Method of manufacturing resin composition, and resin composition
The twin-screw kneading extruder method effectively addresses the imbalance in residual fiber bundles and productivity by optimizing pressure and clearance configurations, resulting in high-quality fiber-reinforced resin compositions for precision molding.
Patent Information
- Application Number
- JP2023078209
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-10
- Publication Date
- 2024-11-21
AI Technical Summary
Existing methods for producing fiber-based filler-reinforced thermoplastic resin compositions fail to achieve a balance between reducing the residual rate of unfibrillated fiber bundles, maintaining fiber length, and improving productivity, particularly in precision molded products where the presence of unfibrillated bundles can cause defects and decreased functionality.
A method involving a twin-screw kneading extruder with specific design features, including first and second supply ports, first and second kneading zones, and resistance portions that generate defined pressures and clearances, to effectively melt-knead thermoplastic resin and fibrous fillers, reducing the residual rate of unfibrillated fiber bundles while maintaining fiber length and productivity.
The method significantly reduces the residual rate of unfibrillated fiber bundles, ensuring improved mechanical strength and productivity, enabling the production of resin compositions suitable for precision molding applications.
Smart Images

Figure 2024162573000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a resin composition and a resin composition. [Background technology]
[0002] Thermoplastic resin compositions containing a thermoplastic resin and a fibrous filler are superior in physical properties such as mechanical strength to thermoplastic resins not containing a fibrous filler, and therefore thermoplastic resin compositions containing a fibrous filler are used as raw materials for automobile parts, parts for electric and electronic products, etc.
[0003] Examples of the method for producing pellets of a fiber-based filler-reinforced thermoplastic resin composition by mixing and kneading a fiber-based filler with a thermoplastic resin include the following methods. First, a thermoplastic resin is fed into an extruder and melted. Next, a fibrous filler is fed into the melted thermoplastic resin and the thermoplastic resin and the fibrous filler are mixed and kneaded in the extruder. Finally, the mixture is cooled and granulated. For example, a single screw extruder or a twin screw extruder (such as a co-rotating intermeshing type twin screw extruder) is used as the extruder. Compared with a single screw extruder, a twin screw extruder tends to have higher productivity and freedom of operation. Therefore, a twin screw extruder is more preferably used for producing pellets of a fiber-based filler reinforced thermoplastic resin composition.
[0004] The fiber-based filler used in the production of the fiber-based filler-reinforced thermoplastic resin composition pellets is, for example, a monofilament having a diameter of 6 to 20 μm, wound into a roving of about 300 to 3000 pieces, or a chopped strand obtained by cutting a roving into a length of 1 to 6 mm, etc. Since chopped strands are easier to use, in the case of industrially producing fiber-based filler-reinforced thermoplastic resin composition pellets, the most common method is to feed a thermoplastic resin to a twin-screw extruder, melt the thermoplastic resin, feed chopped strands from the middle of the twin-screw extruder, mix and knead the molten thermoplastic resin and the fiber-based filler, extrude the mixture, and cool and solidify it.
[0005] The productivity of the fiber-based filler-reinforced thermoplastic resin composition pellets produced using the above-mentioned twin-screw extruder is determined by the plasticizing and mixing / kneading capabilities of the twin-screw extruder. The plasticizing capability of the twin-screw extruder depends on the screw design, the torque generated by the screw, the groove depth of the screw (the difference between the outer diameter and the root diameter of the screw), the screw rotation speed, etc. Patent Document 1 defines the value obtained by dividing the center distance between the two screws by the cube as the torque density, and discloses a twin-screw extruder with high plasticizing capability and excellent productivity.
[0006] The mixing and kneading capacity of a twin-screw extruder also depends on the screw design. As the plasticizing capacity of twin-screw extruders has improved, the residence time has decreased. For this reason, there is a demand for the development of screw designs that have efficient mixing and kneading capacity in a short time. Thus, research is being conducted on technologies to improve the plasticizing and kneading capacity of twin-screw extruders.
[0007] Generally, as the fibrous filler, a bundle of monofilaments is used as described above. This is because, in a method of feeding the fibrous filler to a twin-screw extruder without bundling the monofilaments, the monofilaments tend to become cotton-like, lose fluidity, and become difficult to handle. The chopped strands are, for example, mixed and kneaded in a twin-screw extruder until they are defibrated and turned into monofilaments, and at the same time, the chopped strands are broken by a screw or the like until the length of the monofilaments becomes 200 to 500 μm on average.
[0008] If the mixing and kneading in the twin-screw extruder is insufficient, the chopped strands, which are not defibrated into monofilaments but are in the form of an aggregate of monofilaments (undefibrated fiber-based filler bundles), will remain in the resin composition pellets. If the chopped strands remain in the fiber-based filler-reinforced thermoplastic resin composition pellets, the chopped strands will clog the gate during injection molding, making injection molding impossible, or even if injection molding is possible, the chopped strands will be present in the molded product, which is likely to cause poor appearance or reduced function.
[0009] In particular, in recent years, with the advancement of electronics-related technologies, fiber-based filler reinforced thermoplastic resin compositions used as parts are required to be molded into thin, complex shapes. The gate nozzle of the molding machine used for such precision molding is often 1 mm or less. In precision molded products, the presence of unresolved fiber-based filler bundles is a very serious defect.
[0010] It is said that use of the twin-screw extruder of Patent Document 1 will improve productivity, but particularly in the case of precision molded products such as those described above, the residence time tends to become shorter under conditions of high output, making it more difficult to completely defibrate chopped strands into monofilaments and shorten the fiber length.
[0011] By combining a large number of kneading segments such as kneading disks, it is possible to some extent to increase the kneading intensity and open up the fiber bundle into monofilaments. On the other hand, increasing the kneading intensity tends to significantly shorten the fiber length and reduce the strength. Therefore, Patent Document 2 discloses a method in which a kneading segment having an arc with a predetermined radius of curvature at the top of the flight section is used to promote the reaction between the glass-based inorganic filler and the thermoplastic resin in the molding machine and improve the adhesion between the glass-based inorganic filler and the thermoplastic resin. Patent Document 3 discloses that the use of a single progressive screw element having a flight portion formed with an arc-shaped notch greatly reduces the probability that undefibrated glass fiber bundles remain. [Prior art documents] [Patent documents]
[0012] [Patent Document 1] Special Publication No. 11-512666 [Patent Document 2] JP 2012-140526 A [Patent Document 3] JP 2012-213996 A Summary of the Invention [Problem to be solved by the invention]
[0013] However, none of the above manufacturing methods is sufficient in terms of the balance between the remaining rate of unfibrillated fiber bundles, the remaining fiber length, and the improvement of productivity.
[0014] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a method for producing a resin composition capable of reducing the residual rate of undefibrated fiber bundles. [Means for solving the problem]
[0015] The present inventors have conducted extensive research and have completed the present invention.
[0016] That is, the present invention relates to the following. [1] A method for producing a resin composition, comprising melt-kneading a thermoplastic resin and a fibrous filler using a twin-screw kneading extruder, The twin-screw kneading extruder includes, in order from upstream in a flow direction of the material to be melt-kneaded, a first supply port, a first kneading zone, a second supply port, and a second kneading zone, The thermoplastic resin and the fibrous filler are supplied to the twin-screw kneading extruder through the first supply port and the second supply port, respectively; In the first kneading zone, 50 mass% or more of the thermoplastic resin supplied from the first supply port is melted, The second kneading zone (A) having a single flight and a resistance portion that generates a pressure of 2 MPa or more downstream of the single flight; (B) A double flight has a clearance between the cylinder and the double flight of 1.3% or more of the cylinder diameter, and a resistance portion that generates a pressure of 2 MPa or more downstream of the double flight. (C) having a single flight and a resistance portion that generates a pressure of 1 MPa or more at the downstream end of the single flight and at a position 1D upstream from the downstream end of the single flight; or (D) A method for producing a resin composition having a double flight with a clearance between the double flight and a cylinder of 1.3% or more of the cylinder diameter, and a resistance portion that generates a pressure of 1 MPa or more at a downstream end of the double flight and at a position 1D upstream from the downstream end of the single flight. [2] The method for producing a resin composition according to [1], wherein the clearance between the single flight or the double flight and the cylinder is 2.0% or more of the cylinder diameter. [3] The second kneading zone, (a) A single flight with a clearance between the cylinder and the single flight being 1.3% or more of the cylinder diameter, and a resistance portion that generates a pressure of 4 MPa or more downstream of the single flight. (b) A double flight has a clearance between the cylinder and the double flight of 1.3% or more of the cylinder diameter, and a resistance portion that generates a pressure of 4 MPa or more downstream of the double flight. (c) having a single flight and a resistance portion that generates a pressure of 2 MPa or more at the downstream end of the single flight and at a position 2D upstream from the downstream end of the single flight; or (d) A method for producing a resin composition according to [1], comprising: a double flight having a clearance between the double flight and a cylinder of 1.3% or more of a cylinder diameter; and a resistance portion that generates a pressure of 2 MPa or more at a downstream end of the double flight and at a position 2D upstream from the downstream end of the single flight. [4] The method for producing a resin composition according to any one of [1] to [3], wherein the length of the one flight or the two flights is 3D or more. [5] The method for producing a resin composition according to any one of claims [1] to [4], wherein the fibrous filler is a fiber bundle. [6] The method for producing a resin composition according to any one of [1] to [5], wherein the fibrous filler is glass fiber or carbon fiber. [7] The method for producing a resin composition according to any one of [1] to [6], wherein the thermoplastic resin comprises at least one selected from the group consisting of polypropylene, polyester, polyamide, polycarbonate, polystyrene, polyphenylene ether, ABS resin, AS resin, PPS resin, and liquid crystal polymer. [8] A resin composition obtained by the method for producing a resin composition according to any one of [1] to [7], wherein the thermoplastic resin comprises at least one selected from the group consisting of polypropylene, polyester, polyamide, polycarbonate, polystyrene, polyphenylene ether, ABS resin, AS resin, PPS resin, and liquid crystal polymer. Effect of the Invention
[0017] According to the present invention, there is provided a method for producing a resin composition capable of reducing the residual rate of undefibrated fiber bundles. [Brief description of the drawings]
[0018] [Figure 1] FIG. 1 is a schematic diagram illustrating an example of a twin-screw kneading extruder according to an embodiment of the present invention. [Diagram 2] FIG. 1 is a diagram illustrating the clearance between a single flight and a cylinder. [Diagram 3] FIG. 1 is a diagram explaining the clearance between a double flight and a cylinder. [Figure 4] FIG. 13 is a perspective view showing an example of a cutout segment. [Diagram 5] FIG. 13 is a diagram showing the resin pressure in Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] Hereinafter, several embodiments of the present invention will be described in detail. However, the present invention is not limited to the following embodiments.
[0020] The method for producing a resin composition according to the present embodiment is a method for producing a resin composition in which a thermoplastic resin and a fibrous filler are melt-kneaded using a twin-screw kneading extruder, the twin-screw kneading extruder is provided with, in order from the upstream side as viewed in the flow direction of the materials to be melt-kneaded, a first supply port, a first kneading zone, a second supply port, and a second kneading zone, the thermoplastic resin and the fibrous filler are supplied to the twin-screw kneading extruder from the first supply port and the second supply port, respectively, in the first kneading zone, 50 mass % or more of the thermoplastic resin supplied from the first supply port is melted, the second kneading zone is provided with: (A) a single flight and a pressure of 2 MPa downstream of the single flight; (B) having two flights with a clearance between the cylinder of 1.3% or more of the cylinder diameter and a resistance part downstream of the two flights that generates a pressure of 2 MPa or more; (C) having a single flight and a resistance part that generates a pressure of 1 MPa or more at the downstream end of the single flight and a position 1D upstream from the downstream end of the single flight; or (D) having two flights with a clearance between the cylinder of 1.3% or more of the cylinder diameter and a resistance part that generates a pressure of 1 MPa or more at the downstream end of the two flights and a position 1D upstream from the downstream end of the single flight. According to such a method, the remaining rate of unfibrillated fiber bundles can be reduced. This method is also excellent in productivity of the resin composition. Furthermore, according to this method, the remaining fiber length in the resin composition can be maintained long.
[0021] Single-row and double-row flights are generally used as conveying segments, and in the kneading zone of a twin-screw extruder, screw segments generally used as kneading segments, such as forward kneading disks, reverse kneading disks, neutral kneading, rotors, etc., are generally used in combination. In contrast, in the method according to the present embodiment, single-row and double-row flights are used in the second kneading zone. According to this method, dispersion and mixing of a fibrous filler can be achieved with excellent productivity.
[0022] D usually refers to the approximate value of the diameter of the cylinder. In other words, "a position 1D upstream from the downstream end of the single flight" means a position approximately "1 x D" upstream from the "downstream end of the single flight." In addition, the description "2D" below indicates a length "approximately twice D," and the description "3D" indicates a length "approximately three times D." The same applies to other similar descriptions such as "4D."
[0023] In this specification, 1D is defined as the range of -7.0% to +7.0% of the cylinder diameter. In other words, when the cylinder diameter is defined as D', 1D means "0.93×D' to 1.07×D'". Similarly, "2D" means "0.93×2×D' to 1.07×2×D'", and "3D" means "0.93×3×D' to 1.07×3×D'".
[0024] Fig. 1 is a schematic diagram showing an example of a twin-screw kneading extruder according to the present embodiment. This twin-screw kneading extruder includes a cylinder (not shown), a screw 2 disposed in the cylinder, and a die (not shown) provided at the downstream end of the cylinder. The twin-screw kneading extruder may be configured to include screws that rotate and mesh with each other. Examples of twin-screw kneading extruders include a co-rotating twin-screw kneading extruder and a co-meshing type twin-screw kneading extruder.
[0025] The twin-screw kneading extruder includes, in order from the upstream in the flow direction of the material to be melt-kneaded, a supply zone 20, a first kneading zone 21, a conveying zone 22, a second kneading zone 23, and a conveying zone 24. The supply zone 20 and the conveying zone 22 are provided with a first supply port 1a and a second supply port 1b, respectively, and the conveying zone 24 is provided with a vent port 5. That is, the twin-screw kneading extruder includes, in order from the upstream in the flow direction of the material to be melt-kneaded, a first supply port 1a, a first kneading zone 21, a second supply port 1b, and a second kneading zone 23. For example, a hopper (not shown) is connected to the first supply port 1a and the second supply port 1b.
[0026] The second kneading zone 23 has a mixing / dispersing section 23a on the upstream side and a resistance section 23b on the downstream side as viewed from the direction of flow of the melt-kneaded material. It is believed that the second kneading zone 23 has the resistance section 23b, which makes it easier for the mixture of the molten thermoplastic resin and the fibrous filler to fill the gap between the flight and the cylinder, improving the mixing effect. The resistance section is a region configured as a screw segment in which the pressure is highest at the upstream end of the resistance section 23b and decreases toward the downstream side, and the mixing / dispersing section 23a is a region in which the pressure decreases from the downstream end (upstream end of the resistance section 23b) toward the upstream side.
[0027] The screw elements used in the mixing and dispersing section 23a include, for example, conveying elements having forward flights. Specific examples of the screw elements include single- or double-flighted elements.
[0028] The mixing and dispersing section 23a is composed of one flight or two flights with a clearance between the cylinder of 1.3% or more of the cylinder diameter. The resistance section 23b is a resistance section that generates a pressure of 2 MPa or more. It is preferable that the resistance section 23b is a resistance section that generates a pressure of 4 MPa or more.
[0029] Fig. 2 is a diagram for explaining the clearance between a single flight and a cylinder, in which a indicates the clearance, b indicates the cylinder, c indicates the flight width, and dx indicates the cylinder diameter.
[0030] When a single flight is used, the flight width is preferably 20% or more of the flight lead length, and more preferably about 30%. By widening the flight width, it tends to be easier to obtain the effect of dispersion and mixing in the gap between the screw and the flight.
[0031] Fig. 3 is a diagram for explaining the clearance between the two flights and the cylinder. In Fig. 3, a indicates the clearance, b indicates the cylinder, and dx indicates the cylinder diameter. That is, when the mixing and dispersing section 23a is composed of two flights, a shown in Fig. 3 is 1.3% or more of the cylinder diameter dx.
[0032] When using double flights, it is usually difficult to widen the flight width, but it is preferable to widen the clearance between the flight and the cylinder. This increases the passage rate through the gap between the flight and the cylinder, which tends to make it easier to achieve dispersion and mixing effects. The clearance between the flight and the cylinder may be, for example, 2% or more of the cylinder diameter. The clearance between the flight and the cylinder may be, for example, less than 10% of the cylinder diameter, from the viewpoint of maintaining a relatively high shear rate in the clearance area.
[0033] The length of the single flight or the double flight constituting the mixed dispersion section 23a may be, for example, 2D or more, or 3D or more, from the viewpoint of providing a sufficient area filled with the mixture of fibrous filler and thermoplastic resin.
[0034] The resistance portion 23b may be, for example, a screw element such as a reverse flight, a seal ring, a neutral kneading disk, a reverse kneading disk, a notched segment (a flight or ring with a notch), or a combination of these. From the viewpoint of facilitating the filling of the mixture of the molten thermoplastic resin and the fiber-based filler, the resistance portion 23b may be formed, for example, by adjusting the combination and length of the screw elements so that the conveying force to the downstream side is lower than the discharge amount under the operating conditions of the twin-screw kneading extruder.
[0035] The resistor portion 23b preferably includes a cutout segment. The cutout segment is a segment having a cutout portion. An example of a cutout segment is shown in Fig. 4. The cutout segment 10 shown in Fig. 4 is a cutout segment having a plurality of cutout portions.
[0036] The method for producing a resin composition using the twin-screw kneading extruder is described below. In this method, a thermoplastic resin and a fiber-based filler are melt-kneaded using the twin-screw kneading extruder to produce a resin composition. The obtained resin composition is, for example, a fiber-based filler reinforced thermoplastic resin composition pellet.
[0037] First, a thermoplastic resin is supplied from a first supply port 1a to a supply zone 20. The thermoplastic resin supplied from the first supply port 1a to the supply zone 20 is transported to a first kneading zone 21. In the first kneading zone 21, 50 mass% or more of the thermoplastic resin supplied from the first supply port 1a is melted. The thermoplastic resin leaving the first kneading zone 21 is transported to a conveying zone 22, where it merges with a fibrous filler.
[0038] The fibrous filler is fed from the feed port 1b into the conveying zone 22, where it merges with the thermoplastic resin.
[0039] The thermoplastic resin and the fibrous filler leaving the conveying zone 22 are kneaded in the second kneading zone 23. This causes the fibrous filler to be dispersed in the thermoplastic resin. The above-mentioned resistance portion is formed in the second kneading zone 23.
[0040] The thermoplastic resin and fibrous filler leaving the second kneading zone 23 pass through the conveying zone 24 and are discharged from the die to the outside of the twin-screw kneading extruder. This allows a fiber-filler reinforced thermoplastic resin composition to be obtained. The obtained fiber-filler reinforced thermoplastic resin composition may be pelletized as necessary.
[0041] The manufacturing method of this embodiment may include, for example, a plasticization step in which a thermoplastic resin is supplied to the extruder and plasticized by heating and kneading; a kneading / dispersing step in which, after the plasticization step, one or more bundles of fibrous filler are supplied to the extruder and the defibrated fibrous filler and the plasticized thermoplastic resin are kneaded with a screw while defibrating the fibrous filler bundles; a devolatilization step in which volatile matters are removed as necessary; an extrusion step in which the mixture obtained in the mixing / dispersing step is extruded from a die to the outside of the twin-screw kneading extruder; and a pelletization step in which the mixture extruded from the die is pelletized.
[0042] [Plasticization process] The plasticization step is carried out, for example, in the feed zone 20 and in the first kneading zone 21 .
[0043] In the plasticizing step, the thermoplastic resin (for example, resin pellets) supplied from the supply port 1a is transported and melted.
[0044] Examples of the screw elements used in the supply zone 20 include conveying elements consisting of flights. Examples of the screw elements used in the first kneading zone 21 include screw elements such as reverse flights, seal rings, forward kneading discs, reverse kneading discs, and combinations thereof.
[0045] For example, resin pellets are transported in the supply zone 20. The supply zone 20 functions to transport the resin pellets from the supply port 1a side toward the die.
[0046] As a preparation for plasticization, preheating may be performed using an external heater.
[0047] Since the thermoplastic resin is sandwiched between the rotating screw 2 and the cylinder, frictional force is applied to the thermoplastic resin, generating frictional heat. The preheating and frictional heat may cause the thermoplastic resin to start to melt. In some cases, the groove depth of the screw 2 and the preheating temperature may be adjusted by a conventionally known method in the supply zone 20 so that the transfer of the thermoplastic resin proceeds smoothly.
[0048] In the first kneading zone 21, pressure is applied to the thermoplastic resin transferred from the supply zone 20 to melt the thermoplastic resin. In the first kneading zone 21, a shear stress is applied to the thermoplastic resin, so that the thermoplastic resin is transferred further forward (toward the conveying zone 22) while being melted.
[0049] As described above, 50% by mass or more of the thermoplastic resin is melted in the first kneading zone 21. This tends to reduce breakage of the fibrous filler. It is believed that the breakage of the fibrous filler is reduced by reducing the resin viscosity in the first kneading zone 21.
[0050] The first kneading zone 21 may be provided with an open vent or a vacuum vent for removing excess volatile components after the thermoplastic resin is plasticized and melted.
[0051] The thermoplastic resin (melt) melted in the plasticizing step is joined with the fibrous filler in the conveying zone 22, and then subjected to a kneading and dispersing step in the second kneading zone 23. The fibrous filler is supplied to the extruder from the second supply port 1b. The number of fibrous fillers supplied to the extruder is, for example, one or more bundles.
[0052] [Mixing and dispersing process] In the kneading and dispersion step, the fibrous filler is kneaded with the molten thermoplastic resin, whereby the fiber bundles of the fibrous filler are defibrated and dispersed in the thermoplastic resin.
[0053] The kneading and dispersing step is carried out in the mixing and dispersing section 23a of the second kneading zone 23 and in the resistance section 23b downstream thereof.
[0054] [Post-process] After the kneading and dispersing step, an open vent or a vacuum vent may be provided to remove volatile matters contained in the raw resin, decomposition products of the surface treatment agent of the fibrous filler, and reaction residues of the sizing agent. From the viewpoint of suppressing oxidation and deterioration of the resin, it is preferable to provide a vacuum vent.
[0055] There are no limitations on the fibrous filler and thermoplastic resin used in the method according to this embodiment, but specific examples are shown below.
[0056] [Fiber-based filler] The fibrous filler is, for example, a fiber bundle in which a plurality of monofilaments are bound by a binder or the like. The fiber bundle bound by a binder or the like has excellent handleability during kneading. The number of monofilaments constituting the fiber bundle is not particularly limited, and may be, for example, 300 to 3000, or 1100 to 2200. The fibrous filler may be, for example, a bundle of monofilaments continuously fed to a twin-screw kneading extruder as a roving, or may be fed to a twin-screw kneading extruder in the form of chopped strands obtained by cutting the roving. Chopped strands are preferable as the fibrous filler from the viewpoints of transport and handleability.
[0057] Examples of fibrous fillers include glass fiber, carbon fiber, aramid fiber, and basalt fiber. One type of fibrous filler may be used alone, or two or more types may be used in combination.
[0058] (Glass fiber) The fiber diameter of the monofilaments forming the glass fiber bundle is not particularly limited, but is preferably in the range of, for example, 6 to 20 μm, and those with diameters of 6 μm, 10 μm, and 13 μm are widely distributed on the market.
[0059] The fiber diameter can be determined, for example, by cutting the fibers perpendicular to the fiber direction, measuring the diameters of the cross sections by observing them under a microscope, and calculating the number average of the diameters of 100 or more fibers.
[0060] (Carbon Fiber) The type of carbon fiber is not particularly limited, but examples thereof include PAN (polyacrylonitrile)-based carbon fiber made mainly of acrylonitrile, pitch-based carbon fiber made mainly of tar pitch, and rayon-based carbon fiber. For example, PAN-based carbon fiber is preferred from the viewpoint of composition purity and uniformity. The method for producing carbon fiber is not particularly limited.
[0061] The fiber diameter of the monofilament forming the carbon fiber bundle may be, for example, more than 2 μm and not more than 15 μm, may be 3 to 12 μm, or may be 4 to 10 μm. If the fiber diameter is 2 μm or less, the rigidity of the fiber tends to decrease. If the fiber diameter exceeds 15 μm, the aspect ratio of the fiber (the ratio of length (L) to thickness (D): L / D) decreases, and the rigidity, heat resistance, etc. may decrease.
[0062] As the PAN-based carbon fiber, for example, "Pyrofil" (trade name) manufactured by Mitsubishi Rayon Co., Ltd., "Torayca" (trade name) manufactured by Toray Industries, Inc., or "Besfight" (trade name) manufactured by Toho Tenax Co., Ltd. can be used.
[0063] As the pitch-based carbon fiber, for example, "Dialead" (trade name) manufactured by Mitsubishi Plastics, Inc., "DonaCarbo" (trade name) manufactured by Osaka Gas Chemicals Co., Ltd., or "Kureka" (trade name) manufactured by Kureha Chemical Industry Co., Ltd. can be used.
[0064] (aramid fiber) The aramid constituting the aramid fiber is preferably a meta-aramid, a para-aramid or a copolymerized para-aramid, more preferably a para-aramid or a copolymerized para-aramid, and further preferably a copolymerized para-aramid. Here, the para-aramid refers to an aramid having a structure in which each benzene ring is linearly linked through an amide group (CONH).
[0065] Specific examples of aramid fibers include meta-aramid fibers such as NOMEX (trade name) of DuPont, TEIJINCONEX (trade name) of Teijin Limited, Japan, METASTAR (trade name) of Yantai Limited, China, and X-FIPER (trade name) of SRO Group, China, as well as TWARON (trade name) of Teijin Limited, KEVLAR (trade name) of DuPont, KERMEL TECH (trade name) of Kermel, HERACRON (trade name) of Kolon Industries, etc.
[0066] The fiber diameter of the monofilaments forming the fiber bundle of the aramid fibers may be, for example, 1 to 50 μm, 3 to 30 μm, or 5 to 15 μm, from the viewpoint of increasing the bending strength and impact resistance of the resulting resin composition.
[0067] (Basalt fiber) Basalt fiber is made by melting the mineral basalt in a melting furnace, spinning it into fibers, and is usually composed only of basalt. Basalt fiber usually contains 55-65% by mass of silicon oxide (SiO2), 15-20% by mass of aluminum oxide (Al2O3), and iron oxides (FeO, Fe2O3), etc. As recrystallization occurs during melt spinning, it tends to have a more homogeneous crystal structure than other rock wools.
[0068] The fiber diameter of the monofilaments forming the fiber bundle of the basalt fibers may be, for example, 2 to 15 μm, 6 to 13 μm, or 9 to 13 μm.
[0069] The fibrous filler is preferably glass fiber or carbon fiber.
[0070] In order to improve dispersibility, the fibrous filler may be surface-treated with a surface treatment agent such as an organic silane coupling agent, a titanate coupling agent, an aluminate coupling agent, a zirconate coupling agent, a silicone compound, a higher fatty acid, a fatty acid metal salt, or a fatty acid ester.
[0071] There are no limitations on the binder for bundling the fibrous filler, but for example, when the fibrous filler is an organic fiber, a polar resin or the like is preferably used.
[0072] Examples of polar resins include thermosetting resins such as unsaturated polyesters, vinyl ester resins, epoxy resins, phenolic (e.g., resol type) resins, urea-melamine resins, polyimides, urethane resins, copolymers and modified products thereof; and thermoplastic resins such as saturated polyesters, polyamides, acrylic resins, copolymers and modified products thereof, and acid-modified polyolefins.
[0073] [Thermoplastic resin] Examples of the thermoplastic resin include polycarbonate, polybutylene terephthalate, polyethylene terephthalate, polyethylene naphthalate, various polyamides (PA6, PA66, PA46, PA12, semi-aromatic PA, etc.), acrylonitrile-butadiene-styrene (ABS) resin, acrylonitrile-styrene (AS) resin, methyl methacrylate-styrene (MS) resin, polyethylene, polypropylene, polyacetal, polyamideimide, polyethersulfone, polyimide, polyphenylene oxide, polyphenylene sulfide (PPS resin), polyphenylsulfone, polyetheretherketone, polystyrene, syndiotactic polystyrene, liquid crystal polyester (liquid crystal polymer), thermoplastic polyurethane, polyvinyl chloride, fluororesin, and mixtures thereof. These may be used alone or in combination of two or more. The thermoplastic resin may be appropriately selected from the properties such as heat resistance, chemical resistance, and moldability required depending on the purpose of use.
[0074] The thermoplastic resin preferably contains at least one selected from the group consisting of polypropylene, polyester, polyamide, polycarbonate, polystyrene, polyphenylene ether, ABS resin, AS resin, PPS resin, and liquid crystal polymer.
[0075] Although an example of the method for producing the resin composition according to the present embodiment has been described above, the method is not limited to this.
[0076] For example, in the above description, the second kneading zone 23 has (A) a single flight and a resistance part that generates a pressure of 2 MPa or more downstream of the single flight, or (B) a double flight with a clearance between the cylinder and the double flight of 1.3% or more of the cylinder diameter and a resistance part that generates a pressure of 2 MPa or more downstream of the double flight, but the second kneading zone 23 may be replaced with one having (C) a single flight and a resistance part that generates a pressure of 1 MPa or more at the downstream end of the single flight and at a position 1D upstream from the downstream end of the single flight. In this case, it is more preferable that the second kneading zone 23 has (c) a single flight and a resistance part that generates a pressure of 2 MPa or more at the downstream end of the single flight and at a position 2D upstream from the downstream end of the single flight.
[0077] Similarly, the second kneading zone 23 may be replaced with one having (D) two flights whose clearance with the cylinder is 1.3% or more of the cylinder diameter, and a resistance part that generates a pressure of 1 MPa or more at a position 1D upstream from the downstream end of the two flights and the downstream end of the single flight. In this case, it is more preferable that the second kneading zone 23 has (d) two flights whose clearance with the cylinder is 1.3% or more of the cylinder diameter, and a resistance part that generates a pressure of 2 MPa or more at a position 2D upstream from the downstream end of the two flights and the downstream end of the single flight.
[0078] Also, the vent may or may not be provided.
[0079] The method for producing a resin composition described above is a method for producing a resin composition in which a thermoplastic resin and a fibrous filler are melt-kneaded using a twin-screw kneading extruder, the twin-screw kneading extruder is provided with, in order from upstream as viewed in a flow direction of the materials to be melt-kneaded, a first supply port, a first kneading zone, a second supply port, and a second kneading zone, the thermoplastic resin and the fibrous filler are supplied to the twin-screw kneading extruder from the first supply port and the second supply port, respectively, in the first kneading zone, 50 mass % or more of the thermoplastic resin supplied from the first supply port is melted, the second kneading zone is provided with: (A) a single flight and a pressure of 2 MPa downstream of the single flight; (B) having two flights whose clearance with the cylinder is 1.3% or more of the cylinder diameter and a resistance part that generates a pressure of 2 MPa or more downstream of the two flights, (C) having a single flight and a resistance part that generates a pressure of 1 MPa or more at the downstream end of the single flight and a position 1D upstream from the downstream end of the single flight, or (D) having two flights whose clearance with the cylinder is 1.3% or more of the cylinder diameter and a resistance part that generates a pressure of 1 MPa or more at the downstream end of the two flights and a position 1D upstream from the downstream end of the single flight. According to this method, the remaining rate of undefibrated fiber bundles can be reduced.
[0080] In the above method, the clearance between the single-start flight or the double-start flight and the cylinder may be 2.0% or more of the cylinder diameter.
[0081] In the above method, the second kneading zone may have (a) a single flight having a clearance between the cylinder of 1.3% or more of the cylinder diameter and a resistance portion that generates a pressure of 4 MPa or more downstream of the single flight, (b) a double flight having a clearance between the cylinder of 1.3% or more of the cylinder diameter and a resistance portion that generates a pressure of 4 MPa or more downstream of the double flight, (c) a single flight and a resistance portion that generates a pressure of 2 MPa or more at the downstream end of the single flight and at a position 2D upstream from the downstream end of the single flight, or (d) a double flight having a clearance between the cylinder of 1.3% or more of the cylinder diameter and a resistance portion that generates a pressure of 2 MPa or more at the downstream end of the double flight and at a position 2D upstream from the downstream end of the single flight.
[0082] In the above method, the length of the one-flight or the two-flight may be 3D or more.
[0083] [Resin composition] According to the method for producing a resin composition according to the present embodiment, a resin composition with a reduced residual rate of unfibrillated fiber bundles can be obtained. The resin composition (fiber-based filler reinforced thermoplastic resin composition) obtained by this method has improved mechanical strength due to the fiber-based filler while maintaining the inherent performance of the thermoplastic resin composition. The resin composition can be subjected to various molding methods such as injection molding, extrusion molding, compression molding, blow molding, and injection compression molding. Among them, it is suitable for use in injection molding. The resin composition is suitable for use in, for example, plastic parts that require mechanical strength. The resin composition is particularly suitable for use in automobile parts, building materials, electrical product parts, and the like. EXAMPLES
[0084] The present invention will be described below with reference to examples and comparative examples, but the present invention is not limited to these examples.
[0085] (material) The materials used in the examples and comparative examples are shown below.
[0086] [Thermoplastic resin] AS resin: Cevian N050SF (melt index (MI) 32g / 10min) manufactured by Daicel Miraize Co., Ltd. PA6 resin: Unitika A1020BRL (melt index (MI) 34g / 10min) PP resin: Sumitomo Chemical's Noblen R101 (melt index (MI) 20g / 10min) with 1.5% maleic anhydride modified PP added.
[0087] [Glass fiber bundle] GF(1): Nippon Electronic Glass Co., Ltd. ECS03 T-351 (chopped strands of 3 mm length bundled monofilaments with a diameter of 13 μm) GF(2): Nippon Electronic Glass Co., Ltd. ECS03 T-249H (chopped strands of 3 mm length bundled monofilaments with a diameter of 10.5 μm) GF(3): Nippon Electronic Glass Co., Ltd. ECS03 T-480H (chopped strands of 3 mm length bundled monofilaments with a diameter of 10.5 μm)
[0088] The materials were used so that the resin composition contained 70% by weight of thermoplastic resin and 30% by weight of glass fiber bundles.
[0089] (Extruder configuration and conditions) A twin-screw kneading extruder was used, which was equipped with a first feed port, a first kneading zone, a second feed port, and a second kneading zone in that order from the upstream side in the flow direction of the melt-kneaded material. The thermoplastic resin and the fibrous filler were fed into the twin-screw kneading extruder from the first feed port and the second feed port, respectively, and 50% by mass or more of the thermoplastic resin fed from the first feed port was melted in the first kneading zone. The configuration and conditions of the extruder used are shown below. Extruder: Co-rotating twin screw extruder TEM-26SX (manufactured by Shibaura Machine Co., Ltd.) Cylinder diameter: 26.6mm Extrusion conditions: Cylinder temperature 250℃, extrusion rate 100kg / hour Pressure sensors were installed at the upstream end of the resistor (i.e., the downstream end of the flight), as well as at positions 65.0 mm upstream (equivalent to 2.40 D upstream) and 105.0 mm upstream (equivalent to 4.00 D upstream) from the upstream end of the resistor (i.e., the downstream end of the flight).
[0090] [Screw segment] (1) Screw segment used in the resistance section Notched segment: A screw segment consisting of a ring with 12 notches on the circumference, which is combined into 4 pairs of 1D segments, alternating left and right.
[0091] (2) Screw segment used in the mixing and dispersion section Two-row flight a: A two-row flight with a lead length of 1D and a clearance with the cylinder of 0.66% of the cylinder diameter. Double flight b: A double flight with a lead length of 1D and a clearance to the cylinder of 1.62% of the cylinder diameter. Double flight c: A double flight with a lead length of 1D and a clearance to the cylinder of 3.25% of the cylinder diameter. Single flight a: A single flight with a lead length of 1D, a clearance with the cylinder of 0.66% of the cylinder diameter, and a flight width of 30% of the cylinder diameter. Single flight b: A single flight with a lead length of 1D, a clearance with the cylinder of 3.25% of the cylinder diameter, and a flight width of 33% of the cylinder diameter. Single flight c: A single flight with a lead length of 1D, a clearance with the cylinder of 0.66% of the cylinder diameter, and a flight width of 23% of the cylinder diameter. Forward kneading discs: Seven discs are arranged in 1D, shifted by 30° in the same direction as the screw rotation.
[0092] [Examples 1 to 7 and Comparative Examples 1 to 3] 70% by weight of AS resin and 30% by weight of GF (ECS03 T-351) were melt-kneaded using a co-rotating twin-screw kneading extruder TEM-26SX to obtain a resin composition. The screw configurations of the resistance section and the mixing and dispersing section of the twin-screw kneading extruder, as well as the screw rotation speed, are shown in Table 1. Table 2 also shows the resin pressure at the upstream end of the resistance section (i.e., the downstream end of the flight), and the resin pressure at positions 65.0 mm upstream (corresponding to 2.40D upstream) and 105.0 mm upstream (corresponding to 4.00D upstream) from the upstream end of the resistance section (i.e., the downstream end of the flight).
[0093] (Evaluation of Resin Composition) The resulting resin compositions were evaluated according to the following procedures.
[0094] The obtained thermoplastic resin composition was dried at 120°C for 4 hours, and then molded into test pieces using an injection molding machine (Shibaura Machine IS80EPN-2A) at a cylinder temperature of 240°C and a mold temperature of 60°C.
[0095] [Number of unresolved fibers] Thirty test pieces were visually observed and the number of unresolved fibers was counted.
[0096] [Flexural modulus] The flexural modulus of the test specimen was measured using an A&D Tensilon universal testing machine RTC-1310A.
[0097] The number of unresolved fibers and the flexural modulus of the test specimens are shown in Table 2. [Table 1]
[0098] In the table, the description "notch: 2D" indicates that the notch segment has a length of 2D. The same applies to similar descriptions such as "2-row flight a: 4D."
[0099] [Table 2]
[0100] For Example 3, the resin pressure at the upstream end of the resistance section (i.e., the downstream end of the mixing / dispersing section) and the resin pressure at positions 65.0 mm upstream (corresponding to 2.40 D upstream) and 105.0 mm upstream (corresponding to 4.00 D upstream) from the upstream end of the resistance section (i.e., the downstream end of the mixing / dispersing section) are shown in Figure 5. As is clear from Figure 5, in Example 3, the pressure is highest at the upstream end of the resistance section and decreases toward the downstream, and the mixing / dispersing section has a region configured with screw segments where the pressure decreases from the downstream end (upstream end of the resistance section) toward the upstream side.
[0101] [Examples 8 to 10] A resin composition was obtained by melt-kneading 70% by weight of PA6 resin and 30% by weight of GF (ECS03 T-249H) using a co-rotating twin-screw kneading extruder TEM-26SX. The screw configurations of the resistance section and the mixing and dispersing section of the twin-screw kneading extruder and the screw rotation speed are shown in Table 3. Table 4 also shows the resin pressure at the upstream end of the resistance section (i.e., the downstream end of the flight), and the resin pressure at positions 65.0 mm upstream (corresponding to 2.40D upstream) and 105.0 mm upstream (corresponding to 4.00D upstream) from the upstream end of the resistance section (i.e., the downstream end of the flight).
[0102] (Evaluation of Resin Composition) The resulting resin compositions were evaluated according to the following procedures.
[0103] The obtained thermoplastic resin composition was vacuum dried at 80°C for 24 hours, and then molded into test pieces using an injection molding machine (Shibaura Machine IS80EPN-2A) at a cylinder temperature of 240°C and a mold temperature of 60°C.
[0104] [Number of unresolved fibers] Thirty test pieces were visually observed and the number of unresolved fibers was counted.
[0105] [Flexural modulus] The flexural modulus of the test specimen was measured using an A&D Tensilon universal testing machine RTC-1310A.
[0106] The number of unresolved fibers in the test specimens and the flexural modulus are shown in Table 4.
[0107] [Table 3]
[0108] [Table 4]
[0109] [Examples 11 to 13 and Comparative Example 4] 70% by weight of PP resin and 30% by weight of GF (ECS03 T-480H) were melt-kneaded using a co-rotating twin-screw kneading extruder TEM-26SX to obtain a resin composition. The screw configurations of the resistance section and the mixing and dispersing section of the twin-screw kneading extruder and the screw rotation speed are shown in Table 5. Table 6 also shows the resin pressure at the upstream end of the resistance section (i.e., the downstream end of the flight), and the resin pressure at positions 65.0 mm upstream (corresponding to 2.40D upstream) and 105.0 mm upstream (corresponding to 4.00D upstream) from the upstream end of the resistance section (i.e., the downstream end of the flight).
[0110] (Evaluation of Resin Composition) The resulting resin compositions were evaluated according to the following procedures.
[0111] The obtained thermoplastic resin composition was dried at 120°C for 4 hours, and then molded into test pieces using an injection molding machine (Shibaura Machine IS80EPN-2A) at a cylinder temperature of 240°C and a mold temperature of 60°C.
[0112] [Number of unresolved fibers] Thirty test pieces were visually observed and the number of unresolved fibers was counted.
[0113] [Flexural modulus] The flexural modulus of the test specimen was measured using an A&D Tensilon universal testing machine RTC-1310A.
[0114] The number of unresolved fibers and the flexural modulus of the test specimens are shown in Table 6.
[0115] [Table 5]
[0116] [Table 6]
[0117] It is understood that the method according to the example can reduce the residual rate of unfibrillated fiber bundles compared to the method according to the comparative example. In other words, it is understood that the method according to the example can produce a resin composition having a low residual rate of unfibrillated fiber bundles. [Explanation of symbols]
[0118] 1a, 1b...feed port, 5...vent port, 10...notched segment, 20...feed zone, 21...first kneading zone, 22, 24...conveying zone, 23...second kneading zone, 23b...resistance section, 23a...mixing and dispersion section.
Claims
1. A method for producing a resin composition, comprising melt-kneading a thermoplastic resin and a fibrous filler using a twin-screw kneading extruder, The twin-screw kneading extruder includes, in order from upstream in a flow direction of the material to be melt-kneaded, a first supply port, a first kneading zone, a second supply port, and a second kneading zone, The thermoplastic resin and the fibrous filler are supplied to the twin-screw kneading extruder through the first supply port and the second supply port, respectively; In the first kneading zone, 50 mass% or more of the thermoplastic resin supplied from the first supply port is melted, The second kneading zone (A) having a single flight and a resistance portion that generates a pressure of 2 MPa or more downstream of the single flight; (B) A double flight having a clearance between the cylinder and the double flight of 1.3% or more of the cylinder diameter, and a resistance portion that generates a pressure of 2 MPa or more downstream of the double flight. (C) having a single flight and a resistance portion that generates a pressure of 1 MPa or more at a downstream end of the single flight and at a position 1D upstream from the downstream end of the single flight, or (D) A method for producing a resin composition having a double flight in which the clearance between the double flight and a cylinder is 1.3% or more of the cylinder diameter, and a resistance portion that generates a pressure of 1 MPa or more at a downstream end of the double flight and at a position 1D upstream from the downstream end of the single flight.
2. The method for producing a resin composition according to claim 1 , wherein a clearance between the single-row flight or the double-row flight and a cylinder is 2.0% or more of a cylinder diameter.
3. The second kneading zone (a) having a single flight with a clearance between the cylinder and the single flight being 1.3% or more of the cylinder diameter, and a resistance portion that generates a pressure of 4 MPa or more downstream of the single flight; (b) having a double flight with a clearance between the cylinder and the double flight being 1.3% or more of the cylinder diameter, and a resistance portion that generates a pressure of 4 MPa or more downstream of the double flight; (c) having a single flight and a resistance portion that generates a pressure of 2 MPa or more at a downstream end of the single flight and at a position 2D upstream from the downstream end of the single flight; or (d) a double flight having a clearance between the double flight and a cylinder of 1.3% or more of a cylinder diameter, and a resistance portion that generates a pressure of 2 MPa or more at a downstream end of the double flight and at a position 2D upstream from the downstream end of the single flight. The method for producing a resin composition according to claim 1,
4. The method for producing a resin composition according to any one of claims 1 to 3, wherein the length of the one flight or the two flights is 3D or more.
5. The method for producing a resin composition according to any one of claims 1 to 3, wherein the fibrous filler is a fiber bundle.
6. The method for producing a resin composition according to any one of claims 1 to 3, wherein the fibrous filler is glass fiber or carbon fiber.
7. The thermoplastic resin comprises at least one selected from the group consisting of polypropylene, polyester, polyamide, polycarbonate, polystyrene, polyphenylene ether, ABS resin, AS resin, PPS resin and liquid crystal polymer. The method for producing a resin composition according to any one of claims 1 to 3.
8. A resin composition obtained by the method for producing a resin composition according to any one of claims 1 to 3, wherein the thermoplastic resin comprises at least one selected from the group consisting of polypropylene, polyester, polyamide, polycarbonate, polystyrene, polyphenylene ether, ABS resin, AS resin, PPS resin, and liquid crystal polymer.
Citation Information
Patent Citations
Method of continuous preparation process execution in co-rotating tightly meshing extruders
JP1999512666A
Method for producing thermoplastic resin composition
JP2012140526A
Process for producing pellets of glass-fiber-reinforced thermoplastic resin composition
JP2012213996A