Hardmask composition, hardmask layer, and method of forming patterns

A hard mask composition with aromatic hydrocarbon groups and specific functional groups addresses the limitations of spin-coated hard mask layers by enhancing etching and heat resistance, ensuring effective pattern transfer in semiconductor manufacturing.

JP2024161888AInactive Publication Date: 2024-11-20SAMSUNG SDI CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024050812
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-08
Filing Date
2024-03-27
Publication Date
2024-11-20
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing lithographic techniques struggle to form fine patterns with good profiles due to the limitations of etching resistance and heat resistance in hard mask layers, especially when using spin coating methods, which require improved carbon content without compromising solvent solubility.

Method used

A hard mask composition containing a compound represented by Chemical Formula 1, comprising aromatic hydrocarbon groups and specific functional groups, is used to form a hard mask layer with enhanced etching resistance and solubility, achieved through heat treatment to create a crosslinked polymer with high carbon content.

Benefits of technology

The hard mask layer exhibits excellent etching resistance and heat resistance, maintaining integrity during pattern transfer processes, while allowing for efficient application via spin coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024161888000037
    Figure 2024161888000037
  • Figure 2024161888000001
    Figure 2024161888000001
  • Figure 2024161888000002
    Figure 2024161888000002
Patent Text Reader

Abstract

To provide a hardmask composition capable of forming a hardmask layer that can secure excellent etch resistance and heat resistance, while also exhibiting excellent crosslinking characteristics, a hardmask layer including a cured product of the hardmask composition, and a method of forming patterns using the hardmask composition.SOLUTION: The present invention relates to a hardmask composition including a compound represented by chemical formula 1 and a solvent, a hardmask layer formed from the hardmask composition, and a method of forming patterns using the hardmask composition. The chemical formula 1 is as defined in the specifications.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a hardmask composition, a hardmask layer including a cured product of the hardmask composition, and a pattern forming method using the hardmask composition. [Background technology]

[0002] In recent years, the semiconductor industry has developed from patterns of several hundred nanometers to ultrafine technology with patterns of several to tens of nanometers. Effective lithographic techniques are essential to realize such ultrafine technology.

[0003] A typical lithographic technique includes the steps of forming a material layer on a semiconductor substrate, coating a photoresist layer thereon, exposing and developing to form a photoresist pattern, and then etching the material layer using the photoresist pattern as a mask.

[0004] In recent years, as the size of a pattern to be formed decreases, it is difficult to form a fine pattern having a good profile using only the above-mentioned typical lithographic techniques. Therefore, a supplementary layer called a hard mask layer can be formed between the material layer to be etched and the photoresist layer to form a fine pattern. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Korean Patent Publication No. 10-2022-0092160 Summary of the Invention [Problem to be solved by the invention]

[0006] An object of the present invention is to provide a hard mask composition capable of forming a hard mask layer that can ensure excellent etching resistance and heat resistance, and that has excellent crosslinking properties.

[0007] Another object of the present invention is to provide a hard mask layer comprising a cured product of the above hard mask composition.

[0008] It is still another object of the present invention to provide a pattern forming method using the above hard mask composition. [Means for solving the problem]

[0009] A hard mask composition according to one embodiment of the present invention includes a compound represented by the following Chemical Formula 1, and a solvent:

[0010] [ka]

[0011] In the above chemical formula 1, Ar 1 and Ar 2 each independently represents a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, or a group in which two or more substituted or unsubstituted aromatic hydrocarbon groups having 6 to 30 carbon atoms are linked by a single bond or a substituted or unsubstituted alkylene group having 1 to 30 carbon atoms, R 1 and R 2 each independently represents a hydrogen atom, a deuterium atom, a substituted or unsubstituted saturated or unsaturated aliphatic hydrocarbon group having 1 to 30 carbon atoms, a substituted or unsubstituted saturated or unsaturated alicyclic hydrocarbon group having 3 to 30 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, or a combination thereof; n is an integer from 2 to 6.

[0012] Ar in the above formula 1 1 and Ar 2are each preferably independently a substituted or unsubstituted group having at least one of the structures selected from Group 1 below:

[0013] [ka]

[0014] Ar in the above formula 1 1 and Ar 2 may each independently be a substituted or unsubstituted group having at least one of the structures selected from Group 1-1 below:

[0015] [ka]

[0016] R in the above Chemical Formula 1 1 and R 2 are preferably each independently a hydrogen atom, a deuterium atom, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, or a combination thereof.

[0017] R in the above Chemical Formula 1 1 and R 2 may each independently be a hydrogen atom, a deuterium atom, a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 20 carbon atoms, or a combination thereof.

[0018] Ar in the above formula 1 1 and Ar 2 are each independently a substituted or unsubstituted group having at least one structure selected from the following Group 1-2, R 1 and R 2are each independently a hydrogen atom, a deuterium atom, a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 20 carbon atoms, or a combination thereof, and n may be an integer of 2 to 4.

[0019] [ka]

[0020] In the above formula 1, n is 2 or 3, and all R 1 are identical to each other, and all R 2 are identical to each other, and all Ar 2 may be identical to each other.

[0021] The compound represented by Chemical Formula 1 above may be at least one of the compounds represented by Chemical Formulas 2 to 10 below:

[0022] [ka]

[0023] [ka]

[0024] The molecular weight of the compound represented by the above Chemical Formula 1 is preferably 300 g / mol to 10,000 g / mol.

[0025] The compound is preferably contained in an amount of 0.1% by mass to 30% by mass based on the total mass of the hard mask composition.

[0026] Examples of the solvent include, but are not limited to, propylene glycol, propylene glycol diacetate, methoxypropanediol, diethylene glycol, diethylene glycol butyl ether, tri(ethylene glycol) monomethyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, cyclohexanone, ethyl lactate, γ-butyrolactone, N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidinone, acetylacetone, and ethyl 3-ethoxypropionate.

[0027] According to another aspect of the present invention, there is provided a hardmask layer comprising a cured product of the hardmask composition described above.

[0028] According to yet another aspect of the present invention, there is provided a pattern formation method including the steps of forming a material layer on a substrate, applying the above-described hard mask composition onto the material layer, heat-treating the hard mask composition to form a hard mask layer, forming a photoresist layer on the hard mask layer, exposing and developing the photoresist layer to form a photoresist pattern, selectively removing the hard mask layer using the photoresist pattern to expose a portion of the material layer, and etching the exposed portion of the material layer.

[0029] The step of forming the hard mask layer may include a step of performing a heat treatment at 100°C to 1,000°C. Effect of the Invention

[0030] The hard mask composition according to the present invention has excellent crosslinking properties when cured, and a hard mask layer formed from the hard mask composition can ensure excellent heat resistance and excellent etching resistance. [Brief description of the drawings]

[0031] [Figure 1]FIG. 1 is a diagram for explaining a calculation formula for evaluating the planarization property of a hard mask composition according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0032] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will now be described in detail with reference to exemplary embodiments thereof, so that those skilled in the art will be able to easily practice the present invention. However, the present invention may be embodied in many different forms and is not limited to the embodiments set forth herein.

[0033] Unless otherwise defined in this specification, "substituted" and "substituted" mean that a hydrogen atom in a compound has been replaced with a halogen atom (F, Br, Cl, or I), a hydroxy group, an alkoxy group, a nitro group, a cyano group, an amino group, an azide group, an amidino group, a hydrazino group, a hydrazono group, a carbonyl group, a carbamoyl group, a thiol group, an ester group, a carboxyl group and salts thereof, a sulfonic acid group and salts thereof, a phosphoric acid group and salts thereof, a vinyl group, an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an alkynyl group having 2 to 20 carbon atoms, or a carboxyl group having 2 to 20 carbon atoms. It means that the aryl group is substituted with a substituent selected from the group consisting of an aromatic hydrocarbon group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms, an arylaryl group having 9 to 30 carbon atoms, an alkoxy group having 1 to 30 carbon atoms, a heteroalkyl group having 1 to 20 carbon atoms, a heteroarylalkyl group having 3 to 20 carbon atoms, a cycloalkyl group having 3 to 30 carbon atoms, a cycloalkenyl group having 3 to 15 carbon atoms, a cycloalkynyl group having 6 to 15 carbon atoms, a heterocycloalkyl group having 3 to 30 carbon atoms, and combinations thereof.

[0034] Furthermore, the above-mentioned substituents, i.e., a halogen atom (F, Br, Cl, or I), a hydroxy group, a nitro group, a cyano group, an amino group, an azide group, an amidino group, a hydrazino group, a hydrazono group, a carbonyl group, a carbamoyl group, a thiol group, an ester group, a carboxyl group or a salt thereof, a sulfonic acid group or a salt thereof, a phosphoric acid group or a salt thereof, an alkyl group having 1 to 30 carbon atoms, an alkenyl group having 2 to 30 carbon atoms, an alkynyl group having 2 to 30 carbon atoms, an aromatic hydrocarbon group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms, an alkoxy group having 1 to 30 carbon atoms, a heteroalkyl group having 1 to 20 carbon atoms, a heteroarylalkyl group having 3 to 20 carbon atoms, a cycloalkyl group having 3 to 30 carbon atoms, a cycloalkenyl group having 3 to 15 carbon atoms, a cycloalkynyl group having 6 to 15 carbon atoms, or a heterocyclic group having 2 to 30 carbon atoms, may form a bond with or be condensed to another adjacent substituent to form a ring.

[0035] Unless otherwise defined in this specification, the terms "aromatic hydrocarbon," "aromatic hydrocarbon group," "aromatic hydrocarbon ring," and "aryl group" refer to a group having at least one aromatic hydrocarbon moiety, and include not only non-fused aromatic hydrocarbon rings and fused aromatic hydrocarbon rings, but also forms in which aromatic hydrocarbon moieties are linked by single bonds, fused ring forms having a non-aromatic moiety to which the aromatic hydrocarbon moiety is directly or indirectly fused, and combinations thereof.

[0036] More specifically, the substituted or unsubstituted aromatic hydrocarbon group may be, but is not limited to, a substituted or unsubstituted phenyl group, a substituted or unsubstituted naphthyl group, a substituted or unsubstituted anthracenyl group, a substituted or unsubstituted phenanthryl group, a substituted or unsubstituted naphthacenyl group, a substituted or unsubstituted pyrenyl group, a substituted or unsubstituted biphenylyl group, a substituted or unsubstituted terphenyl group, a substituted or unsubstituted quaterphenyl group, a substituted or unsubstituted chrysenyl group, a substituted or unsubstituted triphenylenyl group, a substituted or unsubstituted perylenyl group, a substituted or unsubstituted indenyl group, a combination thereof, or a condensed form of a combination thereof.

[0037] In this specification, unless otherwise specified, "molecular weight" refers to the sum of the atomic weights of the atoms contained in a molecule. In this specification, the "molecular weight" is measured by dissolving a powder sample in tetrahydrofuran (THF) and then using 1200 series Gel Permeation Chromatography (GPC) manufactured by Agilent Technologies (using an LF-804 column manufactured by Resonac Corporation and polystyrene standard manufactured by Resonac Corporation).

[0038] In the semiconductor industry, there is a constant demand to reduce the size of chips, and to meet this demand, the line width of the resist patterned by lithography technology is required to be several tens of nanometers in size. Therefore, the height that can withstand the line width of the resist pattern is limited, and the resist may not have sufficient resistance in the etching step. To compensate for this, an auxiliary layer called a hardmask layer is used between the material layer to be etched and the photoresist layer. This hardmask layer serves as an intermediate film that transfers the fine pattern of the photoresist to the material layer through selective etching. Therefore, the hardmask layer is required to have etching resistance so that it can withstand the etching process required for pattern transfer.

[0039] Existing hard mask layers have been formed by chemical or physical vapor deposition, which requires large-scale equipment, and the process cost is high, resulting in poor economic efficiency. Therefore, a technology for forming a hard mask layer by a spin coating method has been developed recently. The spin coating method is easier to process than conventional methods, and the gap fill property and planarization property of the hard mask layer manufactured by the spin coating method may be superior, but the hard mask layer formed by the spin coating method may have poor etching resistance. Therefore, it is required that a hard mask composition that can be applied to the spin coating method and the hard mask layer formed by this method have the same etching resistance as the hard mask layer formed by the chemical or physical vapor deposition method.

[0040] Therefore, in order to improve the etching resistance of the hard mask layer, research has been conducted to increase the carbon content of the hard mask composition. However, the more the carbon content of the polymer contained in the hard mask layer increases, the lower the solubility in the solvent tends to be. Therefore, in order to obtain a hard mask layer that can be applied to the spin coating method, it is required to increase the carbon content of the polymer contained in the hard mask layer to improve the etching resistance of the hard mask layer formed therefrom, and to make the compound forming the polymer contained in the hard mask composition sufficiently soluble in the solvent.

[0041] The hard mask composition according to one embodiment of the present invention includes a compound having an aromatic hydrocarbon ring, and can increase the carbon content in the composition. Therefore, the hard mask layer obtained from the composition can ensure excellent etching resistance. In addition, the compound includes a specific functional group, and can ensure excellent solubility in a solvent while increasing the carbon content in the composition.

[0042] Specifically, a hard mask composition according to an embodiment of the present invention includes a compound represented by the following Formula 1, and a solvent.

[0043] [ka]

[0044] In the above chemical formula 1, Ar 1 and Ar 2 each independently represents a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, or a group in which two or more substituted or unsubstituted aromatic hydrocarbon groups having 6 to 30 carbon atoms are linked by a single bond or a substituted or unsubstituted alkylene group having 1 to 30 carbon atoms, R 1 and R 2 each independently represents a hydrogen atom, a deuterium atom, a substituted or unsubstituted saturated or unsaturated aliphatic hydrocarbon group having 1 to 30 carbon atoms, a substituted or unsubstituted saturated or unsaturated alicyclic hydrocarbon group having 3 to 30 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, or a combination thereof; n is an integer from 2 to 6.

[0045] As described above, the compound of the present invention contains an aromatic hydrocarbon ring as represented by Chemical Formula 1 above, and a triple bond carbon atom is directly connected to the central aromatic hydrocarbon ring, thereby increasing the carbon content in the composition and providing excellent crosslinking properties during curing of a hard mask composition containing the compound.

[0046] The compound represented by the above formula 1 is -OR 2 By including a substituent represented by the formula (I), the solubility of the compound in a solvent can be improved, and a hard mask composition including the compound can be effectively applied to a spin coating method. In addition, the compound is crosslinked in a polymer form having a large molecular weight within a short time upon heat treatment, and thus a hard mask layer formed therefrom can have excellent heat resistance and excellent etching resistance.

[0047] Ar in the above formula 1 1 and Ar 2are each preferably independently a substituted or unsubstituted group having at least one structure selected from Group 1 below:

[0048] [ka]

[0049] As an example, Ar 1 and Ar 2 are each independently a substituted or unsubstituted group having at least one structure selected from the following Group 1-1:

[0050] [ka]

[0051] As another example, Ar 1 and Ar 2 are each independently a substituted or unsubstituted group having at least one structure selected from Group 1-2 below.

[0052] [ka]

[0053] R in the above Chemical Formula 1 1 and R 2 may each independently be a hydrogen atom, a deuterium atom, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, or a combination thereof. For example, R 1 and R 2may each independently be a hydrogen atom, a deuterium atom, a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 20 carbon atoms, or a combination thereof. Examples include a hydrogen atom, a methyl group, an ethyl group, a propyl group, a butyl group, a phenyl group, a naphthyl group, a phenanthryl group, an anthryl group, or a pyrenyl group, and examples thereof include, but are not limited to, a hydrogen atom, a methyl group, and a phenyl group.

[0054] In one embodiment, in the compound represented by the above chemical formula 1, 1 and Ar 2 are each independently a substituted or unsubstituted group having at least one structure selected from Group 1-2 above, R 1 and R 2 are each independently a hydrogen atom, a deuterium atom, a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 20 carbon atoms, or a combination thereof, and n is an integer of 2 to 4.

[0055] In the above Chemical Formula 1, n is an integer of 2 to 6, for example, but not limited to, an integer of 2 to 4, for example, n is 2 or 3. When n in the above Chemical Formula 1 is 2 or 3, the solubility of the compound according to one embodiment in a solvent can be further improved, and the etching resistance of a hard mask layer formed from a hard mask composition including the compound can be improved.

[0056] When n in the above chemical formula 1 is 2 or 3, R 1 may be the same or different, and R 2 may be the same or different, and Ar 2 may be the same or different from each other. That is, when n is 2 or 3, two or three R 1 Each may be the same or different from the others, and there may be two or three R 2Each may be the same or different from the others, and there are two or three Ar 2 Each means that they may be the same or different from each other.

[0057] In one embodiment, the compound represented by Chemical Formula 1 is at least one of the compounds represented by Chemical Formulas 2 to 10 below:

[0058] [ka]

[0059] [ka]

[0060] The compound represented by the above formula 1 may have a molecular weight of 300 g / mol to 10,000 g / mol. For example, it may have a molecular weight of 400 g / mol to 10,000 g / mol, for example, 500 g / mol to 10,000 g / mol, for example, 500 g / mol to 9,500 g / mol, for example, 500 g / mol to 9,000 g / mol, for example, 600 g / mol to 8,500 g / mol, for example, 600 g / mol to 8,000 g / mol, for example, 700 g / mol to 7,500 g / mol, for example, 700 g / mol to 7,000 g / mol, but is not limited thereto. By having a molecular weight in the above range, the carbon content and solubility in a solvent of the hard mask composition containing the above compound can be adjusted and optimized.

[0061] The compound represented by the above chemical formula 1 can be synthesized by appropriately referring to a conventionally known synthesis method. More specifically, a person skilled in the art can easily synthesize the compound by referring to the synthesis method described in the Examples.

[0062] The compound may be contained in an amount of 0.1% by mass to 30% by mass based on the total mass of the hard mask composition. For example, it may be 0.2% by mass to 30% by mass, for example, 0.5% by mass to 30% by mass, for example, 1% by mass to 30% by mass, for example, 1% by mass to 25% by mass, for example, 1% by mass to 20% by mass, but is not limited thereto. By containing the compound in the above range, the thickness, surface roughness, and flatness degree of the hard mask can be easily adjusted.

[0063] The hard mask composition according to an embodiment of the present invention may include a solvent, and the solvent may include, but is not limited to, at least one selected from, for example, propylene glycol, propylene glycol diacetate, methoxypropanediol, diethylene glycol, diethylene glycol butyl ether, tri(ethylene glycol) monomethyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, cyclohexanone, ethyl lactate, γ-butyrolactone, N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidinone, acetylacetone, or ethyl 3-ethoxypropionate. The solvent is not particularly limited as long as it has sufficient solubility and / or dispersibility for the compound.

[0064] The hard mask composition may further include additives such as a surfactant, a crosslinking agent, a thermal acid generator, and a plasticizer.

[0065] Examples of the surfactant that can be used include, but are not limited to, fluoroalkyl compounds, alkylbenzenesulfonates, alkylpyridinium salts, polyethylene glycols, and quaternary ammonium salts.

[0066] Examples of the crosslinking agent include melamine-based agents, substituted urea-based agents, and polymers thereof. A crosslinking agent having at least two crosslink-forming substituents is preferable, and for example, compounds such as methoxymethylated glycoluril, butoxymethylated glycoluril, methoxymethylated melamine, butoxymethylated melamine, methoxymethylated benzoguanamine, butoxymethylated benzoguanamine, methoxymethylated urea, butoxymethylated urea, methoxymethylated thiourea, and butoxymethylated thiourea can be used.

[0067] In addition, as the crosslinking agent, a crosslinking agent having high heat resistance can be used. As the crosslinking agent having high heat resistance, a compound containing a crosslinking-forming substituent having an aromatic ring (e.g., a benzene ring or a naphthalene ring) in the molecule can be used.

[0068] Examples of the thermal acid generator that can be used include acidic compounds such as p-toluenesulfonic acid, trifluoromethanesulfonic acid, pyridinium p-toluenesulfonate, salicylic acid, sulfosalicylic acid, citric acid, benzoic acid, hydroxybenzoic acid, and naphthalenecarboxylic acid, and / or 2,4,4,6-tetrabromocyclohexadienone, benzoin tosylate, 2-nitrobenzyl tosylate, and other organic sulfonic acid alkyl esters, but are not limited to these.

[0069] According to another aspect of the present invention, there is provided a hardmask layer comprising a cured product of the hardmask composition described above.

[0070] A method for forming a pattern using the above-described hard mask composition will now be described.

[0071] A pattern formation method according to one embodiment of the present invention includes the steps of forming a material layer on a substrate, applying a hard mask composition containing the above-mentioned compound and a solvent onto the material layer, heat-treating the hard mask composition to form a hard mask layer, forming a photoresist layer on the hard mask layer, exposing and developing the photoresist layer to form a photoresist pattern, selectively removing the hard mask layer using the photoresist pattern to expose a portion of the material layer, and etching the exposed portion of the material layer.

[0072] The substrate may be, for example, a silicon wafer, a glass substrate, or a polymer substrate. The material layer is the material to be ultimately patterned, and may be, for example, a metal layer such as aluminum or copper, a semiconductor layer such as silicon, or an insulating layer such as silicon oxide or silicon nitride. The material layer may be formed, for example, by chemical vapor deposition.

[0073] The hard mask composition may be prepared in the form of a solution and applied by spin coating, as described above. The thickness of the hard mask composition is not particularly limited, but may be, for example, 50 to 200,000 Å.

[0074] The step of heat treating the hard mask composition may be performed for 10 seconds to 1 hour at, for example, 100° C. to 1,000° C. For example, the step of heat treating the hard mask composition may include a plurality of heat treatment steps, for example, a first heat treatment step and a second heat treatment step.

[0075] In one embodiment, the step of heat treating the hard mask composition may include one heat treatment step performed at, for example, 100° C. to 1000° C. for 10 seconds to 1 hour. For example, the heat treatment step may be performed in an air or nitrogen atmosphere, or in an atmosphere having an oxygen concentration of 1% by mass or less.

[0076] In one embodiment, the step of heat treating the hard mask composition includes a first heat treatment step performed at, for example, 100°C to 1,000°C, for example, 100°C to 800°C, for example, 100°C to 500°C, for example, 150°C to 400°C, for example, 30 seconds to 1 hour, for example, 30 seconds to 30 minutes, for example, 30 seconds to 10 minutes, for example, 30 seconds to 5 minutes.

[0077] Also, it may include a second heat treatment step successively performed at, for example, 100° C. to 1,000° C., for example, 300° C. to 1,000° C., for example, 500° C. to 1,000° C., for example, 500° C. to 600° C., for example, 30 seconds to 1 hour, for example, 30 seconds to 30 minutes, for example, 30 seconds to 10 minutes, for example, 30 seconds to 5 minutes. As an example, the first and second heat treatment steps may be performed in an air or nitrogen atmosphere, or in an atmosphere with an oxygen concentration of 1% by mass or less.

[0078] At least one of the steps of heat treating the hard mask composition is performed at a high temperature of 200° C. or more, thereby allowing the hard mask composition to exhibit high etching resistance that can withstand etching gases and chemical solutions to which the hard mask composition is exposed in subsequent processes, including an etching process.

[0079] In one embodiment, forming the hard mask layer may include an ultraviolet-visible (UV / Vis) curing step and / or a near-infrared (near IR) curing step.

[0080] In one embodiment, the step of forming the hard mask layer may include at least one of the steps of the first heat treatment step, the second heat treatment step, the ultraviolet-visible (UV / Vis) curing step, and the near-infrared (near-infrared) curing step, or may include two or more steps consecutively.

[0081] In one embodiment, the method may further include forming a silicon-containing thin film layer on the hard mask layer, the silicon-containing thin film layer being formed of a material such as SiCN, SiOC, SiON, SiOCN, SiC, SiO, and / or SiN.

[0082] In one embodiment, before the step of forming the photoresist layer, a bottom anti-reflective coating (BARC) may be further formed on the silicon-containing thin film layer or the hard mask layer.

[0083] In one embodiment, the step of exposing the photoresist layer can be performed using, for example, ArF, KrF, or EUV, etc. After the exposure, a heat treatment process can be performed at 100°C to 700°C.

[0084] In one embodiment, the step of etching the exposed portions of the material layer can be performed by dry etching using an etching gas, which can be, for example, N2 / O2, CHF3, CF4, Cl2, BCl3, and mixtures thereof.

[0085] The etched material layer can be formed in a variety of patterns, which can be diverse, such as metal patterns, semiconductor patterns, insulating patterns, etc., and can be applied as various patterns within a semiconductor integrated circuit device, for example.

[0086] The above-mentioned embodiments of the present invention will be described in more detail with reference to the following examples. However, the following examples are merely for illustrative purposes and are not intended to limit the scope of the present invention. EXAMPLES

[0087] Compound synthesis Synthesis Example 1 24.7g of potassium tert-butoxide was added to a mixture of 12.6g of 1,3-diethynylbenzene, 21.2g of benzaldehyde, and 200g of tetrahydrofuran (THF) cooled in a nitrogen atmosphere, and the mixture was stirred in an ice bath until all of the 1,3-diethynylbenzene had reacted. After stirring, water was added to stop the reaction. 200g of tetrahydrofuran (THF) was added, washed, and concentrated under reduced pressure, and n-hexane was added. The solid generated was filtered and dried under reduced pressure to obtain compound A represented by the following chemical formula 2-1 (molecular weight = 338.41g / mol).

[0088] [ka]

[0089] Synthesis Example 2 Compound B represented by the following chemical formula 3-1 (molecular weight = 366.46 g / mol) was obtained in the same manner as in Synthesis Example 1 above, except that 24.0 g of acetophenone was used instead of 21.2 g of benzaldehyde.

[0090] [ka]

[0091] Synthesis Example 3 Compound C represented by the following chemical formula 4-1 (molecular weight=490.60 g / mol) was obtained in the same manner as in Synthesis Example 1 above, except that 37.6 g of benzophenone was used instead of 21.2 g of benzaldehyde.

[0092] [ka]

[0093] Synthesis Example 4 Compound D represented by the following chemical formula 5-1 (molecular weight = 586.69 g / mol) was obtained in the same manner as in Synthesis Example 1 above, except that 46.0 g of pyrenecarboxaldehyde was used instead of 21.2 g of benzaldehyde.

[0094] [ka]

[0095] Synthesis Example 5 A mixture of 12.6g of 1,3,5-triethynylbenzene, 58.0g of pyrenecarboxaldehyde, and 600g of tetrahydrofuran (THF) was cooled in a nitrogen atmosphere, to which 31.1g of potassium tert-butoxide was added, and the mixture was stirred in an ice bath until all of the 1,3,5-triethynylbenzene had reacted. After stirring, water was added to stop the reaction. 600g of tetrahydrofuran (THF) was added, washed, and concentrated under reduced pressure, and then n-hexane was added. The solid that was generated was filtered off and dried under reduced pressure to obtain compound E represented by the following chemical formula 6-1 (molecular weight = 840.98g / mol).

[0096] [ka]

[0097] Synthesis Example 6 A mixture of 12.6 g of diethynylpyrene, 21.2 g of benzaldehyde, and 240 g of tetrahydrofuran (THF) cooled in a nitrogen atmosphere was added with 18.6 g of potassium tert-butoxide, and stirred in an ice bath until all of the diethynylpyrene had reacted. After stirring, water was added to stop the reaction. 240 g of tetrahydrofuran (THF) was added thereto, washed and concentrated under reduced pressure, and n-hexane was added. The generated solid was filtered and dried under reduced pressure to obtain compound F represented by the following chemical formula 7-1 (molecular weight = 478.59 g / mol).

[0098] [ka]

[0099] Synthesis Example 7 Compound G represented by the following chemical formula 8-1 was obtained (molecular weight = 506.64 g / mol) in the same manner as in Synthesis Example 6 above, except that 12.1 g of acetophenone was used instead of 21.2 g of benzaldehyde.

[0100] [ka]

[0101] Synthesis Example 8 Compound H represented by the following chemical formula 9-1 (molecular weight = 630.79 g / mol) was obtained in the same manner as in Synthesis Example 6 above, except that 18.6 g of benzophenone was used instead of 21.2 g of benzaldehyde.

[0102] [ka]

[0103] Synthesis Example 9 Compound I represented by the following chemical formula 10-1 (molecular weight=726.88 g / mol) was obtained in the same manner as in Synthesis Example 6 above, except that 23.2 g of pyrenecarboxaldehyde was used instead of 21.2 g of benzaldehyde.

[0104] [ka]

[0105] Comparative synthesis example 1 Terephthalaldehyde (13.4g, 0.1mol) was dissolved in tetrahydrofuran (THF, 300ml) and cooled to 0℃ under nitrogen atmosphere. Then, a THF mixed solution (0.5M, 30ml) in which ethynylmagnesium bromide was dissolved was gradually added dropwise and reacted for 1 hour. Then, the temperature was raised to room temperature and further reacted with stirring for 12 hours, and then quenched with saturated aqueous ammonium chloride solution (sat.NH4Cl(aq)). After the reaction was completed, the mixed solution was separated into an aqueous layer and an organic layer with ethyl acetate, and the aqueous layer was removed to obtain an organic layer. The solvent of the obtained organic layer was removed to obtain a compound represented by the following chemical formula 12-1 (yield 90%) (molecular weight = 338.41g / mol).

[0106] [ka]

[0107] The compound represented by the above formula 12-1 (5.3 g, 0.09 mol) was dissolved in propylene glycol monomethyl ether acetate (PGMEA, 200 ml), and then hydroxypyrene (HO-Pyrene, 43 g, 0.2 mol) was added. The mixed solution was heated to 90° C. and reacted until the compound represented by the above formula 12-1 disappeared. After the reaction, the mixture was purified to obtain comparative compound J represented by the following formula 12 (molecular weight = 338.41 g / mol).

[0108] [ka]

[0109] Comparative synthesis example 2 In a 2L three-neck flask, 27.6g (0.1mol) of benzoperylene and 42g (0.22mol) of naphthoyl chloride were placed together with 500g of a chloroform / dichloromethane mixture, and the mixture was stirred using a stirrer. 61.2g (0.35mol) of aluminum chloride was gradually added and reacted. After the reaction was completed, the aluminum chloride was removed using water. The product obtained from the powder was dissolved in tetrahydrofuran, and 18.98g (0.5mol) of lithium aluminum hydride was gradually added and reacted. After the reaction was completed, impurities generated during the reaction were removed using a water / methanol mixture to obtain a comparative compound K represented by the following chemical formula 13 (molecular weight = 338.41g / mol).

[0110] [ka]

[0111] Preparation of the hard mask composition Examples and Comparative Examples Compounds A to I obtained in Synthesis Examples 1 to 9 and Comparative Synthesis Examples 1 and 2, and Comparative Compounds J and K were dissolved in cyclohexanone and then filtered to produce hard mask compositions having a compound content of 10.0 mass %.

[0112] Evaluation 1: Heat resistance evaluation The hard mask compositions according to Examples 1 to 9 and Comparative Examples 1 and 2 were each coated on a silicon wafer by spin coating, and then heat-treated on a hot plate at 160°C for 1 minute to form a hard mask layer. The thickness of the hard mask layer was measured using a thin film thickness measuring device manufactured by K-MAC. Next, the hard mask layer was re-heat-treated at 400°C for 2 minutes, and the thickness of the hard mask layer was measured. If the change in thickness of the hard mask layer before and after re-heat-treatment at 400°C for 2 minutes was less than 5%, it was evaluated as "A (very good)", if it was 5% or more but less than 10%, it was evaluated as "B (good)", and if it was 10% or more, it was evaluated as "C (poor)". The results are shown in Table 1 below.

[0113] [Table 1]

[0114] Referring to Table 1, it was confirmed that the hard mask layers formed from the compositions according to Examples 1 to 9 had a thickness change rate of less than 5% before and after re-heat treatment, and the hard mask layers formed from the compositions according to Comparative Examples had a thickness change rate of 10% or more before and after re-heat treatment. In other words, it was confirmed that the heat resistance of the hard mask layers formed from the compositions according to the Examples was superior to that of the hard mask layers formed from the compositions according to Comparative Examples.

[0115] Evaluation 2: Gap-fill properties The hard mask compositions according to Examples 1 to 9 and Comparative Examples 1 and 2 were each coated on a patterned silicon wafer by spin coating, and then heat-treated at 400°C for 60 seconds to form a hard mask layer. A field emission scanning electron microscope (FE-SEM) was used to observe the cross-sectional image of the hard mask layer pattern to determine whether voids were generated. The results are shown in Table 2 below.

[0116] [Table 2]

[0117] Referring to Table 2 above, it was found that no voids were generated in the hard mask layers formed from the hard mask compositions according to Examples 1 to 9, whereas voids were generated in the hard mask layer formed from the hard mask composition according to Comparative Example 1. This shows that the gap-fill characteristics of the hard mask layers formed from the hard mask compositions according to the Examples are equivalent to or superior to those of the hard mask layers formed from the hard mask compositions according to Comparative Examples.

[0118] Evaluation 3: Flattening properties The hard mask compositions according to Examples 1 to 9 and Comparative Examples 1 to 2 were coated on a patterned silicon wafer by spin coating, and then heat-treated at 400° C. for 60 seconds. Then, a cross-sectional image of the pattern was observed using a field emission scanning electron microscope (FE-SEM). The thickness of the hard mask layer shown in the cross-sectional image of the pattern was measured, and the planarization characteristics were quantified using the calculation formula in FIG. 1. In FIG. 1, h1 means the average value of the thickness of the hard mask layer measured at three arbitrary points where no pattern was formed, and h2 means the average value of the thickness of the hard mask layer measured at three arbitrary points where a pattern was formed. If the value obtained above is less than 5, it is expressed as “A (very good)”, if it is 5 or more and less than 10, it is expressed as “B (good)”, and if it is 10 or more, it is expressed as “C (poor)”, and the results are shown in Table 3 below.

[0119] [Table 3]

[0120] Referring to Table 3 above, the planarization characteristics of the hard mask layers formed from the hard mask compositions according to Comparative Examples 1 and 2 were either "good" or "poor", whereas the planarization characteristics of the hard mask layers formed from the hard mask compositions according to Examples 1 to 9 were "very good", indicating that the hard mask layers had excellent planarization characteristics.

[0121] Rating 4: Etching resistance The hard mask compositions according to Examples 1 to 9 and Comparative Examples 1 and 2 were coated on a silicon wafer by spin coating, and then heat-treated on a hot plate at 160°C for 1 minute to form a hard mask layer. The hard mask layer was dry-etched for 30 seconds using a mixed gas of CF4 / Ar, and the thickness of the hard mask before and after etching was measured using a thin film thickness measuring device manufactured by K-MAC, and the etching rate (BER) was calculated by the following calculation formula 2. The etching resistance was evaluated by the ratio of the etching rate of the hard mask layer formed from the composition according to Comparative Example 1 to the etching rate of the hard mask layer formed from the composition according to Examples 1 to 9 and Comparative Example 2. Specifically, when the etching rate ratio was less than 0.95, it was expressed as "A (very good)", when it was 0.95 or more and less than 1.00, it was expressed as "B (good)", and when it was 1.00 or more, it was expressed as "C (poor)". The results are shown in Table 4 below.

[0122]

number

[0123] [Table 4]

[0124] Referring to Table 4, the etching rate of the hard mask layer formed from the composition according to Comparative Example 1 was less than 0.95 for the hard mask layer formed from the composition according to Examples 1 to 9, and the etching rate of the hard mask layer formed from the composition according to Comparative Example 2 was greater than or equal to 1. From these results, it was confirmed that the etching resistance of the hard mask layer formed from the composition according to the Examples was superior to that of the hard mask layer formed from the composition according to Comparative Example.

[0125] Although the preferred embodiments of the present invention have been described in detail above, the scope of the present invention is not limited thereto, and various modifications and improvements made by those skilled in the art using the basic concept of the invention defined in the claims below also fall within the scope of the present invention.

Claims

1. A hard mask composition comprising a compound represented by the following Chemical Formula 1 and a solvent: 【Chemistry 1】 In the above Chemical Formula 1, Ar 1 and Ar 2 each independently represents a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, or a group in which two or more substituted or unsubstituted aromatic hydrocarbon groups having 6 to 30 carbon atoms are linked by a single bond or a substituted or unsubstituted alkylene group having 1 to 30 carbon atoms, R 1 and R 2 each independently represents a hydrogen atom, a deuterium atom, a substituted or unsubstituted saturated or unsaturated aliphatic hydrocarbon group having 1 to 30 carbon atoms, a substituted or unsubstituted saturated or unsaturated alicyclic hydrocarbon group having 3 to 30 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, or a combination thereof; n is an integer from 2 to 6.

2. Ar in Formula 1 1 and Ar 2 The hard mask composition according to claim 1 , wherein each of the groups is independently a substituted or unsubstituted group having at least one of the structures selected from Group 1 below: 【Chemistry 2】

3. Ar in Formula 1 1 and Ar 2 The hard mask composition according to claim 1, wherein each of the groups is independently a substituted or unsubstituted group having at least one of the structures selected from the following Group 1-1: 【Chemistry 3】

4. R in Formula 1 1 and R 2 are each independently a hydrogen atom, a deuterium atom, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, or a combination thereof.

5. R in Formula 1 1 and R 2 each independently represents a hydrogen atom, a deuterium atom, a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 20 carbon atoms, or a combination thereof.

6. Ar in Formula 1 1 and Ar 2 are each independently a substituted or unsubstituted group having at least one structure selected from the following Group 1-2, R 1 and R 2 are each independently a hydrogen atom, a deuterium atom, a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 20 carbon atoms, or a combination thereof; and n is an integer from 2 to 4. 【Chemistry 4】

7. In Formula 1, n is 2 or 3, and all R 1 are identical to each other, and all R 2 are identical to each other, and all Ar 2 10. The hardmask composition of claim 1, wherein:

8. 2. The hard mask composition according to claim 1, wherein the compound represented by Formula 1 is at least one of compounds represented by Formulas 2 to 10 below. 【Chemistry 5】 【Chemistry 6】

9. 2. The hard mask composition of claim 1, wherein the compound represented by Formula 1 has a molecular weight of 300 g / mol to 10,000 g / mol.

10. The hard mask composition of claim 1, wherein the compound represented by Formula 1 is present in an amount of 0.1% by weight to 30% by weight based on the total weight of the hard mask composition.

11. 2. The hard mask composition of claim 1, wherein the solvent is at least one of propylene glycol, propylene glycol diacetate, methoxypropanediol, diethylene glycol, diethylene glycol butyl ether, tri(ethylene glycol) monomethyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, cyclohexanone, ethyl lactate, γ-butyrolactone, N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidinone, acetylacetone, and ethyl 3-ethoxypropionate.

12. A hardmask layer comprising a cured product of the hardmask composition according to any one of claims 1 to 11.

13. forming a layer of material on a substrate; applying a hard mask composition according to any one of claims 1 to 11 onto the material layer; heat-treating the hard mask composition to form a hard mask layer; forming a photoresist layer over the hard mask layer; exposing and developing the photoresist layer to form a photoresist pattern; selectively removing the hard mask layer utilizing the photoresist pattern to expose portions of the material layer; and c) etching the exposed portions of the layer of material.

14. The method of claim 13, wherein the step of forming the hard mask layer comprises a step of performing a heat treatment at a temperature of 100° C. to 1,000° C.

Citation Information

Patent Citations

  • Compound, composition for forming organic film, substrate for manufacturing semiconductor device, method of forming organic film, and method of forming pattern

    JP2019172605A

  • Aromatic underlayer

    JP2020071486A

  • Hard mask composition, hard mask layer and patterning method

    JP2023031300A

  • Composition for film formation use, resist underlayer film and method for formation thereof, pattern formation method, and compound

    WO2014208324A1

  • Hardmask composition, hardmask layer and method of forming patterns

    KR1020220092160A