Method for manufacturing resin composition
A resin composition is produced using a specific sulfonium salt with a molecular weight of 500 or more, enhancing adhesion and storage stability by a heating process, addressing reactivity and adhesion issues in conventional resin compositions.
Patent Information
- Application Number
- JP2023077010
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-09
- Publication Date
- 2024-11-21
AI Technical Summary
Conventional resin compositions using sulfonium salts as thermal cationic polymerization initiators face issues with decreased reactivity and adhesion to base materials due to the use of stabilizers, leading to shortened pot life and storage stability concerns.
A method involving a heating step to produce a resin composition with a specific sulfonium salt having a cation moiety with a molecular weight of 500 or more, combined with an epoxy resin, crosslinking agents, and other additives, to enhance adhesion and storage stability.
The method results in a resin composition with improved adhesion to base materials and excellent storage stability, maintaining reactivity and curing properties without light irradiation.
Smart Images

Figure 2024161937000001 
Figure 2024161937000002 
Figure 2024161937000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a resin composition. [Background technology]
[0002] Conventionally, photo-cationically polymerizable adhesives containing epoxy resin as a main component have been used as a type of adhesive used when mounting electronic components such as IC chips on wiring boards. Such photo-cationically polymerizable adhesives contain a photo-cationic polymerization initiator that generates protons by light and starts cationic polymerization. However, when mounting electronic components on wiring boards, there are many cases where light cannot be irradiated onto the joints made by the photo-cationically polymerizable adhesive. In such cases, a thermally polymerizable adhesive that can generate protons only by heat, not by light, is used. Such a thermally polymerizable adhesive contains a thermally polymerizable initiator that generates protons by heat and starts cationic polymerization.
[0003] Patent Document 1 discloses an adhesive (resin composition) using a sulfonium salt as a thermal cationic polymerization initiator. In general, when a highly sensitive polymerizable resin such as an alicyclic epoxy resin and a sulfonium salt are made into a one-component solution, the reaction proceeds at room temperature. This shortens the pot life, which is the time during which the adhesive can be used, and makes the adhesive difficult to handle. Therefore, Patent Document 1 uses a stabilizer in the resin composition to extend the pot life of the adhesive. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2014-31451 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, when a stabilizer is used in a resin composition as in Patent Document 1, there is a concern that the reactivity between the polymerizable resin and the sulfonium salt decreases, and the adhesion of the resin composition to a substrate decreases.
[0006] In view of the above problems, an object of the present invention is to provide a method for producing a resin composition that maintains adhesion to a substrate and has excellent storage stability. [Means for solving the problem]
[0007] In order to solve the above-mentioned problems, the present invention provides a method for producing a resin composition, comprising a heating step of heating a mixture containing an epoxy resin and a sulfonium salt, the sulfonium salt having a structure represented by general formula (1) and a cation moiety having a molecular weight of 500 or more.
[0008] [ka]
[0009] R 1 ~R 3 represents a hydrogen atom, an alkyl group, an alkylthio group, an alkylcarbonyl group, an alkylsulfonyl group, an alkoxy group, an alkoxycarbonyl group, an aryl group, an arylcarbonyl group, an aryloxycarboaryl group, an aryloxy group, an arylthio group, an arylsulfinyl group, a hydroxy group, a hydroxy(poly)alkyleneoxy group, an acyloxy group, a cyano group, a nitro group, a halogen atom, a heterocyclic hydrocarbon group, an optionally substituted silyl group, or an amino group; R 1 ~R 3 may be the same or different. 1 ~R 3 Two or more of the following may be directly connected to each other or -O-, -S-, -SO-, SO 2 A ring structure containing the element S may be formed via -, -NH-, -CO-, -COO-, -CONH-, an alkylene group or a phenylene group. Effect of the Invention
[0010] It is possible to provide a method for producing a resin composition that maintains adhesion to a substrate and has excellent storage stability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] In adhesives (resin compositions) containing epoxy resin as a main component, a method is known in which a photocationic polymerization initiator is blended from the viewpoint of reactivity and storage stability, and the adhesive is bonded by light irradiation. On the other hand, when light irradiation is not possible at the joint, a method is known in which a thermal cationic polymerization initiator capable of generating protons by heat alone is used. As the thermal cationic polymerization initiator, a compound capable of generating a cationic species that initiates polymerization by heating is used, and examples thereof include quaternary ammonium salts, phosphonium salts, and sulfonium salts. In particular, as the thermal cationic polymerization initiator for epoxy resins, sulfonium salts are selected, and those having benzylsulfonium as shown in general formula (2) or heterocyclic derivatives as shown in general formula (3) in the cationic portion are used. However, when these are used, the pot life of the adhesive (resin composition) is shortened, and it has been very difficult to control the adhesion and storage stability of the resin composition to the substrate.
[0012] [ka]
[0013] R 4 is an optionally substituted phenyl group, R 5 represents an alkyl group.
[0014] [ka]
[0015] R 6 represents an optionally substituted alkyl group.
[0016] According to the study by the present inventors, among sulfonium salts generally used as photocationic polymerization initiators, compounds having a specific structure function as thermal cationic polymerization initiators. It has been found that by using such sulfonium salts, it is possible to provide an adhesive (resin composition) that maintains adhesion to a substrate and has excellent storage stability. Specifically, a desired resin composition can be produced by heating a mixture containing an epoxy resin and a specific sulfonium salt. A method for producing a resin composition will be described in detail below with reference to preferred embodiments.
[0017] (sulfonium salts) The mixture according to the present embodiment contains a sulfonium salt. The sulfonium salt has a cation moiety and an anion moiety. First, the cation moiety will be described.
[0018] The sulfonium salt in this embodiment has a structure represented by general formula (1) in a cation moiety having a molecular weight of 500 or more.
[0019] [ka]
[0020] R 1 ~R 3 represents a hydrogen atom, an alkyl group, an alkylthio group, an alkylcarbonyl group, an alkylsulfonyl group, an alkoxy group, an alkoxycarbonyl group, an aryl group, an arylcarbonyl group, an aryloxycarboaryl group, an aryloxy group, an arylthio group, an arylsulfinyl group, a hydroxy group, a hydroxy(poly)alkyleneoxy group, an acyloxy group, a cyano group, a nitro group, a halogen atom, a heterocyclic hydrocarbon group, an optionally substituted silyl group, or an amino group; R 1 ~R 3 may be the same or different. 1 ~R 3 Two or more of the following may be directly connected to each other or -O-, -S-, -SO-, SO 2A ring structure containing the element S may be formed via -, -NH-, -CO-, -COO-, -CONH-, an alkylene group or a phenylene group.
[0021] Conventionally, triphenylsulfonium salts have generally been used as photocationic polymerization initiators, and have required irradiation with light such as ultraviolet light in the curing process of epoxy resins. Therefore, they have not been used in systems that are cured only by heating.
[0022] According to the study of the present inventors, it has been found that among sulfonium salts, sulfonium salts having a structure shown in general formula (1) in the cationic moiety with a molecular weight of 500 or more can harden epoxy resins only by heat treatment without a light irradiation process. Furthermore, by making the skeleton of the cationic moiety the triphenylsulfone structure shown in general formula (1), the degree of SC bonding is improved compared to structures such as general formulas (2) and (3). Furthermore, by making the molecular weight of the cationic moiety 500 or more, the thermal stability of the sulfonium salt is improved.
[0023] Among the structures represented by the general formula (1), preferred specific examples are shown in the following formula.
[0024] [ka]
[0025] Next, the anion portion will be described. The anion portion of the sulfonium salt is SbF 6 - and AsF 6 - And, P.F. 6 - and (Rf) n PF 6-n - (Rf is a perfluoroalkyl group) and BF 4 - And B(C 6 F 5 ) 4 -From the viewpoint of adhesion between the produced resin composition and a substrate, it is preferable to use SbF 6 - , (Rf) n PF 6-n - and B(C 6 F 5 ) 4 - is preferably used, and in particular, the sulfonium salt is SbF 6 - It is preferable that the sulfonium salt contains one kind or a combination of two or more kinds.
[0026] Specific examples of commercially available products include "ADEKA OPTOMER SP-172" (trade name) manufactured by ADEKA, "CPI-310A" (trade name) and "CPI-410S" (trade name) manufactured by SAN-APRO, and "Irgacure290" (trade name) manufactured by BASF. From the viewpoints of curability and adhesion to a substrate, the content of the sulfonium salt in the mixture of the sulfonium salt and the epoxy resin to be cured is preferably 0.1 to 30 parts by mass per 100 parts by mass of the solid content of the epoxy resin to be added.
[0027] (Epoxy resin) The mixture according to the present embodiment contains an epoxy resin. In consideration of the adhesive performance, mechanical strength and swelling resistance of the resin composition, the epoxy resin in the present embodiment is preferably a cationic polymerization type epoxy resin. More specifically, the epoxy resin may be an epoxy resin having a bisphenol skeleton, such as an epoxy resin having an alicyclic skeleton, an epoxy resin having a bisphenol skeleton, such as bisphenol A-type and F-type epoxy resins, an epoxy resin having a phenol novolac skeleton, such as an epoxy resin having a phenol novolac skeleton, an epoxy resin having a cresol novolac skeleton, such as an epoxy resin having a cresol novolac skeleton, an epoxy resin having a norbornene skeleton, an epoxy resin having a terpene skeleton, an epoxy resin having a dicyclopentadiene skeleton, and an epoxy resin having an oxycyclohexane skeleton, and other polyfunctional epoxy resins. As the epoxy resin, one or a combination of two or more of these may be used.
[0028] In order to three-dimensionally crosslink the resin composition and obtain the desired curability, the epoxy resin preferably contains a difunctional or higher epoxy resin. In particular, the epoxy resin preferably contains a trifunctional or higher epoxy resin. Furthermore, it is preferable to use at least one difunctional epoxy resin in addition to the trifunctional or higher epoxy resin.
[0029] As commercially available bifunctional epoxy resins, "jER1004" (trade name), "jER1007" (trade name), "jER1009" (trade name), "jER1010" (trade name), and "jER1256" (trade name) manufactured by Mitsubishi Chemical Corporation, and "EPICLON 4050" (trade name) and "EPICLON 7050" (trade name) manufactured by Dainippon Ink and Chemicals, Inc. are preferably used.
[0030] Commercially available trifunctional or higher epoxy resins include "jER157S70" (trade name), "jER1031S" (trade name) manufactured by Mitsubishi Chemical Corporation, "Epicron N-695" (trade name), "Epicron N-865" (trade name) manufactured by Dainippon Ink and Chemicals, Inc., "Celloxide 2021" (trade name), "GT-300 series", "GT-400 series", "EHPE3150" (trade name) manufactured by Daicel Corporation, "SU8" (trade name) manufactured by Nippon Kayaku Co., Ltd., "VG3101" (trade name), "EPOX-MKR1710) (trade name) manufactured by Printec Co., Ltd., and "Denacol series" manufactured by Nagase ChemteX Corporation.
[0031] (Crosslinking agent) The mixture according to the present embodiment preferably contains a polyol as a crosslinking agent. Here, the polyol is a compound having at least two or more hydroxyl groups in the molecule. By containing a polyol in the mixture containing an epoxy resin and a sulfonium salt, it is possible to promote the cationic polymerization reaction of the epoxy resin and reduce the stress of the resin composition due to the reaction between the ring-opened epoxy group and the hydroxyl group. In other words, it is effective in improving the adhesion of the resin composition to the substrate.
[0032] In addition, from the viewpoint of solubility and reactivity in resins and solvents, the polyol preferably has a number average molecular weight of 3000 or less. Here, the number average molecular weight refers to the simple average of the amount of one polymer chain contained in a polymer. Furthermore, in order for the polyol to not disappear during the heating process of a mixture containing an epoxy resin and a sulfonium salt, the number average molecular weight of the polyol is preferably 200 or more. The number average molecular weight can be calculated in terms of polystyrene by a known method using gel permeation chromatography (for example, manufactured by Shimadzu Corporation). In addition, in order for the polyol to not disappear during the heating process of a mixture containing an epoxy resin and a sulfonium salt, the polyol preferably has a boiling point of 200°C or more.
[0033] Specific examples of polyols include polyethylene glycols (PEG) (200, 300, 400, 600, 1000, 2000) commercially available from various companies. In addition, examples of polyether polyols include ADEKA's "ADEKA Polyether P Series", "BPX Series", "G Series", "SP Series", "SC Series", "CM Series", "AM Series", "EM Series", "BM Series", "PR Series" and "GR Series" (all trade names). Examples of low molecular weight polyols include 1,2- or 1,6-hexanediol, glycerin, trimethylolpropane, 3-methyl-1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,2,6-hexanetriol, 1,5-dihydroxypentan-3-one, 6-hydroxycaproic acid, 2-hydroxymethyl-1 and 3-propanediol, etc. At least one of these can be used. In addition, two or more of these can be used in combination.
[0034] (Silane coupling agent) The mixture of the present embodiment preferably contains a silane coupling agent. Examples of commercially available silane coupling agents include "A-187" (trade name) manufactured by Momentive Performance Materials, Inc.
[0035] (Other Ingredients) The mixture of the present embodiment may contain other components within a range that does not impair the properties of the resin composition. By including other components, it is possible to impart desired properties to the resin composition.
[0036] For example, to adjust the curability or reaction rate, a sensitizer, a basic substance such as an amine, or an acid generator that generates weakly acidic (pKa=-1.5 to 3.0) toluenesulfonic acid may be added to the mixture. Commercially available acid generators that generate toluenesulfonic acid include "TPS-1000" (trade name) manufactured by Midori Chemical Industry Co., Ltd. and "WPAG-367" (trade name) manufactured by Wako Pure Chemical Industries, Ltd.
[0037] (Method of producing resin composition) The method for producing the resin composition of the present invention will be described. First, the method includes a step of mixing an epoxy resin and a sulfonium salt to prepare a mixture containing them. The mixture may contain the above-mentioned crosslinking agent (polyol), silane coupling agent, and other components. Next, the method may include a dissolving step of dissolving the mixture in a solvent. As the solvent, for example, propylene glycol monomethyl ether acetate (PGMEA) is preferably used. Next, the method includes a heating step of heating the mixture containing the epoxy resin and the sulfonium salt. By heating the mixture, the reaction proceeds and the resin composition can be produced. The heating temperature in the heating step is preferably 90°C or higher and 300°C or lower. The heating temperature in the heating step here is sufficient if it is raised to a temperature of 90°C or higher and 300°C or lower, and there is no need to maintain the temperature at 90°C or higher and 300°C or lower throughout the entire heating step. In addition, the heating time at the heating temperature is preferably 1 hour. If the heating temperature is 90°C or lower, the resin composition may not be cured sufficiently, and the adhesion to the substrate may be reduced. On the other hand, there is a risk that the epoxy resin may decompose if the heating temperature is 300° C. or higher. Furthermore, the heating temperature in the heating step is more preferably 100° C. or higher and 250° C. or lower.
[0038] In addition, when the dissolving step is performed, it is preferable to perform a drying treatment for drying the solvent in the mixture before the heating step of the mixture. The temperature and time of the drying treatment may be, for example, heating at 90°C for 5 minutes.
[0039] Through the above steps, the resin composition according to the present invention can be produced. EXAMPLES
[0040] The following examples of the present invention will be described.
[0041] (Examples 1 to 27) A mixture having the composition shown in Tables 2 to 6 was applied onto a substrate by spin coating, and the solvent was dried at 90° C. for 5 minutes. Furthermore, a heating step was performed in which the mixture was heated at the temperature shown in each example, to obtain a resin composition.
[0042] (Comparative Examples 1 to 4) The resin composition was cured on the substrate in the same manner as in Example 1, except that the composition shown in Table 7 was used as the mixture.
[0043] The structure of the cation moiety of the sulfonium salt used in the examples and comparative examples is shown in the following formula.
[0044] [ka]
[0045] [ka]
[0046] Table 1 shows a summary of the cationic and anionic moieties of the sulfonium salts contained in the mixture.
[0047] [Table 1]
[0048] [Evaluation method 1] The adhesion to a substrate was evaluated for the resin compositions prepared by the methods of Examples 1 to 27 and Comparative Examples 1 to 4. The resin compositions were immersed in a 20 wt % aqueous solution of 1,2-hexanediol and stored at 70°C, and the presence or absence of peeling between the resin composition and the substrate was observed using an optical microscope. Excellent adhesion: No peeling even after one month Adhesion: Peeling occurs within one week to one month Adhesion: ×: Peeling occurs within one week [Evaluation method 2] The rate of change in viscosity when stored at room temperature was confirmed for the resin compositions used in Examples 1 to 27 and Comparative Examples 1 to 4. The viscosity was measured using an E-type viscometer (manufactured by Toki Sangyo Co., Ltd.). Storage stability: Viscosity increase rate after one month is less than 10% Storage stability ×: Viscosity change rate after one month is 10% or more Tables 2 to 7 show the evaluation results for each of the examples and comparative examples.
[0049] [Table 2]
[0050] [Table 3]
[0051] [Table 4]
[0052] [Table 5]
[0053] [Table 6]
[0054] [Table 7]
[0055] [Evaluation Results] As shown in Tables 2 to 6, the method according to the present invention was able to provide a resin composition having excellent adhesion to a substrate and excellent storage stability.
[0056] In Table 2, Examples 1 to 12, in which a sulfonium salt having a structure represented by general formula (1) was used in the cation moiety with a molecular weight of 500 or more, gave good results in terms of adhesion to the substrate and storage stability. 6 - Examples 1, 7, 8, 10 and 12 containing the compound were particularly excellent in adhesion.
[0057] In Table 3, Examples 13 and 14, in which the amount of sulfonium salt added in the mixture was 0.1 to 30 parts by mass relative to 100 parts by mass of the epoxy resin, showed better adhesion than Examples 12 and 15.
[0058] In Table 4, Examples 17 and 18, which used jER157S70 and EHPE3150, respectively, other than N-695, as the tri- or higher functional epoxy resin, also showed good adhesion. Also, Example 19, which used a combination of a tri- or higher functional epoxy resin and a di- or higher functional epoxy resin as the epoxy resin, showed good adhesion to the substrate.
[0059] In Table 5, in Examples 20 to 23, which contained a polyol as a crosslinking agent, the resin composition had good adhesion to the substrate. The number average molecular weight and boiling point of the polyol used in each Example are as follows. ·PEG200: Number average molecular weight 190~210, boiling point 250℃ or higher ·PEG600: Number average molecular weight 570~630, boiling point 250℃ or higher ·PEG1000: Number average molecular weight 950~1050, boiling point 250℃ or higher Also in Example 23, in which a silane coupling agent was used, a resin composition having good adhesion to the substrate was obtained.
[0060] In Table 6, Examples 25 and 26, in which the mixture curing temperatures were 100°C and 250°C, respectively, had better adhesion to the substrate of the resulting resin composition than Examples 24 and 27, in which the mixture curing temperatures were 90°C and 300°C, respectively.
[0061] On the other hand, in Table 7, in Comparative Example 1, in which an iodonium salt was used instead of a sulfonium salt, the viscosity change rate after one month of storage was 10% or more. In Comparative Example 2, in which the cationic moiety of the sulfonium salt does not have the structure shown in general formula (1), the viscosity also increased by 10% or more after one week of storage. Furthermore, in Comparative Examples 3 and 4, in which the cationic moiety of the sulfonium salt has the structure shown in general formula (1) but has a molecular weight of less than 500, a resin composition having good adhesion to the substrate was not obtained.
[0062] As described above, when the sulfonium salt contained in the mixture has a structure represented by general formula (1) in the cation moiety having a molecular weight of 500 or more, a resin composition having excellent storage stability while maintaining adhesion to the substrate can be produced.
[0063] The resin composition of the present invention is suitable as an adhesive for bonding a flow path forming substrate that forms a flow path of an inkjet head and a discharge port forming substrate that discharges liquid.The resin composition of the present invention is also suitable as an adhesive for bonding a flow path forming substrate that forms a flow path and a damper film (polyimide) that suppresses vibration of the liquid in an inkjet head.
[0064] To summarize the present invention as described above, the present invention includes the following configurations.
[0065] (Configuration 1) A method for producing a resin composition, comprising: A heating step of heating a mixture containing an epoxy resin and a sulfonium salt, The method for producing a resin composition, wherein the sulfonium salt has a structure represented by general formula (1) and has a cation moiety with a molecular weight of 500 or more.
[0066] [ka]
[0067] R 1 ~R 3represents a hydrogen atom, an alkyl group, an alkylthio group, an alkylcarbonyl group, an alkylsulfonyl group, an alkoxy group, an alkoxycarbonyl group, an aryl group, an arylcarbonyl group, an aryloxycarboaryl group, an aryloxy group, an arylthio group, an arylsulfinyl group, a hydroxy group, a hydroxy(poly)alkyleneoxy group, an acyloxy group, a cyano group, a nitro group, a halogen atom, a heterocyclic hydrocarbon group, an optionally substituted silyl group, or an amino group; R 1 ~R 3 may be the same or different. 1 ~R 3 Two or more of the following may be directly connected to each other or -O-, -S-, -SO-, SO 2 A ring structure containing the element S may be formed via -, -NH-, -CO-, -COO-, -CONH-, an alkylene group or a phenylene group.
[0068] (Configuration 2) 2. The method for producing a resin composition according to claim 1, wherein the heating temperature in the heating step is 90° C. or higher and 300° C. or lower.
[0069] (Configuration 3) 3. The method for producing a resin composition according to claim 1 or 2, wherein the heating temperature in the heating step is 100° C. or higher and 250° C. or lower.
[0070] (Configuration 4) The method for producing a resin composition according to any one of the above aspects 1 to 3, wherein the epoxy resin contains a tri- or higher functional epoxy resin.
[0071] (Configuration 5) The method for producing a resin composition according to any one of claims 1 to 4, wherein the epoxy resin contains a difunctional epoxy resin.
[0072] (Configuration 6) The method for producing a resin composition according to any one of Structures 1 to 5, wherein the epoxy resin includes at least one selected from the group consisting of an epoxy resin having an alicyclic skeleton, an epoxy resin having a bisphenol skeleton, an epoxy resin having a phenol novolac skeleton, an epoxy resin having a cresol novolac skeleton, an epoxy resin having a norbornene skeleton, an epoxy resin having a terpene skeleton, an epoxy resin having a dicyclopentadiene skeleton, and an epoxy resin having an oxycyclohexane skeleton.
[0073] (Configuration 7) The anion portion of the sulfonium salt is SbF 6 - and AsF 6 - And, P.F. 6 - and (Rf) n PF 6-n - (Rf is a perfluoroalkyl group) and BF 4 - And B(C 6 F 5 ) 4 - and at least one selected from the group consisting of:
[0074] (Configuration 8) The anion portion of the sulfonium salt is SbF 6 - The method for producing the resin composition according to any one of Configurations 1 to 7,
[0075] (Configuration 9) 9. The method for producing a resin composition according to any one of configurations 1 to 8, wherein the content of the sulfonium salt in the mixture is 0.1 to 30 parts by mass per 100 parts by mass of a solid content of the epoxy resin.
[0076] (Configuration 10) 10. The method for producing a resin composition according to any one of claims 1 to 9, wherein the mixture contains a polyol having at least two hydroxyl groups in the molecule.
[0077] (Configuration 11) 11. The method for producing a resin composition according to claim 10, wherein the polyol has a number average molecular weight of 3,000 or less.
[0078] (Configuration 12) 12. The method for producing a resin composition according to claim 10 or 11, wherein the polyol has a number average molecular weight of 200 or more.
[0079] (Configuration 13) 13. The method for producing a resin composition according to any one of claims 10 to 12, wherein the polyol has a boiling point of 200°C or higher.
[0080] (Configuration 14) 14. The method for producing a resin composition according to any one of claims 1 to 13, wherein the mixture contains a silane coupling agent.
[0081] (Configuration 15) 15. The method for producing a resin composition according to any one of claims 1 to 14, wherein the mixture contains a solvent.
[0082] (Configuration 16) 16. The method for producing a resin composition according to claim 15, wherein the solvent is propylene glycol monomethyl ether acetate.
Claims
1. A method for producing a resin composition, comprising: A heating step of heating a mixture containing an epoxy resin and a sulfonium salt, The sulfonium salt has a structure represented by general formula (1) and has a cation moiety with a molecular weight of 500 or more. [Formula 1] (R 1 ~R 3 represents a hydrogen atom, an alkyl group, an alkylthio group, an alkylcarbonyl group, an alkylsulfonyl group, an alkoxy group, an alkoxycarbonyl group, an aryl group, an arylcarbonyl group, an aryloxycarboaryl group, an aryloxy group, an arylthio group, an arylsulfinyl group, a hydroxy group, a hydroxy(poly)alkyleneoxy group, an acyloxy group, a cyano group, a nitro group, a halogen atom, a heterocyclic hydrocarbon group, an optionally substituted silyl group, or an amino group; R 1 ~R 3 may be the same or different. 1 ~R 3 Two or more of these are directly connected to each other or -O-, -S-, -SO-, SO 2 A ring structure containing the element S may be formed via -, -NH-, -CO-, -COO-, -CONH-, an alkylene group or a phenylene group.
2. The method for producing a resin composition according to claim 1 , wherein the heating temperature in the heating step is 90° C. or higher and 300° C. or lower.
3. The method for producing a resin composition according to claim 1 , wherein the heating temperature in the heating step is 100° C. or higher and 250° C. or lower.
4. The method for producing a resin composition according to claim 1 , wherein the epoxy resin comprises a tri- or higher functional epoxy resin.
5. The method for producing a resin composition according to claim 1 or 4, wherein the epoxy resin comprises a difunctional epoxy resin.
6. 2. The method for producing a resin composition according to claim 1, wherein the epoxy resin includes at least one selected from the group consisting of epoxy resins having an alicyclic skeleton, epoxy resins having a bisphenol skeleton, epoxy resins having a phenol novolac skeleton, epoxy resins having a cresol novolac skeleton, epoxy resins having a norbornene skeleton, epoxy resins having a terpene skeleton, epoxy resins having a dicyclopentadiene skeleton, and epoxy resins having an oxycyclohexane skeleton.
7. The anion portion of the sulfonium salt is SbF 6 - and AsF 6 - And, P.F. 6 - and (Rf) n P.F. 6-n - (Rf is a perfluoroalkyl group) and BF 4 - And B (C 6 F 5 ) 4 - The method for producing a resin composition according to claim 1, further comprising at least one selected from the group consisting of:
8. The anion portion of the sulfonium salt is SbF 6 - The method for producing the resin composition according to claim 1,
9. The method for producing a resin composition according to claim 1, wherein the content of the sulfonium salt in the mixture is 0.1 to 30 parts by mass per 100 parts by mass of a solid content of the epoxy resin.
10. The method for producing a resin composition according to claim 1 , wherein the mixture contains a polyol having at least two hydroxyl groups in the molecule.
11. The method for producing a resin composition according to claim 10, wherein the polyol has a number average molecular weight of 3,000 or less.
12. The method for producing a resin composition according to claim 10 or 11, wherein the polyol has a number average molecular weight of 200 or more.
13. The method for producing a resin composition according to claim 10, wherein the polyol has a boiling point of 200°C or higher.
14. The method for producing a resin composition according to claim 1 , wherein the mixture contains a silane coupling agent.
15. The method for producing a resin composition according to claim 1 , wherein the mixture contains a solvent.
16. The method for producing a resin composition according to claim 15, wherein the solvent is propylene glycol monomethyl ether acetate.
Citation Information
Patent Citations
Thermal cation generator composition, thermosetting composition, and anisotropic conductive connection material
JP2014031451A