Method for producing thermoplastic resin extruded foam board
A blend of polystyrene resin and polyethylene terephthalate copolymer addresses moldability issues in extruded foam boards, enhancing both foam moldability and long-term heat insulation properties.
Patent Information
- Application Number
- JP2023077679
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-10
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2043-05-10
AI Technical Summary
Existing extruded foam boards using aliphatic hydrocarbons as physical foaming agents face issues with foam moldability, leading to decreased performance and difficulty in forming consistent shapes.
A method involving a specific blend of polystyrene resin and polyethylene terephthalate copolymer, with controlled ratios and compositions of dicarboxylic and glycol components, is used to enhance foam moldability and maintain long-term heat insulation properties.
The solution results in extruded foam boards with improved foam moldability, surface properties, and long-term heat insulation, reducing the likelihood of snagging at the edges during production.
Smart Images

Figure 2024162305000001 
Figure 2024162305000002 
Figure 2024162305000003
Abstract
Description
[Technical field]
[0001] The present invention relates to the technology of extruded thermoplastic resin foam boards. [Background technology]
[0002] Extruded thermoplastic resin foam boards (hereinafter, simply referred to as "extruded foam boards") using a thermoplastic resin (such as polystyrene resin) as a base resin have excellent heat insulating properties and mechanical strength and are therefore widely used as heat insulating materials. For example, extruded foam boards are suitably used as heat insulating materials for the walls, floors, roofs, and the like of buildings. Extruded foam boards are generally produced by heating and melting a thermoplastic resin in an extruder, and then injecting and kneading a physical foaming agent into the resulting molten material to obtain a foamable molten resin kneaded material, which is extruded into a low pressure region from a flat die or the like attached to the tip of the extruder to foam it, and then forming it into a plate shape using a molding tool.
[0003] In recent years, the demand for energy saving in houses, buildings, etc. has been increasing, and there is a further demand for extruded foam boards with excellent thermal insulation. In order to improve the thermal insulation of an extruded foam board, it is necessary to reduce the thermal conductivity of the extruded foam board. For example, Patent Document 1 discloses that by using a mixture of polystyrene resin and a specific amorphous polyester resin as a base resin, an extruded foam board with a reduced thermal conductivity and excellent long-term thermal insulation can be obtained. In the technology of Patent Document 1, specifically, MeCl (methyl chloride) is used as a physical foaming agent. However, since MeCl is a heavy burden on the environment, conversion to other foaming agents is being considered.
[0004] In recent years, aliphatic hydrocarbons with 3 to 5 carbon atoms (hydrofluoroolefins and saturated aliphatic hydrocarbons with 3 to 5 carbon atoms) have been used as physical foaming agents in extruded foam boards because they have little impact on the environment and human body, have low thermal conductivity, and tend to remain in the extruded foam board for long periods of time. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2012-007094 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, in the technology of Patent Document 1, when an aliphatic hydrocarbon having 3 to 5 carbon atoms is used as a physical foaming agent, the edges of the molded body may get caught, resulting in poor foam moldability. In consideration of the above circumstances, the present invention aims to provide an extruded foam board that is excellent not only in long-term heat insulation but also in foam moldability when an aliphatic hydrocarbon having 3 to 5 carbon atoms is used as a physical foaming agent. [Means for solving the problem]
[0007] [1] A method for producing an extruded thermoplastic resin foam plate by extruding and foaming a foamable resin melt obtained by kneading a thermoplastic resin and a physical foaming agent containing an aliphatic hydrocarbon having 3 to 5 carbon atoms, wherein the thermoplastic resin is a mixture of a polystyrene resin and a polyethylene terephthalate copolymer, or a polyethylene terephthalate copolymer, the mass ratio of the polystyrene resin to the polyethylene terephthalate copolymer (polystyrene resin:polyethylene terephthalate copolymer) being 45:55 to 0:100, the polyethylene terephthalate copolymer containing a terephthalic acid component and an isophthalic acid component as dicarboxylic acid components, and containing an ethylene glycol component and a glycol component having a cyclic ether skeleton as glycol components, the content of the isophthalic acid component in the dicarboxylic acid component being 5 mol% or more and 50 mol% or less, and the content of the glycol component having a cyclic ether skeleton in the glycol component being 10 mol% or more and less than 30 mol%.
[0008] [2] The method for producing an extruded thermoplastic resin foam board according to [1], wherein a mass ratio of the polystyrene-based resin to the polyethylene terephthalate copolymer (polystyrene-based resin:polyethylene terephthalate copolymer) is 40:60 to 5:95. Effect of the Invention
[0009] According to the production method of the present invention, an extruded foam board can be obtained which is excellent not only in long-term heat insulation properties but also in foam moldability and surface properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The production method according to the present invention is a method for producing an extruded thermoplastic resin foam board obtained by extruding and foaming a foamable resin melt containing a thermoplastic resin (A) and a physical foaming agent (B) containing an aliphatic hydrocarbon having 3 to 5 carbon atoms.
[0011] The extruded thermoplastic resin foam board (hereinafter, simply referred to as "extruded foam board") obtained by the production method of the present invention is generally produced as follows. First, a thermoplastic resin (A), a flame retardant, and other additives added as necessary are melted and kneaded under heating in an extruder to obtain a molten kneaded product, and a physical foaming agent (B) is injected into the molten kneaded product and further kneaded to obtain a foamable resin melt. Next, the foamable resin melt is adjusted to a temperature suitable for foaming, extruded from the high-pressure extruder through a flat die to a low-pressure region to foam, and passed through a molding tool (e.g., a molding die or a molding roll) arranged at the outlet of the flat die to form a plate-shaped extruded foam board.
[0012] The thermoplastic resin (A) used in the present invention is a mixture of a polystyrene resin and a specific polyethylene terephthalate copolymer (hereinafter also referred to as a "resin mixture"), or the polyethylene terephthalate copolymer (when a polyethylene terephthalate copolymer is used without a polystyrene resin). The content of the resin mixture or the polyethylene terephthalate copolymer (when a polyethylene terephthalate copolymer is used without a polystyrene resin) in the thermoplastic resin is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more. It is particularly preferable that the thermoplastic resin (A) is substantially composed of only the resin mixture or only the polyethylene terephthalate copolymer.
[0013] In addition, when a mixture of a polystyrene-based resin and a specific polyethylene terephthalate copolymer is used as the thermoplastic resin (A), the polystyrene-based resin and the specific polyethylene terephthalate copolymer may be kneaded in advance and then fed to the extruder, or the polystyrene-based resin and the specific polyethylene terephthalate copolymer may be fed separately to the extruder to form a resin mixture.
[0014] [Polystyrene resin] Examples of the polystyrene resin used in the production method of the present invention include polystyrene, styrene-methyl acrylate copolymers containing 50 mol% or more of styrene unit components, styrene-ethyl acrylate copolymers, styrene-methyl methacrylate copolymers, styrene-ethyl methacrylate copolymers, styrene-acrylic acid copolymers, styrene-methacrylic acid copolymers, styrene-maleic anhydride copolymers, styrene-polyphenylene ether copolymers, styrene-acrylonitrile copolymers, styrene-methylstyrene copolymers, styrene-dimethylstyrene copolymers, styrene-ethylstyrene copolymers, and styrene-diethylstyrene copolymers. Among these, polystyrene can be preferably used. In addition to the styrene unit components, polystyrene may contain unit components derived from a branching agent such as a polyfunctional monomer or a polyfunctional macromonomer. The content of the styrene component units in these copolymers is preferably 60 mol% or more, more preferably 80 mol% or more, and even more preferably 90 mol% or more.
[0015] In addition, the polystyrene resin may be a recycled material obtained by recovering used polystyrene resin foam beads molded bodies used in commercial general-purpose polystyrene or fish boxes, or a recycled material obtained by recovering extruded polystyrene resin foam boards (e.g., scraps and crushed materials generated during the manufacture of extruded polystyrene resin foam boards). The recycled material described above can be reused as a polystyrene resin by, for example, crushing and melting the material to form pellets.
[0016] The density of the polystyrene resin is preferably 1000 kg / m 3 That's all. The density of polystyrene resin is approximately 1100 kg / m 3 The density is measured according to the method described in ISO 1183-3.
[0017] For polystyrene-based resins, the heat of fusion in a DSC (Differential Scanning Calorimetry) curve obtained under the following <Condition 1> is preferably 1 J / g or less (including 0), more preferably 0.5 J / g or less, and even more preferably 0 J / g.
[0018] <Condition 1>: A polystyrene-based resin is used as a test piece, and the test piece is held at 200°C for 15 minutes and then allowed to stand at 145°C for 4 days. Then, heat flux differential scanning calorimetry based on JIS K7122-1987 is performed to obtain a DSC curve at a heating rate of 10°C / min.
[0019] From the viewpoint of the production stability of the extruded foam board from the resin mixture, the glass transition temperature of the polystyrene resin is preferably 80° C. or more and 110° C. or less. From the above viewpoint, the glass transition temperature of the polystyrene resin is more preferably 85° C. or more and 105° C. or less.
[0020] The glass transition temperature of a polystyrene resin is the midpoint glass transition temperature measured based on a DSC curve obtained at a heating rate of 10°C / min using a heat flux differential scanning calorimeter (hereinafter referred to as DSC device) in accordance with "measurement of glass transition temperature after a certain heat treatment" (the heating rate and cooling rate in conditioning the test piece are both 10°C / min) as described in JIS K7121-1987.
[0021] [Polyethylene terephthalate copolymer] The polyethylene terephthalate copolymer used in the production method of the present invention is a polyester resin having dicarboxylic acid component (a) units and glycol component (b) units as main component units. The polyethylene terephthalate copolymer contains a terephthalic acid component and an isophthalic acid component as the dicarboxylic acid component (a), and an ethylene glycol component and a glycol component having a cyclic ether skeleton as the glycol component (b). The polyethylene terephthalate copolymer contains 5 mol% to 50 mol% of an isophthalic acid component as the dicarboxylic acid component, and 10 mol% to less than 30 mol% of a glycol component having a cyclic ether skeleton as the glycol component. By containing 5 mol% to 50 mol% of an isophthalic acid component as the dicarboxylic acid component and 10 mol% to less than 30 mol% of a glycol component having a cyclic ether skeleton as the glycol component, the polyethylene terephthalate copolymer can suppress the occurrence of snagging at the width direction edge when the extruded foam plate is continuously molded, and can provide an extruded foam plate having excellent foam moldability and surface properties.
[0022] The polyethylene terephthalate copolymer contains 5 mol% or more and 50 mol% or less of an isophthalic acid component as the dicarboxylic acid component (a). When the polyethylene terephthalate copolymer contains the isophthalic acid component, the crystallinity of the copolymer is reduced, and the foam moldability and surface properties can be improved. From the above viewpoints, the content of the isophthalic acid component in the dicarboxylic acid component (a) is preferably 10 mol% or more and 40 mol% or less, more preferably 15 mol% or more and 30 mol% or less. Since an extruded foam board having a high closed cell ratio and capable of maintaining low thermal conductivity can be obtained, it is particularly preferable that the content of the isophthalic acid component in the dicarboxylic acid component (a) is more than 20 mol% and 30 mol% or less. The total ratio of the terephthalic acid component and the isophthalic acid component in the dicarboxylic acid component (a) is preferably 90 mol% or more, more preferably 95 mol% or more, and further preferably substantially composed of only the terephthalic acid component and the isophthalic acid component.
[0023] As the dicarboxylic acid component (a) other than isophthalic acid and terephthalic acid, for example, dicarboxylic acid or its ester-forming derivative can be used. Examples of the ester-forming derivative include ester derivatives such as alkyl esters having about 1 to 4 carbon atoms, salts such as diammonium salts, and acid halides such as dichlorides. Examples of the dicarboxylic acid include aromatic dicarboxylic acids such as 2,6-naphthalenedicarboxylic acid, phthalic acid (1,2-benzenedicarboxylic acid), 4,4'-diphenyldicarboxylic acid, 3,4'-diphenyldicarboxylic acid, 1,4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 2,5-naphthalenedicarboxylic acid, and 2,7-naphthalenedicarboxylic acid, or derivatives thereof such as acid anhydrides, aliphatic dicarboxylic acids such as oxalic acid, succinic acid, adipic acid, sebacic acid, and dodecanedioic acid, or derivatives thereof, and alicyclic dicarboxylic acids such as 1,4-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, decalindicarboxylic acid, and tetralindicarboxylic acid. The dicarboxylic acid components exemplified above may be used alone or in combination of two or more kinds.
[0024] The amorphous polyethylene terephthalate copolymer contains 10 mol% or more and less than 30 mol%, preferably 10 mol% or more and less than 25 mol% of a glycol component having a cyclic ether skeleton as the glycol component (b). By containing a glycol component having a cyclic ether skeleton, the heat resistance of the extruded foam board can be improved, and the extruded foam board is suitable as an insulating material for external insulation construction such as roofs and exterior walls that require dimensional stability at high temperatures. In addition, since an extruded foam board having a high closed cell ratio and capable of maintaining low thermal conductivity can be obtained, it is particularly preferable that the content of the glycol component having a cyclic ether skeleton in the glycol component (b) is 10 mol% or more and less than 20 mol%. The total ratio of the ethylene glycol component and the glycol component having a cyclic ether skeleton in the glycol component (b) is preferably 90 mol% or more, more preferably 95 mol% or more, and further preferably substantially composed of only the ethylene glycol component and the glycol component having a cyclic ether skeleton.
[0025] As the glycol component (b), other glycol components than the ethylene glycol component and the glycol component having a cyclic ether skeleton can be used, such as aliphatic and aromatic diols (including dihydric phenols) or their ester-forming derivatives, and specifically, can be exemplified by aliphatic diols such as propylene glycol, trimethylene glycol, diethylene glycol, 1,4-butanediol, and neopentyl glycol, alicyclic diols such as 1,4-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, and 1,6-cyclohexanediol, aromatic diols such as bisphenol A, and glycols having a cyclic ether skeleton such as 3,9-bis(1,1-dimethyl-2-hydroxyethyl)2,4,8,10-tetraoxaspiro[5.5]undecane (hereinafter referred to as "spiroglycol") and (1,1-dimethyl-2-hydroxyethyl)-5-ethyl-5-hydroxymethyl-1,3-dioxane (hereinafter referred to as dioxane glycol). The glycol components exemplified above can be used alone or in combination of two or more kinds.
[0026] The polyethylene terephthalate copolymer may have its molecular ends blocked with a small amount of component units derived from monofunctional compounds such as benzoic acid, benzoylbenzoic acid, methoxypolyethylene glycol, etc. Also, it may contain a small amount of component units derived from polyfunctional compounds such as pyromellitic acid, trimellitic acid, trimesic acid, glycerin, pentaerythritol, etc.
[0027] The density of the polyethylene terephthalate copolymer is preferably 1200 kg / m 3 More preferably, it is 1250 kg / m 3 More preferably, it is 1280 kg / m 3 That's all. The density of polyethylene terephthalate copolymer is approximately 1350 kg / m 3 The density of the polyethylene terephthalate copolymer is determined according to the method described in ISO 1183-3.
[0028] The air permeability coefficient of the polyethylene terephthalate copolymer is preferably 8.0×10 -17 [mol m / (m 2 s Pa)] or less, and more preferably 5.0 × 10 -17 [mol m / (m 2 s Pa)] or less, and more preferably 4.0 × 10 -17 [mol m / (m 2 The air permeability coefficient is measured using a known gas permeability tester (for example, a gas permeability tester BT-3 manufactured by Toyo Seiki Co., Ltd.) in accordance with JIS K7126-1:2006 Plastics - Films and sheets - Gas permeability test method - Part 1: Differential pressure method under a temperature condition of 23°C ± 2°C.
[0029] For the polyethylene terephthalate copolymer, the heat of fusion of the DSC curve obtained under the above <Condition 1> is preferably less than 1 J / g (including 0). For the above <Condition 1>, the test piece is a polyethylene terephthalate copolymer. When the heat of fusion of the polyethylene terephthalate copolymer is less than 1 J / g, the catching at the width direction end of the extruded foam plate is suppressed, and the foam moldability is improved. From the above viewpoints, the heat of fusion of the polyethylene terephthalate copolymer is preferably 1 J / g or less, more preferably less than 0.5 J / g. The catching at the width direction end of the extruded foam plate refers to the extruded foam plate being caught at the width direction end of the molding die and curled up due to excessive solidification of a part of the foamed resin melt during extrusion foaming. If the width direction end of the extruded foam plate is caught, the width direction end of the extruded foam plate will not be smooth and will have a poor appearance. If the catching is severe, cracks will occur at the width direction end of the extruded foam plate, and an extruded foam plate with the desired width direction length may not be obtained.
[0030] In the above <Condition 1>, the resin is held at 200°C for 15 minutes to reset the change in the crystallization state and adjust the state. After that, the resin is left at rest for 4 days at 145°C to promote crystallization. In the present invention, it has been found that even in the case of low-crystalline resins in which no endothermic peak was observed by the conventional method of determining the endothermic peak heat, an endothermic peak may be observed by leaving the resin at 145°C for 4 days. In <Condition 1>, when a resin containing a polyethylene terephthalate copolymer having a heat of fusion of 1 J / g or less (including 0) is used to continuously mold an extruded foam board, the occurrence of snagging at the width direction edge can be suppressed. In addition, the relationship between the heat of fusion observed in <Condition 1> (i.e., the crystalline component of the resin) and the snagging at the width direction edge of the extruded foam board can be confirmed by cutting a test piece from the width direction edge of the extruded foam board and measuring the heat of fusion under <Condition 1>. In the present invention, it has been confirmed that the greater the heat of fusion of an extruded foam board obtained under <Condition 1> using a test piece cut from the widthwise end of the extruded foam board, the more frequently the extruded foam board will have snagging at its widthwise end, and it is believed that the progress of resin crystallization during the production of the extruded foam board makes the extruded foam board more susceptible to snagging at its widthwise end. As a conventional method for determining the endothermic peak heat, for example, there is a method for determining the endothermic peak heat associated with the melting of a resin based on a DSC curve obtained under the following <Condition 2>.
[0031] <Condition 2>: "When the heat of fusion is measured after a certain heat treatment" described in JIS K7122-1987 (the heating rate and cooling rate in conditioning the test piece are both 10°C / min) is adopted, and a DSC curve is obtained at a heating rate of 10°C / min using a heat flux differential scanning calorimeter.
[0032] The glass transition temperature of the polyethylene terephthalate copolymer is preferably 75°C or higher. By having a glass transition temperature of 75°C or higher, an extruded foam board having excellent foam moldability and surface properties can be obtained. In addition, by having a glass transition temperature of 75°C or higher, an extruded foam board having excellent heat resistance can be obtained. Furthermore, from the viewpoint of improving the heat resistance of the extruded foam board, the glass transition temperature of the polyethylene terephthalate copolymer is preferably 80°C or higher, more preferably 85°C or higher. From the viewpoint of foam moldability, the upper limit of the glass transition temperature of the polyethylene terephthalate copolymer is preferably 105°C or lower, more preferably 100°C or lower. The glass transition temperature of the polyethylene terephthalate copolymer is measured in the same manner as the glass transition temperature of the polystyrene resin.
[0033] The mass ratio of the polystyrene resin to the polyethylene terephthalate copolymer (polystyrene resin:polyethylene terephthalate copolymer) is 45:55 to 0:100. When the mass ratio of the polystyrene resin to the polyethylene terephthalate copolymer is within the above range, the long-term heat insulation of the extruded foam board is good. Furthermore, from the viewpoint of improving the surface properties and foam moldability of the obtained extruded foam board, the mass ratio of the polystyrene resin to the polyethylene terephthalate copolymer is preferably 40:60 to 5:95. When the (polystyrene resin:polyethylene terephthalate copolymer) is 0:100, the thermoplastic resin does not contain a resin mixture and is composed only of the polyethylene terephthalate copolymer. In this case, the long-term heat insulation of the extruded foam board is particularly good.
[0034] Since the polyethylene terephthalate copolymer has a smaller air permeability coefficient than polystyrene resins, it exhibits good gas barrier properties that suppress the escape of the blowing agent from the extruded foam board and the inflow of air into the extruded foam board. However, in the past, foam molding tended to become difficult when the blending amount of the polyethylene terephthalate copolymer was large. In the present invention, by using a polyethylene terephthalate copolymer consisting of a dicarboxylic acid component containing 10 mol % to 50 mol % of an isophthalic acid component and a glycol component, foam molding is possible even when the blending amount of the polyethylene terephthalate copolymer is large, and an extruded foam board with excellent surface properties and foam moldability can be obtained.
[0035] The thermoplastic resin may contain polymers other than the polystyrene resin and the specific polyethylene terephthalate copolymer described above within the scope in which the object and effect of the present invention are achieved. Examples of other polymers include thermoplastic resins such as polyethylene resins (a mixture of one or more selected from the group consisting of ethylene homopolymers and ethylene copolymers having an ethylene unit content of 50 mol% or more), polypropylene resins (a mixture of one or more selected from the group consisting of propylene homopolymers and propylene copolymers having an ethylene unit content of 50 mol% or more), polyphenylene ether resins, and polymethyl methacrylate, as well as thermoplastic elastomers such as styrene-butadiene-styrene block copolymers, styrene-isoprene-styrene block copolymers, hydrogenated styrene-butadiene-styrene block copolymers, hydrogenated styrene-isoprene-styrene block copolymers, and styrene-ethylene copolymers.
[0036] [Physical foaming agent] Examples of the physical foaming agent (B) containing an aliphatic hydrocarbon having 3 to 5 carbon atoms include hydrofluoroolefins (HFOs) and / or saturated aliphatic hydrocarbons having 3 to 5 carbon atoms. The physical foaming agent (B) containing an aliphatic hydrocarbon having 3 to 5 carbon atoms is a physical foaming agent that has a relatively slow gas permeation rate and is likely to remain in the extruded foam plate. By using the physical foaming agent (B) containing an aliphatic hydrocarbon having 3 to 5 carbon atoms, the extruded foam plate can be made to have excellent long-term heat insulation properties because the physical foaming agent remains in the extruded foam plate for a long time after extrusion foaming. From the above viewpoints, the amount of the physical foaming agent (B) containing an aliphatic hydrocarbon having 3 to 5 carbon atoms added is preferably 0.5 mol to 1.1 mol, more preferably 0.6 mol to 1 mol, and even more preferably 0.7 mol to 0.9 mol per kg of the thermoplastic resin (A). The thermoplastic resin in the present invention has improved gas barrier properties by containing a specific ratio of polyethylene terephthalate copolymer, so that the gas permeation rate of the physical foaming agent through the thermoplastic resin is further slowed, and as a result, the heat insulation performance is further improved.
[0037] Examples of hydrofluoroolefins (HFOs) include 1,3,3,3-tetrafluoropropene (HFO-1234ze), 1-chloro-3,3,3-trifluoropropene (HFO-1233zd), 1-chloro-2,3,3,3-tetrafluoropropene (HFO-1224yd), 2,3,3,3-tetrafluoropropene (HFO-1234yf), 1,1,1,4,4,4-hexafluoro-2-butene (HFO-1336mzz), etc. Among these, HFO-1233zd is preferred from the viewpoint of excellent foamability and facilitating the production of a foamed board having a low apparent density.
[0038] The amount of HFO added is preferably 0.05 mol to 0.6 mol, more preferably 0.1 mol to 0.4 mol, and even more preferably 0.15 mol to 0.3 mol, per kg of thermoplastic resin (A). When the amount of HFO added is within the above range, an effective amount of HFO remains in the extruded foam plate after extrusion foaming, and the extruded foam plate has excellent long-term heat insulation properties.
[0039] Examples of saturated aliphatic hydrocarbons having 3 to 5 carbon atoms include propane, n-butane, i-butane, n-pentane, i-pentane, cyclopentane, and neopentane.
[0040] The amount of the saturated aliphatic hydrocarbon having 3 to 5 carbon atoms added is preferably 0.05 mol to 1 mol, more preferably 0.1 mol to 0.8 mol, and even more preferably 0.2 mol to 0.7 mol, per kg of the thermoplastic resin (A). When the amount of the saturated aliphatic hydrocarbon having 3 to 5 carbon atoms added is within the above range, an extruded foam board having an excellent balance between long-term heat insulation and foam moldability is easily obtained.
[0041] Here, the aliphatic hydrocarbon having 3 to 5 carbon atoms is a foaming agent that contributes to maintaining the long-term thermal conductivity of the extruded foam board low. However, compared with the conventionally used methyl chloride, the aliphatic hydrocarbon having 3 to 5 carbon atoms has a slightly inferior foaming property, and it tends to be difficult to manufacture an extruded foam board with excellent surface properties. In contrast, the present invention has an advantage that, since the foaming stability is excellent by including the specific polyethylene terephthalate copolymer described above, even if the aliphatic hydrocarbon having 3 to 5 carbon atoms is used as the foaming agent, an extruded foam board with excellent foam moldability and surface properties can be obtained.
[0042] In the present invention, other physical foaming agents may be used in addition to the physical foaming agent (B). Examples of other physical foaming agents include aliphatic alcohols having 1 to 5 carbon atoms, ethers, alkyl chlorides, water, carbon dioxide, and nitrogen. These foaming agents may be used alone or in combination of two or more.
[0043] Examples of aliphatic alcohols having 1 to 5 carbon atoms include methyl alcohol (methanol), ethyl alcohol (ethanol), n-propyl alcohol, isopropyl alcohol, butyl alcohol, sec-butyl alcohol (isobutyl alcohol), tert-butyl alcohol, aryl alcohol, crotyl alcohol, propargyl alcohol, n-amyl alcohol, sec-amyl alcohol, isoamyl alcohol, tert-amyl alcohol, neopentyl alcohol, 3-pentanol, 2-methyl-1-butanol, 3-methyl-2-butanol, etc. Among these, ethanol is preferred because of its excellent safety to the environment and the human body.
[0044] The amount of the aliphatic alcohol having 1 to 5 carbon atoms added is preferably 0.01 mol or more and 0.5 mol or less, more preferably 0.03 mol or more and 0.4 mol or less, and even more preferably 0.05 mol or more and 0.25 mol or less, per 1 kg of the thermoplastic resin (A).
[0045] Examples of the ethers include dimethyl ether, diethyl ether, ethyl methyl ether, di-n-butyl ether, and diisopropyl ether.
[0046] Examples of alkyl chlorides include formate esters such as methyl formate, ethyl formate, butyl formate, etc., ethyl chloride, etc. In the present invention, it is preferable that the physical blowing agent does not contain methyl chloride.
[0047] The amount of water added is preferably 0.05 mol to 0.5 mol, more preferably 0.1 mol to 0.4 mol, and even more preferably 0.15 mol to 0.25 mol, per kg of thermoplastic resin (A). By using water within the above range together with the saturated aliphatic hydrocarbon, HFO, and aliphatic alcohol, the expansion ratio of the resulting extruded foam plate can be further improved and the apparent density can be reduced.
[0048] The total amount of the physical foaming agent added is appropriately selected in relation to the desired apparent density, but is preferably 0.8 mol or more and 2 mol or less, more preferably 1 mol or more and 1.5 mol or less, per kg of the thermoplastic resin (A).
[0049] [Flame retardant] The extruded foam board of the present invention is used mainly as a heat insulating material for building materials, and is imparted with flame retardancy by containing a flame retardant, which is blended with a thermoplastic resin.
[0050] The flame retardant is not particularly limited, but a brominated flame retardant is preferable. Examples of the brominated flame retardant include brominated butadiene-based polymers such as brominated butadiene-styrene copolymers, tetrabromobisphenol-A-bis(2,3-dibromo-2-methylpropyl ether), tetrabromobisphenol-S-bis(2,3-dibromo-2-methylpropyl ether), tetrabromobisphenol-F-bis(2,3-dibromo-2-methylpropyl ether), tetrabromobisphenol-A-bis(2,3-dibromopropyl ether), tetrabromobisphenol-B-bis(2,3-dibromopropyl ether), tetrabromobisphenol-C-bis(2,3-dibromopropyl ether), tetrabromobisphenol-D ... Examples of the brominated flame retardants include brominated bisphenol compounds such as tetrabromobisphenol-S-bis(2,3-dibromopropyl ether) and tetrabromobisphenol-F-bis(2,3-dibromopropyl ether), and brominated isocyanurates such as tris(2,3-dibromopropyl)isocyanurate, mono(2,3,4-tribromobutyl)isocyanurate, di(2,3,4-tribromobutyl)isocyanurate, and tris(2,3,4-tribromobutyl)isocyanurate. These brominated flame retardants may be used alone or in combination of two or more.
[0051] In addition to the bromine-based flame retardants, nitrogen-containing cyclic compounds such as cresyl di-2,6-xylenyl phosphate, antimony trioxide, diantimony pentoxide, ammonium sulfate, zinc stannate, cyanuric acid, pentabromotoluene, isocyanuric acid, triallyl isocyanurate, melamine cyanurate, melamine, melam, and melem, silicone-based compounds, inorganic compounds such as boron oxide, zinc borate, and zinc sulfide, phosphorus-based compounds such as phosphate esters represented by triphenyl phosphate, red phosphorus, ammonium polyphosphate, phosphazene, and hypophosphites, and the like can be used in combination.
[0052] Among the flame retardants exemplified above, it is preferable to use a flame retardant containing one or more of brominated butadiene-styrene copolymer, tetrabromobisphenol A-bis(2,3-dibromopropyl ether), tetrabromobisphenol A-bis(2,3-dibromo-2-methylpropyl ether), and tris(2,3-dibromopropyl)isocyanurate, because it can impart high flame retardancy to the extruded foam board. Among these, it is more preferable to use a flame retardant containing a brominated butadiene-styrene copolymer, or a flame retardant using a combination of tetrabromobisphenol A-bis(2,3-dibromopropyl ether) and tetrabromobisphenol A-bis(2,3-dibromo-2-methylpropyl ether), because it can impart high flame retardancy, it is difficult to decompose the polystyrene resin during extrusion, and it is easy to stably obtain an extruded foam board even in the case of a low apparent density (high expansion ratio) and a large cross-sectional area.
[0053] The amount of flame retardant added to the extruded foam board is preferably 0.1 to 10 parts by mass, more preferably 1 to 8 parts by mass, and even more preferably 2 to 7 parts by mass, per 100 parts by mass of thermoplastic resin (A), since high flame retardancy can be imparted to the extruded foam board while suppressing deterioration of extrusion foamability and deterioration of mechanical properties. If the content of the flame retardant is within the above range, the flame retardant does not inhibit foamability, and an extruded foam board that has flame retardancy can be obtained.
[0054] [Flame retardant synergist] In the present invention, in order to further improve the flame retardancy of the extruded foam board, a flame retardant auxiliary can be used in combination with the above flame retardant. Examples of the flame retardant auxiliary include one or more selected from diphenylalkanes and diphenylalkenes such as 2,3-dimethyl-2,3-diphenylbutane, 2,3-diethyl-2,3-diphenylbutane, 3,4-dimethyl-3,4-diphenylhexane, 3,4-diethyl-3,4-diphenylhexane, 2,4-diphenyl-4-methyl-1-pentene, and 2,4-diphenyl-4-ethyl-1-pentene, and polyalkylated aromatic compounds such as poly-1,4-diisopropylbenzene.
[0055] The amount of the flame retardant auxiliary added to the extruded foam board is preferably 0.01 to 1 part by mass, more preferably 0.05 to 0.5 parts by mass, based on 100 parts by mass of the thermoplastic resin (A).
[0056] [Radiation suppressant] In the present invention, the foamable resin melt composition may contain a radiation suppressor in order to improve the heat insulating property by suppressing heat transfer due to infrared radiation.
[0057] The amount of the radiation inhibitor added to the extruded foam board is, from the viewpoint of improving the heat insulation while minimizing the effect on the production stability of the extruded foam board, for example, from 0.3 to 10 parts by mass, preferably from 0.5 to 8 parts by mass, and more preferably from 1.2 to 5 parts by mass, per 100 parts by mass of the thermoplastic resin (A).
[0058] The radiation suppressant may contain graphite. Examples of graphite include flake graphite, scaly graphite, artificial graphite, and earthy graphite, and it is preferable to use graphite whose main component is flake graphite. As described later, it is preferable to use graphite as a master batch in which the graphite is mixed at a high concentration with a polystyrene resin. Graphite having a fixed carbon content of 90% or more is preferable because it has good workability when producing a master batch and has an excellent effect of improving the heat insulation of the resulting extruded foam board. In order to further improve the heat insulation of the extruded foam board, graphite having a fixed carbon content of 93% or more is more preferable, and graphite having a fixed carbon content of 95% or more is even more preferable. The fixed carbon content of graphite refers to a value measured by the method described in JIS M8511:2014.
[0059] The amount of graphite added to the extruded foam plate is, for example, 0.3 parts by mass or more and 10 parts by mass or less, based on 100 parts by mass of the thermoplastic resin (A). When the amount of graphite added is within the above range, the heat insulating property is improved, and an extruded foam plate with a desired low thermal conductivity can be obtained. From the above viewpoints, the amount of graphite added is preferably 0.3 parts by mass or more and 3 parts by mass or less, more preferably 0.4 parts by mass or more and 2 parts by mass or less, and even more preferably 0.4 parts by mass or more and less than 1 part by mass, based on 100 parts by mass of the thermoplastic resin (A).
[0060] In the conventional technology, the addition of graphite tends to result in finer bubbles, making it difficult to produce an extruded foam plate. In contrast, the present invention has the advantage that the extruded foam plate contains the specific polyethylene terephthalate copolymer described above, which provides excellent foaming stability, and therefore allows the extruded foam plate to be stably produced even if it contains graphite.
[0061] In order to further improve the heat insulating properties, the foamable resin melt composition may contain a component other than graphite as a radiation suppressant.
[0062] Examples of components other than graphite include one or more selected from metal oxides such as titanium oxide, metals such as aluminum, ceramics, carbon black, infrared shielding pigments, hydrotalcite, etc. The amount of each of these components added is preferably 0.5 parts by mass or more and 5 parts by mass or less, and more preferably 1 part by mass or more and 4 parts by mass or less, relative to 100 parts by mass of the thermoplastic resin (A).
[0063] [Foam regulator] In the present invention, it is preferable to form a foamable resin melt by blending a cell regulator with the thermoplastic resin.
[0064] The bubble adjusting agent may be one or a mixture of two or more of inorganic powders such as talc, kaolin, mica, silica, calcium carbonate, barium sulfate, titanium oxide, clay, aluminum oxide, bentonite, diatomaceous earth, etc. Among these, talc is preferred because it is easy to adjust the bubble size and to reduce the bubble size without impairing flame retardancy, and fine talc with a 50% particle size (light transmission centrifugal sedimentation method) of 0.1 to 20 μm is particularly preferred, with fine talc with a 50% particle size (light transmission centrifugal sedimentation method) of 0.5 to 15 μm being preferred.
[0065] The amount of the bubble regulator added varies depending on the type of regulator, the desired bubble diameter, etc., but when talc is used as the bubble regulator, the amount is preferably 0.02 parts by mass or more and 7 parts by mass or less, more preferably 0.05 parts by mass or more and 5 parts by mass or less, and even more preferably 0.1 parts by mass or more and 3 parts by mass or less, per 100 parts by mass of the thermoplastic resin (A).
[0066] In the present invention, other known additives may be appropriately added as necessary. Examples of other additives include various additives such as colorants such as pigments or dyes, heat stabilizers, and fillers. The total amount of other additives is preferably 50 parts by mass or less per 100 parts by mass of the thermoplastic resin (A).
[0067] In the production of the extruded foam board of the present invention, the method of adding the flame retardant and other additives to the thermoplastic resin can be adopted by feeding a predetermined ratio of the flame retardant and other additives together with the thermoplastic resin to a feed section provided upstream of the extruder and kneading them in the extruder. In addition, a method of feeding the flame retardant and other additives into the molten resin from a feed section provided in the middle of the extruder can also be adopted. Specifically, a method of feeding a dry blend of the flame retardant, other additives and the thermoplastic resin to the extruder and melt-kneading it, a method of feeding a melt-kneaded product obtained by kneading the flame retardant, other additives and the thermoplastic resin with a kneader or the like to the extruder, a method of preparing a master batch in which a high concentration of the flame retardant and other additives is blended in advance with a polystyrene resin, feeding the master batch to the extruder and melt-kneading it with the thermoplastic resin, etc. can be adopted. In particular, from the viewpoint of dispersibility, it is preferable to adopt a method of preparing a flame retardant master batch and feeding it to the extruder.
[0068] As described above, the extruded foam board of the present invention can be obtained by extruding and foaming a foamable resin melt obtained by melting a thermoplastic resin, additives such as a radiation suppressant and a flame retardant, and a physical foaming agent under atmospheric pressure, and then shaping the extruded foam board into a plate shape using a molding tool.
[0069] <Physical properties of extruded foam board> [Cross-section area and dimensions] The extruded foam board according to the present invention is in the form of a plate. The cross-sectional area of the extruded foam board perpendicular to the extrusion direction is 100 cm 2 It is preferable that the length is more than 200 cm. 2 The upper limit of the cross-sectional area perpendicular to the extrusion direction of the extruded foam plate is, for example, 1500 cm 2 The cross-sectional area perpendicular to the extrusion direction refers to the area of the cross section of the extruded foam board perpendicular to the extrusion direction.
[0070] When the extruded foam board is used as a heat insulating material, the thickness of the extruded foam board is preferably 10 mm or more and 150 mm or less, and more preferably 15 mm or more and 120 mm or less.
[0071] The width of the extruded foam plate is preferably 800 mm or more, more preferably 900 mm or more, and the upper limit of the width of the extruded foam plate is, for example, 1200 mm.
[0072] [Apparent Density] The apparent density of the extruded foam board is 20 kg / m 3 More than 50kg / m 3 It is preferable that the thickness is less than 30 kg / m 3 More than 45kg / m 3 It is more preferable that the apparent density is within the above range. When the apparent density is within the above range, the extruded foam board has sufficient mechanical strength and is lightweight, and can be suitably used, for example, as a heat insulating material. The apparent density is determined by measuring the mass of the extruded foam board and dividing the mass by the volume.
[0073] [Closed bubble rate] The closed cell ratio of the extruded foam board is preferably 85% or more, and more preferably 90% or more. When the closed cell ratio is within the above range, the extruded foam board can have excellent long-term insulation properties and mechanical strength.
[0074] The closed cell ratio of the extruded foam board is measured according to procedure C of ASTM-D2856-70 using a Toshiba Beckman Co., Ltd. air comparison type specific gravity meter Model 930 (a cut sample without a molded skin cut into a size of 25 mm x 25 mm x 20 mm from the extruded foam board is placed in a sample cup and measured. However, if the thickness is too thin to cut a 20 mm cut sample in the thickness direction, for example, two cut samples of a size of 25 mm x 25 mm x 10 mm may be placed in the sample cup at the same time and measured.) using the true volume Vx of the extruded foam board (cut sample) and calculate the closed cell ratio S (%) using the following formula (1), and obtain the average value of N = 3.
[0075] S(%)=(Vx-W / ρ)×100 / (VA-W / ρ)···(1) Vx: True volume of cut sample (cm 3) (This corresponds to the sum of the volume of the resin that constitutes the cut sample of the extruded foam board and the total volume of the air bubbles in the closed cell portion of the cut sample.) VA: Apparent volume (cm) of the cut sample calculated from the outer dimensions of the cut sample used for measurement 3 ) W: Total weight of cut sample used for measurement (g) ρ: Density of the resin that composes the extruded foam board (g / cm 3 )
[0076] [Average bubble diameter in thickness direction] In the present invention, the average bubble diameter in the thickness direction is preferably in the range of 50 to 200 μm, and more preferably in the range of 80 to 150 μm. The method for measuring the average bubble diameter in the thickness direction is as follows.
[0077] First, in the center part (a part 5 mm above and below the center part in the width direction from the center, centered on the line that bisects the foam board in the thickness direction) of the vertical cross section of the foam board in the extrusion direction (a vertical cross section parallel to the extrusion direction of the extruded foam) that divides the foam board in half in the thickness direction, enlarged photographs are obtained by adjusting the magnification to about 50 to 200 times so that the number of cells in the photograph is about 200 to 500. On each photograph, the bubble diameter in the thickness direction of each bubble is obtained using image processing software NS2K-pro manufactured by Nano System Co., Ltd., and the average bubble diameter in the thickness direction of the vertical cross section of the foam board in the extrusion direction is obtained by arithmetically averaging. Next, in the center part (a vertical cross section perpendicular to the extrusion direction of the extruded foam) that divides the foam board in the thickness direction, the average bubble diameter in the thickness direction of the vertical cross section of the foam board in the width direction is obtained in the same manner as the vertical cross section of the foam board in the extrusion direction. The average cell diameter in the thickness direction is calculated by taking the geometric mean of the average cell diameter in the thickness direction of the cross section perpendicular to the extrusion direction of the foamed plate and the average cell diameter in the thickness direction of the cross section perpendicular to the width direction of the foamed plate.
[0078] [Bubble deformation rate] In the present invention, the cell deformation ratio is preferably from 0.7 to 1.3, and more preferably from 0.8 to 1.2.
[0079] The bubble deformation ratio can be calculated by arithmetically averaging the average bubble diameter in the thickness direction and the average bubble diameter in the width direction, and dividing the average bubble diameter in the thickness direction by the average bubble diameter in the width direction, in the same manner as the above measurement of the average bubble diameter in the thickness direction. The smaller the bubble deformation ratio is than 1.0, the flatter the bubbles are, and the larger the bubble deformation ratio is than 1.0, the longer the bubbles are. By having the bubble deformation ratio within the above range, the extruded foam board can be made to have excellent mechanical strength and higher thermal insulation.
[0080] [Thermal Conductivity] (Thermal conductivity after 44 days) The thermal conductivity of the extruded foam board 44 days after production is preferably 0.026 W / m·K or less, more preferably 0.025 W / m·K or less, and even more preferably 0.024 W / m·K or less.
[0081] (Thermal conductivity after 250 days) The thermal conductivity of the extruded foam board 250 days after production is preferably 0.027 W / m·K or less, more preferably 0.026 W / m·K or less, and even more preferably 0.025 W / m·K or less.
[0082] The thermal conductivity of the extruded foam board can be measured based on the heat flow meter method described in JIS A1412-2:1999 (one test piece, symmetrical configuration, high temperature side 38°C, low temperature side 8°C, average temperature 23°C).
[0083] [10% compressive strength] Compressive strength is measured by the following method. From the center of the width of the extruded foam board, a rectangular parallelepiped shape of 25 mm in the extrusion direction, 25 mm in the width direction, and 25 mm thick (excluding the skin layer) is cut out. In this case, the center of the width of the extruded foam board and the center of the width of the test piece are aligned. Next, the test piece is compressed at a speed of 10% x T mm / min (where T is the initial thickness of the test piece), and the maximum force reached within a deformation rate of 10% based on JIS K7220:2006 is calculated, and the compressive strength is calculated by dividing this by the pressure-receiving area of the test piece. The above operation is performed for each of the extrusion direction, width direction, and thickness direction of the test piece, and the arithmetic average value is taken as the 10% compressive strength. EXAMPLES
[0084] The present invention will be described in detail with reference to examples, but the present invention is not limited to the examples.
[0085] In the examples and comparative examples, extruded foam boards were produced as follows. In the examples and comparative examples, the polyethylene terephthalate copolymers shown in Table 1 and the polystyrene resins shown in Table 2 were used as thermoplastic resins.
[0086] The air permeability coefficient, crystallinity, and glass transition temperature were measured for the polyethylene terephthalate copolymers in Table 1 and the polystyrene resins in Table 2. In Table 1, "TPA" is terephthalic acid, "IPA" is isophthalic acid, "EG" is ethylene glycol, and "SPG" is spiroglycol.
[0087] Air permeability coefficient [mol m / (m 2 ·s·Pa) was measured using a gas permeability tester BT-3 manufactured by Toyo Seiki Co., Ltd., in accordance with JIS K7126-1:2006 Plastics - Films and sheets - Gas permeability test method - Part 1: Differential pressure method, at a temperature of 23±2°C.
[0088] Regarding crystallinity, the heat of fusion [J / g] of the DSC curve obtained as follows was measured. For the heat of fusion (condition 1), a polyethylene terephthalate copolymer or a polystyrene resin was used as a test piece, and the heat of fusion was obtained from the DSC curve obtained under the following <condition 1>. Regarding the end temperature of the measurement, if a melting peak was detected, the sample was heated to a temperature 30°C higher than the end of the melting peak to obtain a DSC curve. If no melting peak was detected, the sample was heated to 250°C to obtain a DSC curve.
[0089] <Condition 1>: The test piece was held at 200°C for 15 minutes, then left to stand at 145°C for 4 days, and then subjected to heat flux differential scanning calorimetry based on JIS K7122-1987 to obtain a DSC curve at a heating rate of 10°C / min.
[0090] The heat of fusion (condition 2) was calculated from the DSC curve obtained under the following <condition 2> using polyethylene terephthalate copolymer or polystyrene resin as a test piece. Regarding the end temperature of the measurement, if a melting peak was detected, the sample was heated to a temperature 30°C higher than the end of the melting peak to obtain a DSC curve. If no melting peak was detected, the sample was heated to 250°C to obtain a DSC curve.
[0091] <Condition 2>: "When the heat of fusion is measured after a certain heat treatment" described in JIS K7122-1987 (the heating rate and cooling rate in conditioning the test piece are both 10°C / min) was adopted, and a DSC curve was obtained at a heating rate of 10°C / min using a heat flux differential scanning calorimeter.
[0092] The glass transition temperature [°C] was determined according to "the case where the glass transition temperature is measured after a certain heat treatment" as described in JIS K7121 (1987) (the heating rate and cooling rate in the conditioning of the test piece are both 10°C / min), using a heat flux differential scanning calorimeter (hereinafter referred to as DSC device). The midpoint glass transition temperature measured based on a DSC curve obtained at a heating rate of 10°C / min was taken as the glass transition temperature in the present invention.
[0093] [Table 1]
[0094] [Table 2]
[0095] An extruded foam board was manufactured using the components shown in Table 3. Details of each component are as follows. The polyethylene terephthalate copolymer and polystyrene resin are as shown in Tables 1 and 2.
[0096] [Flame retardant] GR134BG: tetrabromobisphenol A bis(2,3-dibromo-2-methylpropyl ether) ("SR-130" manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), tetrabromobisphenol A bis(2,3-dibromopropyl ether) ("SR-720" manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), GR134BG (SR-130 / SR-720) = 60 / 40 (mass ratio) [Radiation suppressant] Graphite: manufactured by Resino Color Kogyo Co., Ltd., product name: SBF-T-1683, flake graphite powder, average particle size 17 μm, 40% master batch Titanium oxide: "JR-405" manufactured by Teika Co., Ltd., primary particle size (d50) = 0.2 μm [Foam regulator] Talc: Matsumura Sangyo Co., Ltd., product name: High Filler #12, particle size (d50) 7.5 μm [Physical foaming agent] i-Bu: Isobutane: Mitsui Chemicals HFO-1233zd: 1-chloro-3,3,3-trifluoropropene (manufactured by Honeywell, product name "Solstice 1233zd") DME: Dimethyl ether: Mitsubishi Gas Chemical Company, Inc. Ethanol: Yamaichi Chemical Industry Co., Ltd. water
[0097] Specifically, the base resin (polystyrene resin, polyethylene terephthalate copolymer), radiation suppression powder, bubble control agent, and flame retardant master batch were fed to the first extruder in the formulation shown in Table 3, heated to 200°C and kneaded, and the physical foaming agents were fed from the physical foaming agent injection port provided in the first extruder in the amounts shown in Table 3 at each foaming agent injection pressure, and further kneaded to form a foamable resin melt.
[0098] Next, the obtained foamable resin melt is transferred to a second extruder to adjust the resin temperature, and then extruded into a guider at a discharge rate of 400 kg / hr. The resin is foamed while passing through the guider to be molded (shaped) into a plate. The length is then adjusted by cutting to produce an extruded foam plate (width 1000 mm, length 1820 mm, thickness 30 mm, cross-sectional area perpendicular to the extrusion direction: 300 cm). 2 ) was manufactured.
[0099] For the examples and comparative examples, the closed cell ratio, apparent density, thermal conductivity (after 44 days and 250 days), average cell diameter in the thickness direction, cell deformation rate, surface properties, foam moldability, and crystallization state at the product ends were evaluated as follows.
[0100] [Closed bubble rate] The closed cell ratio of the extruded foam board was measured according to procedure C of ASTM-D2856-70 using a Toshiba Beckman Co., Ltd. air comparison type specific gravity meter Model 930 (a cut sample without a molded skin cut into a size of 25 mm x 25 mm x 20 mm was placed in a sample cup and measured. However, if the thickness is too thin to cut a 20 mm cut sample in the thickness direction, for example, two cut samples with a size of 25 mm x 25 mm x 10 mm may be placed in the sample cup at the same time for measurement.) using the true volume Vx of the extruded foam board (cut sample), the closed cell ratio S (%) was calculated using the following formula (1), and the average value of N = 3 was obtained.
[0101] S(%)=(Vx-W / ρ)×100 / (VA-W / ρ)···(1) Vx: True volume of cut sample (cm 3) (This corresponds to the sum of the volume of the resin that constitutes the cut sample of the extruded foam board and the total volume of the air bubbles in the closed cell portion of the cut sample.) VA: Apparent volume (cm) of the cut sample calculated from the outer dimensions of the cut sample used for measurement 3 ) W: Total weight of cut sample used for measurement (g) ρ: Density of the resin that composes the extruded foam board (g / cm 3 )
[0102] [Apparent Density] The apparent density of the foam board was determined by the following method: A rectangular parallelepiped sample of 50 mm length × 50 mm width × 20 mm thickness was cut from the position that divided the obtained foam board into two equal parts in the length direction and from the center and both ends in the width direction of the obtained foam board, and the mass was measured and the apparent density of each sample was determined by dividing the mass by the volume, and the arithmetic average of the masses was regarded as the apparent density.
[0103] [10% compressive strength] The compressive strength is a value measured by the following method. From the center of the width direction of the extruded foam plate, a rectangular parallelepiped shape of 25 mm in the extrusion direction, 25 mm in the width direction, and 25 mm in thickness (excluding the skin layer) was cut out. In this case, the center of the width direction of the extruded foam plate and the center of the width direction of the test piece were made to coincide. Next, the compression speed of this test piece was set to 10% x Tmm / min (where T is the initial thickness of the test piece), and the maximum force reached within a deformation rate of 10% based on JIS K7220:2006 was calculated, and this was divided by the pressure-receiving area of the test piece to calculate the compressive strength. The above operation was performed for each of the extrusion direction, width direction, and thickness direction of the test piece, and the arithmetic average value thereof was determined as the 10% compressive strength.
[0104] [Average bubble diameter in thickness direction] The average bubble diameter was measured as follows. At the center of the foam board that divides the thickness direction of the vertical cross section (a vertical cross section parallel to the extrusion direction of the extruded foam in half at the center in the width direction) in half, the magnification was adjusted to about 50 to 200 times so that the number of cells in the photograph was about 200 to 500, and the bubble diameter in the thickness direction of each bubble was obtained using image processing software NS2K-pro manufactured by Nano System Co., Ltd., and the average bubble diameter in the thickness direction of the vertical cross section of the foam board in the extrusion direction was calculated by arithmetic averaging. Next, at the center of the foam board that divides the thickness direction of the vertical cross section of the foam board in half (a vertical cross section perpendicular to the extrusion direction of the extruded foam) in the thickness direction, the average bubble diameter in the thickness direction of the vertical cross section of the foam board in the width direction was calculated in the same manner as the vertical cross section of the foam board in the extrusion direction. The average cell diameter in the thickness direction was calculated by taking the geometric mean of the average cell diameter in the thickness direction of the cross section perpendicular to the extrusion direction of the foam plate and the average cell diameter in the thickness direction of the cross section perpendicular to the width direction of the foam plate.
[0105] [Bubble deformation rate] The bubble deformation ratio was measured as follows: In the same manner as in the above measurement of the average bubble diameter in the thickness direction, the bubble deformation ratio was calculated by calculating the arithmetic average of the average bubble diameter in the thickness direction and the average bubble diameter in the width direction, and dividing the average bubble diameter in the thickness direction by the average bubble diameter in the width direction.
[0106] [Thermal Conductivity] The thermal conductivity of the extruded foam board was measured by cutting a test piece without the skin, measuring 200 mm long x 200 mm wide x 10 mm, from the extruded foam board immediately after production and storing it in an atmosphere of 23°C and 50% humidity, according to the flat plate heat flow meter method described in JIS A1412-2:1999 (two heat flow meter method, high temperature side 38°C, low temperature side 8°C, average temperature 23°C).
[0107] The thermal conductivity measurements 44 to 250 days after manufacture were taken from extruded foam boards subjected to test method A of the accelerated long-term change test for thermal resistance in accordance with JIS A1486:2014. Specifically, the thermal conductivity measured 7 days after manufacture using a sample obtained by slicing a 25 mm-thick extruded foam board to a thickness of 10 mm was deemed equivalent to the thermal conductivity of the extruded foam board 44 days after manufacture, and the thermal conductivity measured 40 days after manufacture was deemed equivalent to the thermal conductivity of the extruded foam board 250 days after manufacture.
[0108] [Superficiality] The surface properties were visually evaluated according to the following criteria. ⊚: There are no gas spots, and the surfaces of the base plate and the extruded foam plate are free of defects such as roughness. ◯: There are gas spots on the surface of the original plate, but there are no defects such as gas spots or roughness on the foam surface of the extruded foam plate. Δ: Gas spots were observed, and the surfaces of the base plate and extruded foam plate were rough or otherwise defective. ×: Many gas spots were generated, and molding was difficult.
[0109] [Foam moldability] The foam moldability was visually evaluated according to the following criteria. ⊚: The foaming state is good, and there is no sticking at the width direction edges of the extruded foam plate. ◯: The foaming state is good, but the width direction edges of the extruded foam plate are occasionally caught. Δ: The foaming state is poor, and continuous snagging occurs at the widthwise edges of the extruded foam plate. ×: The foaming state is poor and it is not possible to form it into a plate.
[0110] [Crystallization state] The degree of crystallization of the polyethylene terephthalate copolymer at the end of the extruded foam plate was evaluated by measuring the heat of fusion of the extruded foam plate. The heat of fusion of the extruded foam plate [J / g] was calculated from the melting peak area of the DSC curve and the sample weight by randomly cutting out 3-5 mg test pieces from the end of the width direction of the extruded foam plate including the skin layer, adopting the "measurement of transition heat by adjusting under standard conditions" described in JIS K7122-1987, and performing heat flux differential scanning calorimetry using a DSC device and heating from 30°C to 250°C at a heating rate of 10°C / min.
[0111] [Table 3]
[0112] As can be seen from Table 3, in Examples 1 to 5, compared with Comparative Examples 1 to 4, it was confirmed that not only the long-term heat insulation properties but also the foam moldability and surface properties were excellent, and there was almost no catching at the width direction end. In particular, Comparative Examples 2 to 4 were poor in foamability, and it was difficult to mold them into a plate. In Comparative Examples 2 to 4, the molding was difficult, so the physical properties were not evaluated. Comparing Examples 1 and 2 with Example 3, it was also confirmed that the surface properties and foam moldability were further improved by using a polyethylene terephthalate copolymer in combination with a polystyrene-based resin compared to using a polyethylene terephthalate copolymer alone.
[0113] As described above, in the present invention, by using a specific polyethylene terephthalate copolymer, the extruded foam board can have good long-term heat insulation properties, foam moldability, and surface properties, even when a physical foaming agent made of an aliphatic hydrocarbon having 3 to 5 carbon atoms is used.
Claims
1. A method for producing an extruded thermoplastic resin foam plate, comprising extruding and foaming a foamable resin melt obtained by kneading a thermoplastic resin and a physical foaming agent containing an aliphatic hydrocarbon having 3 to 5 carbon atoms, the method comprising the steps of: The thermoplastic resin is a mixture of a polystyrene resin and a polyethylene terephthalate copolymer, or a polyethylene terephthalate copolymer; a mass ratio of the polystyrene-based resin to the polyethylene terephthalate copolymer (polystyrene-based resin:polyethylene terephthalate copolymer) is 45:55 to 0:100; a polyethylene terephthalate copolymer containing a terephthalic acid component and an isophthalic acid component as dicarboxylic acid components, and containing an ethylene glycol component and a glycol component having a cyclic ether skeleton as glycol components, the content of the isophthalic acid component in the dicarboxylic acid component being 5 mol % or more and 50 mol % or less, and the content of the glycol component having a cyclic ether skeleton in the glycol component being 10 mol % or more and less than 30 mol %.
2. The method for producing an extruded thermoplastic resin foam plate according to claim 1, wherein the mass ratio of the polystyrene resin to the polyethylene terephthalate copolymer (polystyrene resin:polyethylene terephthalate copolymer) is 40:60 to 5:95.
Citation Information
Patent Citations
Thermoplastic resin extrusion foamed heat insulating plate
JP2012007094A