Method for manufacturing seal tape from mixture of talc and polytetrafluoroethylene
By controlling temperatures and using dry ice to maintain low mixing conditions, the method addresses the challenges of PTFE fibrillation and volume change, producing a stable, colored sealing tape suitable for threaded joints.
Patent Information
- Application Number
- JP2023077228
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-09
- Publication Date
- 2024-11-21
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods for manufacturing PTFE tapes for threaded joint seals fail to specify how to mix PTFE and talc at low temperatures to prevent fibrillation, and the use of dry ice during stirring can lead to excessive temperature rises.
A method involving the controlled use of dry ice to maintain temperatures below the room temperature transition point of PTFE (around 19°C) during mixing, combined with specific stirring techniques to pulverize PTFE emulsion polymer particles and talc, followed by granulation, extrusion, and rolling to produce a sealing tape.
The method effectively prevents PTFE fibrillation and volume changes, allowing for the production of a stable sealing tape that can be colored for identification and used without damaging threaded joints.
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a talc and polytetrafluoroethylene mixed sealing tape, and more particularly to a method for producing an unsintered polytetrafluoroethylene sealing tape for sealing threaded joints, which contains a specific inorganic powder, i.e., talc powder. Hereinafter, "polytetrafluoroethylene" is simply referred to as "PTFE". [Background technology]
[0002] The following Patent Document 1 describes that in the manufacture of unsintered PTFE tape for sealing screw joints, an aqueous dispersion of PTFE fine powder is mixed with talc to co-coagulate, and the coagulated PTFE fine powder and talc are mixed at a low temperature so as not to cause fibrillation of PTFE.
[0003] Patent Document 2 describes that when mixing thermoplastic resin powder and fluororesin powder, the temperature inside the mixer is controlled to be below the softening point (glass transition point) of the fluororesin, and that the method of temperature control is to add dry ice to keep the temperature below the softening point of the fluororesin.
[0004] Patent Document 3 describes a method in which, in order to disintegrate the PTFE fine powder, the PTFE fine powder and dry ice are charged into a cutter mixer, and then simply stirred and mixed at low speed and at high speed. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication WO96 / 30458 [Patent Document 2] Japanese Patent Application Publication No. 10-237254 [Patent Document 2] JP2015-151543A Summary of the Invention [Problem to be solved by the invention]
[0006] Patent Document 1 describes mixing at a low temperature so as to prevent PTFE from fibrillating, but does not specifically disclose how to mix at a low temperature.
[0007] Patent Document 2 describes controlling the temperature inside the mixer to below the softening point (glass transition point) of the fluororesin. However, since the glass transition point of PTFE is 115°C, simply lowering the temperature to below 115°C may cause a change in volume. In addition, the document simply describes fluororesin powder, and makes no mention of the use of PTFE emulsion polymerization particles, which are highly susceptible to fibrillation.
[0008] The crushing method in Patent Document 3 had a problem that the temperature would rise too much unless dry ice was added during stirring and mixing.
[0009] The present invention provides a method for producing a talc and PTFE mixed sealing tape, in which the temperature is controlled to below about 19°C, the room temperature transition point at which PTFE does not undergo volume change, during the production process by paste extrusion molding using talc powder and PTFE emulsion polymerized particle powder, which is highly susceptible to fibrillation, and which specifically clarifies a means for mixing the talc powder and the PTFE emulsion polymerized particle powder. [Means for solving the problem]
[0010] The method for producing a talc and PTFE mixed sealing tape according to claim 1 of the present invention is characterized by being produced by the following steps. First step: A talc powder having a particle size of 2 to 5 μm, a PTFE emulsion polymerized particle powder having an average particle size of 500 μm in which PTFE particles having a particle size of 0.2 to 0.3 μm are aggregated, and dry ice are prepared. Second step: 100 parts by weight of the mixed powder of 40 to 60 parts by weight of the talc powder and PTFE emulsion polymerization particle powder, and 30 to 50 parts by weight of crushed dry ice are placed in the container of a cutter mixer equipped with a container and a rotating blade, and low-speed stirring and mixing is performed by small movements of the rotating blade of the cutter mixer 4 to 6 times at intervals of 2 to 4 seconds at an average rotation speed of 1500 rpm, followed by high-speed stirring and mixing by repeated operations 4 to 6 times at intervals of 15 to 25 seconds at an average rotation speed of 3000 rpm, to pulverize the PTFE emulsion polymerization particle powder, and a mixed pulverized powder of PTFE emulsion polymerization particle pulverized powder and talc powder having a particle size of 30 μm or less is produced in an environment of 10°C or less. Third step: The mixed and crushed powder is transferred to a granulation vessel, and a granulation liquid is poured into it. The granulation mixture is produced under an environment of 10°C or less while stirring. Thereafter, the granulation mixture is heated to 110-130°C to evaporate and dry the granulation liquid, producing a granulated mixed powder. Fourth step: 15 to 25 parts by weight of a petroleum-based solvent is added as an auxiliary to the granulated mixed powder, the mixture is heated to 25 to 60°C, and compressed at 10 to 20 kg / cm 2 A pressure of 1000 psi is applied to create a preform. Fifth step: Using an extrusion die consisting of a cylindrical cylinder portion and a flat die portion having a flared outlet portion, the preform is inserted into the cylinder portion and extruded from the flat die portion to produce an extruded sheet having a thickness of 2 to 3 mm. Sixth step: The extruded sheet is rolled with a rolling roll to produce a rolled film having a thickness of 50 to 200 μm. Seventh step: The auxiliary contained in the rolled film is removed by heating at 250° C. or less, and a thin film is produced by stretching the film in the extrusion direction from 1.5 times to 3 to 4 times using a heated roll. Eighth step: The thin film is cut in the extrusion direction to a width of 5 to 20 mm to prepare a ribbon-shaped sealing tape.
[0011] In addition, the manufacturing method of a talc and PTFE mixed sealing tape according to claim 2 of the present invention is characterized in that in the second step in claim 1, a total of 100 parts by weight of talc powder and PTFE emulsion polymerized particle powder, 30 to 50 parts by weight of crushed dry ice, and 0.5 to 2 parts by weight of a colorant are put into the container of a cutter mixer.
[0012] Furthermore, the manufacturing method of a talc and PTFE mixed sealing tape according to claim 3 of the present invention is characterized in that the second step in claim 1 comprises: putting 40 to 60 parts by weight of PTFE emulsion polymerization particle powder and 30 to 50 parts by weight of crushed dry ice into a container of a cutter mixer, stirring and mixing at low speed by small movements of the rotary blade of the cutter mixer 4 to 6 times at intervals of 2 to 4 seconds at an average rotation speed of 1500 rpm, and then stirring and mixing at high speed by repeated operations 4 to 6 times at intervals of 15 to 25 seconds at an average rotation speed of 3000 rpm to pulverize the PTFE emulsion polymerization particle powder, and then putting talc powder in an amount such that the sum of the talc powder and the PTFE emulsion polymerization particle powder put in is 100 parts by weight, and stirring and mixing at low speed to produce a mixed pulverized powder of PTFE emulsion polymerization particle pulverized powder having a particle size of 30 μm or less and talc powder in an environment of 10° C. or less. Effect of the Invention
[0013] The method for producing a talc and PTFE mixed sealing tape according to claim 1 of the present invention has the advantage that, by adding an appropriate amount of dry ice, the talc powder and the PTFE emulsion polymerization particle powder, which is very susceptible to fibrillation, can be stirred and mixed at or below the room temperature transition point of about 19°C, at which no volume change occurs in PTFE, and further, by using a specific stirring and mixing method that involves low-speed stirring and mixing and high-speed stirring and mixing, the PTFE emulsion polymerization particle powder can be pulverized to a particle size of 30 μm or less, and a step of adding dry ice during the stirring and mixing process is not required.
[0014] In addition, the manufacturing method of the talc and PTFE mixed sealing tape according to claim 2 has the advantage that the finished sealing tape is colored, which serves as an indication that the sealing tape contains talc powder.
[0015] Furthermore, in the manufacturing method of the talc and PTFE mixed sealing tape according to claim 3, the talc powder is mixed at a low speed by stirring and mixing, so that the talc powder is mixed with the pulverized powder of PTFE emulsion polymerization particles without being damaged, and therefore, when the finished sealing tape is used as a threaded joint seal, no wear or damage occurs in the threaded portion. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The best mode for carrying out the invention will now be described. EXAMPLES
[0017] The talc and PTFE mixed sealing tape according to this embodiment was manufactured by the following manufacturing method.
[0018] [Material preparation (step 1)] First, talc powder, PTFE emulsion polymerized particle powder, and dry ice are prepared.
[0019] The talc powder prepared had a D50 particle size of 2.8 μm as measured by a laser diffraction method (product name: Micro Ace P-8, manufactured by Nippon Talc Co., Ltd.) and a Mohs hardness of 1. The particle size of the talc powder may be in the range of 2 to 5 μm.
[0020] The PTFE emulsion polymerization particle powder is an agglomeration of nearly spherical PTFE particles having a particle size of 0.2 to 0.3 μm as measured by an electron microscope, and 750 g of PTFE fine powder (product name F-104, manufactured by Daikin Industries, Ltd.) formed of secondary particles having an average particle size of 500 μm according to the sieving test method JIS Z 8815 was prepared.
[0021] The content of the talc powder in the sealing tape is set to 40 parts by weight or more for economical effect and sustainability of global resources, and 60 parts by weight or less that enables stable tape formation, relative to 100 parts by weight of the total amount of the talc powder and the PTFE emulsion polymerized particle powder. In this embodiment, it is 50 parts by weight.
[0022] Then, 600 g of crushed dry ice was prepared. The appropriate amount of dry ice is 30 to 50 parts by weight per 100 parts by weight of the total amount of the talc powder and the PTFE emulsion polymerized particle powder.
[0023] [Pulverization of PTFE emulsion polymerized particle powder (2nd process)] 1500g of the mixed powder of the talc powder and PTFE emulsion polymerized particle powder and 600g of crushed dry ice were placed in a polyethylene bag and lightly stirred, and then placed in the container of a cutter mixer (DITO SAMA Food Processor Cutter Mixer 3.5LT-2Speed 1500RPM and 3000RPM). The cutter mixer is equipped with a container and a rotary blade, the container being a stainless steel tank, and the rotary blade is a cutter knife type with an upward-facing flat blade. The skipper at the bottom where compression occurs was removed. The baffle was made of stainless steel.
[0024] <Low speed mixing> After the mixed powder and dry ice were put into the cutter mixer, the rotating blade of the cutter mixer was rotated at an average speed of 1500 rpm, and low-speed stirring and mixing was performed by performing small movements four times at intervals of about 2 to 3 seconds. Note that it is appropriate to perform small movements four to six times at intervals of about 2 to 4 seconds in the low-speed stirring and mixing.
[0025] When the powder temperature was measured with an alcohol thermometer after the rotation had stopped, it was found to be -35°C, which is below the room temperature transition point of PTFE, around 19°C.
[0026] <High-speed stirring and mixing> Following this low-speed stirring and mixing, high-speed stirring and mixing was performed by repeatedly operating the rotary blade of the cutter mixer at an average rotation speed of 3000 rpm four times at 30-second intervals to pulverize the secondary agglomerates of the PTFE emulsion polymerization particle powder, and a mixed pulverized powder of PTFE emulsion polymerization particle pulverized powder with a D50 particle size of 30 μm or less by the laser diffraction method and talc powder was produced. The repeated operation of high-speed stirring and mixing is appropriately performed four to six times at intervals of 15 to 25 seconds.
[0027] The powder temperature after the rotation stopped was -30°C, which is below the room temperature transition point of PTFE, which is around 19°C. The temperature was measured with an infrared thermometer (A&D Company, Limited). At this point, the mixed and ground powder was produced in an environment of 10°C or less due to the effect of adding dry ice.
[0028] [Preparation of granulated mixed powder (3rd step)] The mixed pulverized powder was transferred to a granulation vessel consisting of a stainless steel ball with a diameter of 300 mm, and 400 cc of a 50% aqueous solution of isopropyl alcohol was poured into the granulation vessel as a granulation liquid, and a granulation mixture was prepared while stirring with an electric whipper. The temperature until the end of this process was -10°C, which is below the room temperature transition point of PTFE, which is about 19°C. At this point, the granulation mixture was also prepared in an environment of 10°C or less due to the effect of the dry ice injection.
[0029] The granulated mixture was placed in an oven and heated at a temperature of about 120°C (110 to 130°C is appropriate) for 4 hours to evaporate and dry the 50% aqueous solution of isopropyl alcohol, producing a granulated mixed powder. The average particle size of the granulated mixed powder at this time was about 800 μm.
[0030] A sealing tape was produced from the granulated mixed powder thus prepared by the following method.
[0031] [Preparation of preform (4th step)] <Mixing auxiliary agents> 23 parts by weight, i.e. 115 g, of a petroleum-based solvent (Isopar-H, Exxon Chemical Co., Ltd.) was poured into 500 g of the granulated mixed powder stored in a polyethylene container, and the mixture was left for 24 hours in an insulated box at 30°C, which is above the room temperature transition point of PTFE at 19°C, to prepare an auxiliary-injected mixed powder. The appropriate amount of the auxiliary is 15 to 25 parts by weight. The appropriate temperature of the insulated box is 25 to 60°C.
[0032] <Preforming> First, a 50 mm square die was used as a die for preparing a preform so that it could be inserted into the cylinder of the extrusion die in the extrusion process described below, and the auxiliary-injected mixed powder (equivalent to 500 g) was poured into the die and compressed at 15 kg / cm 2 The preform was prepared by applying a pressure of 10 to 20 kg / cm. 2 is appropriate.
[0033] [Preparation of extruded sheet (5th process)] To produce the extruded sheet, an extrusion die consisting of a cylindrical cylinder and a flat die with a flared outlet is used. The preform is inserted into the cylinder and extruded from the flat die to produce an extruded sheet with a flared width of 150 mm and a thickness of 2.5 mm. The width and thickness depend on the size of the outlet of the flat die, but it is appropriate to extrude to a thickness of 2 to 3 mm.
[0034] [Preparation of rolled film (6th process)] The extruded sheet was heated in hot water at 50° C., and rolled into a 100 μm thick film using a rolling roll having a diameter of 200 mm.
[0035] [Preparation of thin film (7th step)] The auxiliary agent contained in the rolled film was evaporated and dried in an oven at 200°C. The specific gravity of the film at this stage was 1.4 g / CC. Furthermore, a thin film was produced by stretching the film in the extrusion direction to twice its original length between a pair of heating rolls with a diameter of 300 mm and a temperature of 300°C. The specific gravity was 0.8 g / CC.
[0036] The film rolled by the rolling rolls has a thickness in the range of 50 to 200 μm, and it is appropriate to produce a thin film by stretching it 1.5 times to 3 to 4 times depending on the thickness.
[0037] [Preparation of sealing tape (8th process)] Furthermore, the thin film was cut in the extrusion direction to a width of 10 mm to produce a ribbon-shaped sealing tape as a finished product. The appropriate width of the sealing tape is 5 to 20 mm depending on the application. EXAMPLES
[0038] The grinding of the PTFE emulsion polymerized particle powder in Example 1 can be changed as follows.
[0039] Before the low-speed stirring and mixing of [Pulverization of PTFE emulsion polymerization particle powder (second step)] in Example 1, 1.5 g of red iron oxide (pigment) equivalent to 1 part by weight of the total amount of talc powder and PTFE emulsion polymerization particle powder was added as a colorant. That is, a total of 1500 g (100 parts by weight) of talc powder and PTFE emulsion polymerization particle powder and 50 parts by weight of crushed dry ice were added to the container of the cutter mixer together with 1.5 g of red iron oxide (pigment) equivalent to 1 part by weight of the total amount of talc powder and PTFE emulsion polymerization particle powder. The amount of colorant added is appropriately 0.5 to 2 parts by weight of the total amount of talc powder and PTFE emulsion polymerization particle powder.
[0040] Then, in the same manner as in Example 1, a colored sealing tape was completed.
[0041] The use of such a manufacturing method has the advantage that it provides an indication that the sealing tape contains talc powder, and it can be identified by its coloring which is different from conventional products. EXAMPLES
[0042] The grinding of the PTFE emulsion polymerized particle powder in Example 1 can be changed as follows.
[0043] 50 parts by weight of PTFE emulsion polymerization particle powder and 50 parts by weight of crushed dry ice are placed in the container of a cutter mixer, and low-speed stirring and mixing is performed by small movements of the rotating blade of the cutter mixer five times at intervals of about 3 seconds at an average rotation speed of 1500 rpm, followed by high-speed stirring and mixing by repeated operations five times at intervals of 20 seconds at an average rotation speed of 3000 rpm to pulverize the PTFE emulsion polymerization particle powder, and then 50 parts by weight of talc powder is placed in the container of the cutter mixer and low-speed stirring and mixing is performed to produce a mixed pulverized powder of PTFE emulsion polymerization particle pulverized powder with a particle size of 30 μm or less and talc powder in an environment of 10°C or less.
[0044] Then, the same procedure as in Example 1 was carried out to complete the sealing tape.
[0045] When this method is adopted, the talc powder is mixed with the PTFE emulsion polymerized particle powder without being damaged because the talc powder is mixed at a low speed by stirring, and therefore, when the sealing tape is used as a threaded joint seal, the threaded portion does not wear or get damaged.
[0046] Although the embodiment of the present invention has been described above, this embodiment is presented as an example and is not intended to limit the scope of the invention. This embodiment can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the gist of the invention. This embodiment and its modifications are included in the scope of the invention and its equivalents described in the claims, as well as in the scope and gist of the invention.
Claims
1. A method for producing a talc and polytetrafluoroethylene mixed sealing tape, comprising the steps of: First step: talc powder having a particle size of 2 to 5 μm, polytetrafluoroethylene emulsion polymerized particle powder having an average particle size of 500 μm which is an aggregate of polytetrafluoroethylene having a particle size of 0.2 to 0.3 μm, and dry ice are prepared. Second step: 100 parts by weight of the mixed powder of 40 to 60 parts by weight of the talc powder and the polytetrafluoroethylene emulsion polymerization particle powder, and 30 to 50 parts by weight of crushed dry ice are placed in the container part of a cutter mixer equipped with a container part and a rotary blade, and low-speed stirring and mixing is performed by small operation of the rotary blade of the cutter mixer 4 to 6 times at intervals of 2 to 4 seconds at an average rotation speed of 1500 rpm, followed by high-speed stirring and mixing by repeated operation 4 to 6 times at intervals of 15 to 25 seconds at an average rotation speed of 3000 rpm, to pulverize the polytetrafluoroethylene emulsion polymerization particle powder, thereby producing a mixed pulverized powder of the talc powder and the pulverized powder of the polytetrafluoroethylene emulsion polymerization particle having a particle size of 30 μm or less in an environment of 10° C. or less. Third step: The mixed and pulverized powder is transferred to a granulation vessel, a granulation liquid is poured into the vessel, and a granulation mixture is produced under stirring at an environment of 10°C or less. Thereafter, the granulation mixture is heated to 110 to 130°C to evaporate and dry the granulation liquid, thereby producing a granulated mixed powder. Fourth step: 15 to 25 parts by weight of a petroleum-based solvent is added as an auxiliary to the granulated mixed powder, and the mixture is heated to 25 to 60°C and compressed at 10 to 20 kg / cm 2 A pressure of 1000 psi is applied to create a preform. Fifth step: Using an extrusion die consisting of a cylindrical cylinder portion and a flat die portion having a flared outlet portion, the preform is inserted into the cylinder portion and extruded from the flat die portion to produce an extruded sheet having a thickness of 2 to 3 mm. Sixth step: The extruded sheet is rolled with a rolling roll to produce a rolled film having a thickness of 50 to 200 μm. Seventh step: The auxiliary contained in the rolled film is removed by heating at 250° C. or less, and a thin film is produced by stretching the film in the extrusion direction from 1.5 times to 3-4 times using a heated roll. Eighth step: The thin film is cut in the extrusion direction to a width of 5 to 20 mm to prepare a ribbon-shaped sealing tape.
2. In the second step of claim 1, a total of 100 parts by weight of talc powder and polytetrafluoroethylene emulsion polymerized particle powder, 30 to 50 parts by weight of crushed dry ice, and 0.5 to 2 parts by weight of a colorant are charged into the container of a cutter mixer.
2. The method for producing the talc and polytetrafluoroethylene mixed sealing tape according to claim 1 .
3. The second step in claim 1 is to feed 40 to 60 parts by weight of polytetrafluoroethylene emulsion polymerization particle powder and 30 to 50 parts by weight of crushed dry ice into a container of a cutter mixer, and perform low-speed stirring and mixing by performing 4 to 6 small movements of the rotary blade of the cutter mixer at an average rotation speed of 1500 rpm at intervals of 2 to 4 seconds, and then perform high-speed stirring and mixing by performing 4 to 6 repeated operations at an average rotation speed of 3000 rpm at intervals of 15 to 25 seconds to pulverize the polytetrafluoroethylene emulsion polymerization particle powder, and then feed talc powder in an amount that makes the sum of the charged polytetrafluoroethylene emulsion polymerization particle powder and the charged polytetrafluoroethylene emulsion polymerization particle powder 100 parts by weight, and perform low-speed stirring and mixing to produce a mixed and pulverized powder of polytetrafluoroethylene emulsion polymerization particle pulverized powder having a particle size of 30 μm or less and talc powder in an environment of 10° C. or less.
2. The method for producing the talc and polytetrafluoroethylene mixed sealing tape according to claim 1 .
Citation Information
Patent Citations
Method for mixing thermoplastic resin with fluoro resin and method for producing fluoro-resin-containing thermoplastic resin composition
JP1998237254A
Powder for paste extrusion molding and method for producing the same
JP2015151543A
Tape for sealing screw joints
WO1996030458A1