transfer chamber 14) is set to 1.33×10 -5 The pressure is set to be equal to or lower than Pa. In the Ru film formation module 154, a Ru film 66 is formed so that Ru is embedded in the upper surface side of the TiSi layer 64 formed in the recess 60 (P14 in FIG. 4; a process of embedding a conductor).
[0047] Specifically, the wafer W is carried into the processing chamber 210 of the Ru film forming module 154 and placed on the mounting table 22, and the wafer W is heated by the heater 220 to, for example, 150° C. within a range of 130 to 200° C. Further, the pressure inside the processing chamber 210 is adjusted, and Ru is introduced into the processing chamber 210. 3 (CO) 12 Gas (including CO gas as a carrier gas) is supplied.
[0048] As a result, the Ru supplied into the processing vessel 210 3 (CO)12 Thermal CVD proceeds, in which the Ru film 66 is thermally decomposed on the wafer W. By carrying out thermal CVD for a preset period of time, as shown in FIG. 5C, the Ru film 66 can be filled into the recess 60 from which the deposited Ti 65 has been removed.
[0049] After the formation of the Ru film 66 is completed, the wafer W is transferred to the load lock chamber 12 via the second transfer mechanism 141, the delivery unit 17, and the first transfer mechanism 131. Next, the atmosphere in the load lock chamber 12 is switched to an atmospheric pressure atmosphere, and then the processed wafer W is returned to the carrier C by the atmospheric transfer mechanism 111.
[0050] According to the above embodiment, the Ti 65 deposited on the sidewall surface of the recess 60 is replaced with WCl 5 As a result, it is possible to suppress an increase in the wiring resistance after the Ru film 66 (Ru wiring 66a) is buried in the recess 60.
[0051] Here, the technology of the present disclosure is WCl 5 The adhering Ti 65 is removed by dry etching using a gas (second metal halide gas). Therefore, unlike the case where wet etching is performed, the adhering Ti 65 can be removed in a series of substrate processing steps from the process of removing the native oxide film on the surface of the Si layer 61 (COR process, PHT) to the process of forming the Ru film 66. As a result, it is possible to perform substrate processing in the common substrate processing apparatus 1 without exposing the wafer W to the air atmosphere, and the formation of unnecessary native oxide films can be suppressed.
[0052] 3, the first processing module for forming the Ti layer 64a and the second processing module for removing the adhered Ti 65 are not limited to being configured to share the mounting table 22 and the processing container 210. The first processing module and the second processing module may be configured as separate entities.
[0053] The substrate processing apparatus 1a shown in FIG. 6 includes a Ti film-forming module 153a, which is a first processing module having only a Ti film-forming function, and a WCl 5 6 and 7, a pre-cleaning module 155, which is a second processing module having only a function of removing adhering Ti65 by gas, is provided separately. In the substrate processing apparatuses 1a and 1b shown in FIG. 6 and FIG. 7, components common to the substrate processing apparatus 1 described with reference to FIG. 2 are denoted by the same reference numerals as those shown in the drawings.
[0054] In this substrate processing apparatus 1a, one Ti film formation module 153a is connected to each of the left and right walls of the first substrate transfer chamber 13. In addition, a pre-cleaning module 155 is connected to one wall of the second substrate transfer chamber 14. By providing the pre-cleaning module 155, the substrate processing apparatus 1a of this example has three Ru film formation modules 154 installed, compared to the substrate processing apparatus 1 shown in FIG.
[0055] <Second embodiment> Next, the configuration and operation of a substrate processing apparatus 1b according to a second embodiment will be described with reference to Figs. 7 and 8. The substrate processing apparatus 1a according to the second embodiment performs a process for oxidizing Ti 65 deposited on the sidewall surface of the recess 60, and then performs a process for removing WCl 5 The substrate processing apparatus 1b is configured to remove the adhering Ti65 by using a gas. The substrate processing apparatus 1b includes an oxidation processing module 156 that performs a process of oxidizing the adhering Ti65.
[0056] Although not shown separately, the oxidation process module 156 is similar to the Ti film formation module 153 described with reference to FIG. 3 in that it includes a process chamber 210 and a mounting table 22. The oxidation process module 156 is configured such that an oxidation gas for oxidizing the deposited Ti 65 is supplied to the process chamber 210 via a gas supply path 40. The oxidation gas used here is O 2 Gas and O 3 Gas, H 2 O gas, H 2 O 2 Gas, N 2 O gas, N 2 O2 The Ti film forming module 153 may have a function of converting an oxidizing gas into plasma, or may use the oxidizing gas as it is without converting it into plasma.
[0057] 7, a Ti film formation module 153a having only a Ti film formation function and an oxidation treatment module 156 are connected to the first substrate transfer chamber 13. Also, a pre-cleaning module 155 is connected to the second substrate transfer chamber 14.
[0058] Processing of a wafer W using this substrate processing apparatus 1b will be described with reference to Fig. 8. In Fig. 8, differences from the substrate processing according to the first embodiment described with reference to Fig. 4 will be mainly described.
[0059] After the COR process and the PHT process are performed on the wafer W to be processed using the COR module 151 and the PHT module 152 (P11 in FIG. 8), the wafer W is loaded into the Ti film forming module 153a to form a Ti layer 64a (process P12 in FIG. 8). Thereafter, the wafer W after the Ti layer 64a (TiSi layer 64) is subjected to a process for oxidizing the Ti 65 attached to the sidewall surface of the recess 60 (P13A in FIG. 8, a process for oxidizing the first metal).
[0060] Specifically, the wafer W is carried into the processing vessel 210 of the oxidation processing module 156 and placed on the mounting table 22, and the wafer W is heated by the heater 220 to a temperature in the range of, for example, 100 to 400° C. Then, the pressure inside the processing vessel 210 is adjusted, and an oxidizing gas is supplied into the processing vessel 210. At this time, when the oxidizing gas is turned into plasma, energy such as high-frequency power is supplied.
[0061] By the above operation, the oxidation of the attached Ti65 proceeds under the atmosphere of the supply of the oxidizing gas. Then, after the process with the oxidizing gas is performed for a preset period, the supply of the oxidizing gas and the heating of the wafer W are stopped, and the wafer W is transferred to the pre-cleaning module 155.
[0062] In the pre-cleaning module 155, the wafer W housed in the processing vessel 210 and placed on the placement table 22 is heated to a temperature in the range of 300 to 500° C., for example, 450° C. Then, the pressure in the processing vessel 210 is adjusted, and WCl is introduced into the processing vessel 210. 5 As a result, WCl 5 When the gas arrives, the reaction shown in formula (2) below proceeds. 2WCl 5 (g) + TiO(s) → TiOCl 2 (g) + 2WCl 4 (g) …(2)
[0063] By proceeding with the above formula (2), it is possible to remove Ti 65 adhering to the side wall surface of the recess 60 in the same manner as in the first embodiment described with reference to FIG. 5B (process P13B in FIG. 4). As shown in formula (2), WCl 5 Since the reaction product of and TiO is a gaseous substance, there is almost no effect of remaining tungsten (W).
[0064] Here, the TiSi layer 64 formed on the bottom of the recess 60 may be oxidized under the supply of an oxidizing gas, resulting in the formation of TiSiO. The SiO contained in the TiSiO is WCl 5 It is difficult to remove the Ti layer 64a by gas. To avoid such a state, when forming the Ti layer 64a, the thickness of the Ti layer 64a may be increased to such an extent that silicon atoms diffused from the Si layer 61 have difficulty in reaching the surface of the Ti layer 64a. When forming the TiSi layer 64 with a thickness of 5 nm, the thickness of the Ti layer 64a may be set to about 1.5 to 2 times the thickness of the TiSi layer 64.
[0065] By adjusting the thickness of the Ti layer 64a in this way, it is possible to prevent TiSi from being exposed at the bottom of the recess 60, and suppress the formation of TiSiO. At the bottom of the recess 60, the Ti layer with no exposed silicon atoms is exposed, and this Ti layer is oxidized to form a TiO layer. 5When the TiO layer is removed by gas, the TiSi layer 64 is exposed at the bottom of the recess 60, similar to the example shown in FIG. 5B.
[0066] After removing the adhering Ti 65, the process of forming the Ru film 66 and the operation of unloading the processed wafer W are similar to those in the case of using the substrate processing apparatus 1 described above, and therefore will not be described again.
[0067] <Variations> In the above-described substrate processing method, the second halide gas used to remove the adhering Ti65 is WCl 5 The gas examples are not limited to WCl 6 Gas and MoCl 5 A gas may also be used. Moreover, the first metal formed in the recess 60 is not limited to Ti, and the metal film formed using the first metal halide gas may be another metal. Even in this case, the first metal attached to the sidewall surface of the recess 60 can be removed by supplying a second metal halide gas that reacts with the first metal.
[0068] The embodiments disclosed herein should be considered to be illustrative and not restrictive in all respects. The above-described embodiments may be omitted, substituted, or modified in various forms without departing from the scope and spirit of the appended claims. EXAMPLES
[0069] (experiment) A film containing Ti was formed on the surface of a silicon wafer, and WCl 5 The effect of gas removal was confirmed.
[0070] A. Experimental Conditions (Reference example) TiCl 4 A TiN layer was formed on the surface of the flat wafer W by plasma CVD using a deposition gas containing TiN and a Ru layer was further laminated on the surface of the TiN layer. (Example) After forming a TiN layer on the surface of a flat wafer W by the same method as in the reference example, the wafer W was heated to 450° C. and treated with WCl at a pressure of 1200 Pa and a flow rate of 1.8 sccm. 5 Gas was supplied for 20 seconds. After that, H was supplied at a flow rate of 1200 sccm while maintaining the temperature and pressure. 2 Gas was supplied for 100 seconds.
[0071] B. Experimental Results TEM (Transmission Electron Microscopy) photographs of the wafer W according to the reference example and the embodiment are shown in Fig. 9(a) and (b). Comparing these figures, in the embodiment of Fig. 9(b), the WCl 5 It can be seen that the thickness of the TiN layer is reduced by the gas treatment. 5 It was confirmed that the Ti layer could be removed using WCl gas, just like the TiN layer. 5 It has been confirmed that it can be removed using gas. [Explanation of symbols]
[0072] 1, 1a, 1b Substrate Processing Equipment 153 Ti deposition module 22 Placement table 210 Processing vessel 410 TiCl 4 Gas supply source 510 WCl 5 Gas supply source
Claims
1. 1. A method for processing a substrate, comprising: supplying a first metal halide gas to the substrate, the substrate having an insulating layer stacked on silicon and a recess formed in the insulating layer, to form a metal layer of a first metal contained in the first metal halide on a surface of the silicon exposed in the recess; next, supplying a second metal halide gas containing a second metal different from the first metal and reacting with the first metal to the substrate on which a metal silicide layer has been formed by diffusing the silicon into the metal layer, and removing the first metal adhering to the sidewall surface of the recess.
2. a step of heating the substrate in an atmosphere containing an oxidizing gas after the step of forming the metal layer is performed, and oxidizing the first metal attached to the side wall surface; The method according to claim 1 , wherein the step of removing the first metal comprises removing the first metal oxidized in the step of oxidizing the first metal.
3. 2. The method of claim 1, wherein said first metal is titanium and said metal silicide is titanium silicide.
4. The first metal halide gas is TiCl 4 The method of claim 3 , wherein the gas is a gas.
5. The second metal halide gas is WCl 5 The method of claim 3 , wherein the gas is a gas.
6. The method according to claim 1 , further comprising the step of depositing a conductor on the substrate and embedding the conductor in the recess after performing the step of removing the first metal.
7. An apparatus for processing a substrate, comprising: a first processing module including a processing vessel including a mounting table on which the substrate is placed, and a first gas supply unit for supplying a first metal halide gas to the processing vessel; a second processing module including a processing vessel having a mounting table on which the substrate is placed, and a second gas supply unit for supplying a second metal halide gas containing a second metal different from the first metal and reacting with the first metal to the processing vessel; A control unit, the control unit is configured to output a control signal to execute the steps of: placing the substrate, in which an insulator layer is laminated on silicon and a recess is formed in the insulator layer, on a mounting table of the first processing module, supplying the first metal halide gas from the first gas supply unit to a processing vessel of the first processing module, and forming a metal layer of a first metal contained in the first metal halide on a surface of the silicon exposed in the recess; and then placing the substrate, in which a metal silicide layer is formed by diffusing the silicon into the metal layer, on a mounting table of the second processing module, supplying the second metal halide gas from the second gas supply unit to the processing vessel of the second processing module, and removing the first metal adhering to a sidewall surface of the recess.
8. The apparatus according to claim 7 , wherein the first processing module and the second processing module share the mounting table and the processing container.
9. a vacuum transfer chamber to which the processing container of the first processing module and the processing container of the second processing module are connected, and a substrate transfer mechanism disposed in the vacuum transfer chamber, 8. The apparatus of claim 7, wherein the control unit is configured to, after performing a step of forming a metal layer of the first metal, perform a step of transporting the substrate from the mounting table of the first processing module to the mounting table of the second processing module via the vacuum transfer chamber by the substrate transport mechanism, and then output a control signal for executing a step of removing the first metal.
10. a third processing module including a processing vessel including a mounting table on which the substrate is placed, and a third gas supply unit for supplying an oxidizing gas to the processing vessel; 8. The apparatus of claim 7, wherein the control unit is configured to, after performing the step of forming the metal layer, place the substrate on the mounting table of the third processing module, heat the substrate under an atmosphere of the oxidizing gas supplied from the third gas supply unit, and perform a step of oxidizing the first metal adhering to the side wall surface, and in the step of removing the first metal, output a control signal for removing the first metal oxidized in the step of oxidizing the first metal.
11. 8. The device of claim 7, wherein said first metal is titanium and said metal silicide is titanium silicide.
12. The first metal halide gas is TiCl 4 The device of claim 11 which is a gas.
13. The second metal halide gas is WCl 5 The device of claim 11 which is a gas.
14. a fourth processing module including a processing vessel including a mounting table on which the substrate is placed, and a fourth gas supply unit for supplying a source gas of a conductor to the processing vessel; 8. The apparatus of claim 7, wherein the control unit is configured to output a control signal for executing a step of placing the substrate on the mounting table of the fourth processing module after performing the step of removing the first metal, supplying the raw material gas from the fourth gas supply unit to the processing vessel to deposit a conductor on the substrate, and embedding the conductor in the recess.
Citation Information
Patent Citations
Method of depositing tungsten on feature with high aspect ratio
JP2011035366A
Forming method of titanium silicide region
JP2018186123A
Methods for etching via atomic layer deposition (ALD) cycles
US20160276214A1
Contacts and Interconnect Structures in Field-Effect Transistors
US20200098623A1
Method of manufacturing semiconductor device and semiconductor device