Film deposition method

The film-forming method addresses the issues of uneven smoothness and grain growth in copper films by controlling substrate temperature and applying a magnetic field, resulting in low resistance and smooth copper films on large glass substrates.

JP2024162567APending Publication Date: 2024-11-21ULVAC INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023078196
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-10
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Existing methods for forming thick copper films on large glass substrates face issues with uneven surface smoothness and excessive grain growth due to high substrate temperatures, leading to warpage and increased specific resistance values.

Method used

A film-forming method that maintains the substrate temperature below 100°C by setting a heat transfer coefficient of 50W/m²·K or higher, applies a leakage magnetic field with a maximum horizontal magnetic field strength of 400G, and controls the discharge voltage during sputtering to form a copper film with a thickness of 1 μm or more.

Benefits of technology

The method achieves a copper film with low resistance and good smoothness, maintaining warpage below 1 mm and specific resistance values around 2 μΩcm, while ensuring high productivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024162567000001_ABST
    Figure 2024162567000001_ABST
Patent Text Reader

Abstract

To provide a film deposition method capable of depositing a copper film low in resistance and excellent in smoothness in a larger thickness.SOLUTION: A film deposition method comprises depositing a copper film on the surface of a substrate Sw in a film thickness of 1 μm or more by sucking the substrate on a stage 2 provided in a vacuum chamber 1, introducing sputtering gas so as to hold the inside of the vacuum chamber having a vacuum atmosphere in a predetermined pressure range, inputting electric power to copper targets Tg1-Tg6 arranged to face the substrate, forming a plasma atmosphere in a space between the substrate and the target and sputtering each target. The substrate is held at a temperature equal to or less than a predetermined temperature by heat exchange with the stage during the sputtering, and at this time, a heat transfer rate coefficient between the substrate and the stage is 50 W / m2 K or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a film forming method, and more particularly to a method for forming a copper film with a thickness of 1 μm or more by a sputtering method. [Background technology]

[0002] In recent years, micro LED displays and mini LED displays, which are mounted with tiny LED chips in the pixels of a circuit board, have been developed as next-generation displays because of their superior device characteristics, such as lower power consumption and higher contrast and brightness compared to liquid crystal displays and organic electroluminescence displays. Examples of circuit boards that drive LED chips include those that include a light-transmitting substrate such as a glass substrate, a quartz substrate, or a sapphire substrate and a TFT formed on the substrate, and copper is used for wiring to drive the micro LED and other circuits (see Patent Document 1). For this reason, it is expected that there will be an increased demand for a technology that forms a copper (wiring) film with a thickness in the range of 1 μm to 10 μm on the surface of a relatively large glass substrate with at least one side of 1 mm or more.

[0003] To form such a copper film, it is considered to use a magnetron sputtering device using a copper target (see, for example, Patent Document 2). This type of sputtering device generally has a vacuum chamber capable of forming a vacuum atmosphere, a copper target is disposed in the upper part of the vacuum chamber, and a stage on which a substrate on which a film is to be formed is placed is provided in the lower part of the vacuum chamber facing directly to the target. The stage has a base and a chuck plate provided on the upper surface of the base, and an electrode for electrostatic chucking is embedded in the chuck plate. A DC voltage is applied to the electrode from a chuck power supply, so that the substrate placed with the film-forming surface facing upwards can be electrostatically attracted to the upper surface of the chuck plate.

[0004] The base is formed with a coolant circulation path for circulating the coolant supplied from the chiller unit, so that the substrate adsorbed on the upper surface of the chuck plate can be kept at a predetermined temperature or lower by heat exchange with the stage during sputtering of the target. At this time, the heat transfer coefficient between the stage and the substrate can be increased by supplying an assist gas (e.g., Ar gas or He gas) to the back surface of the substrate electrostatically adsorbed to the chuck plate. Then, with the substrate electrostatically adsorbed to the stage, a rare gas is introduced into a vacuum chamber in a vacuum atmosphere, and DC power with a negative potential or AC power with a predetermined frequency is applied to the target. As a result, a plasma atmosphere is formed in the vacuum chamber, and ions of the rare gas ionized in the plasma collide with the target to sputter it, and sputtered particles scattered from the target adhere and deposit on the surface of the substrate, forming a copper film.

[0005] When a copper film is formed on a glass substrate surface with a thickness of 1 μm or more by the above-mentioned sputtering device, a film formation rate of 0.5 μm / min or more, preferably about 1 μm / min, is required in consideration of productivity, but this requires not only increasing the power input to the target but also increasing the film formation time. For this reason, it is expected that the heat input from the plasma to the substrate during film formation will increase. In such a case, if the substrate temperature during sputtering becomes high, the grain growth of copper is excessively promoted, and the surface of the formed copper film becomes uneven, impairing its surface smoothness, while it is generally known that if the substrate temperature during sputtering is too low, the grain size of the crystal grains of the copper film becomes small, resulting in a high resistivity value. On the other hand, if the substrate is large and thin (thickness is 0.5 mm to 0.7 mm), the substrate warps as the substrate temperature rises during sputtering, which may locally impair the surface smoothness of the formed copper film. The amount of warping at this time tends to be significantly large in the case of a substrate having at least one side that is 1 m or longer. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Patent Publication No. 2022-36709 [Patent Document 2] International Publication No. 2020 / 136964 Summary of the Invention [Problem to be solved by the invention]

[0007] The present invention has been made in consideration of the above points, and an object of the present invention is to provide a film formation method capable of forming a copper film having low resistance and good smoothness with a relatively large thickness. [Means for solving the problem]

[0008] In order to solve the above problems, the film formation method of the present invention includes a film formation step of adsorbing a substrate to be subjected to film formation processing onto a stage provided within a vacuum chamber, introducing a sputtering gas so that the inside of the vacuum chamber in a vacuum atmosphere is maintained at a predetermined pressure range, supplying power to a copper target disposed opposite the substrate, forming a plasma atmosphere in a space between the substrate and the target, and sputtering the target to form a copper film with a thickness of 1 μm or more on the surface of the substrate, and further includes a holding step of holding the substrate at a predetermined temperature or lower by heat exchange with the stage during sputtering of the target, and maintaining a heat transfer coefficient between the substrate and the stage at a temperature of 50 W / m or lower. 2 The characteristic of the present invention is that the temperature is 0.5 to 100°C.

[0009] Here, the inventors of the present application have conducted extensive research focusing on the amount of warping per unit length during film formation by sputtering, and have discovered that if the amount of warping per unit length (m) can be kept to 1 mm or less by controlling the substrate temperature during film formation, a copper film with good smoothness can be formed. Then, the film stress and thermal stress when a copper film of a specified thickness is formed on a glass substrate of a specified plate thickness are obtained, and the amount of warping of the substrate is calculated based on this using the Stoney formula and the substrate temperature. It has been found that if the substrate temperature during film formation can be kept below 100°C, the amount of warping can be kept to 1 mm or less, and this can be achieved by maintaining the heat transfer coefficient between the substrate and the stage at 50 W / m 2We found that it is sufficient to set the value to 0.K or more.

[0010] According to the above, even if the deposition rate is set to 0.5 μm / min or more to maintain productivity, the substrate temperature can be maintained at 100° C. or less, so that a copper film with good smoothness can be deposited, and furthermore, there is no problem that the surface of the deposited copper film becomes uneven due to excessive promotion of copper grain growth, which would impair the surface smoothness. The upper limit of the heat transfer coefficient is appropriately set within a range in which the grain size of the crystal grains in the copper film does not become small and the resistivity value does not become high. In this case, the heat transfer coefficient is set to 100 W / m 2 It was confirmed that a low resistivity value of approximately 2 μΩcm was obtained when the temperature was 1.0 K.

[0011] In the present invention, it is preferable that while power is being applied to the copper target, a leakage magnetic field having a maximum horizontal magnetic field strength of 400 G or more is applied to the sputtering surface of the target, and the discharge voltage during sputtering is set to 550 V or less. It has been confirmed that this makes it possible to form a copper film with a lower resistivity.

[0012] In the present invention, it is preferable that the holding step includes a step of introducing an assist gas to the back surface of the substrate adsorbed to the stage, and that the deposition rate in the deposition step is set to 0.5 μm / min or more. It is also preferable that the substrate has at least one side having a length of 1 m or more, and that the target is composed of a plurality of targets arranged in parallel, and that DC power having a negative potential is input to each target from a sputtering power supply. [Brief description of the drawings]

[0013] [Figure 1] FIG. 2 is a schematic cross-sectional view of a sputtering apparatus capable of carrying out the film formation direction of the present embodiment. [Diagram 2] 1 is a graph showing the relationship between substrate temperature and substrate warpage amount. [Diagram 3] 1 is a graph showing the relationship between substrate temperature and heat transfer coefficient. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, with reference to the drawings, an embodiment of the film forming method of the present invention will be described by taking as an example a case where a copper film is formed on the surface of the substrate Sw to a thickness within a range of 1 μm to 10 μm by a sputtering method using a large-area, thin glass substrate (hereinafter referred to as "substrate Sw") used in the manufacture of flat panel displays, a copper target of a predetermined purity, and argon gas as the sputtering gas. In the following, terms indicating directions such as up and down are based on FIG. 1.

[0015] 1, a sputtering apparatus Sm capable of carrying out the film forming method of this embodiment is a so-called magnetron type multi-cathode type, and includes an earthed vacuum chamber 1. A vacuum pump 12 is connected to the vacuum chamber 1 via an exhaust pipe 11, and the inside of the vacuum chamber 1 can be evacuated to a predetermined pressure (vacuum level). A gas pipe 14a, which is connected to an argon gas source and has a mass flow controller 13a interposed therein, is connected to a side wall of the vacuum chamber 1. Then, argon gas, the flow rate of which is controlled by each mass flow controller 13a, can be introduced into the vacuum chamber 1 in a vacuum atmosphere at a predetermined flow rate.

[0016] A stage 2 is provided in the vacuum chamber 1. The stage 2 has a metal base 21 arranged on the inside of the bottom surface of the vacuum chamber 1 via an insulator Ip, and an electrostatic chuck 22 provided on the upper surface of the base 21. The base 21 is formed with a coolant passage 21a for circulating a coolant such as cooling water, and a coolant at a predetermined temperature is circulated from a chiller unit Ch to cool the base 21. On the other hand, the electrostatic chuck 22 is not particularly limited as long as it can adsorb the substrate Sw as an insulator in an orientation with its film formation surface Sw1 facing upward and in close contact over its entire surface at the beginning of film formation, and can maintain a state of close contact over the entire surface even after a conductive copper film has been formed on the film formation surface Sw1. As the electrostatic chuck 22, for example, a known one (for example, Japanese Patent No. 6511212) capable of exhibiting both an adsorption force dominated by electrostatic force or Johnsen-Rahbek force and an adsorption force dominated by gradient force can be used, and therefore a detailed description thereof will be omitted here. As shown in FIG. 1, a recess 22a recessed downward in the upper surface of the electrostatic chuck 22 may be formed, and a gas pipe 14b having a mass flow controller 13b interposed therein may be connected to the recess 22a to supply an assist gas (e.g., Ar gas or He gas) to the back surface of the substrate Sw attracted to the electrostatic chuck 22, thereby increasing the heat transfer coefficient between the stage 2 and the substrate Sw.

[0017] The vacuum chamber 1 is provided with a cathode unit Sc facing the stage 2. The cathode unit Sc is provided with six copper targets Tg1 to Tg6, each of which is installed with its sputtering surface Tgs facing downward and is arranged in parallel at equal intervals in the X-axis direction in an XY plane parallel to the film formation surface Sw1 of the substrate Sw adsorbed by the stage 2. The targets Tg1 to Tg6 are of the same shape formed into a flat plate, and the width in the X-axis direction and the length in the Y-axis direction of each target Tg1 to Tg6 are set so that the area in which the targets Tg1 to Tg6 are arranged in parallel is slightly larger than the outline of the substrate Sw. The TS distance between the sputtering surface Tgs of each target Tg1 to Tg6 and the substrate Sw is set in the range of 150 mm to 400 mm. The number of targets arranged in parallel is not limited to this, and can be set appropriately depending on the size (area) of the substrate Sw, etc. A backing plate 31 is bonded to each of the targets Tg1 to Tg6 via a bonding material (not shown) such as indium or tin, and each backing plate 31 is attached to a single support plate 32 in a state in which they are electrically insulated from each other. A shield plate 33 that functions as an anode is attached to the support plate 32 so as to surround each of the targets Tg1 to Tg6. An output from a DC power source Ps is also connected to each of the targets Tg1 to Tg6, and a predetermined power having a negative potential is input.

[0018] Magnet units Mu1 to Mu6 are provided above the backing plates 31 of the targets Tg1 to Tg6. Each of the magnet units Mu1 to Mu6 has the same shape and includes a yoke 41 made of a magnetic material arranged parallel to the film formation surface Sw1 of the substrate Sw. The yoke 41 has a length that covers almost the entire length of each of the targets Tg1 to Tg6, and a central magnet 42 extending in the Y-axis direction and a peripheral magnet 43 surrounding the periphery of the central magnet 42 are arranged in the center of the lower surface of the yoke 41 with the polarity on the target Tg1 to Tg6 side changed. As a result, a balanced closed loop leakage magnetic field acts on the space between the sputtering surface Tgs of each of the targets Tg1 to Tg6 and the substrate Sw. In this embodiment, the central magnet 42 and the peripheral magnet 43 are designed so that a leakage magnetic field having a maximum horizontal magnetic field strength of 400 G or more acts on the sputtering surface Tgs of each of the targets Tg1 to Tg6. Each of the magnet units Mu1 to Mu6 is also connected to a drive shaft 51 of a drive means 5 such as a linear motor or an air cylinder, and during film formation by sputtering, each of the magnet units Mu1 to Mu6 can reciprocate together in the X-axis direction at a predetermined stroke value.

[0019] When a copper film is formed on the film-forming surface Sw1 of the substrate Sw, the substrate Sw is transported to the vacuum chamber 1 by a transport robot (not shown) and placed on the upper surface of the stage 2 (electrostatic chuck 22) with the film-forming surface Sw1 facing upward. When the substrate Sw is placed, a DC voltage is applied to the electrodes (not shown) of the electrostatic chuck 22, and for example, a chucking force dominated by gradient force is generated, and the substrate Sw is chucked in a state of being in close contact over its entire surface. At this time, a refrigerant at a predetermined temperature is circulated from the chiller unit Ch to start cooling the base 21. Then, when the inside of the vacuum chamber 1 reaches a predetermined pressure, argon gas whose flow rate is adjusted by the mass flow controller 13a is introduced. The flow rate of the argon gas introduced into the vacuum chamber 1 is set to 100 sccm to 1000 sccm (the pressure inside the vacuum chamber 1, which is evacuated at a constant exhaust speed, is maintained in the range of 0.1 Pa to 1 Pa). At the same time, DC power having a negative potential is applied to each of the targets Tg1 to Tg6 by the DC power source Ps.

[0020] The input power is set so that a film formation rate in the range of 1 μm / min is obtained, for example, while the discharge voltage is set in the range of 150V to 550V. If the discharge voltage is lower than 150V, a high film formation rate cannot be obtained, resulting in poor productivity. On the other hand, if the discharge voltage is higher than 550V, the smoothness of the surface of the copper film is locally impaired. Then, plasma is formed in the space between each of the targets Tg1 to Tg6 and the substrate Sw in the vacuum chamber 1. As a result, the sputtering surfaces Tgs of each of the targets Tg1 to Tg6 are sputtered by ions of argon gas in the plasma, and the sputtered particles scattered from each of the targets Tg1 to Tg6 according to a predetermined cosine law are attached to and deposited on the surface of the substrate Sw to form a copper film, which is continued for a sputtering time until the copper film is formed to a thickness in the range of 1 μm to 10 μm (film formation process). During sputtering of each of the targets Tg1 to Tg6, the substrate Sw is maintained at a predetermined temperature or lower by heat exchange with the stage 2 (maintenance step). During sputtering, in order to erode the sputtering surface Tgs approximately uniformly, each of the magnet units Mu1 to Mu6 is reciprocated in the X-axis direction by the driving means 5 at a predetermined stroke value. When a copper film is formed on the film formation surface Sw1 of the substrate Sw, for example, a DC voltage is applied to another electrode (not shown) of the electrostatic chuck 22 to generate an electrostatically dominant attracting force, so that the substrate Sw is constantly maintained in a state of being attracted (closely attached) to the electrostatic chuck 22 with a constant attracting force.

[0021] Here, when a film is formed by sputtering, the amount of warping of the substrate Sw per unit length (m) is considered, and in order to form a copper film with good smoothness, the amount of warping must be kept below 1 mm / m. In this case, the film stress and thermal stress when a copper film is formed to a thickness of 4.5 μm on a glass substrate with a plate thickness of 0.5 mm are calculated, and based on these, the relationship between the temperature of the substrate Sw and the amount of warping of the substrate Sw per unit length (m) is graphed using the known Stoney's formula, as shown in FIG. 2. According to this, it is found that if the temperature of the substrate Sw during film formation can be kept below 100° C., the amount of warping can be kept below 1 mm / m. Then, taking into consideration the amount of heat input from the plasma when the film formation rate is set to 1 μm / min, the emissivity of the lower surface of the substrate Sw (0.9), the emissivity of the substrate attracting surface of the electrostatic chuck 22 (0.8), and the coolant temperature (25° C.), the heat transfer coefficient (W / m 2 The relationship between the heat transfer coefficient (K) and the substrate Sw temperature is shown in Figure 3. 2 .K or more, the amount of warping of the substrate can be made 1 mm / m or less even when the deposition rate is set to 1 μm / min. In this embodiment, the temperature and flow rate of the coolant circulating from the chiller unit Ch to the coolant passage 21a are controlled to achieve a heat transfer coefficient of 50 W / m 2 It was made to be K or higher.

[0022] According to the above, even if the film formation rate is set to 0.5 μm / min or more, preferably 1 μm / min or more to maintain productivity, the substrate temperature can be maintained at 100° C. or less, so that a copper film with good smoothness can be formed, and furthermore, there is no problem that the surface of the formed copper film becomes uneven due to excessive promotion of copper grain growth, and the surface smoothness is impaired. Moreover, during sputtering, a leakage magnetic field having a maximum horizontal magnetic field strength of 400 G or more is applied to the sputtering surface Tgs of the targets Tg1 to Tg6, and the discharge voltage during sputtering is set to 550 V or less, so that a copper film with a lower resistivity can be formed. The upper limit of the heat transfer coefficient is appropriately set within a range in which the grain size of the crystal grains in the copper film does not become small and the resistivity does not become high.

[0023] In order to confirm the above-mentioned effect, the following experiment was carried out using the sputtering device Sm. In this experiment, the substrate Sw was a so-called G8.5 glass substrate on which a Ti film was formed as an adhesive layer with a thickness of 50 nm (Mo or Cr can also be used as the adhesive layer, and the film thickness can be appropriately set within the range of 5 to 100 nm). As sputtering conditions, each magnet unit Mu1 to Mu6 was configured so that a leakage magnetic field (weak magnetic field) with a maximum horizontal magnetic field strength of 260 G acts on the sputtering surface Tgs, the distance between TS was set to 57 mm, the DC power with a negative potential input to each target Tg1 to Tg6 was set to 7.5 kW, and the amount of argon gas introduced was set so that the pressure in the vacuum chamber 1 was maintained at 0.3 Pa, and a copper film was formed in a sputtering time of 4 minutes (the film formation rate at this time was about 1 μm / min). In the invention experiment 1, the heat transfer coefficient during heat exchange between the stage 2 and the substrate Sw during film formation was 70 W / m 2 While the chiller unit Ch was controlled so that the temperature was kept at 100° C., in a comparative experiment, the chiller unit Ch was stopped and film formation was performed without cooling the substrate Sw.

[0024] In the comparative experiment, the substrate temperature easily exceeded 100°C before the sputtering time elapsed, and the unit area (5 μm 2 The surface roughness (Ra) per unit area (5 μm2) was measured to be 12.9 nm. The specific resistance of the copper film was measured to be 2.3 μΩcm. In contrast, in invention experiment 1, the substrate temperature was kept below 85°C until the sputtering time had elapsed, and the surface roughness (Ra) per unit area (5 μm2) of the deposited copper film was 12.9 nm. 2 When the surface roughness (Ra) per unit area was measured, it was found to have decreased to 7.1 nm, confirming that the smoothness had improved. In addition, the resistivity of the copper film was found to be 2.4 μΩ cm, confirming that the grain size of the crystal grains in the copper film had not become significantly smaller.

[0025] Next, as invention experiment 2, each magnet unit Mu1 to Mu6 was configured so that a leakage magnetic field (strong magnetic field) with a maximum horizontal magnetic field strength of 450 G acts on the sputtering surface Tgs, and a copper film was formed under the same conditions as in invention experiment 1. According to this, the substrate temperature was kept below 85°C until the sputtering time elapsed, and the surface roughness (Ra) per unit area (5 μm2) of the copper film after film formation was measured and further decreased to 6.7 nm, confirming that the smoothness was further improved. In addition, the resistivity value of the copper film was measured and found to be 2.0 μΩcm, and it was confirmed that an even lower resistivity value could be obtained. It was also confirmed that a low resistivity value of about 2 μΩcm could be obtained even when the heat transfer coefficient was set to 100 W / m2·K.

[0026] Although the embodiment of the present invention has been described above, various modifications are possible without departing from the scope of the technical concept of the present invention. In the above embodiment, the sputtering apparatus for carrying out the film forming method of the present invention is described as an example in which a plurality of flat targets Tg1 to Tg6 are arranged in parallel, but the present invention is not limited to this, and for example, a known so-called rotary cathode having a cylindrical target can be used. [Explanation of symbols]

[0027] Sm: sputtering device, Sw: substrate, Ch: chiller unit, Tg1 to Tg6: targets, Mu1 to Mu6: magnet units, 1: inside vacuum chamber, 2: stage, 14: sputtering gas introduction pipe.

Claims

1. A substrate to be subjected to a film forming process is adsorbed on a stage provided in a vacuum chamber, A sputtering gas is introduced so that the inside of the vacuum chamber in a vacuum atmosphere is maintained at a predetermined pressure range; A film formation method including a film formation step of applying power to a copper target disposed opposite the substrate, forming a plasma atmosphere in a space between the substrate and the target, and sputtering the target to form a copper film having a thickness of 1 μm or more on the surface of the substrate, a holding step of holding the substrate at or below a predetermined temperature by heat exchange with the stage during sputtering of the target, The heat transfer coefficient between the substrate and the stage is 50 W / m 2 A film forming method characterized in that the temperature is K or higher.

2. The film forming method according to claim 1, characterized in that while power is being supplied to the copper target, a leakage magnetic field having a maximum horizontal magnetic field strength of 400 G or more is applied to the sputtering surface of the target, and the discharge voltage during sputtering is set to 550 V or less.

3. the holding step includes a step of supplying an assist gas to a rear surface of the substrate adsorbed on the stage, 3. The method according to claim 1, wherein the deposition rate in the deposition step is set to 0.5 [mu]m / min or more.

4. 4. The film forming method according to claim 3, wherein the substrate has at least one side having a length of 1 m or more, the target is configured by arranging a plurality of targets in parallel, and each target is supplied with DC power having a negative potential from a sputtering power supply.

Citation Information

Patent Citations

  • Display device

    JP2022036709A

  • Vacuum processing apparatus

    WO2020136964A1