Acrylic resin, resin composition and hot-melt adhesive
The acrylic resin, with controlled pH and composition, addresses the issues of initial adhesive strength, discoloration, and VOC content in conventional hot melt adhesives, providing improved performance and stability.
Patent Information
- Application Number
- JP2023077188
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-09
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2043-05-09
AI Technical Summary
Conventional reactive hot melt adhesives suffer from issues such as insufficient initial adhesive strength, discoloration, and high viscosity due to heating, as well as high VOC content, which affects their appearance and application process.
An acrylic resin with a pH of 4.0 to 8.0, containing specific copolymers and monomers, and a controlled particle size and molecular weight, is formulated to minimize thickening and discoloration, and is produced without alkaline compounds to reduce VOCs.
The acrylic resin and hot melt adhesive exhibit improved initial adhesive strength, reduced discoloration, and lower VOC content, ensuring better appearance and process stability.
Smart Images

Figure 2024162037000001 
Figure 2024162037000002 
Figure 2024162037000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an acrylic resin, a resin composition, and a hot melt adhesive. [Background technology]
[0002] Hot melt adhesives are solid or semi-solid at room temperature, and become fluid when heated. In particular, those whose main component is a urethane prepolymer with an isocyanate group at the end are called reactive hot melt adhesives, and most of them are moisture-curing urethane adhesives, usually in the form of a urethane prepolymer with an isocyanate group, which is formed by condensation polymerization of a polyol component and an isocyanate component.
[0003] These reactive hot melt adhesives are applied to a substrate in a heated and molten state, and after cooling and solidifying, moisture curing occurs through a chemical crosslinking reaction between isocyanate groups and water, forming a coating (adhesive layer) that is tough, heat-resistant, and chemical-resistant.
[0004] Conventional reactive hot melt adhesives exhibit excellent adhesive properties when chemical crosslinks are formed by moisture curing, but have the problem that chemical crosslinks hardly occur immediately after application. In addition, the adhesive has a high temperature immediately after heating and melting, and has fluidity due to the characteristics of thermoplastic polymers, so that the initial adhesive strength to the substrate is insufficient. Note that the initial adhesive strength means the adhesive strength after application to the substrate and before moisture curing. Furthermore, conventional reactive hot melt adhesives have the problem that the adhesive turns yellow immediately after heating and melting, which deteriorates the appearance. As a means for increasing the initial adhesive strength, a method is known in which a thermoplastic resin is blended with a hot melt adhesive to improve the initial adhesive strength. Patent Document 1 discloses an acrylic resin powder for reactive hot melt adhesives that is easily soluble in polyalkylene glycol.
[0005] Reactive hot melt adhesives are melted and applied using a machine that applies the adhesive according to the intended use. If the adhesive thickens due to the application of heat for a certain period of time, this is undesirable as it will cause work defects during the application process. Also, discoloration will result in poor appearance in applications where people can see the adhesive, such as furniture. Furthermore, in recent years, volatile organic compounds (VOCs) generated from chemical substances have become a problem, and regulations are becoming stricter in each country. There is a demand for the development of acrylic resins for reactive hot melt adhesives that contain as little low molecular weight VOCs as possible. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] International Publication No. 2018 / 012234 Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention has been made to solve these problems. That is, an object of the present invention is to provide an acrylic resin powder, a resin composition, and a hot melt adhesive that are less prone to thickening or discoloration due to heating, have a good appearance, and have a low VOC content compared to conventional products. [Means for solving the problem]
[0008] The present invention relates to the following items [1] to
[13] . [1] An acrylic resin whose pH when dissolved in a 40% by weight aqueous solution is between 4.0 and 8.0 and which does not contain any alkaline compounds. [2] The acrylic resin according to [1], which contains a copolymer having a structural unit derived from a (meth)acrylic monomer. [3] The acrylic resin according to [1] or [2], wherein the primary particles have a volume average particle size of 0.1 to 10 μm, and the secondary particles have a volume average particle size of 20 to 80 μm. [4] The acrylic resin according to any one of [1] to [3], which has a mass average molecular weight of 100,000 or less. [5] The acrylic resin according to any one of [1] to [4], which has a structural unit derived from a hydroxyalkyl (meth)acrylate. [6] The acrylic resin according to any one of [1] to [5], wherein the acrylic resin is soluble when the acrylic resin is mixed with polypropylene glycol having a number average molecular weight of 1,000 to give a concentration of 10% by mass and stirred at 60°C for 60 minutes. [7] A resin composition comprising the resin according to any one of [1] to [6] and a polyalkylene glycol. [8] The resin composition according to [7], wherein the polyalkylene glycol has a number average molecular weight of 200 to 5,000. [9] The resin composition according to [7] or [8], further comprising a polyester polyol.
[10] The resin composition according to any one of [7] to [9], further comprising an isocyanate.
[11] A hot melt adhesive comprising the resin composition according to any one of [7] to
[10] .
[12] Use of the resin composition according to any one of [7] to
[10] for producing a hot melt adhesive.
[13] A hot melt adhesive, which is a heat-melt product of the resin composition according to any one of [7] to
[10] . Effect of the Invention
[0009] According to the present invention, it is possible to provide an acrylic resin powder, a resin composition, and a hot melt adhesive which are less prone to thickening or discoloration due to heating, have a good appearance, and have a low VOC content compared to conventional products. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The present invention will be described in detail below. In addition, unless otherwise specified, in this specification, a numerical range expressed using "to" means a range that includes the numerical values before and after "to" as the lower limit and upper limit. "(Meth)acrylic" is a general term for acrylic and methacrylic.
[0011] <Acrylic resin> The acrylic resin of the present invention has a pH of 4.0 or more and 8.0 or less when made into a 40% by mass aqueous solution, and does not contain any alkaline compounds. The acrylic resin of the present invention preferably contains a copolymer having a structural unit derived from a (meth)acrylic monomer, since this makes it easier to adjust the glass transition temperature. The acrylic resin of the present invention preferably has a powdery appearance in terms of ease of handling.
[0012] (copolymer) Examples of the (meth)acrylic monomer include (meth)acrylic acid esters, (meth)acrylic acid, (meth)acrylic acid amide, (meth)acrylonitrile, etc., and (meth)acrylic acid esters and (meth)acrylic acid are preferred, (meth)acrylic acid alkyl esters having 5 to 10 carbon atoms and (meth)acrylic acid are more preferred, methyl methacrylate, n-butyl methacrylate, 2-hydroxyethyl methacrylate and methacrylic acid are further preferred, and methyl methacrylate is particularly preferred. By having a structural unit derived from a (meth)acrylic monomer, the initial adhesive strength of the hot melt adhesive is improved.
[0013] The copolymer may have, in addition to the structural units derived from methyl methacrylate, structural units derived from other monomers copolymerizable with methyl methacrylate. Examples of the other monomers include (meth)acrylic acid alkyl esters having a linear or branched alkyl group, (meth)acrylic acid cycloalkyl esters, and other (meth)acrylic acid alkyl esters having a linear, branched, or cyclic alkyl group; (meth)acrylic acid esters having a hydroxyl group (hereinafter also referred to as "hydroxyalkyl (meth)acrylates"), (meth)acrylic acid, (meth)acrylic acid esters having a carboxyl group, (meth)acrylic acid esters having a carbonyl group, (meth)acrylic acid esters having an epoxy group, and (meth)acrylic acid esters having an amino group; other monomers having a carboxyl group, and styrene and derivatives thereof.
[0014] Examples of the (meth)acrylic acid alkyl ester include methyl acrylate, n-butyl (meth)acrylate, i-butyl (meth)acrylate, t-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and octyl (meth)acrylate. Examples of the cycloalkyl (meth)acrylate include cyclohexyl (meth)acrylate and isobornyl (meth)acrylate. Examples of the (meth)acrylic acid ester having a hydroxyl group include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate. The acrylic resin of the present invention preferably contains a structural unit derived from a hydroxyalkyl (meth)acrylate, since this improves the final strength of the hot melt adhesive. Examples of (meth)acrylic acid include acrylic acid and methacrylic acid. Examples of (meth)acrylic acid esters having a carboxyl group include 2-(meth)acryloylhexahydrophthalic acid, 2-(meth)acryloyloxypropylhexahydrophthalic acid, 2-(meth)acryloyloxyethyltetrahydrophthalic acid, 2-(meth)acryloyloxypropyltetrahydrophthalic acid, 5-methyl-2-(meth)acryloyloxyethylhexahydrophthalic acid, 2-(meth)acryloyloxyethylphthalic acid, 2-(meth)acryloyloxypropylphthalic acid, 2-(meth)acryloyloxyethylmaleic acid, 2-(meth)acryloyloxypropylmaleic acid, 2-(meth)acryloyloxyethylsuccinic acid, 2-(meth)acryloyloxypropylsuccinic acid, 2-(meth)acryloyloxyethyloxalic acid, and 2-(meth)acryloyloxypropyloxalic acid. An example of a (meth)acrylic acid ester having a carbonyl group is 2-acetoacetoxyethyl (meth)acrylate. An example of the (meth)acrylic acid ester having an epoxy group is glycidyl (meth)acrylate. Examples of the (meth)acrylic acid ester having an amino group include 2-dimethylaminoethyl (meth)acrylate and 2-diethylaminoethyl (meth)acrylate. Examples of other monomers having a carboxyl group include crotonic acid, fumaric acid, maleic acid, itaconic acid, and sorbic acid. These may be used alone or in combination of two or more.
[0015] In terms of good compatibility with polyalkylene glycol, the copolymer preferably has a structural unit derived from a methacrylic acid C4-C8 alkyl ester, which is an ester of an aliphatic alcohol having 4 to 8 carbon atoms and methacrylic acid, in addition to a structural unit derived from methyl methacrylate. Here, the "C4-C8 alkyl group" refers to the number of carbon atoms in the alkyl group. Examples of the methacrylic acid C4-C8 alkyl ester include n-butyl methacrylate, i-butyl methacrylate, t-butyl methacrylate, 2-ethylhexyl methacrylate, and octyl methacrylate. Among them, it is industrially advantageous to use n-butyl methacrylate, i-butyl methacrylate, and t-butyl methacrylate in the copolymer, since they are inexpensive and easily available.
[0016] The copolymer preferably has a structural unit derived from a monomer having a carboxyl group, in order to promote the reaction between the isocyanate and the polyol in the resin composition and to improve the initial adhesion to the substrate when the hot melt adhesive is applied and the adhesive strength after curing. In addition, it is more preferable to have a structural unit derived from methacrylic acid, since it has good copolymerizability with the structural unit derived from methyl methacrylate and the structural unit derived from a C4-C8 alkyl ester of methacrylic acid.
[0017] The mass proportion of the structural units derived from methyl methacrylate relative to all structural units of the copolymer is preferably from 20 to 80 mass %, more preferably from 25 to 75 mass %, and even more preferably from 30 to 75 mass %. The mass ratio of the structural units derived from monomers other than methyl methacrylate to the total structural units of the copolymer is preferably 20 to 80 mass%, more preferably 25 to 75 mass%, and even more preferably 25 to 70 mass%. By setting the mass ratio of the structural units derived from monomers other than methyl methacrylate within the above range, it is possible to achieve both solubility in polyalkylene glycol and initial adhesive strength of the hot melt adhesive.
[0018] When the copolymer contains structural units derived from C5-10 (meth)acrylic acid alkyl esters other than methyl methacrylate, the mass ratio of the structural units derived from C5-10 (meth)acrylic acid alkyl esters other than methyl methacrylate to the total structural units of the copolymer is preferably 20-80 mass%, more preferably 25-75 mass%, and even more preferably 25-70 mass%. By setting the mass ratio of the structural units within the above range, compatibility with polyalkylene glycol is improved.
[0019] When the copolymer contains a structural unit derived from a C4-C8 alkyl ester of methacrylic acid other than methyl methacrylate, the proportion of the structural unit derived from a C4-C8 alkyl ester of methacrylic acid relative to the total structural units of the copolymer is preferably 20-80% by mass, more preferably 25-75% by mass, and even more preferably 25-70% by mass. By setting the mass ratio of the structural unit within the above range, compatibility with polyalkylene glycol is improved.
[0020] When the copolymer contains a structural unit derived from a (meth)acrylic monomer having a polar group, the mass ratio of the structural unit derived from a (meth)acrylic monomer having a polar group to the total structural units of the copolymer is preferably 20 mass% or less, more preferably 10 mass% or less, even more preferably 0.1 to 10 mass%, particularly preferably 0.5 to 5.0 mass%, and most preferably 1.0 to 3.0 mass%. By setting the mass ratio of the structural unit within the above range, the storage stability of the hot melt adhesive is improved and the initial adhesive strength of the hot melt adhesive can be further increased.
[0021] When the copolymer contains a structural unit derived from a hydroxyalkyl (meth)acrylate, the mass ratio of the structural unit derived from a hydroxyalkyl (meth)acrylate to the total structural units of the copolymer is preferably 20 mass% or less, more preferably 10 mass% or less, even more preferably 0.1 to 1.0 mass%, and particularly preferably 0.2 to 0.5 mass%. By setting the mass ratio of the structural unit within the above range, the storage stability of the hot melt adhesive is improved.
[0022] When the copolymer contains a structural unit derived from (meth)acrylic acid, the mass ratio of the structural unit derived from (meth)acrylic acid to the total structural units of the copolymer is preferably 0.1 to 5.0 mass%, more preferably 0.3 to 3.0 mass%, further preferably 0.5 to 2.5 mass%, and particularly preferably 1.0 to 2.0 mass%. By setting the mass ratio of the structural unit within the above range, the initial adhesive strength of the hot melt adhesive can be further increased.
[0023] (Volume average particle size of primary particles) The volume average particle diameter of the primary particles of the acrylic resin of the present invention is preferably 0.1 to 10 μm, more preferably 0.1 to 5 μm, even more preferably 0.2 to 2 μm, particularly preferably 0.3 to 1 μm, and most preferably 0.5 to 0.9 μm. In this specification, the term "primary particles" refers to the smallest unit of resin particles constituting the acrylic resin. If the volume average particle diameter of the primary particles is equal to or less than the upper limit, the surface area of the particles is large, so that the solubility in a medium such as polyalkylene glycol is good. In addition, if the volume average particle diameter of the primary particles is equal to or more than the lower limit, the thermal fusion of the volume average particle diameter of the secondary particles when made into a powder is suppressed, and the dispersibility in a medium such as polyalkylene glycol is good.
[0024] (Volume average particle size of secondary particles) The volume average particle diameter of the secondary particles of the acrylic resin of the present invention is preferably 20 to 80 μm, more preferably 20 to 60 μm, and even more preferably 30 to 50 μm. In this specification, "secondary particles" refers to aggregated particles in which a large number of primary particles are aggregated. If the volume average particle diameter of the secondary particles is equal to or greater than the lower limit, dusting is suppressed, making the particles easy to handle. In addition, if the volume average particle diameter of the secondary particles is equal to or less than the upper limit, the particles have good solubility in polyalkylene glycol. In the case of such an aggregated structure, it is preferable that the primary particles are not strongly bonded to each other and are loosely aggregated. Specifically, it is preferable that the volume average particle size after irradiating the secondary particles with ultrasonic waves for 5 minutes in an aqueous medium is 0.2 to 20 μm, and within this range, when dissolving in polyalkylene glycol, dispersion precedes dissolution, resulting in a larger surface area and faster dissolution. That is, it is preferable that the volume average particle diameter of the primary particles of the acrylic resin of the present invention is 0.1 to 10 μm, and the volume average particle diameter of the secondary particles is 20 to 80 μm.
[0025] (mass average molecular weight) The mass average molecular weight of the acrylic resin of the present invention, as determined by GPC (gel permeation chromatography), is preferably 100,000 or less, more preferably 10,000 to 100,000, and even more preferably 30,000 to 80,000. If the mass average molecular weight is equal to or greater than the lower limit, the initial adhesive strength of the adhesive tends to be good. If the mass average molecular weight is equal to or less than the upper limit, the viscosity of the resin composition and the hot melt adhesive is suppressed.
[0026] The acrylic resin of the present invention is preferably soluble when the resin is mixed with a polyalkylene glycol having a number average molecular weight of 1000 to a concentration of 10% by mass, and stirred at 60° C. for 60 minutes. An example of the polyalkylene glycol having a number average molecular weight of 1000 is polypropylene glycol having a number average molecular weight of 1000. If the resin is soluble, the coating properties of the resin when made into a resin composition or a hot melt adhesive are good, and it is easy to form a uniform coating film. Here, "stirring" means, for example, using a total of 100 g of polypropylene glycol and acrylic resin, using a glass sample bottle with a full volume of 144 mL, a body diameter of 55 mm, and an overall height of 95 mm as a container, and stirring at 250 rpm using a magnetic stirrer and an octagonal stirrer with a diameter of 8 mm and a length of 40 mm.
[0027] "Soluble when mixed with polypropylene glycol having a number average molecular weight of 1000 to a concentration of 10% by mass and stirred at 60°C for 60 minutes" means that it is determined to be soluble by the following determination method.
[0028] Judgment method: The mixture is acrylic resin / polypropylene glycol (number average molecular weight 1000) = 10 / 90 (mass%), and the resin is dissolved in polypropylene glycol by stirring for 60 minutes on a 60°C water bath, and the degree of dispersion is measured by visual inspection and the measurement method described in JIS K5600-2-5. If the measured degree of dispersion is 20 μm or less, the resin containing the acrylic resin is judged to be soluble in polypropylene glycol.
[0029] (pH of acrylic resin) The pH is measured by mixing ordinary tap water with the resin to a concentration of 40% by mass, stirring for 2 minutes at 2000 rpm using a PRIMIX TK Homo Disper 2.5 model, and then using an AS ONE Lacom Tester pH meter (pHTestr10). As a result of intensive investigation, it has been found that when an aqueous solution of an acrylic resin with a low pH (high acidity) is mixed with polypropylene glycol (e.g., polypropylene glycol with a number average molecular weight of 1000) and heated (e.g., heated at 180°C for 2 hours), the color changes from transparent to yellow. In reactive hot melts, acrylic resins and polyalkylene glycols such as polypropylene glycol are the main materials, and the acidity of the aqueous solution in which these materials are dissolved is one of the factors that cause discoloration of the reactive hot melt. Therefore, it is preferable that the aqueous solution of the acrylic resin is not too acidic. The preferred pH for suppressing discoloration is 4.0 or more, more preferably 4.5 or more, and even more preferably 5.0 or more. On the other hand, the higher the pH (the stronger the basicity), the more the reaction of the isocyanate is promoted, causing the thickening of the reactive hot melt adhesive during heating and application. Therefore, it is preferable that the aqueous solution of the acrylic material is not too basic. The preferred pH for suppressing thickening is 8.0 or less, more preferably 7.5 or less, and even more preferably 7.0 or less. Therefore, the preferred pH range for suppressing both discoloration and thickening is 4.0 to 8.0.
[0030] (acrylic resin that does not contain alkaline compounds) The acrylic resin of the present invention does not contain an alkaline compound. The acrylic resin of the present invention can also be obtained by spray drying an emulsion synthesized by a soap-free emulsion polymerization method. In the soap-free emulsion polymerization method, persulfate is often used as a polymerization initiator, and when persulfate is used, the pH decreases. In order to suppress the decrease in pH, the addition of an alkaline compound is exemplified in Japanese Patent Application No. 2018-214500. However, such a treatment requires the reinforcement of production equipment and the management of alkaline compounds, and also increases the number of production steps, resulting in an increase in production costs. In addition, since inorganic salts are generated by the treatment with alkaline compounds, inorganic salts remain in the acrylic resin obtained by spray-drying the treated acrylic resin, and therefore application to a reactive hot melt adhesive is not preferable because insoluble inorganic matter remains. In addition, when the pH is high, thickening occurs for the above-mentioned reasons, which is similarly undesirable, and it is appropriate not to include alkaline compounds. In other words, the method for producing an acrylic resin of the present invention by a soap-free emulsion polymerization method preferably does not include a step of adding an alkaline compound. Examples of the alkaline compound include inorganic alkaline compounds and organic alkaline compounds. Examples of inorganic alkaline compounds include alkali metal hydroxides such as sodium hydroxide and potassium hydroxide, alkali metal silicates such as sodium orthosilicate, sodium metasilicate and sodium sesquisilicate, alkali metal phosphates such as trisodium phosphate, alkali metal carbonates such as disodium carbonate, sodium hydrogen carbonate and dipotassium carbonate, alkali metal borates such as sodium borate, and alkali earth metal hydroxides such as magnesium hydroxide and calcium hydroxide. Examples of the organic alkaline compound include hydroxyalkylamines and quaternary ammonium salts. Examples of the hydroxyalkylamines include monoethanolamine, diethanolamine, triethanolamine, methylethanolamine, methyldiethanolamine, monopropanolamine, dipropanolamine, tripropanolamine, methylpropanolamine, methyldipropanolamine, and aminoethylethanolamine. Examples of the quaternary ammonium salts include tetramethylammonium hydroxide and choline.
[0031] The content of alkaline compounds in the acrylic resin of the present invention is preferably 500 ppm by mass or less, more preferably 10 ppm by mass or less, and even more preferably 1 ppm by mass or less.
[0032] (Vinyl monomer content in acrylic resin) The acrylic resin of the present invention may contain unreacted monomers used in the production of the copolymer, but it is preferable that the amount is as small as possible from the viewpoint of reducing the content of volatile organic compounds in the hot melt adhesive. The content of volatile organic compounds (content of unreacted vinyl monomers) of acrylic resins obtained by commonly used suspension polymerization generally exceeds 3000 ppm by mass, and it is desirable to reduce the content of unreacted vinyl monomers. From the viewpoint of reducing the content of volatile organic compounds, the content of unreacted vinyl monomers of the acrylic resin of the present invention is preferably 3000 ppm by mass or less, more preferably 1500 ppm by mass or less.
[0033] The acrylic resin of the present invention may contain additives such as an antifoaming agent, if necessary.
[0034] The acrylic resin of the present invention may contain additives such as an emulsifier and a chain transfer agent, and an acid or a salt thereof derived from a polymerization initiator, which are used in the production process described below. From the viewpoint of reducing the content of volatile organic compounds, the content of the chain transfer agent in the acrylic resin of the present invention is preferably 3000 ppm by mass or less, more preferably 1500 ppm by mass or less.
[0035] Examples of the acid or salt thereof derived from the polymerization initiator include benzoic acid, phenol, sulfuric acid, salts of benzoic acid, salts of phenol, sulfates, etc. These may be contained alone or in combination of two or more.
[0036] <Method of manufacturing acrylic resin> The acrylic resin of the present invention can be produced by a soap-free emulsion polymerization method. The above-mentioned production method preferably does not include a step of adding an alkaline compound as a pH adjuster. The emulsifier, chain transfer agent, and polymerization initiator may be the same as those exemplified above in the description of the acrylic resin. The amount of the emulsifier used may be determined in consideration of the balance between the amount of the monomer charged and the amount of the polymerization initiator used.
[0037] An example of a method for producing the acrylic resin of the present invention includes the following steps I to III. Step I: (a) In a medium mainly composed of water, a monomer mixture (a) is polymerized in the presence of an emulsifier at or below the critical micelle concentration and a water-soluble radical polymerization initiator to obtain a polymer dispersion (A) containing a polymer of the monomer mixture (a). Next, (b) a monomer mixture (b) and a chain transfer agent are dropped into the polymer dispersion (A) to polymerize the monomer mixture (b) to obtain a polymer dispersion (B). Step III: An acrylic resin is obtained from the polymer dispersion (B).
[0038] (Process I(a)) In step I(a), the monomer mixture (a) is polymerized in a medium mainly composed of water in the presence of an emulsifier at or below the critical micelle concentration and a water-soluble radical polymerization initiator. This allows the preparation of seed particles having a relatively large particle size. By preparing seed particles having a relatively large particle size, the generation of new particles can be suppressed in the subsequent step I(b), and the particle size of the resulting polymer becomes relatively large. As a result, the acrylic resin obtained in step III has good dispersibility in a medium such as polyalkylene glycol.
[0039] The term "medium containing water as a main component" refers to a medium containing tap water, pure water, ultrapure water, distilled water, or ion-exchanged water as a main component. These may be used alone or in combination of two or more.
[0040] Examples of the emulsifier include anionic surfactants and nonionic surfactants. Examples of anionic surfactants include alkylbenzene sulfonates, alkyl sulfonates, alkyl sulfates, fatty acid metal salts, polyoxyalkyl ether sulfates, polyoxyethylene carboxylate sulfates, polyoxyethylene alkylphenyl ether sulfates, dialkyl succinate sulfonates (e.g., sodium dioctyl sulfosuccinate, etc.), and sodium polyoxyethylene alkyl (12-15) ether phosphate (trade name: Phosphanol RS-610NA, manufactured by Toho Chemical Industry Co., Ltd.). These may be used alone or in combination of two or more.
[0041] Examples of nonionic surfactants include polyoxyethylene alkylphenyl ether, polyoxyethylene alkyl ether, polyoxyethylene fatty acid ester, polyoxyethylene sorbitan fatty acid ester, polyoxyethylene alkyl ether glycerin borate ester, polyoxyethylene alkyl ether phosphate ester, sorbitan fatty acid ester, fatty acid glycerin ester, glycerin fatty acid ester, and pentaerythritol fatty acid ester. In addition, compounds having a polyoxyethylene chain in the molecule and having surface activity (polyoxyethylene, etc.), and compounds having a polyoxyalkylene chain consisting of oxyethylene and oxypropylene instead of the polyoxyethylene chain in the above compounds can also be used. These may be used alone or in combination of two or more.
[0042] The critical micelle concentration can be taken from the New Surfactant Handbook (4th edition, 2000, Kogyo Tosho Co., Ltd.). For example, the critical micelle concentration of sodium n-dodecylbenzenesulfonate is 1.2 mmol / L (75°C), and the critical micelle concentration of disodium dioctyl sulfosuccinate is 0.7 g / L (25°C).
[0043] The monomer mixture (a) is a mixture of monomers that has a solubility of 0.02% by mass or more in a medium mainly composed of water at 20° C. and whose polymer is not dissolved in the medium mainly composed of water. By using such a monomer mixture (a), the seed polymerization is facilitated, and the obtained polymer is less likely to dissolve in the medium, making it easier to obtain seed particles.
[0044] Examples of monomers used in the monomer mixture (a) include alkyl acrylates such as methyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and octyl (meth)acrylate, cycloalkyl (meth)acrylates such as cyclohexyl (meth)acrylate, and hydroxyl group-containing (meth)acrylic esters such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate. These may be used alone or in combination of two or more. From the viewpoint of polymerization stability, it is preferable to use a combination of methyl methacrylate and a C4 to C8 alkyl methacrylate in the monomer mixture (a).
[0045] Examples of the water-soluble radical polymerization initiator include persulfates, water-soluble azo compounds, thermal decomposition polymerization initiators, and redox polymerization initiators. Examples of persulfates include potassium persulfate, ammonium persulfate, and sodium persulfate. Examples of water-soluble azo compounds include 2,2'azobis(2-amidinopropane) trihydrochloride and 4,4'-azobis(4-cyanopentanoic acid). Examples of thermal decomposition polymerization initiators include hydrogen peroxide. Examples of redox polymerization initiators include hydrogen peroxide and ascorbic acid, tert-butyl hydroperoxide and Rongalite, potassium persulfate and metal salts, and ammonium persulfate and sodium hydrogen sulfite. These polymerization initiators may be used alone or in combination of two or more. As the water-soluble radical polymerization initiator, persulfates are preferred since they are suitable for soap-free polymerization which can give relatively large seed particles.
[0046] (Step I (b)) In step I(b), a monomer mixture (b) containing methyl methacrylate and a chain transfer agent are dropped into the polymer dispersion (A) in the presence of a water-soluble radical polymerization initiator to polymerize it, thereby obtaining a polymer dispersion (B) containing particles in which the polymer of the monomer mixture (b) is coated on the polymer of the monomer mixture (a) contained in the polymer dispersion (A). The chain transfer agent may be mixed with the monomer mixture (b) and then dropped, or may be dropped separately from and simultaneously with the monomer mixture (b).
[0047] The monomer mixture (b) contains methyl methacrylate. The monomer mixture (b) may contain, in addition to methyl methacrylate, other monomers exemplified in the description of the acrylic resin.
[0048] By using a chain transfer agent in step I(b), the molecular weight of the acrylic resin can be adjusted. Examples of chain transfer agents include mercaptans such as n-dodecyl mercaptan, primary or secondary mercapto compounds, thioglycolic acid esters such as octyl thioglycolate, α-methylstyrene dimer, and terpinolene. Among these, primary or secondary mercapto compounds are preferred because they improve the physical properties of the hot melt adhesive using the acrylic resin of the present invention.
[0049] Examples of primary or secondary mercapto compounds include alkyl mercaptans, thioglycolic acid esters, and mercaptopropionic acid esters. Examples of alkyl mercaptans include n-butyl mercaptan, sec-butyl mercaptan, n-octyl mercaptan, n-dodecyl mercaptan, and n-octadecyl mercaptan. Examples of thioglycolic acid esters include 2-ethylhexyl thioglycolate, methoxybutyl thioglycolate, and trimethylolpropane tris(thioglycolate). Examples of mercaptopropionic acid esters include 2-ethylhexyl β-mercaptopropionate, 3-methoxybutyl β-mercaptopropionate, and trimethylolpropane tris(β-thiopropionate). Among these, n-octyl mercaptan, n-dodecyl mercaptan, and 2-ethylhexyl thioglycolate, which have large chain transfer constants, are preferred, and n-dodecyl mercaptan and 2-ethylhexyl thioglycolate are more preferred from the viewpoint of odor. These may be used alone or in combination of two or more.
[0050] The amount of the chain transfer agent used is preferably 0.1 to 3 parts by mass, more preferably 0.3 to 2 parts by mass, based on 100 parts by mass of the monomer mixture (b). If the amount of the chain transfer agent used is equal to or more than the lower limit, the molecular weight of the acrylic resin is reduced by chain transfer of radicals, improving adhesion to the substrate. If the amount of the chain transfer agent used is equal to or less than the upper limit, the amount of unreacted monomer and the amount of the chain transfer agent remaining is reduced, reducing odor.
[0051] In step I(ii), a radical polymerization initiator may be further added. Examples of the radical polymerization initiator used include the same water-soluble radical polymerization initiators as exemplified in step I(i). The total amount of the water-soluble radical polymerization initiator used in step I(a) and step I(b) is preferably 0.03 parts by mass or more, more preferably 0.05 to 1.0 parts by mass, relative to 100 parts by mass of the total amount of the monomer mixture (a) and the monomer mixture (b). When the total amount of the water-soluble radical polymerization initiator used is equal to or more than the lower limit, an acrylic resin having good solubility in polyalkylene glycol is obtained, and the viscosity of the resin composition dissolved in polyalkylene glycol is reduced, resulting in good handleability.
[0052] An emulsifier may be used in step I(ii). Examples of the emulsifier used in step I(ii) include the same emulsifiers as those exemplified in the explanation of step I(i). The polymerization temperature in step I(a) and step (b) may be set according to the type of water-soluble radical polymerization initiator and the polymerization conditions. For example, when a water-soluble inorganic peroxide such as potassium persulfate or ammonium persulfate is used alone as the water-soluble radical polymerization initiator, the polymerization can be carried out at a temperature equal to or higher than the 10-hour half-life temperature of the polymerization initiator. From the viewpoint of polymerization stability and time reduction, a temperature 5°C or higher than the 10-hour half-life temperature of the water-soluble radical polymerization initiator is preferable. The polymerization time in step I(a) and step I(b) may be set according to the type of polymerization initiator and the polymerization conditions. Although the suitable polymerization time varies depending on the polymerization temperature, it is preferable to carry out the polymerization within a time period during which the polymerization initiator can thermally decompose and generate radicals.
[0053] (Step I(C)) The method for producing an acrylic resin of the present invention may further include step I(iii) after step I(ii) and before steps II and III described below. In step I(iii), the monomer mixture (c) and the chain transfer agent are dropped into the polymer dispersion (B) in the presence of a water-soluble radical polymerization initiator to polymerize it, thereby obtaining a polymer dispersion (C) containing particles in which the polymer of the monomer mixture (a) is coated with the polymer of the monomer mixture (b), and the particles are further coated with the polymer of the monomer mixture (c). In step I(c), the same raw materials, reagents, and reaction conditions as those in step I(b) can be used. In step I(iii), a water-soluble radical polymerization initiator may or may not be added. When the polymerization initiator added in steps I(i) and I(ii) remains in the polymer dispersion (B) and the polymerization reaction in step I(iii) proceeds sufficiently due to the remaining polymerization initiator, it is preferable not to add a polymerization initiator in step I(iii). By not adding a polymerization initiator, it becomes easier to adjust the pH of the resulting aqueous solution of the acrylic resin to a desired range.
[0054] (Process II) The method for producing an acrylic resin of the present invention may further include step II after step I(b) or step I(c) and before step III described below. In step II, an alkaline compound is added to the polymer dispersion (B) obtained in step I(b) or the polymer dispersion (C) obtained in step I(c) to obtain a polymer dispersion (B') or a polymer dispersion (C'). The alkaline compound to be used is preferably added within the range of the amount required to neutralize the acid derived from the polymerization initiator used so that it does not remain in the obtained acrylic resin. This makes it easier to adjust the pH of the obtained aqueous solution of the acrylic resin to a desired range, and prevents the viscosity of the hot melt adhesive containing the acrylic resin from becoming too high after heating. Step II may or may not be performed, but is preferably not performed from the viewpoint of reducing production costs.
[0055] The pH of the polymer dispersion (B), polymer dispersion (B'), polymer dispersion (C), and polymer dispersion (C') is preferably 2.0 or more, more preferably 2.5 or more, and even more preferably 3.0 or more. The pH of the polymer dispersion (B), polymer dispersion (B'), polymer dispersion (C), and polymer dispersion (C') is preferably 9.0 or less, more preferably 8.5 or less, and even more preferably 8.0 or less. By setting the pH of the polymer dispersion (B), polymer dispersion (B'), polymer dispersion (C), and polymer dispersion (C') within the above range, discoloration when mixed with polyalkylene glycol and heated can be easily suppressed, and the viscosity of the hot melt adhesive containing the acrylic resin after heating can be prevented from becoming too high.
[0056] (Process III) In the step III, the acrylic resin is recovered from the polymer dispersion (B), the polymer dispersion (B'), the polymer dispersion (C), or the polymer dispersion (C'). The method for recovering the acrylic resin from the polymer dispersion (B), polymer dispersion (B'), polymer dispersion (C), or polymer dispersion (C') is not particularly limited, and examples thereof include a spray drying method and a method of drying after acid coagulation or salt coagulation. The spray drying method is preferred because the primary particles are not strongly bonded to each other and can be easily brought into a primary particle state by weak shear force.
[0057] The acrylic resin obtained in step III includes primary particles and secondary particles. The higher-order structure of the secondary particles is not particularly limited, and it is possible for the secondary particles to have secondary structures such as particles in which the primary particles are aggregated with weak cohesive force, particles in which the primary particles are aggregated with strong cohesive force, and particles fused together by heat. Furthermore, it is also possible to give these secondary particles a higher-order structure by subjecting them to a process such as granulation. The higher-order structure can be formed for the purpose of improving workability, for example, by suppressing dusting of the powder or increasing fluidity, or can be formed for the purpose of improving physical properties, for example, by improving the dispersion state of the powder in polyalkylene glycol, and can be designed according to the application and requirements.
[0058] ≪Resin composition≫ The resin composition of the present invention preferably contains the acrylic resin of the present invention and a polyalkylene glycol as a polyol component, since it can be used as a material for a hot melt adhesive.
[0059] (Polyalkylene glycol) Examples of polyalkylene glycols include polyalkylene glycols having structural units derived from two or more glycols, such as polymethylene glycol, polyethylene glycol, polypropylene glycol, polyoxytetramethylene glycol, polyhexamethylene glycol, copolymers of ethylene oxide and propylene oxide, and branched polyalkylene glycols using polyfunctional alcohols, such as glycerin. These may be used alone or in combination of two or more.
[0060] The number average molecular weight of the polyalkylene glycol is preferably 200 to 5000, more preferably 700 to 3000. When the number average molecular weight of the polyalkylene glycol is equal to or higher than the lower limit, the adhesive strength of the hot melt adhesive after curing is good. When the number average molecular weight of the polyalkylene glycol is equal to or lower than the upper limit, the viscosity of the resin composition is low, and the coatability is good. In the resin composition of the present invention, the polyalkylene glycol preferably has a number average molecular weight of 200 to 5,000.
[0061] (Polyester polyol) The resin composition of the present invention preferably further contains a polyester polyol in view of being a material for a hot melt adhesive. As the polyester polyol, crystalline polyester polyol and amorphous polyester polyol are known. Specific examples thereof include aliphatic polyester polyol and aromatic polyester polyol. Crystalline polyester polyols and amorphous polyester polyols can be easily distinguished from each other by differential scanning calorimetry (DSC). More specifically, the melting point of crystalline polyester polyols is observed by DSC as an endothermic peak when the temperature rises, and as an exothermic peak when the temperature falls. When the melting point of amorphous polyester polyols is measured by DSC, no endothermic peak or exothermic peak is clearly observed, so that it can be distinguished from crystalline polyester polyols.
[0062] The aliphatic polyester polyol can be obtained by reacting an aliphatic dicarboxylic acid with a diol. Examples of the aliphatic dicarboxylic acid include adipic acid, sebacic acid, azelaic acid, and decamethylenedicarboxylic acid. The aliphatic dicarboxylic acid may be used alone or in combination of two or more. Examples of diols include low molecular weight diols having 2 to 12 carbon atoms, such as ethylene glycol, 1-methylethylene glycol, 1-ethylethylene glycol, propylene glycol, butanediol, pentanediol, hexanediol, heptanediol, octanediol, nonanediol, decanediol, dodecanediol, neopentyl glycol, 2-methyl-1,3-propanediol, cyclohexanedimethanol, and 2,4-dimethyl-1,5-pentanediol. Among these, at least one of ethylene glycol, butanediol, hexanediol, octanediol, and decanediol is preferred. One diol may be used alone, or two or more diols may be used in combination.
[0063] Examples of the aliphatic polyester polyol include polyhexamethylene adipate, polyhexamethylene sebacate, polyhexamethylene dodecanate, and polybutylene adipate.
[0064] The aromatic polyester polyol is preferably a compound obtained by the reaction of an aromatic polycarboxylic acid or an aromatic dicarboxylic acid with the diol. Examples of the aromatic polycarboxylic acid or the aromatic dicarboxylic acid include phthalic acid, isophthalic acid, and terephthalic acid. These may be used alone or in combination of two or more. Examples of aromatic polyester polyols include polyalkylene phthalate, polyalkylene isophthalate, and polyalkylene terephthalate.
[0065] Polyester polyols have low viscosity and good handling properties, and are suitable for dissolving acrylic resins. In addition, polyester polyols have high heat resistance, high solvent resistance, and high strength, so it is preferable to use polyalkylene glycols and polyester polyols in combination.
[0066] (Isocyanate) The resin composition of the present invention preferably further contains an isocyanate since the adhesive strength is increased by moisture curing. Examples of isocyanates include ethylene diisocyanate, ethylidene diisocyanate, propylene diisocyanate, butylene diisocyanate, hexamethylene diisocyanate, toluene diisocyanate, cyclopentylene-1,3-diisocyanate, cyclohexylene-1,4-diisocyanate, cyclohexylene-1,2-diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,2-diphenylpropane-4,4'-diisocyanate, p-phenylene diisocyanate, m-phenylene diisocyanate, xylylene diisocyanate, 1,4-naphthyl diisocyanate, Examples include diisocyanate, 1,5-naphthylene diisocyanate, diphenyl-4,4'-diisocyanate, azobenzene-4,4'-diisocyanate, diphenylsulfone-4,4'-diisocyanate, dichlorohexamethylene diisocyanate, furfuridene diisocyanate, 1-chlorobenzene-2,4-diisocyanate, 4,4',4"-triisocyanate-triphenylmethane, 1,3,5-triisocyanate-benzene, 2,4,6-triisocyanate-toluene, and 4,4'-dimethyldiphenylmethane-2,2',5,5'-tetraisocyanate.
[0067] From the viewpoint of high adhesive strength after moisture curing, the isocyanate is preferably a compound having an average of 1 to 3 isocyanate groups per molecule, and more preferably a bifunctional isocyanate, i.e., a diisocyanate. One type of isocyanate may be used alone, or two or more types may be used in combination. Among them, 4,4'-diphenylmethane diisocyanate is preferred from the viewpoint of high adhesive strength after moisture curing.
[0068] Although a monol, a monoisocyanate, a trifunctional polyol, and a trifunctional isocyanate can also be used, a combination of a difunctional polyol (diol) and a difunctional isocyanate (diisocyanate) is preferred in terms of the viscosity of the resin composition. It is preferable to use 2 moles of a difunctional isocyanate per mole of a difunctional polyol, since this allows the desired urethane prepolymer to be produced relatively easily.
[0069] The resin composition of the present invention may contain other additives to the extent that they do not adversely affect the reaction between the polyol and the isocyanate that forms the urethane prepolymer. Examples of additives include plasticizers, antioxidants, pigments, light stabilizers, flame retardants, curing catalysts, and waxes. In addition, wetting agents, thickeners, defoamers, rheology adjusters, and the like may also be added as necessary. The content of the additives relative to the total mass of the resin composition of the present invention is preferably 0 to 5% by mass.
[0070] <Hot melt adhesive> In the present invention, the term "hot melt adhesive" refers to an adhesive that is melted by applying heat of 80 to 150°C before use. The hot melt adhesive of the present invention preferably contains the resin composition of the present invention. By containing the resin composition of the present invention, the odor when the hot melt adhesive of the present invention is heated and melted and used as a hot melt adhesive is reduced, and thus coating workability is improved.
[0071] When the hot melt adhesive contains an acrylic resin, a polyester polyol, and an isocyanate, it is preferable that the acrylic resin is 1 to 50 parts by mass, and the total amount of the polyester polyol and the isocyanate is 50 to 99 parts by mass, relative to 100 parts by mass of the total of the acrylic resin, the polyester polyol, and the isocyanate. It is more preferable that the acrylic resin is 5 to 30 parts by mass, and the total amount of the polyester polyol and the isocyanate is 70 to 95 parts by mass. If the acrylic resin is equal to or more than the lower limit, the initial adhesive strength tends to be good. If the acrylic resin is equal to or less than the upper limit, the adhesive strength after curing tends to be improved.
[0072] The hot melt adhesive of the present invention can be used in the same manner as conventional hot melt adhesives, and the method of use is not particularly limited. The heating temperature for melting the hot melt adhesive is preferably 80 to 140° C., more preferably 90 to 110° C. Within the above temperature range, each component is well dissolved, the viscosity of the hot melt adhesive is reduced, and the handleability is improved. Furthermore, the reaction between the isocyanate and the polyalkylene glycol proceeds sufficiently. The heating time is not particularly limited, but is preferably 30 to 300 minutes, and more preferably 60 to 180 minutes.
[0073] The initial viscosity of the hot melt adhesive varies depending on the process, but from the viewpoints of preventing dripping and ease of processing, a viscosity range of 10 to 150 Pa·s is preferable. The viscosity increase rate (%) of the hot melt adhesive is preferably from 0 to 100%, more preferably from 0 to 80%, further preferably from 0 to 50%, and particularly preferably 0 to 30%. The viscosity difference represented by [viscosity of the hot melt adhesive after heating] - [initial viscosity of the hot melt adhesive] is preferably 0 to 35 Pa·s, more preferably 0 to 20 Pa·s, even more preferably 0 to 10 Pa·s, and particularly preferably 0 to 7.0 Pa·s. The initial viscosity, viscosity after heating, and viscosity increase rate of the hot melt adhesive can be measured by the methods described in the examples.
[0074] The initial strength of the hot melt adhesive is preferably from 50 to 400 kPa, more preferably from 80 to 300 kPa, and even more preferably from 100 to 250 kPa. The final strength of the hot melt adhesive is preferably from 0.5 to 20 MPa, more preferably from 0.8 to 20 MPa, and even more preferably from 1.0 to 20 MPa. The initial strength and final strength of the hot melt adhesive can be measured by the method described in the Examples.
[0075] The open time of the hot melt adhesive is preferably from 5 to 100 minutes, more preferably from 10 to 90 minutes, and even more preferably from 20 to 80 minutes. The open time of the hot melt adhesive can be measured by the method described in the Examples.
[0076] The hot melt adhesive of the present invention can be used in fields where hot melt adhesives have been used conventionally, such as the architectural interior field (or architectural field), the electronic material field, the automotive interior field, etc. Specifically, it can be used, for example, for attaching automotive interior components, attaching decorative materials to architectural interior components, for woodworking, paper processing, fiber processing, and as a general-purpose adhesive.
[0077] For example, when attaching an adherend to a substrate, the hot melt adhesive may be applied to one or more surfaces of the substrate side and the adherend side. The adherend and the substrate may be any commonly used material, such as a molding material, a film sheet, or a fibrous material made by weaving synthetic or natural fibers in a spinning machine into a sheet.
[0078] The raw material of the molding material, film and sheet is not particularly limited, and is preferably a thermoplastic resin. Examples of the raw material of the molding material, film and sheet include polyolefin resin, polyester resin, acetate resin, polystyrene resin, ABS resin, vinyl chloride resin and polycarbonate resin. Examples of the polyolefin resin include polyethylene and polypropylene. Examples of the polyester resin include polyethylene terephthalate.
[0079] A laminate obtained by bonding an adherend and a substrate with the hot melt adhesive of the present invention can be used in various applications such as construction, electronic materials, and the automotive field. There is no need to use special equipment to manufacture the laminate, and it can be manufactured using commonly known manufacturing equipment including a conveyor, a coater, a press, a heater, and a cutter. For example, the laminate can be manufactured as follows. While the substrate and the adherend are flowing on a conveyor, the hot melt adhesive of the present invention is applied to the substrate or the adherend with a coater. The temperature during application is controlled to a predetermined temperature by a heater. The adherend is lightly pressed against the substrate with a press, and the adherend and substrate are bonded together via the hot melt adhesive. The bonded adherend and substrate are then allowed to cool, and are then flowed on a conveyor to solidify the hot melt adhesive. The substrate to which the adherend is attached is then cut to an appropriate size with a cutter.
[0080] The laminate has a high initial adhesive strength of the hot melt adhesive of the present invention and has excellent heat resistance after moisture curing, so that the substrate and the adherend are unlikely to peel off even in summer. It is also possible to produce a laminate by applying the adhesive without using a coater. EXAMPLES
[0081] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to the following descriptions.
[0082] The various measurement and evaluation methods are shown below.
[0083] (mass average molecular weight) The polystyrene equivalent value measured under the following conditions by GPC (gel permeation chromatography) was used as the mass average molecular weight of the resin. <Measurement conditions> High-speed GPC equipment (Tosoh Corporation, product name: HLC-8220GPC) Four columns (manufactured by Tosoh Corporation, product name: TSKgel SuperHZM-M) were connected in series. Oven temperature: 40℃ Eluent: Tetrahydrofuran Sample concentration: 0.1% by mass Eluent flow rate: 0.35mL / min Sample injection volume: 1μL Detector: RI (differential refractometer)
[0084] (Volume average particle size) The particle size of the obtained powdered acrylic resin was measured using a laser diffraction / scattering type particle size distribution analyzer (Horiba, product name: LA-960) after irradiating it with ultrasonic waves for 5 minutes using ion-exchanged water as the dispersion medium. The median size (volume average particle size) was used as the particle size. The relative refractive index of the resin particles and the dispersion medium was 1.12 for all cases.
[0085] (pH) The pH was measured by mixing ordinary tap water with the resin at a concentration of 40% by mass, stirring the mixture at 2000 rpm for 2 minutes using a PRIMIX TK Homo Disper 2.5 model, and then using an AS ONE Lacom Tester pH meter (pHTestr10).
[0086] (PPG solubility) A powdered acrylic resin / polypropylene glycol (hereinafter also referred to as "PPG", number average molecular weight 1000, product name: Adeka Polyether P-1000, manufactured by ADEKA) was mixed at a ratio of 10 / 90 (mass%) and stirred at 60°C for 60 minutes to dissolve the resin in polypropylene glycol. Stirring was carried out at 250 rpm using a glass sample bottle with a full volume of 144 mL, a body diameter of 55 mm, and a total height of 95 mm as a container, and using a magnetic stirrer and an octagonal stirrer with a diameter of 8 mm and a length of 40 mm. Thereafter, the appearance was observed, and the presence or absence of insoluble components with a diameter of 1 mm or more was visually judged, and evaluated according to the following criteria. <Evaluation Criteria 1> ○: No insoluble matter with a diameter of 1 mm or more. ×: Insoluble matter with a diameter of 1 mm or more is present. <Evaluation Criteria 2> The degree of dispersion was measured by the method described in JIS K5600-2-5. When the measured degree of dispersion was 20 μm or less, the acrylic resin was determined to be soluble in polypropylene glycol.
[0087] (Vinyl monomer content in acrylic resin) The content of vinyl monomer remaining in the powdered acrylic resin obtained was measured using a gas chromatograph HP-7890A (column: HP-5, manufactured by Agilent Corporation) manufactured by Agilent.
[0088] (Appearance after heating PPG solution) A powdered acrylic resin / polypropylene glycol (mass average molecular weight 1000, product name: Adeka Polyether P-1000, manufactured by ADEKA) was mixed at 20 / 80 (mass%) and stirred at 80°C for 60 minutes to dissolve the resin in polypropylene glycol. Stirring was performed at 250 rpm using a glass sample bottle with a full volume of 144 mL, a body diameter of 55 mm, and a total height of 95 mm as a container, and a magnetic stirrer and an octagonal stirrer with a diameter of 8 mm and a length of 40 mm. The resulting solution was transferred to a test tube and heated in a drying furnace at 180°C for 2 hours, and the appearance of the solution after heating was visually observed. In order to quantify the color change before and after heating the PPG solution containing the acrylic resin, it was evaluated by UV-Vis spectrum measurement under the following conditions. <Measurement conditions> Equipment: U-1900 spectrophotometer (Hitachi High-Tech Corporation) Cell: Quartz cell Cell length: 10mm Scan speed: 200nm / min Measurement range: 350~800nm ·Measurement temperature: 23℃ Sample: Resin was dissolved in polypropylene glycol and heated at 180°C for 2 hours. The solution (hereafter referred to as the "heated sample") was mixed with ethyl acetate in a ratio of 1 mL:2 mL to prepare the sample. Reference sample: Polypropylene glycol (mass average molecular weight 1000, product name: Adeka Polyether P-1000, manufactured by ADEKA) was heated in a drying oven at 180°C for 2 hours (hereinafter referred to as the "heated PPG sample"). This was mixed with the heated PPG sample and ethyl acetate in a ratio of 1 mL:2 mL as described above to prepare the reference sample. - Method of calculating absorbance difference: When yellow discoloration is confirmed, absorption is observed in the shorter wavelength side of the visible light range of its complementary color. Therefore, the absorbance at 400 nm is used as the standard, and the absorbance is calculated as follows to compare the appearance. Absorbance at 400 nm = [absorbance of sample at 400 nm] - [absorbance of reference sample at 400 nm] <Evaluation criteria> ◯: Transparent and has excellent appearance (absorbance below 0.060). △: Light yellow in appearance and usable level (absorbance greater than 0.06 and less than 0.0.10). ×: Yellow and poor appearance (absorbance of 0.10 or more).
[0089] (Initial adhesive strength) Two flat bars (wooden, 1.7 cm wide, 7.5 cm long, 1.5 mm thick) were prepared, and hot melt adhesive that had been heated and melted at 120°C was applied to one of the bars to a thickness of 0.36 mm over an area of 1.5 cm x 1.7 cm, and the other flat bar was placed on top of it, clamped with a double clip, and left to stand for 5 minutes to allow the hot melt adhesive to cool and solidify. After leaving it to stand, the double clip was removed, and a precision universal testing machine (product name: AGS-X, manufactured by Shimadzu Corporation) was used as the tensile tester to perform a tensile shear test under the following measurement conditions, and the initial adhesive strength was measured. <Measurement conditions> Tensile speed: 5.0 mm / min Chuck distance: 50mm Measurement temperature: 23℃
[0090] (final strength) Two adherends (ABS plates, width 2.5 cm, length 10 cm, thickness 2.0 mm) were prepared, and hot melt adhesive that had been heated and melted at 120°C was applied to one of the flat bars to a thickness of 0.36 mm over an area of 1.5 cm x 2.5 cm, and the other flat bar was placed on top of it, clamped with a double clip, and left to stand for three days to allow the hot melt adhesive to solidify. After leaving it to stand, the double clip was removed, and a tensile shear test was performed under the following measurement conditions using a precision universal testing machine (product name: AG-Xplus, manufactured by Shimadzu Corporation) as the tensile tester, and the final strength was measured. <Measurement conditions> Tensile speed: 5.0 mm / min Chuck distance: 50mm Measurement temperature: 23℃
[0091] (Hot melt initial viscosity) The initial viscosity of the prepared hot melt adhesive was measured under the following conditions using a HAAKE MARS60 (manufactured by Thermo Scientific), and the data after 2 minutes from the start of the measurement was recorded. Rotor Shape: Cone Rotor diameter: 50mm Rotor angle: 2° ·Measurement temperature 100℃ Shear rate: 1 (1 / s)
[0092] (Hot melt viscosity after heating) The post-heating viscosity of the prepared hot melt adhesive was measured in the same manner as the initial hot melt viscosity after placing 20 to 30 g of the hot melt adhesive in a glass bottle with a capacity of 144 mL, a body diameter of 55 mm, and an overall height of 95 mm, and heating at 100°C for 4 hours.
[0093] (Thickening rate) The viscosity increase rate was calculated as follows. Viscosity increase rate (%) = (viscosity of hot melt after heating - initial viscosity of hot melt) ÷ initial viscosity of hot melt x 100
[0094] (Method of measuring open time) The hot melt adhesive was applied to a dried flat bar (wooden, 1.7 cm wide, 7.5 cm long, 1.5 mm thick) and heated to 120°C in a Geer oven. After that, pieces of kraft paper were attached to the bar by applying pressure with a finger at one-minute intervals at room temperature, and the kraft paper pieces were quickly peeled off. The open time was the time from when the hot melt adhesive was applied to the flat bar to when the kraft paper pieces were peeled off and no paper fibers remained on the adhesive surface.
[0095] (Example 1) Acrylic resin (P-1) [Process I (A)] 583 g of ion-exchanged water was placed in a 2-liter four-neck flask equipped with a thermometer, a nitrogen gas inlet tube, a stirring rod, a dropping funnel, and a cooling tube, and nitrogen gas was passed through the flask for 30 minutes to replace the dissolved oxygen in the ion-exchanged water. Next, the nitrogen gas was stopped, and the flask was heated to 80°C while stirring at 200 rpm. When the internal temperature reached 80°C, a monomer mixture (a) consisting of 26 g of methyl methacrylate and 20 g of n-butyl methacrylate was added all at once, and then 0.80 g of potassium persulfate and 20 g of ion-exchanged water were added, and the mixture was held for 45 minutes to obtain a resin dispersion (A-1).
[0096] [Step I (b)] A mixture of 1.38 g of Neopelex G-15 (sodium dodecylbenzenesulfonate, active ingredient (emulsifier) 15%, manufactured by Kao Corporation) and 3.51 g of ion-exchanged water was added to the resin dispersion (A-1) obtained in step I (a), and 15 minutes later, a monomer mixture (b) consisting of 526 g of methyl methacrylate, 215 g of n-butyl methacrylate, 9.6 g of methacrylic acid, 3.2 g of hydroxyethyl methacrylate, 5.92 g of Phosphanol RS-610NA, 14.4 g of n-dodecyl mercaptan, and 400 g of ion-exchanged water was added dropwise over 5 hours. After completion of the dropwise addition, the mixture was kept at 80 ° C for 1 hour to complete polymerization, and a resin dispersion (B-1) was obtained. The polymerization was carried out in an environment where 25 mL of nitrogen gas was passed per minute.
[0097] [Process III] The resin dispersion (B-1) was spray-dried using a spray dryer (manufactured by Okawara Chemical Engineering Co., Ltd., product name: L-8i type) under conditions of an inlet temperature of 150°C, an outlet temperature of 60°C, and a disk rotation speed of 20,000 rpm, to produce a powdered acrylic resin (P-1).
[0098] (Examples 2 to 3) Acrylic resins (P-2 to P-3) Powdered acrylic resins (P-2 to P-3) were produced in the same manner as in Example 1, except that the amount of the polymerization initiator (KPS) in step I(a) was changed to the amount shown in Table 1.
[0099] (Example 4) Acrylic resin (P-4) [Process I (A)] In the same manner as in Example 2, a resin dispersion (A-2) was obtained.
[0100] [Step I (b)] A mixture of 1.38 g of Neopelex G-15 (sodium dodecylbenzenesulfonate, active ingredient (emulsifier) 15%, manufactured by Kao Corporation) and 3.51 g of ion-exchanged water was added to the resin dispersion (A-2) obtained in step I (a), and 15 minutes later, a monomer mixture (b) consisting of 104 g of methyl methacrylate, 243 g of n-butyl methacrylate, 5.76 g of methacrylic acid, 1.04 g of hydroxyethyl methacrylate, 2.96 g of Phosphanol RS-610NA, 4.0 g of n-dodecyl mercaptan, and 200 g of ion-exchanged water was added dropwise over 2.5 hours. After completion of the dropwise addition, the mixture was kept at 80 ° C for 1 hour to complete polymerization, and a resin dispersion (B-2) was obtained. The polymerization was carried out in an environment where 25 mL of nitrogen gas was passed per minute.
[0101] [Step I (Ha)] A monomer mixture (c) consisting of 272 g of methyl methacrylate, 120 g of n-butyl methacrylate, 7.0 g of methacrylic acid, 1.20 g of hydroxyethyl methacrylate, 2.96 g of Phosphanol RS-610NA, 4.0 g of n-dodecyl mercaptan, and 200 g of ion-exchanged water was added dropwise to the resin dispersion (B-2) obtained in [Step I(b)] over a period of 2.5 hours. The temperature was maintained at 80° C. for 1 hour to complete the polymerization, thereby obtaining a multi-stage resin dispersion (C-1). The polymerization was carried out in an environment where nitrogen gas was passed through at 25 mL per minute.
[0102] [Process III] The resin dispersion (C-1) was spray-dried under the same conditions as in Example 1 to produce a powdered acrylic resin (P-4).
[0103] (Examples 5 to 6) Acrylic resins (P-5 to P-6) Powdered acrylic resins (P-5 to P-6) were produced in the same manner as in Example 4, except that the amount of the polymerization initiator (KPS) in step I (a) was changed to the amount shown in Tables 1 and 2.
[0104] (Example 7) Acrylic resin (P-7) A powdered acrylic resin (P-7) was produced in the same manner as in Example 6, except that in step I(b) of Example 6, a mixed solution of an emulsifier (Neopelex G-15 (sodium dodecylbenzenesulfonate) and ion-exchanged water was added, and then a mixed solution of 0.4 g of potassium persulfate and 10 g of ion-exchanged water was added.
[0105] (Comparative Example 1) Acrylic resin (P-8) [Process I (A)] In the same manner as in Example 1, a resin dispersion (A-1) was obtained. [Step I (b)] A mixture of 1.38g of Neopelex G-15 (sodium dodecylbenzenesulfonate, active ingredient (emulsifier) 15%, manufactured by Kao Corporation) and 3.51g of ion-exchanged water was added to the resin dispersion (A-1) obtained in step I (a), followed by a mixture of 0.4g of potassium persulfate and 10g of ion-exchanged water, and 15 minutes later, a monomer mixture (b) consisting of 526g of methyl methacrylate, 215g of n-butyl methacrylate, 9.6g of methacrylic acid, 3.2g of hydroxyethyl methacrylate, 5.92g of Phosphanol RS-610NA, 14.4g of n-dodecyl mercaptan, and 400g of ion-exchanged water was added dropwise over 5 hours. After completion of the dropwise addition, the mixture was kept at 80°C for 1 hour to complete polymerization, and a resin dispersion (B-3) was obtained. The polymerization was carried out in an environment where 25mL of nitrogen gas was passed per minute. [Process II] The resin dispersion (B-3) obtained in step I(ii) was cooled to room temperature, and then 16.8 g of an aqueous KOH solution adjusted to a concentration of 5% by mass was added to obtain a resin dispersion (B'-3). [Process III] The resin dispersion (B'-3) was spray-dried under the same conditions as in Example 1 to produce a powdered acrylic resin (P-8).
[0106] (Comparative Example 2) Acrylic resin (P-9) [Process I (A)] In the same manner as in Example 1, a resin dispersion (A-1) was obtained. [Step I (b)] A mixture of 1.6g of potassium persulfate and 64g of ion-exchanged water was added to the resin dispersion (A-1) obtained in step I (a), and 15 minutes later, a monomer mixture (b) consisting of 529g of methyl methacrylate, 220g of n-butyl methacrylate, 4.8g of methacrylic acid, 6.88g of PELLEX OT-P (sodium dialkyl sulfosuccinate, active ingredient 70%, Kao Corporation), 8.0g of n-octyl mercaptan, and 400g of ion-exchanged water was added dropwise over 5 hours. After completion of the dropwise addition, the mixture was kept at 80°C for 1 hour to complete polymerization, and a resin dispersion (B-4) was obtained. The polymerization was carried out in an environment where 25mL of nitrogen gas was passed per minute. Thereafter, a powdered acrylic resin (P-9) was produced in the same manner as in Example 1, except that the amounts of the raw materials in step I(b) were changed to the amounts shown in Table 2.
[0107] Table 3 shows the evaluation results of each of the acrylic resins (P-1 to P-9).
[0108] [Table 1]
[0109] [Table 2]
[0110] [Table 3]
[0111] The abbreviations in Tables 1 and 2 represent the following compounds. "MMA": Methyl methacrylate (manufactured by Mitsubishi Chemical Corporation) "n-BMA": n-butyl methacrylate (manufactured by Mitsubishi Chemical Corporation) "MAA": Methacrylic acid (manufactured by Mitsubishi Chemical Corporation) 2-HEMA: 2-hydroxyethyl methacrylate (Mitsubishi Chemical Corporation) "n-DM": n-dodecyl mercaptan (manufactured by NOF Corporation) "n-OM": n-octyl mercaptan (manufactured by Wako Pure Chemical Industries, Ltd.) "KPS": Potassium persulfate (manufactured by Mitsubishi Gas Chemical Co., Ltd.) "OT-P": Pelex OT-P, disodium dioctyl sulfosuccinate, 70% active ingredient (Kao Corporation) "G-15": Neopelex G-15, sodium dodecylbenzenesulfonate, active ingredient (emulsifier) 15% (Kao Corporation) "RS-610NA": Phosphanol RS-610NA, sodium polyoxyethylene alkyl (12-15) ether phosphate
[0112] As shown in Table 3, the acrylic resins of Examples 1 to 7 obtained by the manufacturing method of the present invention suppressed the generation of low molecular weight components that could be a cause of odor, the PPG solution containing the acrylic resin showed little discoloration after heating, and had excellent solubility. In addition, when used as hot melt adhesives in Examples 8 to 14, there was no increase in viscosity, and it was found that these are acrylic resins suitable for reactive hot melt adhesives. On the other hand, the pH of a 40% by mass aqueous solution was outside the range specified in the present application, and Comparative Example 1, in which an acrylic resin containing an alkaline compound was used, showed a high viscosity increase rate when made into a hot melt adhesive in Comparative Example 3, and it was found that this acrylic resin is not suitable as an acrylic resin for reactive hot melt adhesives. In addition, it was found that the acrylic resin of Comparative Example 2, which does not contain an alkaline compound in the resin dispersion, is not suitable as an acrylic resin for reactive hot melt adhesives because the PPG solution significantly discolors after heating.
[0113] (Example 8) Hot melt adhesive (RHM-1) [Dissolution process] A 300 mL four-neck flask equipped with a thermometer, a stirring rod, and a cooling tube was charged with 41.1 g of polypropylene glycol having a mass average molecular weight of approximately 2000 (product name Adeka Polyether P-2000, manufactured by ADEKA) as a polyol, 3.0 g of polypropylene glycol having a mass average molecular weight of approximately 400 (product name Adeka Polyether P-400, manufactured by ADEKA), 0.3 g of "Modaflow 2100" (manufactured by Allnex) as a defoaming agent, and 23.7 g of powdered acrylic resin (P-1). The internal temperature was heated to 100°C and stirred for 1 hour to obtain a uniform solution-like resin composition.
[0114] [Decompression dehydration process] The resin composition was heated and stirred at 15 kPa and 100° C. for 1 hour, and then dehydrated under reduced pressure. 24.5 g of polyester polyol "HS 2H-351A" (Toyokuni Oil, polyester polyol of hexanediol and adipic acid, molecular weight 3500, melting point 55°C, hydroxyl value = 32 mgKOH / g) as polyol, 14.0 g of 4,4'-diphenylmethane diisocyanate as isocyanate, and 0.1 g of 2,2'-dimorpholinodiethyl ether (Mitsui Chemicals Fine) as curing catalyst were added and stirred at 15 kPa and 100°C for 3 hours. After cooling, the obtained hot melt adhesive was collected and stored in a sealed state.
[0115] (Examples 9 to 14, Comparative Examples 3 and 4) Hot melt adhesives (RHM-2 to 9) Except for changing the type of acrylic resin as shown in Table 4, the same procedures as in Example 8 were followed to produce hot melt adhesives.
[0116] [Table 4]
[0117] The abbreviations in Table 4 represent the following compounds. "P-2000": Adeka Polyether P-2000, a polypropylene glycol with a mass average molecular weight of approximately 2000 (manufactured by ADEKA) "P-400": Adeka Polyether P-400, a polypropylene glycol with a mass average molecular weight of approximately 400 (manufactured by ADEKA) Modaflow2100: Modaflow 2100, defoamer (manufactured by Allnex) ·HS 2H-351A: Polyester polyol (Toyokuni Oil Co., Ltd.) DMDEE: 2,2'-dimorpholinodiethyl ether (Mitsui Chemicals Fine Chemicals) ·MDI: 4,4'-diphenylmethane diisocyanate (manufactured by Tosoh)
[0118] As shown in Table 4, the hot melt adhesives of Examples 8 to 14, which used the acrylic resin obtained by the production method of the present invention, had a low viscosity increase rate and high work stability when applying the adhesive. On the other hand, Comparative Example 3, which used the acrylic resin P-8 containing the alkaline compound obtained in Comparative Example 1, had a high viscosity increase rate and poor workability when applying the adhesive, and was therefore found to be unsuitable as an acrylic resin for reactive hot melt adhesives. Comparative Example 4, which used the acrylic resin P-9 obtained in Comparative Example 2, which has a low pH when made into an aqueous solution, was found to be unsuitable as an acrylic resin for reactive hot melt adhesives, as it was colored and had a poor appearance. [Industrial Applicability]
[0119] According to the present invention, it is possible to provide an acrylic resin suitable for hot melt adhesives, which has a lower VOC content, is transparent and has a good appearance, and exhibits little viscosity increase, as compared with conventional products. Therefore, the acrylic resin of the present invention can be suitably used in fields where hot melt adhesives have been used conventionally, such as the field of architectural interiors, the field of electronic materials, and the field of automotive interiors, and is extremely important industrially.
Claims
1. The pH of a 40% by mass aqueous solution is 4.0 or more and 8.0 or less, Acrylic resin that does not contain alkaline compounds.
2. The acrylic resin according to claim 1 , comprising a copolymer having a structural unit derived from a (meth)acrylic monomer.
3. 3. The acrylic resin according to claim 1, wherein the primary particles have a volume average particle size of 0.1 to 10 μm, and the secondary particles have a volume average particle size of 20 to 80 μm.
4. 3. The acrylic resin according to claim 1, having a mass average molecular weight of 100,000 or less.
5. The acrylic resin according to claim 1 or 2, which has a structural unit derived from a hydroxyalkyl (meth)acrylate.
6. 3. The acrylic resin according to claim 1, wherein the acrylic resin is soluble when the acrylic resin is mixed with polypropylene glycol having a number average molecular weight of 1,000 to a concentration of 10% by mass and stirred at 60°C for 60 minutes.
7. A resin composition comprising the resin according to claim 1 or 2 and a polyalkylene glycol.
8. The resin composition according to claim 7, wherein the polyalkylene glycol has a number average molecular weight of 200 to 5,000.
9. The resin composition according to claim 7, further comprising a polyester polyol.
10. The resin composition according to claim 9, further comprising an isocyanate.
11. A hot melt adhesive comprising the resin composition according to claim 9.
12. Use of the resin composition according to claim 9 for producing a hot melt adhesive.
13. A hot melt adhesive which is a heated and melted product of the resin composition according to claim 9.
Citation Information
Patent Citations
Emulsion composition
JP1995018156A
Water dispersion type resin composition containing amphiphilic polymer as dispersion
JP1997299782A
Aqueous emulsion composition
JP1999256046A
Acrylic emulsion and method for producing the same
JP2010065091A
Method for forming multi-layer coating films
JP2013535311A