Silicon carbide semiconductor device and method for manufacturing silicon carbide semiconductor device
A silicon carbide semiconductor device with a phosphorus delta-doped interlayer insulating film addresses the challenge of capturing metal impurities, enhancing adhesion and reducing threshold voltage fluctuations by using ion implantation and low-pressure CVD to form a dense film structure.
Patent Information
- Application Number
- JP2023078589
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-11
- Publication Date
- 2024-11-21
AI Technical Summary
Existing silicon carbide semiconductor devices face challenges in efficiently capturing metal impurities, particularly sodium, due to irregularities formed on the surface when high concentrations of phosphorus atoms are included in the PSG film, which affects the adhesion and integrity of the interlayer insulating film.
Incorporating a phosphorus delta-doped layer in the interlayer insulating film, formed through ion implantation and low-pressure CVD at high temperatures, to create a dense film structure that efficiently captures metal impurities and improves adhesion with the barrier metal film.
The solution effectively reduces fluctuations in threshold voltage and prevents cracks in the interlayer insulating film by enhancing the capture of metal impurities like sodium, thereby improving the film's adhesion and structural integrity.
Smart Images

Figure 2024162734000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to silicon carbide semiconductor devices and methods of manufacturing silicon carbide semiconductor devices. [Background technology]
[0002] 2. Description of the Related Art Silicon carbide semiconductor devices are known that have an interlayer insulating film including a phosphorus silicate glass (PSG) film. The PSG film is formed by, for example, atmospheric pressure chemical vapor deposition (CVD) method. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2016-86064 A [Patent Document 2] JP 2018-82054 A Summary of the Invention [Problem to be solved by the invention]
[0004] When forming a PSG film using atmospheric pressure CVD, if a high concentration of phosphorus atoms is included, unevenness is likely to form on the surface. Therefore, it is difficult to include a high concentration of phosphorus atoms in the PSG film. If the concentration of phosphorus atoms in the PSG film is low, it is difficult to efficiently capture metal impurities such as sodium.
[0005] An object of the present disclosure is to provide a silicon carbide semiconductor device having an interlayer insulating film capable of efficiently capturing metal impurities, and a method for manufacturing the silicon carbide semiconductor device. [Means for solving the problem]
[0006] A silicon carbide semiconductor device of the present disclosure comprises a silicon carbide substrate having a first main surface, a gate insulating film provided on the first main surface of the silicon carbide substrate, a gate electrode provided on the gate insulating film, and an interlayer insulating film provided to cover the gate electrode, wherein the interlayer insulating film includes a phosphorus delta-doped layer. Effect of the Invention
[0007] Advantageous Effects of Invention According to the present disclosure, it is possible to provide a silicon carbide semiconductor device having an interlayer insulating film capable of efficiently capturing metal impurities, and a method for manufacturing a silicon carbide semiconductor device. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a cross-sectional view showing a silicon carbide semiconductor device according to an embodiment. [Diagram 2] FIG. 2 is a cross-sectional view showing an interlayer insulating film. [Diagram 3] FIG. 3 is a diagram showing the phosphorus concentration distribution in the depth direction of the interlayer insulating film. [Figure 4] 4A to 4C are cross-sectional views (part 1) illustrating the method for manufacturing a silicon carbide semiconductor device according to the embodiment. [Diagram 5] FIG. 5 is a cross-sectional view (part 2) illustrating the method for manufacturing a silicon carbide semiconductor device according to the embodiment. [Figure 6] 6A to 6C are cross-sectional views (part 3) illustrating the method for manufacturing a silicon carbide semiconductor device according to the embodiment. [Figure 7] 7A to 7C are cross-sectional views (part 4) illustrating the method for manufacturing a silicon carbide semiconductor device according to the embodiment. [Figure 8] 8A to 8C are cross-sectional views (part 5) illustrating the method for manufacturing a silicon carbide semiconductor device according to the embodiment. [Figure 9] FIG. 9 is a cross-sectional view (part 6) illustrating the method for manufacturing a silicon carbide semiconductor device according to the embodiment. [Figure 10] FIG. 10 is a cross-sectional view (part 7) illustrating the method for manufacturing a silicon carbide semiconductor device according to the embodiment. [Figure 11]FIG. 11 is a cross-sectional view (part 8) illustrating the method for manufacturing a silicon carbide semiconductor device according to the embodiment. [Figure 12] FIG. 12 is a ninth cross-sectional view illustrating the method for manufacturing a silicon carbide semiconductor device according to the embodiment. [Figure 13] FIG. 13 is a cross-sectional view (part 10) illustrating the method for manufacturing a silicon carbide semiconductor device according to the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The embodiments for carrying out the invention are described below.
[0010] [Description of the embodiments of the present disclosure] First, the embodiments of the present disclosure will be described. In the following description, the same or corresponding elements are denoted by the same reference numerals, and the same description thereof will not be repeated.
[0011] [1] A silicon carbide semiconductor device according to one embodiment of the present disclosure includes a silicon carbide substrate having a first main surface, a gate insulating film provided on the first main surface of the silicon carbide substrate, a gate electrode provided on the gate insulating film, and an interlayer insulating film provided to cover the gate electrode, the interlayer insulating film including a delta-doped layer of phosphorus (P). In this case, metal impurities such as sodium can be efficiently captured and prevented from penetrating into the gate insulating film. Therefore, the fluctuation of the threshold voltage can be reduced.
[0012] [2] In the above [1], the peak concentration of phosphorus atoms in the delta doped layer is 5×10 16 cm -3 More than 1×10 19 cm -3 It may be less than 5×10 16 cm -3 If the concentration is more than 1×10, metal impurities such as sodium are easily captured by the interlayer insulating film. 19 cm -3If the thickness is less than 100 nm, unevenness is unlikely to form on the surface of the interlayer insulating film, which improves adhesion between the interlayer insulating film and the barrier metal film and makes it difficult for cracks to occur in the interlayer insulating film in subsequent processes.
[0013] [3] In [1] or [2], the thickness of the delta doped layer may be 0.05 μm or more and 0.3 μm or less. If the thickness is 0.05 μm or more, metal impurities such as sodium are easily captured by the interlayer insulating film. If the thickness is 0.3 μm or less, irregularities are not easily formed on the surface of the interlayer insulating film. Therefore, the adhesion between the interlayer insulating film and the barrier metal film is improved, and cracks are not easily generated in the interlayer insulating film in a later process.
[0014] [4] In any one of [1] to [3], the interlayer insulating film may have a plurality of the delta doped layers spaced apart from each other in a depth direction. In this case, metal impurities such as sodium are easily captured by the interlayer insulating film.
[0015] [5] A method for manufacturing a silicon carbide semiconductor device according to another embodiment of the present disclosure includes forming a gate insulating film on a first main surface of a silicon carbide substrate having a first main surface, forming a gate electrode on the gate insulating film, and forming an interlayer insulating film to cover the gate electrode, the interlayer insulating film forming step includes forming an insulating film to cover the gate electrode, and forming a delta-doped layer in which phosphorus atoms are doped in the insulating film by ion implantation, and in the insulating film forming step, the silicon carbide substrate is heated to a temperature of 800° C. or higher. In this case, the surface unevenness of the interlayer insulating film is reduced, and the adhesion between the interlayer insulating film and the barrier metal film is improved. In addition, metal impurities such as sodium can be efficiently captured and their intrusion into the gate insulating film can be suppressed. Therefore, the fluctuation of the threshold voltage can be reduced.
[0016] [6] In the method of [5], the insulating film may be formed by low-pressure CVD, which has a high film formation temperature and is therefore likely to form an insulating film with a dense film quality.
[0017] [Details of the embodiment of the present disclosure] Hereinafter, embodiments of the present disclosure will be described in detail, but the present disclosure is not limited thereto.
[0018] (Silicon carbide semiconductor device) The following describes a silicon carbide semiconductor device 100 according to an embodiment. Fig. 1 is a cross-sectional view showing a silicon carbide semiconductor device 100 according to an embodiment.
[0019] As shown in FIG. 1, the silicon carbide semiconductor device 100 according to the embodiment mainly has a silicon carbide substrate 10, a gate insulating film 81, a gate electrode 82, an interlayer insulating film 83, a barrier metal film 84, a source electrode 60, and a drain electrode 70.
[0020] The silicon carbide substrate 10 includes a silicon carbide single crystal substrate 50 and a silicon carbide epitaxial layer 40 on the silicon carbide single crystal substrate 50. The silicon carbide substrate 10 has a first main surface 1 and a second main surface 2 opposite to the first main surface 1. The silicon carbide epitaxial layer 40 constitutes the first main surface 1, and the silicon carbide single crystal substrate 50 constitutes the second main surface 2. The silicon carbide single crystal substrate 50 and the silicon carbide epitaxial layer 40 are made of, for example, hexagonal silicon carbide of polytype 4H. The silicon carbide single crystal substrate 50 contains an n-type impurity such as nitrogen (N) and has an n-type. A field effect transistor is formed on the silicon carbide substrate 10 as an example of a semiconductor element.
[0021] The silicon carbide epitaxial layer 40 mainly includes a drift region 11, a body region 12, a source region 13, and a contact region .
[0022] Drift region 11 contains n-type impurities such as nitrogen or phosphorus and has n-type conductivity.
[0023] The body region 12 is provided on the drift region 11. The body region 12 contains p-type impurities such as aluminum (Al) and has the p-type.
[0024] The source region 13 is provided on the body region 12 so as to be separated from the drift region 11 by the body region 12. The source region 13 contains an n-type impurity such as nitrogen or phosphorus and has an n-type. The source region 13 constitutes the first main surface 1.
[0025] The contact region 18 contains a p-type impurity such as aluminum and has a p-type. The contact region 18 constitutes the first main surface 1. The contact region 18 penetrates the source region 13 and contacts the body region 12.
[0026] A plurality of gate trenches 5 are provided on the first main surface 1. Each gate trench 5 extends, for example, in a first direction parallel to the first main surface 1. The plurality of gate trenches 5 are arranged, for example, in a second direction parallel to the first main surface 1 and perpendicular to the first direction. Each gate trench 5 has a bottom surface 4 made of a drift region 11. Each gate trench 5 has a side surface 3 that penetrates the source region 13 and the body region 12 and continues to the bottom surface 4. The bottom surface 4 is, for example, a plane parallel to the second main surface 2. The angle of the side surface 3 with respect to a plane including the bottom surface 4 is, for example, 50° or more and 65° or less. This angle may be, for example, 55° or more. This angle may be, for example, 60° or less. The angle of the side surface 3 with respect to a plane including the bottom surface 4 may be 90°.
[0027] The gate insulating film 81 contacts the side surface 3 and the bottom surface 4. The gate insulating film 81 contacts the drift region 11 at the bottom surface 4. The gate insulating film 81 contacts each of the source region 13, the body region 12, and the drift region 11 at the side surface 3. The gate insulating film 81 may be in contact with the source region 13 at the first main surface 1. The gate insulating film 81 is, for example, an oxide film. The gate insulating film 81 is made of, for example, a material containing silicon dioxide.
[0028] The gate electrode 82 is provided on the gate insulating film 81. The gate electrode 82 is made of, for example, polysilicon (poly-Si) containing conductive impurities. The gate electrode 82 is disposed inside the gate trench 5. A part of the gate electrode 82 may be disposed on the first main surface 1.
[0029] The interlayer insulating film 83 is provided in contact with the gate insulating film 81 and the gate electrode 82. The interlayer insulating film 83 is made of a material containing, for example, silicon dioxide. The interlayer insulating film 83 electrically insulates the source electrode 60 from the gate electrode 82. A part of the interlayer insulating film 83 may be provided inside the gate trench 5. The interlayer insulating film 83 will be described in detail later.
[0030] Contact holes 90 are formed in the gate insulating film 81 and the interlayer insulating film 83 at regular intervals in the second direction. The contact holes 90 are provided such that, when viewed in a plan view from a direction perpendicular to the first main surface 1, the gate trench 5 is located between the contact holes 90 adjacent to each other in the second direction. The contact holes 90 extend in the first direction. Through the contact holes 90, the source region 13 and the contact region 18 are exposed from the gate insulating film 81 and the interlayer insulating film 83.
[0031] The barrier metal film 84 covers the side surface of the gate insulating film 81 and the upper surface and side surfaces of the interlayer insulating film 83. The barrier metal film 84 is in contact with both the gate insulating film 81 and the interlayer insulating film 83. The barrier metal film 84 is made of a material containing, for example, titanium nitride (TiN). The barrier metal film 84 is, for example, a laminated film of a titanium (Ti) film and a titanium nitride film.
[0032] The source electrode 60 is in contact with the first main surface 1. The source electrode 60 has a contact electrode 61 and a source wiring 62.
[0033] The contact electrode 61 may be in contact with the source region 13 and the contact region 18 on the first main surface 1. The contact electrode 61 has, for example, a first electrode region 61a and a second electrode region 61b. The first electrode region 61a is in contact with the source region 13 and the contact region 18. The first electrode region 61a forms an ohmic junction with the source region 13 and the contact region 18. The first electrode region 61a is made of, for example, a material containing nickel silicide (NiSi). The first electrode region 61a may be made of a material containing titanium, aluminum, and silicon. The second electrode region 61b covers the upper surface and side surface of the barrier metal film 84. The second electrode region 61b may not be provided. The second electrode region 61b is made of, for example, a material containing nickel.
[0034] The source wiring 62 covers the upper surface and side surfaces of the contact electrode 61. The source wiring 62 is made of a material containing, for example, aluminum or copper (Cu). The source wiring 62 may be made of a material containing aluminum and copper. The source electrode 60 is electrically insulated from the gate electrode 82 by an interlayer insulating film 83.
[0035] The drain electrode 70 is in contact with the second main surface 2. The drain electrode 70 is in contact with the silicon carbide single crystal substrate 50 at the second main surface 2. The drain electrode 70 is electrically connected to the drift region 11. The drain electrode 70 is made of a material containing nickel silicide, for example. The drain electrode 70 may be made of a material containing titanium, aluminum, and silicon. The drain electrode 70 forms an ohmic junction with the silicon carbide single crystal substrate 50.
[0036] Next, the interlayer insulating film 83 will be described. Fig. 2 is a cross-sectional view showing the interlayer insulating film 83. Fig. 3 is a diagram showing the phosphorus concentration distribution in the depth direction of the interlayer insulating film 83. In Fig. 3, the horizontal axis indicates the depth position of the interlayer insulating film 83, and the vertical axis indicates the phosphorus concentration of the interlayer insulating film 83.
[0037] The interlayer insulating film 83 is a high temperature silicon oxide film (HTO: High Temperature Oxide). The thickness of the interlayer insulating film 83 is, for example, 0.6 μm. The interlayer insulating film 83 includes a delta-doped layer 83a. The delta-doped layer 83a is a layer in which phosphorus atoms are delta-doped in the depth direction. The distribution of phosphorus atoms contained in the delta-doped layer 83a in the depth direction is approximated by a Gaussian distribution.
[0038] The peak concentration of phosphorus atoms in the delta doped layer 83a is 5×10 16 cm -3 In this case, metal impurities such as sodium are easily captured by the interlayer insulating film 83. The peak concentration of phosphorus atoms in the delta doped layer 83a is 1×10 19 cm -3 or less. In this case, irregularities are less likely to be formed on the surface of the interlayer insulating film 83. Therefore, the adhesion between the interlayer insulating film 83 and the barrier metal film 84 is improved, and cracks are less likely to occur in the interlayer insulating film 83 in a later process. The phosphorus concentration of the interlayer insulating film 83 can be measured by, for example, secondary ion mass spectrometry (SIMS).
[0039] The thickness of the delta doped layer 83a may be 0.05 μm or more. In this case, metal impurities such as sodium are easily captured by the interlayer insulating film 83. The thickness of the delta doped layer 83a may be 0.3 μm or less. In this case, irregularities are unlikely to be formed on the surface of the interlayer insulating film 83. Therefore, the adhesion between the interlayer insulating film 83 and the barrier metal film 84 is improved, and cracks are unlikely to occur in the interlayer insulating film 83 in a later process. The thickness of the delta doped layer 83a is the spread width of the peak at a height Y / 2, which is half the height Y of the peak, in the concentration profile of phosphorus atoms in the depth direction of the delta doped layer 83a, as shown in FIG. 3, for example.
[0040] The interlayer insulating film 83 may have a plurality of delta doped layers 83a spaced apart from each other in the depth direction. In this case, metal impurities such as sodium are easily captured by the interlayer insulating film 83. The plurality of delta doped layers 83a may be provided at equal intervals in the depth direction of the interlayer insulating film 83.
[0041] As described above, the silicon carbide semiconductor device 100 according to the embodiment has the interlayer insulating film 83 including the phosphorus delta-doped layer 83a. In this case, metal impurities such as sodium can be captured and prevented from penetrating into the gate insulating film 81. This can reduce the variation in threshold voltage.
[0042] (Method for manufacturing silicon carbide semiconductor device) A method for manufacturing the silicon carbide semiconductor device 100 according to the embodiment will now be described. Figures 4 to 13 are cross-sectional views illustrating the method for manufacturing the silicon carbide semiconductor device 100 according to the embodiment.
[0043] First, as shown in FIG. 4, a silicon carbide single crystal substrate 50 is prepared. Next, a silicon carbide epitaxial layer 40 is formed on the silicon carbide single crystal substrate 50. For example, the silicon carbide single crystal substrate 50 contains an n-type impurity such as nitrogen and has an n-type. For example, the silicon carbide epitaxial layer 40 can be formed by epitaxial growth with the addition of an n-type impurity such as nitrogen. In this manner, a silicon carbide substrate 10 having a first main surface 1 and a second main surface 2 is obtained.
[0044] Next, as shown in Fig. 5, ions are implanted into the silicon carbide epitaxial layer 40. For example, the body region 12, the source region 13, and the contact region 18 are formed by the ion implantation. The remaining portion of the silicon carbide epitaxial layer 40 functions as the drift region 11. In the ion implantation for forming the body region 12 or the contact region 18, for example, a p-type impurity such as aluminum is ion-implanted. In the ion implantation for forming the source region 13, for example, an n-type impurity such as phosphorus is ion-implanted.
[0045] 6, a plurality of gate trenches 5 are formed in the source region 13, the body region 12, and the drift region 11. The gate trenches 5 can be formed as follows.
[0046] First, a mask (not shown) having an opening is formed on a region where the gate trench 5 is to be formed. Next, using the mask, a part of the source region 13, a part of the body region 12, and a part of the drift region 11 are removed by etching. The etching is, for example, reactive ion etching (RIE). By the etching, a recess having a side portion substantially perpendicular to the first main surface 1 and a bottom portion that is continuous with the side portion and substantially parallel to the first main surface 1 is formed in the region where the gate trench 5 is to be formed.
[0047] Next, thermal etching is performed in the recess. The thermal etching can be performed, for example, by heating in an atmosphere containing a reactive gas having at least one or more types of halogen atoms, with the mask formed on the first main surface 1. The at least one or more types of halogen atoms include at least one of chlorine (Cl) atoms and fluorine (F) atoms. The atmosphere includes, for example, chlorine (Cl2), boron trichloride (BCl3), sulfur hexafluoride (SF6), or carbon tetrafluoride (CF4). For example, a mixed gas of chlorine gas and oxygen (O2) gas is used as the reactive gas, and the thermal etching is performed at a heat treatment temperature of 800°C or more and 900°C or less. The reactive gas may contain a carrier gas in addition to the above-mentioned chlorine gas and oxygen gas. For example, nitrogen (N2) gas, argon (Ar) gas, or helium (He) gas can be used as the carrier gas. A gate trench 5 is formed in the first main surface 1 by the thermal etching. The gate trench 5 has a bottom surface 4 formed from the drift region 11, and a side surface 3 that penetrates the source region 13 and the body region 12 and is continuous to the bottom surface 4. After the thermal etching, the mask is removed from the first main surface 1.
[0048] Next, as shown in FIG. 7, a gate insulating film 81 is formed. For example, the silicon carbide substrate 10 is thermally oxidized to form the gate insulating film 81 in contact with the source region 13, the body region 12, the drift region 11, and the contact region 18. Specifically, the silicon carbide substrate 10 is heated in an atmosphere containing oxygen at a temperature of, for example, 1300° C. or higher and 1400° C. or lower. As a result, the gate insulating film 81 in contact with the first main surface 1, the side surface 3, and the bottom surface 4 is formed. When the gate insulating film 81 is formed by thermal oxidation, strictly speaking, a part of the silicon carbide substrate 10 is taken into the gate insulating film 81. Therefore, in the subsequent processing, it is assumed that the first main surface 1, the side surface 3, and the bottom surface 4 have moved slightly to the interface between the gate insulating film 81 and the silicon carbide substrate 10 after the thermal oxidation.
[0049] 8, a gate electrode 82 is formed. The gate electrode 82 is formed on the gate insulating film 81. The gate electrode 82 is formed by, for example, a low-pressure CVD method. The gate electrode 82 is formed so as to face each of the source region 13, the body region 12, and the drift region 11.
[0050] 9, an interlayer insulating film 83 is formed. The interlayer insulating film 83 can be formed as follows.
[0051] First, an insulating film (not shown) for the interlayer insulating film 83 is formed so as to cover the gate electrode 82 and to be in contact with the gate insulating film 81. The insulating film is, for example, a high-temperature silicon oxide film. The insulating film is formed, for example, by a CVD method. The film formation temperature of the insulating film may be, for example, 800° C. or higher. In this case, an insulating film having a dense film quality can be formed. Therefore, the unevenness of the surface of the interlayer insulating film 83 is reduced, and the adhesion between the interlayer insulating film 83 and the barrier metal film 84 is improved. The insulating film is formed, for example, by a low-pressure CVD method. In the low-pressure CVD method, since the film formation temperature is high, an insulating film having a dense film quality can be easily formed. A part of the insulating film may be formed inside the gate trench 5.
[0052] Next, a delta-doped layer 83a is formed by doping phosphorus atoms inside the insulating film by ion implantation into the insulating film. This forms an interlayer insulating film 83 including the delta-doped layer 83a. In the ion implantation into the insulating film, ion implantation may be performed multiple times while changing the acceleration voltage into the insulating film to form a plurality of delta-doped layers 83a separated from each other in the depth direction of the insulating film. This makes it possible to form an interlayer insulating film 83 having a plurality of delta-doped layers 83a separated from each other in the depth direction. In this case, metal impurities such as sodium are easily captured by the interlayer insulating film 83.
[0053] 10 , the gate insulating film 81 and the interlayer insulating film 83 are etched to form contact holes 90 in the gate insulating film 81 and the interlayer insulating film 83. As a result, the source region 13 and the contact region 18 are exposed from the gate insulating film 81 and the interlayer insulating film 83.
[0054] 11, a barrier metal film 84 is formed to cover the side surface of the gate insulating film 81 and the upper surface and side surface of the interlayer insulating film 83. The barrier metal film 84 is made of a material containing titanium nitride, for example. The barrier metal film 84 is a laminated film of a titanium film and a titanium nitride film, for example. The barrier metal film 84 is formed by a sputtering method, for example.
[0055] 12, a metal film (not shown) for a contact electrode 61 in contact with the source region 13 and the contact region 18 on the first main surface 1 is formed. The metal film for the contact electrode 61 is formed by, for example, a sputtering method. The metal film for the contact electrode 61 is made of, for example, a material containing nickel. Next, a metal film for a drain electrode 70 in contact with the silicon carbide single crystal substrate 50 on the second main surface 2 is formed. The metal film for the drain electrode 70 is made of, for example, a material containing nickel.
[0056] Next, alloying annealing is performed. The metal film for the contact electrode 61 and the metal film for the drain electrode 70 are held at a temperature of, for example, 900° C. or more and 1100° C. or less for about 5 minutes. As a result, at least a part of the metal film for the contact electrode 61 and at least a part of the metal film for the drain electrode 70 react with silicon contained in the silicon carbide substrate 10 and are silicided. As a result, a first electrode region 61a that makes ohmic contact with the source region 13 and the contact region 18, and a drain electrode 70 that makes ohmic contact with the silicon carbide single crystal substrate 50 are formed. In addition, a second electrode region 61b that is not silicided is formed on the upper surface and side surface of the barrier metal film 84. The first electrode region 61a may be made of a material containing titanium, aluminum, and silicon. The drain electrode 70 may be made of a material containing titanium, aluminum, and silicon.
[0057] Next, as shown in FIG. 13, a source wiring 62 is formed. Specifically, the source wiring 62 is formed to cover the contact electrode 61. The source wiring 62 is formed by, for example, a sputtering method. The source wiring 62 is made of, for example, a material containing aluminum or copper. The source wiring 62 may be made of a material containing aluminum and copper. In this manner, a source electrode 60 having the contact electrode 61 and the source wiring 62 is formed.
[0058] In this manner, silicon carbide semiconductor device 100 including a field effect transistor can be manufactured.
[0059] As described above, according to the method for manufacturing the silicon carbide semiconductor device 100 according to the embodiment, first, an insulating film is formed at a film formation temperature of 800° C. or higher, and then a delta-doped layer 83a is formed in which phosphorus atoms are doped inside the insulating film by ion implantation into the insulating film. This forms an interlayer insulating film 83 including the delta-doped layer 83a. In this case, the surface irregularities of the interlayer insulating film 83 are reduced, and the adhesion between the interlayer insulating film 83 and the barrier metal film 84 is improved. In addition, metal impurities such as sodium can be efficiently captured and their intrusion into the gate insulating film 81 can be suppressed. As a result, the fluctuation of the threshold voltage can be reduced.
[0060] Although the embodiments have been described in detail above, the present invention is not limited to the specific embodiments, and various modifications and changes are possible within the scope of the claims. [Explanation of symbols]
[0061] 1 First main surface 2 Second main surface 3. Aspects 4 Bottom 4 Polytype 5. Gate trench 10 Silicon carbide substrate 11 Drift Region 12 Body Region 13 Source Area 18 Contact Area 40 Silicon carbide epitaxial layer 50 Silicon carbide single crystal substrate 60 Source electrode 61 Contact electrode 61a 1st electrode area 61b 2nd electrode area 62 Source wiring 70 Drain electrode 81 Gate insulating film 82 Gate electrode 83 Interlayer insulating film 83a Delta-doped layer 84 Barrier metal film 90 Contact Hole 100 Silicon carbide semiconductor device
Claims
1. a silicon carbide substrate having a first main surface; a gate insulating film provided on the first main surface of the silicon carbide substrate; a gate electrode provided on the gate insulating film; an interlayer insulating film provided so as to cover the gate electrode; having the interlayer insulating film includes a delta-doped layer of phosphorus; Silicon carbide semiconductor devices.
2. The peak concentration of phosphorus atoms in the delta doped layer is 5×10 16 cm -3 Above 1 x 10 19 cm -3 Below is the The silicon carbide semiconductor device according to claim 1 .
3. The thickness of the delta doped layer is 0.05 μm or more and 0.3 μm or less. The silicon carbide semiconductor device according to claim 1 .
4. the interlayer insulating film has a plurality of the delta doped layers spaced apart from each other in a depth direction; The silicon carbide semiconductor device according to claim 1 .
5. forming a gate insulating film on a first main surface of a silicon carbide substrate; forming a gate electrode on the gate insulating film; forming an interlayer insulating film so as to cover the gate electrode; having The step of forming an interlayer insulating film includes: forming an insulating film to cover the gate electrode; forming a delta doped layer by doping the insulating film with phosphorus atoms by ion implantation; Including, In the step of forming the insulating film, the silicon carbide substrate is heated to a temperature of 800° C. or more. A method for manufacturing a silicon carbide semiconductor device.
6. In the step of forming the insulating film, the insulating film is formed by a low pressure CVD method. The method for manufacturing a silicon carbide semiconductor device according to claim 5 .
Citation Information
Patent Citations
Semiconductor device and manufacture thereof
JP1991278435A
Semiconductor device and method for manufacturing the same
JP1998098040A
Silicon carbide semiconductor device
JP2016086064A
Method for manufacturing silicon carbide semiconductor device, and silicon carbide semiconductor device
JP2018082054A