Resin composition

The resin composition, combining epoxy resin, active ester resin, and organic filler, addresses resin seepage issues in printed wiring boards, ensuring uniform thickness and enhanced bending resistance while maintaining low dielectric properties.

JP2024163031APending Publication Date: 2024-11-21AJINOMOTO CO INC

Patent Information

Application Number
JP2024066917
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-10
Filing Date
2024-04-17
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Existing resin compositions for printed wiring boards face issues with resin seepage during lamination, leading to non-uniform thickness and difficulty in controlling the thickness of insulating layers, which compromises bending resistance and reliability.

Method used

A resin composition comprising epoxy resin, active ester resin with an allyl group, and a predetermined amount of organic filler, along with optional components like curing agents and inorganic fillers, to control resin flow and enhance bending resistance.

Benefits of technology

The composition effectively suppresses resin seepage, achieves excellent bending resistance, and results in a cured product with low dielectric loss tangent and dielectric constant, suitable for insulating layers in printed wiring boards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024163031000001
    Figure 2024163031000001
  • Figure 2024163031000002
    Figure 2024163031000002
  • Figure 2024163031000003
    Figure 2024163031000003
Patent Text Reader

Abstract

To provide a resin composition or the like that minimizes the amount of resin leakage and yields a cured product with superior bending resistance.SOLUTION: A resin composition contains (A) an epoxy resin, (B) an active ester resin with an allyl group and (C) an organic filler, where the content of component (C) is 6 mass% or less when the nonvolatile component in the resin composition is 100 mass%.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition. The present invention further relates to a resin sheet, a printed wiring board, and a semiconductor device obtained by using the resin composition. [Background technology]

[0002] 2. Description of the Related Art A known manufacturing technique for printed wiring boards is a build-up method in which insulating layers and conductor layers are alternately stacked.

[0003] As insulating materials for printed wiring boards used in such insulating layers, for example, Patent Documents 1 and 2 disclose resin compositions. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2022 / 038893 [Patent Document 2] Patent Publication No. 2021-14577 Summary of the Invention [Problem to be solved by the invention]

[0005] In recent years, in order to improve the reliability of printed wiring boards, materials with high strength, especially bending resistance, are also required.

[0006] In addition, when forming an insulating layer using a resin composition layer of a resin sheet, if the viscosity of the resin composition layer is low, when the resin sheet and the inner layer substrate are laminated, the amount of resin exudation (resin flow amount) in which the resin component in the resin composition layer flows out from the part between the support of the resin sheet and the inner layer substrate tends to increase. If the amount of resin exudation increases, the resin composition layer protrudes outside the edge of the support of the resin sheet. If the amount of resin exudation increases, the thickness of the resin composition layer at the end of the resin sheet tends to be thinned by the amount of the resin composition that has flowed out. Therefore, if the amount of resin exudation is large, the thickness of the resin composition layer becomes non-uniform, making it difficult to control the thickness.

[0007] The present invention has been devised in view of the above-mentioned problems, and aims to provide a resin composition which suppresses the amount of resin seepage and gives a cured product having excellent bending resistance; a resin sheet containing the resin composition; and a printed wiring board and a semiconductor device which have an insulating layer formed using the resin composition. [Means for solving the problem]

[0008] Means for Solving the Problems The present inventors have conducted intensive research into the above-mentioned problems and have found that the above-mentioned problems can be solved by incorporating a combination of (A) an epoxy resin, (B) an active ester resin having an allyl group, and a predetermined amount of (C) an organic filler, thereby completing the present invention.

[0009] That is, the present invention includes the following. [1] (A) epoxy resin, (B) an active ester resin having an allyl group, and (C) a resin composition containing an organic filler, A resin composition, the content of the component (C) being 6% by mass or less, when the total amount of non-volatile components in the resin composition is taken as 100% by mass. [2] The resin composition according to [1], further comprising (D) a curing agent. [3] The resin composition according to [2], wherein the component (D) includes one or more selected from the group consisting of a phenol-based curing agent, a naphthol-based curing agent, a carbodiimide-based curing agent, an active ester-based curing agent (excluding those corresponding to the component (B)), a benzoxazine-based curing agent, and a cyanate ester-based curing agent. [4] The resin composition according to any one of [1] to [3], further comprising (E) an inorganic filler. [5] The resin composition according to any one of [1] to [4], wherein the component (B) contains any one of a compound represented by general formula (B-1), a compound represented by general formula (B-2), and a compound represented by general formula (B-3). [ka] (In general formula (B-1), Ar 11 each independently represents a monovalent aromatic hydrocarbon group which may have a substituent, Ar 12 each independently represents a divalent aromatic hydrocarbon group which may have a substituent; Ar 13 each independently represents a divalent aromatic hydrocarbon group which may have a substituent, a divalent aliphatic hydrocarbon group which may have a substituent, an oxygen atom, a sulfur atom, or a divalent group consisting of a combination thereof. n represents an integer of 0 to 10. [ka] (In general formula (B-2), Ar 21 each independently represents a monovalent aromatic hydrocarbon group which may have a substituent, Ar 22 each independently represents a divalent hydrocarbon group which may have a substituent; Ar 23 each independently represents a divalent aromatic hydrocarbon group which may have a substituent, and m represents an integer of 0 to 10. [ka] (In general formula (B-3), Ar 21 each independently represents a monovalent aromatic hydrocarbon group which may have a substituent, Ar 31each independently represents a divalent aromatic hydrocarbon group which may have a substituent; Ar 13 each independently represents a divalent aromatic hydrocarbon group which may have a substituent, a divalent aliphatic hydrocarbon group which may have a substituent, an oxygen atom, a sulfur atom, or a divalent group consisting of a combination thereof. Each of mb and nb independently represents 0 or more. [6] The resin composition according to any one of [1] to [5], wherein the content of component (B) is 1% by mass or more and 25% by mass or less, when the total amount of non-volatile components in the resin composition is 100% by mass. [7] The resin composition according to any one of [1] to [6], wherein the component (C) contains core-shell particles. [8] A resin sheet comprising a support and a resin composition layer provided on the support, the resin composition layer comprising the resin composition according to any one of [1] to [7]. [9] A printed wiring board comprising an insulating layer formed from a cured product of the resin composition according to any one of [1] to [7].

[10] A semiconductor device comprising the printed wiring board described in [9]. Effect of the Invention

[0010] According to the present invention, it is possible to provide a resin composition which can suppress the amount of resin seeping out and give a cured product which has excellent bending resistance; a resin sheet containing the resin composition; a printed wiring board having an insulating layer formed using the resin composition, and a semiconductor device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present invention will be described in detail below with reference to preferred embodiments. However, the present invention is not limited to the following embodiments and examples, and can be modified and implemented as desired without departing from the scope of the claims of the present invention and their equivalents.

[0012] [Resin composition] The resin composition of the present invention is a resin composition containing (A) an epoxy resin, (B) an active ester resin having an allyl group, and (C) an organic filler, and the content of the (C) component is 6% by mass or less when the non-volatile components in the resin composition are 100% by mass. In the present invention, by containing the (A) component, the (B) component, and a predetermined amount of the (C) component in combination, the amount of resin bleeding is suppressed, and a cured product having excellent bending resistance can be obtained. In addition, a cured product having a low dielectric tangent and dielectric constant can usually be obtained.

[0013] The resin composition may further contain optional components in combination with the components (A) to (C). Examples of the optional components include a curing agent (D) (excluding those corresponding to the component (B)), an inorganic filler (E), a curing accelerator (F), other additives (G), and a solvent (H). Each component contained in the resin composition will be described in detail below.

[0014] <(A) Epoxy resin> The resin composition contains an epoxy resin (A) as component (A). By containing the epoxy resin (A) in the resin composition, a cured product exhibiting good mechanical strength and insulation reliability can be obtained. The epoxy resin (A) may be used alone or in combination of two or more kinds.

[0015] Examples of the epoxy resin (A) include bixylenol type epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, bisphenol AF type epoxy resin, dicyclopentadiene type epoxy resin, trisphenol type epoxy resin, naphthol novolac type epoxy resin, phenol novolac type epoxy resin, tert-butyl-catechol type epoxy resin, naphthalene type epoxy resin, naphthol type epoxy resin, anthracene type epoxy resin, glycidylamine type epoxy resin, glycidyl ester type Examples of the epoxy resin include epoxy resins, glycidyl cyclohexane type epoxy resins, alkyl diglycidyl ether type epoxy resins, cresol novolac type epoxy resins, biphenyl type epoxy resins, linear aliphatic epoxy resins, epoxy resins having a butadiene structure, alicyclic epoxy resins, heterocyclic epoxy resins, spiro ring-containing epoxy resins, cyclohexane type epoxy resins, cyclohexane dimethanol type epoxy resins, naphthylene ether type epoxy resins, trimethylol type epoxy resins, tetraphenylethane type epoxy resins, phenolphthalimidine type epoxy resins, etc. The epoxy resins may be used alone or in combination of two or more.

[0016] The resin composition preferably contains, as component (A), an epoxy resin having two or more epoxy groups in one molecule. From the viewpoint of significantly obtaining the desired effects of the present invention, the proportion of the epoxy resin having two or more epoxy groups in one molecule relative to 100% by mass of the epoxy resin (A) is preferably 50% by mass or more, more preferably 60% by mass or more, and particularly preferably 70% by mass or more.

[0017] Epoxy resins include epoxy resins that are liquid at a temperature of 20° C. (hereinafter sometimes referred to as "liquid epoxy resins") and epoxy resins that are solid at a temperature of 20° C. (hereinafter sometimes referred to as "solid epoxy resins"). The resin composition may contain only a liquid epoxy resin as component (A), may contain only a solid epoxy resin, or may contain a combination of a liquid epoxy resin and a solid epoxy resin. Of these, from the viewpoint of achieving the effects of the present invention significantly, it is preferable to contain a combination of a liquid epoxy resin and a solid epoxy resin.

[0018] The liquid epoxy resin is preferably a liquid epoxy resin having two or more epoxy groups in one molecule.

[0019] As the liquid epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol AF type epoxy resin, naphthalene type epoxy resin, glycidyl ester type epoxy resin, glycidyl amine type epoxy resin, phenol novolac type epoxy resin, alicyclic epoxy resin having an ester skeleton, cyclohexane type epoxy resin, cyclohexane dimethanol type epoxy resin, glycidyl amine type epoxy resin, epoxy resin having a butadiene structure, glycidyl cyclohexane type epoxy resin, phenolphthalimidine type epoxy resin, alkyl diglycidyl ether type epoxy resin are preferred, bisphenol A type epoxy resin, bisphenol F type epoxy resin, alkyl diglycidyl ether type epoxy resin are more preferred, and naphthalene type epoxy resin is even more preferred.

[0020] Specific examples of liquid epoxy resins include "HP4032", "HP4032D", and "HP4032SS" (naphthalene type epoxy resins) manufactured by DIC Corporation; "828US", "jER828EL", "825", and "Epikote 828EL" (bisphenol A type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER807" and "1750" (bisphenol F type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER152" (phenol novolac type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "630" and "630LSD" (glycidylamine type epoxy resins) manufactured by Mitsubishi Chemical Corporation; and "ZX1" manufactured by Nippon Steel Chemical & Material Co., Ltd. Examples of epoxy resins include "EX-721" (a mixture of bisphenol A type epoxy resin and bisphenol F type epoxy resin) manufactured by Nagase ChemteX Corporation, "Celloxide 2021P" (an alicyclic epoxy resin having an ester skeleton) manufactured by Daicel Corporation, "PB-3600" (an epoxy resin having a butadiene structure) manufactured by Daicel Corporation, "ZX1658" and "ZX1658GS" (liquid 1,4-glycidylcyclohexane type epoxy resin) manufactured by Nippon Steel Chemical & Material Corporation, and "YED216D" (an alkyl diglycidyl ether type epoxy resin) manufactured by Mitsubishi Chemical Corporation. These may be used alone or in combination of two or more types.

[0021] As the solid epoxy resin, a solid epoxy resin having two or more epoxy groups in one molecule is preferable, a solid epoxy resin having three or more epoxy groups in one molecule is more preferable, and an aromatic solid epoxy resin having three or more epoxy groups in one molecule is even more preferable.

[0022] As the solid epoxy resin, bixylenol type epoxy resin, naphthalene type epoxy resin, naphthalene type tetrafunctional epoxy resin, cresol novolac type epoxy resin, dicyclopentadiene type epoxy resin, trisphenol type epoxy resin, naphthol type epoxy resin, biphenyl type epoxy resin, naphthylene ether type epoxy resin, anthracene type epoxy resin, bisphenol A type epoxy resin, bisphenol AF type epoxy resin, and tetraphenylethane type epoxy resin are preferred, and naphthalene type epoxy resin and biphenyl type epoxy resin are more preferred.

[0023] Specific examples of solid epoxy resins include "HP4032H" (naphthalene type epoxy resin), "HP-4700", "HP-4710" (naphthalene type tetrafunctional epoxy resin), "N-690" (cresol novolac type epoxy resin), "N-695" (cresol novolac type epoxy resin), "HP-7200", "HP-7200HH", "HP-7200H" (dicyclopentadiene type epoxy resin), "EXA-7311", "EXA-7311-G3", "EXA-7311-G4", "EXA-7311-G4S", "HP6000", "HP6000L" (naphthylene ether type epoxy resin), and "EPPN-502H" (trisphenol type epoxy resin), "NC7000L" (naphthol novolac type epoxy resin), "NC3000H", "NC3000", "NC3000L" manufactured by Nippon Kayaku Co., Ltd. Examples of epoxy resins include "NC3100" (biphenyl type epoxy resin); "ESN475V" (naphthalene type epoxy resin) and "ESN485" (naphthol novolac type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "YX4000H", "YL6121" (biphenyl type epoxy resin), "YX4000HK" (bixylenol type epoxy resin), and "YX8800" (anthracene type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "PG-100" and "CG-500" manufactured by Osaka Gas Chemical Co., Ltd.; "YL7760" (bisphenol AF type epoxy resin), "YL7800" (fluorene type epoxy resin), "jER1010" (solid bisphenol A type epoxy resin), and "jER1031S" (tetraphenylethane type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd.; and "WHR-991S" (phenolphthalimidine type epoxy resin) manufactured by Nippon Kayaku Co., Ltd. These may be used alone or in combination of two or more.

[0024] When a liquid epoxy resin and a solid epoxy resin are used in combination as component (A), the ratio by mass (liquid epoxy resin:solid epoxy resin) is preferably 1:0.1 to 1:20, more preferably 1:0.15 to 1:10, and particularly preferably 1:0.2 to 1:5. When the ratio by mass of the liquid epoxy resin and the solid epoxy resin is within this range, the desired effects of the present invention can be significantly obtained.

[0025] The epoxy equivalent of the (A) component is preferably 50 g / eq. to 5000 g / eq., more preferably 50 g / eq. to 3000 g / eq., even more preferably 80 g / eq. to 2000 g / eq., and even more preferably 110 g / eq. to 1000 g / eq. Within this range, a cured product of the resin composition can be obtained with sufficient crosslink density. The epoxy equivalent is the mass of an epoxy resin containing one equivalent of epoxy groups. This epoxy equivalent can be measured according to JIS K7236.

[0026] From the viewpoint of significantly obtaining the desired effects of the present invention, the weight average molecular weight (Mw) of the component (A) is preferably 100 to 5000, more preferably 150 to 3000, and even more preferably 200 to 1500. The weight average molecular weight of the epoxy resin is a polystyrene-equivalent weight average molecular weight measured by gel permeation chromatography (GPC).

[0027] From the viewpoint of obtaining a cured product exhibiting good mechanical strength and insulation reliability, the content of the (A) component is preferably 1% by mass or more, more preferably 5% by mass or more, and even more preferably 8% by mass or more, based on 100% by mass of the non-volatile components in the resin composition. The upper limit is preferably 30% by mass or less, more preferably 20% by mass or less, and particularly preferably 15% by mass or less.

[0028] In the present invention, unless otherwise specified, the content of each component in the resin composition is a value when the non-volatile components in the resin composition are 100 mass %, and the non-volatile components mean all non-volatile components in the resin composition excluding the solvent.

[0029] <(B) Active ester resin having allyl group> The resin composition contains an active ester resin having an allyl group as the component (B). The component (B) does not include the above-mentioned component (A). By including the component (B) in the resin composition, a cured product having excellent bending resistance can be obtained. The component (B) may be used alone or in combination of two or more types.

[0030] As the component (B), a compound having an active ester site that reacts with the component (A) and an allyl group can be used.

[0031] The active ester site of the component (B) is preferably an aromatic ester skeleton. The aromatic ester skeleton represents a skeleton having an ester bond and an aromatic ring bonded to one end or both ends of the ester bond. Among them, the aromatic ester skeleton is preferably one having an aromatic ring at both ends of the ester bond. Examples of groups having such a skeleton include an arylcarbonyloxy group, an aryloxycarbonyl group, an arylenecarbonyloxy group, an aryleneoxycarbonyl group, an arylcarbonyloxyarylene group, an aryloxycarbonylarylene group, an arylenecarbonyloxyarylene group, and an aryleneoxycarbonylarylene group. The number of carbon atoms of the group having such a skeleton is preferably 7 to 20, more preferably 7 to 15, and even more preferably 7 to 11. The aromatic hydrocarbon group such as an aryl group and an arylene group may have a substituent.

[0032] The aryl group is preferably an aryl group having 6 to 30 carbon atoms, more preferably an aryl group having 6 to 20 carbon atoms, and even more preferably an aryl group having 6 to 10 carbon atoms. Examples of such aryl groups include those obtained by removing one hydrogen atom from a monocyclic aromatic compound such as a phenyl group, a furanyl group, a pyrrolyl group, a thiophene group, an imidazolyl group, a pyrazolyl group, an oxazolyl group, an isoxazolyl group, a thiazolyl group, an isothiazolyl group, a pyridinyl group, a pyrimidinyl group, a pyridazinyl group, a pyrazinyl group, or a triazinyl group; and those obtained by removing one hydrogen atom from a condensed ring aromatic compound such as a naphthyl group, anthracenyl group, a phenalenyl group, a phenanthrenyl group, a quinolinyl group, an isoquinolinyl group, a quinazolyl group, a phthalazinyl group, a pteridinyl group, a coumarinyl group, an indole group, a benzimidazolyl group, a benzofuranyl group, or an acridinyl group.

[0033] The arylene group is preferably an arylene group having 6 to 30 carbon atoms, more preferably an arylene group having 6 to 20 carbon atoms, and further preferably an arylene group having 6 to 10 carbon atoms. Examples of such arylene groups include a phenylene group, a naphthylene group, an anthracenylene group, and a biphenylene group (-C6H4-C6H4-).

[0034] The terminal of component (B) is preferably a monovalent aromatic hydrocarbon group. Examples of the monovalent aromatic hydrocarbon group include aryl groups, and the aryl groups are as described above. The monovalent aromatic hydrocarbon group at the terminal of component (B) is preferably a phenyl group.

[0035] In addition to the allyl group and aromatic ester skeleton, component (B) may have any of an aromatic hydrocarbon group, an aliphatic hydrocarbon group, an oxygen atom, a sulfur atom, and a group consisting of a combination thereof. The term "aromatic hydrocarbon group" means a hydrocarbon group containing an aromatic ring, and the aromatic ring may be any of a monocyclic, polycyclic, and heterocyclic ring.

[0036] The aromatic hydrocarbon group is preferably a divalent aromatic hydrocarbon group, more preferably an arylene group or an aralkylene group, and even more preferably an arylene group. The arylene group is preferably an arylene group having 6 to 30 carbon atoms, more preferably an arylene group having 6 to 20 carbon atoms, and even more preferably an arylene group having 6 to 10 carbon atoms. Examples of such an arylene group include a phenylene group, a naphthylene group, an anthracenylene group, and a biphenylene group. The aralkylene group is preferably an aralkylene group having 7 to 30 carbon atoms, more preferably an aralkylene group having 7 to 20 carbon atoms, and even more preferably an aralkylene group having 7 to 15 carbon atoms. Among these, a phenylene group and a naphthylene group are preferable.

[0037] The aliphatic hydrocarbon group is preferably a divalent aliphatic hydrocarbon group, more preferably a divalent saturated aliphatic hydrocarbon group, and further preferably an alkylene group or a cycloalkylene group. The alkylene group is preferably an alkylene group having 1 to 10 carbon atoms, more preferably an alkylene group having 1 to 6 carbon atoms, and further preferably an alkylene group having 1 to 3 carbon atoms. Examples of the alkylene group include a methylene group, an ethylene group, a propylene group, a 1-methylmethylene group, a 1,1-dimethylmethylene group, a 1-methylethylene group, a 1,1-dimethylethylene group, a 1,2-dimethylethylene group, a butylene group, a 1-methylpropylene group, a 2-methylpropylene group, a pentylene group, and a hexylene group, and the 1,1-dimethylmethylene group is preferred.

[0038] The cycloalkylene group is preferably a cycloalkylene group having 3 to 20 carbon atoms, more preferably a cycloalkylene group having 3 to 15 carbon atoms, and even more preferably a cycloalkylene group having 5 to 10 carbon atoms. The cycloalkylene group may have a monocyclic structure or a polycyclic structure. Examples of the cycloalkylene group include a cyclopropylene group, a cyclobutylene group, a cyclopentylene group, a cyclohexylene group, a cyclopentylene group, a cycloheptylene group, and cycloalkylene groups represented by the following formulas (a) to (d). In the formulas (a) to (d), "*" represents a bond. [ka]

[0039] The group consisting of these combinations is preferably a divalent group, and examples thereof include a group consisting of a combination of an aliphatic hydrocarbon group and an aromatic hydrocarbon group, a group consisting of a combination of an aromatic hydrocarbon group, an aliphatic hydrocarbon group and an aromatic hydrocarbon group, etc. One embodiment of the group consisting of these combinations is a group consisting of a combination of arylene-alkylene-arylene, and a group consisting of a combination of phenylene-1,1-dimethylmethylene-phenylene is preferred.

[0040] The component (B) has an allyl group. From the viewpoint of obtaining a cured product having excellent bending resistance, the number of allyl groups per molecule of the component (B) is preferably 1 or more, more preferably 2 or more, and is preferably 10 or less, more preferably 8 or less, and even more preferably 5 or less.

[0041] The allyl group contained in component (B) may be present as a substituent on a terminal monovalent aromatic hydrocarbon group, or may be present as a substituent on an aromatic hydrocarbon group or an aliphatic hydrocarbon group. When an allyl group is present as a substituent on a terminal monovalent aromatic hydrocarbon group, it is more preferable that the allyl group is present as a substituent on aromatic hydrocarbon groups at both ends.

[0042] The aromatic ester skeleton, aromatic hydrocarbon group, aliphatic hydrocarbon group, and unsaturated hydrocarbon group may have a substituent. Examples of the substituent include an unsaturated hydrocarbon group, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, and a halogen atom. The substituent may be contained alone or in combination of two or more kinds.

[0043] The substituent is not particularly limited, and examples thereof include halogen atoms, -OH, -OC 1-6 Alkyl group, -N(C 1-10 Alkyl group) 2, C 1-20 Alkyl group, C 2-30 Alkenyl group, C 2-30An alkynyl group, C 6-10 An aryl group, -NH2, -CN, -C(O)O-C 1-10 An alkyl group, -COOH, -C(O)H, -NO2, etc. are exemplified. Here, the term "C p-q " (p and q are positive integers and p < q is satisfied.) represents that the number of carbon atoms of the organic group described immediately after this term is p to q. For example, the expression "C 1-10 alkyl group" indicates an alkyl group having 1 to 10 carbon atoms. These substituents may be bonded to each other to form a ring, and the ring structure includes a spiro ring and a fused ring.

[0044] (Component (B) is preferably any one of a compound represented by the following general formula (B-1), a compound represented by the following general formula (B-2), and a compound represented by the following general formula (B-3). [Chemical formula] (In general formula (B-1), Ar 11 each independently represents a monovalent aromatic hydrocarbon group which may have a substituent, Ar 12 each independently represents a divalent aromatic hydrocarbon group which may have a substituent, Ar 13 each independently represents a divalent group composed of a divalent aromatic hydrocarbon group which may have a substituent, a divalent aliphatic hydrocarbon group which may have a substituent, an oxygen atom, a sulfur atom, or a combination thereof. n represents an integer from 0 to 10.) [Chemical formula] (In general formula (B-2), Ar 21 each independently represents a monovalent aromatic hydrocarbon group which may have a substituent, Ar 22 each independently represents a divalent hydrocarbon group which may have a substituent, Ar 23 each independently represents a divalent aromatic hydrocarbon group which may have a substituent. m represents an integer from 0 to 10.) [Chemical formula] (In general formula (B-3), Ar 21 each independently represents a monovalent aromatic hydrocarbon group which may have a substituent, Ar 31 each independently represents a divalent aromatic hydrocarbon group which may have a substituent; Ar 13 each independently represents a divalent aromatic hydrocarbon group which may have a substituent, a divalent aliphatic hydrocarbon group which may have a substituent, an oxygen atom, a sulfur atom, or a divalent group consisting of a combination thereof. Each of mb and nb independently represents 0 or more.

[0045] In general formula (B-1), Ar 11 Each of the groups independently represents a monovalent aromatic hydrocarbon group which may have a substituent. Examples of the monovalent aromatic hydrocarbon group include monocyclic aromatic compounds such as phenyl, furanyl, pyrrolyl, thiophene, imidazolyl, pyrazolyl, oxazolyl, isoxazolyl, thiazolyl, isothiazolyl, pyridinyl, pyrimidinyl, pyridazinyl, pyrazinyl, and triazinyl groups from which one hydrogen atom has been removed; and condensed aromatic compounds such as naphthyl, anthracenyl, phenalenyl, phenanthrenyl, quinolinyl, isoquinolinyl, quinazolyl, phthalazinyl, pteridinyl, coumarinyl, indole, benzimidazolyl, benzofuranyl, and acridinyl groups from which one hydrogen atom has been removed. Among them, Ar 11 From the viewpoint of obtaining the effects of the present invention remarkably, a phenyl group is preferable.

[0046] Ar 11 It is preferable that Ar has an allyl group as a substituent. 11 The monovalent aromatic hydrocarbon group represented by may have a substituent other than an allyl group. The substituent is the same as the substituent that the aromatic ester skeleton may have.

[0047] In general formula (B-1), Ar 12 each independently represents a divalent aromatic hydrocarbon group which may have a substituent. The divalent aromatic hydrocarbon group is as described above.

[0048] Ar 12 The divalent aromatic hydrocarbon group represented by may have a substituent. The substituent is the same as the substituent that the aromatic ester skeleton may have.

[0049] In general formula (B-1), Ar 13 each independently represents a divalent aromatic hydrocarbon group which may have a substituent, a divalent aliphatic hydrocarbon group which may have a substituent, an oxygen atom, a sulfur atom, or a divalent group consisting of a combination thereof, and a divalent group consisting of a combination thereof is preferred. The divalent aromatic hydrocarbon group and the divalent saturated aliphatic hydrocarbon group are as described above.

[0050] The divalent group formed from these combinations is preferably a divalent group formed by combining a divalent aromatic hydrocarbon group which may have a substituent, a divalent aliphatic hydrocarbon group which may have a substituent, and an oxygen atom, and more preferably a divalent group formed by alternately combining a plurality of divalent aromatic hydrocarbon groups which may have a substituent, and a plurality of divalent aliphatic hydrocarbon groups which may have a substituent. The divalent group formed from these combinations is the same as the group formed from these combinations. Specific examples of the divalent group formed from these combinations include the following divalent groups (B1) to (B15). In the formula, b1 to b7 represent integers of 0 to 10, preferably integers of 0 to 5. a1 to a9 represent integers of 0 to 10, preferably integers of 0 to 6, more preferably integers of 0 to 5. "*" represents a bond, and the wavy line represents a structure obtained by reaction of an aromatic compound, an acid halide of an aromatic compound, or an ester of an aromatic compound used in synthesizing the component (B). [ka] [ka] [ka]

[0051] Ar 13 The divalent aromatic hydrocarbon group and the divalent aliphatic hydrocarbon group represented by may have a substituent. The substituent is the same as the substituent that the aromatic ester skeleton may have.

[0052] In general formula (B-1), n ​​represents an integer of 0 to 10, preferably an integer of 0 to 5, and more preferably an integer of 0 to 3. When the compound represented by general formula (B-1) is an oligomer or polymer, n represents the average value thereof.

[0053] The compound represented by general formula (B-1) is preferably a compound represented by general formula (B-4). [ka] In the formula, Ar 31 each independently represents a monovalent aromatic hydrocarbon group which may have a substituent, Ar 32 each independently represents a divalent aromatic hydrocarbon group which may have a substituent, Ar 33 each independently represents a divalent group consisting of a divalent aromatic hydrocarbon group which may have a substituent, a divalent aliphatic hydrocarbon group which may have a substituent, and an oxygen atom. n1 represents an integer of 0 to 10.

[0054] Ar 31 each independently represents a monovalent aromatic hydrocarbon group which may have a substituent, and Ar 11 is the same as:

[0055] Ar 32 each independently represents a divalent aromatic hydrocarbon group which may have a substituent, and Ar 12 is the same as:

[0056] Ar 33each independently represents a divalent group consisting of a combination of a divalent aromatic hydrocarbon group which may have a substituent, a divalent aliphatic hydrocarbon group which may have a substituent, and an oxygen atom; Ar 13 is the same as a divalent group formed by a combination thereof represented by the following formula:

[0057] n1 represents an integer of 0 to 10 and is the same as n in formula (B-1).

[0058] In general formula (B-2), Ar 21 represents a monovalent aromatic hydrocarbon group which may have a substituent. Examples of the monovalent aromatic hydrocarbon group include monocyclic aromatic compounds such as phenyl, furanyl, pyrrolyl, thiophene, imidazolyl, pyrazolyl, oxazolyl, isoxazolyl, thiazolyl, isothiazolyl, pyridinyl, pyrimidinyl, pyridazinyl, pyrazinyl, and triazinyl groups from which one hydrogen atom has been removed; and condensed aromatic compounds such as naphthyl, anthracenyl, phenalenyl, phenanthrenyl, quinolinyl, isoquinolinyl, quinazolyl, phthalazinyl, pteridinyl, coumarinyl, indole, benzimidazolyl, benzofuranyl, and acridinyl groups from which one hydrogen atom has been removed. Among these, Ar 21 From the viewpoint of obtaining the effects of the present invention remarkably, Ar is preferably a phenyl group or a naphthyl group. 21 The monovalent aromatic hydrocarbon group represented by may have a substituent. The substituent is the same as the substituent that the aromatic ester skeleton may have.

[0059] In general formula (B-2), Ar 22 Each of the groups independently represents a divalent hydrocarbon group which may have a substituent. Examples of the divalent hydrocarbon group include a divalent aliphatic hydrocarbon group, a divalent aromatic hydrocarbon group, and a divalent group formed from a combination thereof, and a divalent group formed from a combination thereof is preferred. As for the divalent aliphatic hydrocarbon group, Ar 13The divalent aromatic hydrocarbon group is the same as the divalent aliphatic hydrocarbon group represented by Ar 12 is the same as:

[0060] The group consisting of these combinations is the same as the group consisting of these combinations described above. Specifically, a divalent group consisting of a divalent aromatic hydrocarbon group which may have a substituent and a divalent aliphatic hydrocarbon group which may have a substituent is preferred, a divalent group consisting of a divalent aromatic hydrocarbon group which may have a substituent-a divalent aliphatic hydrocarbon group which may have a substituent-a divalent aromatic hydrocarbon group which may have a substituent in this order is more preferred, and a divalent group consisting of phenylene-1,1-dimethylmethylene-phenylene in this order is even more preferred. The divalent group consisting of phenylene-1,1-dimethylmethylene-phenylene in this order is represented by the above formula (B10).

[0061] Ar 22 It is preferable that Ar has an allyl group as a substituent. The allyl group is preferably present on a divalent aromatic hydrocarbon group. 22 In the case where the group is a combination of these, the allyl group is preferably contained in a divalent aromatic hydrocarbon group. 22 may have a substituent other than an allyl group. The substituent is the same as the substituent that the aromatic ester skeleton may have.

[0062] In general formula (B-2), Ar 23 Each of Ar independently represents a divalent aromatic hydrocarbon group which may have a substituent. 23 represents Ar in general formula (B-1). 12 The same applies to the divalent aromatic hydrocarbon group represented by Ar 23 The divalent aromatic hydrocarbon group represented by may have a substituent. The substituent is the same as the substituent that the aromatic ester skeleton may have.

[0063] In formula (B-2), m represents an integer of 0 to 10, preferably an integer of 1 to 5, more preferably an integer of 1 to 3, and particularly preferably 1. When the compound represented by formula (B-2) is an oligomer or polymer, n represents the average value thereof.

[0064] The compound represented by general formula (B-2) is preferably a compound represented by general formula (B-5). [ka] In the formula, Ar 41 each independently represents a monovalent aromatic hydrocarbon group which may have a substituent, Ar 42 , and Ar 44 each independently represents a divalent aromatic hydrocarbon group which may have a substituent, Ar 43 each independently represents a divalent aliphatic hydrocarbon group which may have a substituent. m1 represents an integer of 0 to 10.

[0065] Ar 41 each independently represents a monovalent aromatic hydrocarbon group which may have a substituent, and Ar 21 is the same as:

[0066] Ar 42 , and Ar 44 each independently represents a divalent aromatic hydrocarbon group which may have a substituent, and Ar 12 is the same as:

[0067] Ar 43 each independently represents a divalent aliphatic hydrocarbon group which may have a substituent, and Ar 13 is the same as the optionally substituted divalent aliphatic hydrocarbon group represented by the formula (1).

[0068] m1 represents an integer of 0 to 10 and is the same as m in formula (B-2).

[0069] In general formula (B-3), Ar 21each independently represents a monovalent aromatic hydrocarbon group which may have a substituent. 21 represents Ar in formula (B-2). 21 is the same as:

[0070] In general formula (B-3), Ar 31 Each of Ar independently represents a divalent aromatic hydrocarbon group which may have a substituent. 31 represents Ar in formula (B-1). 12 is the same as:

[0071] In general formula (B-3), Ar 13 each independently represents a divalent aromatic hydrocarbon group which may have a substituent, a divalent aliphatic hydrocarbon group which may have a substituent, an oxygen atom, a sulfur atom, or a divalent group consisting of a combination thereof. 13 represents Ar in formula (B-1). 13 is the same as:

[0072] Specific examples of the (B) component include the following compounds. Specific examples of the (B) component include the compounds described in paragraphs 0068 to 0071 of International Publication No. 2018 / 235424 and paragraphs 0113 to 0115 of International Publication No. 2018 / 235425. However, the (B) component is not limited to these specific examples. In the formula, s represents an integer of 0 or 1 or more, and r represents an integer of 1 to 10. The average value of m2 is 1. n and m are 0 or more. [ka]

[0073] The component (B) may be synthesized by a known method. The component (B) can be synthesized by, for example, the method described in WO 2018 / 235424 or WO 2018 / 235425.

[0074] From the viewpoint of significantly obtaining the effects of the present invention, the weight average molecular weight of component (B) is preferably at least 150, more preferably at least 200, and even more preferably at least 250, and is preferably at most 5000, more preferably at most 3000, and even more preferably at most 2000. The weight average molecular weight of component (B) is a polystyrene-equivalent weight average molecular weight measured by gel permeation chromatography (GPC).

[0075] From the viewpoint of obtaining the effects of the present invention significantly, the allyl group equivalent of the (B) component is preferably 50 g / eq or more, more preferably 100 g / eq or more, even more preferably 150 g / eq, and is preferably 2000 g / eq or less, more preferably 1000 g / eq or less, even more preferably 500 g / eq or less. The allyl group equivalent is the mass of the (B) component containing one equivalent of an allyl group.

[0076] The ratio of the amount of the (A) component to the (B) component is preferably 1:0.01 to 1:10, more preferably 1:0.3 to 1:5, and even more preferably 1:0.4 to 1:4, in terms of the ratio of [total number of epoxy groups in the (A) component] to [total number of allyl groups in the (B) component]. Here, the "total number of epoxy groups in the epoxy resin" refers to the total value obtained by dividing the mass of the non-volatile components of the (A) component present in the resin composition by the epoxy equivalent. In addition, the "total number of allyl groups in the (B) component" refers to the total value obtained by dividing the mass of the non-volatile components of the (B) component present in the resin composition by the allyl group equivalent. By setting the ratio of the amount of the (B) component to the (A) component within this range, the effects of the present invention can be obtained significantly.

[0077] From the viewpoint of suppressing the amount of resin bleeding, the content of the (B) component is 1 mass% or more, preferably 2 mass% or more, more preferably 3 mass% or more, and is 25 mass% or less, preferably 20 mass% or less, and even more preferably 16 mass% or less, based on 100 mass% of the non-volatile components in the resin composition.

[0078] <(C)Organic filler> The resin composition contains an organic filler (C) as the component (C). The organic filler (C) as the component (C) does not include those corresponding to the above-mentioned components (A) to (B). The resin composition can obtain a cured product having excellent bending resistance by containing the component (B), but it becomes difficult to suppress the amount of resin seepage. However, in the present invention, the resin composition contains a combination of the component (B) and a predetermined amount of the component (C), so that a cured product having excellent bending resistance can be obtained and the amount of resin seepage can be suppressed. This is considered to be because the resin composition is given thixotropy by containing the component (C), and as a result, the flowability of the resin composition can be appropriately controlled. The component (C) may be used alone or in combination of two or more.

[0079] From the viewpoint of obtaining a cured product having excellent bending resistance, the content of the (C) component is 6% by mass or less, preferably 5% by mass or less, more preferably 4% by mass or less, and more preferably 3% by mass or less, when the non-volatile components in the resin composition are taken as 100% by mass. From the viewpoint of suppressing the amount of exudation of the resin, the lower limit is preferably 0.1% by mass or more, more preferably 0.3% by mass or more, even more preferably 0.5% by mass or more, or 0.8% by mass or more.

[0080] The component (C) is present in the resin composition in the form of particles. Examples of the component (C) include rubber particles, polyamide fine particles, silicone particles, and core-shell type particles. In the present invention, from the viewpoint of significantly obtaining the desired effects of the present invention, it is preferable to use either the rubber particles or the core-shell type particles, and it is more preferable to use the core-shell type particles.

[0081] Examples of the rubber component contained in the rubber particles include polybutadiene, polyisoprene, polychlorobutadiene, ethylene-vinyl acetate copolymer, styrene-butadiene copolymer, styrene-isoprene copolymer, styrene-isobutylene copolymer, acrylonitrile-butadiene copolymer, isoprene-isobutylene copolymer, isobutylene-butadiene copolymer, ethylene-propylene-diene terpolymer, ethylene-propylene-butene terpolymer, and other olefin-based thermoplastic elastomers; poly(propyl meth)acrylate, poly(butyl meth)acrylate, poly(cyclohexyl meth)acrylate, poly(octyl meth)acrylate, and other acrylic thermoplastic elastomers, and preferably olefin-based thermoplastic elastomers, and more preferably styrene-butadiene copolymers. Furthermore, the rubber component may be mixed with silicone-based rubbers such as polyorganosiloxane rubber. The rubber component contained in the rubber particles has a glass transition temperature of, for example, 0° C. or lower, preferably −10° C. or lower, more preferably −20° C. or lower, and even more preferably −30° C. or lower.

[0082] As the rubber particles, commercially available products may be used, for example, "EXL2655" manufactured by Dow Chemical Japan, "AC3401N" and "AC3816N" manufactured by Aica Kogyo Co., Ltd.

[0083] The core-shell type particles are particulate organic fillers consisting of a core particle containing a rubber component as described above and one or more shell layers covering the core particle. Furthermore, the core-shell type particles are preferably core-shell type graft copolymer particles consisting of a core particle containing a rubber component as described above and a shell portion obtained by graft copolymerization of a monomer component copolymerizable with the rubber component contained in the core particle. The core-shell type as used herein does not necessarily refer only to particles in which the core particle and the shell portion are clearly distinguishable, but also includes particles in which the boundary between the core particle and the shell portion is unclear, and the core particle does not necessarily have to be completely covered with the shell portion.

[0084] The rubber component is preferably contained in the core-shell graft copolymer particles in an amount of 40% by mass or more, more preferably 50% by mass or more, and even more preferably 60% by mass or more. The upper limit of the rubber component content in the core-shell graft copolymer particles is not particularly limited, but is preferably, for example, 95% by mass or less, and more preferably 90% by mass, from the viewpoint of sufficiently covering the core particles with the shell portion.

[0085] Examples of monomer components forming the shell portion of the core-shell type graft copolymer particles include (meth)acrylic acid esters such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, cyclohexyl (meth)acrylate, octyl (meth)acrylate, and glycidyl (meth)acrylate; (meth)acrylic acid; N-substituted maleimides such as N-methylmaleimide and N-phenylmaleimide; maleimide; α,β-unsaturated carboxylic acids such as maleic acid and itaconic acid; aromatic vinyl compounds such as styrene, 4-vinyltoluene, and α-methylstyrene; and (meth)acrylonitrile. Of these, (meth)acrylic acid esters are preferred, and methyl (meth)acrylate is more preferred.

[0086] Examples of commercially available core-shell type graft copolymer particles include "CHT" manufactured by Samsung SDI; "B602" manufactured by Techno UMG; "Paraloid EXL2602", "Paraloid EXL2603", "Paraloid EXL2655", "Paraloid EXL2311", "Paraloid EXL2313", "Paraloid EXL2315", "Paraloid KM330", "Paraloid KM336P", and "Paraloid KCZ201" manufactured by Dow Chemical Japan; "Metabrene C-223A", "Metabrene E-901", "Metabrene S-2001", "Metabrene W-450A", and "Metabrene SRK-200" manufactured by Mitsubishi Rayon; and "Kane Ace M-511", "Kane Ace M-600", "Kane Ace M-400", "Kane Ace M-580", and "Kane Ace MR-01" manufactured by Kaneka Corporation. These may be used alone or in combination of two or more.

[0087] The average particle size (average primary particle size) of the core-shell graft copolymer particles is not particularly limited, but is preferably 20 nm or more, more preferably 50 nm or more, even more preferably 80 nm or more, particularly preferably 100 nm or more, preferably 5,000 nm or less, more preferably 2,000 nm or less, even more preferably 1,000 nm or less, particularly preferably 500 nm or less. The average particle size (average primary particle size) of the core-shell graft copolymer particles can be measured using a zeta potential particle size distribution measuring device or the like.

[0088] When the nonvolatile components in the resin composition are taken as 100% by mass, the mass ratio of the (B) component to the (C) component ((B) / (C) component) is preferably 1 or more, more preferably 3 or more, even more preferably 5 or more, or 8 or more, and is preferably 30 or less, more preferably 20 or less, and even more preferably 15 or less. By adjusting the contents of the (B) component and the (C) component so that the mass ratio of the (B) component to the (C) component is within this range, a cured product having excellent bending resistance can be obtained and the amount of resin seeping out can be suppressed.

[0089] When the contents of the (A), (B), and (C) components are A1, B1, and C1, respectively, when the nonvolatile components in the resin composition are taken as 100% by mass, A1 / (B1+C1) is preferably 0.1 or more, more preferably 0.3 or more, and even more preferably 0.5 or more, and is preferably 5 or less, more preferably 3 or less, and even more preferably 1 or less. By adjusting the contents of the (A), (B), and (C) components so that A1 / (B1+C1) falls within this range, a cured product having excellent bending resistance can be obtained and the amount of resin seeping out can be suppressed.

[0090] <(D) Hardener> The resin composition may further contain a (D) curing agent as an optional component in addition to the above-mentioned components. The (D) curing agent as this (D) component does not include those corresponding to the above-mentioned (A) to (C) components. As the (D) curing agent, a compound having a function of reacting with the (A) component to cure the resin composition can be used, and examples thereof include phenol-based curing agents, naphthol-based curing agents, carbodiimide-based curing agents, active ester-based curing agents (excluding those corresponding to the (B) component), benzoxazine-based curing agents, and cyanate ester-based curing agents. Among them, from the viewpoint of obtaining the effects of the present invention significantly, the (D) curing agent preferably contains one or more selected from phenol-based curing agents, naphthol-based curing agents, carbodiimide-based curing agents, active ester-based curing agents (excluding those corresponding to the (B) component), benzoxazine-based curing agents, and cyanate ester-based curing agents, and more preferably contains one or more of phenol-based curing agents and carbodiimide-based curing agents, and further preferably contains a phenol-based curing agent. The (D) curing agent may be used alone or in combination of two or more kinds.

[0091] As the phenol-based curing agent and naphthol-based curing agent, from the viewpoint of heat resistance and water resistance, a phenol-based curing agent having a novolac structure or a naphthol-based curing agent having a novolac structure is preferable. Also, from the viewpoint of adhesion to the conductor layer, a nitrogen-containing phenol-based curing agent is preferable, and a triazine skeleton-containing phenol-based curing agent is more preferable.

[0092] Specific examples of phenol-based curing agents and naphthol-based curing agents include, for example, "MEH-7700", "MEH-7810", and "MEH-7851" manufactured by Meiwa Kasei Co., Ltd., "NHN", "CBN", "GPH", and "KAYAHARD GPH103" manufactured by Nippon Kayaku Co., Ltd., "SN170", "SN180", "SN190", "SN475", "SN485", "SN495", "SN-495V", "SN375", and "SN395" manufactured by Nippon Steel & Sumikin Chemical Co., Ltd., and "TD-2090", "LA-7052", "LA-7054", "LA-1356", "LA3018-50P", "EXB-9500", and "KA-1163" manufactured by DIC Corporation.

[0093] The carbodiimide curing agent is a compound having one or more carbodiimide groups (-N=C=N-) in one molecule, and the carbodiimide curing agent is preferably a compound having two or more carbodiimide groups in one molecule.

[0094] Specific examples of carbodiimide-based curing agents include Carbodilite V-03 (carbodiimide group equivalent: 216 g / eq., V-05 (carbodiimide group equivalent: 262 g / eq.), V-07 (carbodiimide group equivalent: 200 g / eq.), V-09 (carbodiimide group equivalent: 200 g / eq.), all manufactured by Nisshinbo Chemical Inc.; and Stavaxol P (carbodiimide group equivalent: 302 g / eq.), all manufactured by Lanxess AG.

[0095] The active ester curing agent is not particularly limited, but generally, compounds having two or more highly reactive ester groups in one molecule, such as phenol esters, thiophenol esters, N-hydroxyamine esters, and esters of heterocyclic hydroxy compounds, are preferably used. The active ester curing agent is preferably one obtained by a condensation reaction between a carboxylic acid compound and / or a thiocarboxylic acid compound and a hydroxy compound and / or a thiol compound. In particular, from the viewpoint of improving heat resistance, an active ester curing agent obtained from a carboxylic acid compound and a hydroxy compound is preferred, and an active ester curing agent obtained from a carboxylic acid compound and a phenol compound and / or a naphthol compound is more preferred. Examples of the carboxylic acid compound include benzoic acid, acetic acid, succinic acid, maleic acid, itaconic acid, phthalic acid, isophthalic acid, terephthalic acid, and pyromellitic acid. Examples of phenol compounds or naphthol compounds include hydroquinone, resorcin, bisphenol A, bisphenol F, bisphenol S, phenolphthaline, methylated bisphenol A, methylated bisphenol F, methylated bisphenol S, phenol, o-cresol, m-cresol, p-cresol, catechol, α-naphthol, β-naphthol, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, dihydroxybenzophenone, trihydroxybenzophenone, tetrahydroxybenzophenone, phloroglucin, benzenetriol, dicyclopentadiene-type diphenol compounds, phenol novolac, etc. Here, the term "dicyclopentadiene-type diphenol compounds" refers to diphenol compounds obtained by condensing one molecule of dicyclopentadiene with two molecules of phenol.

[0096] Specifically, active ester compounds containing a dicyclopentadiene-type diphenol structure, active ester compounds containing a naphthalene structure, active ester compounds containing an acetylated product of phenol novolac, and active ester compounds containing a benzoylated product of phenol novolac are preferred, and among these, active ester compounds containing a naphthalene structure and active ester compounds containing a dicyclopentadiene-type diphenol structure are more preferred. The "dicyclopentadiene-type diphenol structure" refers to a divalent structural unit consisting of phenylene-dicyclopentylene-phenylene.

[0097] Commercially available active ester curing agents include active ester compounds containing a dicyclopentadiene-type diphenol structure, such as "EXB-9451", "EXB-9460", "EXB-9460S", "HPC-8000-65T", "HPC-8000H-65TM", and "HPC-8000L-65TM" (manufactured by DIC Corporation); active ester compounds containing a naphthalene structure, such as "EXB-9416-70BK", "EXB-8100L-65T", "EXB-8150-65T", "EXB-8150L-65T", "HPC-8150-60T", "HPC-8150-62T", and "HP-B-8151-62T" (manufactured by DIC Corporation); and phenol novolac. Examples of the active ester compound containing an acetylated product of phenol novolac include "DC808" (manufactured by Mitsubishi Chemical Corporation), an active ester compound containing a benzoylated product of phenol novolac includes "YLH1026" (manufactured by Mitsubishi Chemical Corporation), an active ester curing agent which is an acetylated product of phenol novolac includes "DC808" (manufactured by Mitsubishi Chemical Corporation), an active ester curing agent which is a benzoylated product of phenol novolac includes "YLH1026" (manufactured by Mitsubishi Chemical Corporation), "YLH1030" (manufactured by Mitsubishi Chemical Corporation), and "YLH1048" (manufactured by Mitsubishi Chemical Corporation), and an active ester compound containing a styryl group includes "PC1300-02-65MA" (manufactured by Air Water Corporation).

[0098] Specific examples of benzoxazine-based curing agents include "HFB2006M" manufactured by Showa Polymer Co., Ltd., and "Pd" and "Fa" manufactured by Shikoku Chemical Industry Co., Ltd.

[0099] Examples of the cyanate ester curing agent include bifunctional cyanate resins such as bisphenol A dicyanate, polyphenol cyanate, oligo(3-methylene-1,5-phenylene cyanate), 4,4'-methylenebis(2,6-dimethylphenyl cyanate), 4,4'-ethylidene diphenyl dicyanate, hexafluorobisphenol A dicyanate, 2,2-bis(4-cyanate)phenylpropane, 1,1-bis(4-cyanate phenylmethane), bis(4-cyanate-3,5-dimethylphenyl)methane, 1,3-bis(4-cyanate phenyl-1-(methylethylidene))benzene, bis(4-cyanate phenyl)thioether, and bis(4-cyanate phenyl)ether; polyfunctional cyanate resins derived from phenol novolac and cresol novolac; and prepolymers in which these cyanate resins are partially converted to triazine. Specific examples of cyanate ester-based curing agents include arxada's "PT30" and "PT60" (phenol novolac type multifunctional cyanate ester resins), "ULL-950S" (multifunctional cyanate ester resin), "BA230" and "BA230S75" (prepolymers in which part or all of bisphenol A dicyanate has been triazine-converted into a trimer).

[0100] The ratio of the amount of the (A) component to the (D) component is preferably 1:0.01 to 1:10, more preferably 1:0.05 to 1:5, and even more preferably 1:0.08 to 1:3, in terms of the ratio of [total number of epoxy groups in the (A) component] to [total number of active groups in the (D) component]. Here, the "total number of epoxy groups in the epoxy resin" refers to the total value obtained by dividing the mass of the non-volatile component of the (A) component present in the resin composition by the epoxy equivalent. In addition, the "total number of active groups in the (D) component" refers to the total value obtained by dividing the mass of the non-volatile component of the (D) component present in the resin composition by the active group equivalent. By setting the ratio of the amount of the (D) component to the (A) component within this range, the effects of the present invention can be obtained significantly.

[0101] The ratio of the amount of the (A) component to the (B) and (D) components is preferably 1:0.01 to 1:10, more preferably 1:0.3 to 1:5, and even more preferably 1:0.4 to 1:4, in terms of the ratio of [total number of epoxy groups in the (A) component] to [total number of active groups in the (B) and (D) components]. Here, the "total number of active groups in the (B) and (D) components" refers to the total value of the mass of the non-volatile components of the (B) and (D) components present in the resin composition divided by the active group equivalent. By setting the ratio of the amount of the (A) component to the (B) and (D) components within this range, the effects of the present invention can be significantly obtained.

[0102] From the viewpoint of obtaining the desired effect of the present invention remarkably, the content of the (D) component is preferably 0.5% by mass or more, more preferably 0.8% by mass or more, and even more preferably 1% by mass or more, based on 100% by mass of the non-volatile components in the resin composition. The upper limit is preferably 25% by mass or less, more preferably 20% by mass or less, and even more preferably 15% by mass or less.

[0103] <(E) Inorganic filler> The resin composition of the present invention may contain an inorganic filler (E) as an optional component. The inorganic filler (E) is contained in the resin composition in the form of particles.

[0104] (E) An inorganic compound is used as the material of the inorganic filler. (E) Examples of the material of the inorganic filler include silica, alumina, glass, cordierite, silicon oxide, barium sulfate, barium carbonate, talc, clay, mica powder, zinc oxide, hydrotalcite, boehmite, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, magnesium oxide, boron nitride, aluminum nitride, manganese nitride, aluminum borate, strontium carbonate, strontium titanate, calcium titanate, magnesium titanate, bismuth titanate, titanium oxide, zirconium oxide, barium titanate, barium zirconate titanate, barium zirconate, calcium zirconate, zirconium phosphate, and zirconium tungstate phosphate. Among these, silica is particularly suitable. Examples of silica include amorphous silica, fused silica, crystalline silica, synthetic silica, and hollow silica. In addition, spherical silica is preferable as the silica. The (E) inorganic filler may be used alone or in combination of two or more kinds in any ratio.

[0105] The average particle size of the (E) inorganic filler is not particularly limited, but is preferably 10 μm or less, more preferably 5 μm or less, even more preferably 2 μm or less, even more preferably 1 μm or less, and particularly preferably 0.7 μm or less. The lower limit of the average particle size of the (E) inorganic filler is not particularly limited, but is preferably 0.01 μm or more, more preferably 0.05 μm or more, even more preferably 0.1 μm or more, and particularly preferably 0.2 μm or more. The average particle size of the (E) inorganic filler can be measured by a laser diffraction / scattering method based on the Mie scattering theory. Specifically, the particle size distribution of the inorganic filler is prepared on a volume basis using a laser diffraction / scattering type particle size distribution measuring device, and the median diameter is taken as the average particle size. The measurement sample can be prepared by weighing 100 mg of the inorganic filler and 10 g of methyl ethyl ketone into a vial and dispersing it by ultrasonic waves for 10 minutes. The measurement sample was measured using a laser diffraction type particle size distribution measuring device with blue and red light source wavelengths, and the particle size distribution of the inorganic filler on a volume basis was measured using a flow cell method, and the average particle size was calculated as the median diameter from the particle size distribution obtained. An example of a laser diffraction type particle size distribution measuring device is the "LA-960" manufactured by Horiba, Ltd.

[0106] The specific surface area of ​​the (E) inorganic filler is not particularly limited, but is preferably 0.1 m 2 / g or more, more preferably 0.5m 2 / g or more, more preferably 1m 2 / g or more, particularly preferably 3m 2 The upper limit of the specific surface area of ​​the (E) inorganic filler is not particularly limited, but is preferably 100 m 2 / g or less, more preferably 70m 2 / g or less, more preferably 50m 2 / g or less, particularly preferably 40m 2 The specific surface area of ​​the inorganic filler is obtained by adsorbing nitrogen gas onto the surface of a sample using a specific surface area measuring device (Macsorb HM-1210 manufactured by Mountech Co., Ltd.) according to the BET method, and calculating the specific surface area using the BET multipoint method.

[0107] The (E) inorganic filler may be a non-hollow inorganic filler with a porosity of 0 volume % (preferably non-hollow silica), or a hollow inorganic filler with a porosity of more than 0 volume % (preferably hollow silica), or may contain both. The porosity of the hollow inorganic filler is preferably 70 volume % or less, more preferably 50 volume % or less, and particularly preferably 30 volume % or less. The lower limit of the porosity of the (E) inorganic filler may be, for example, more than 0 volume %, 1 volume % or more, 5 volume % or more, 10 volume % or more, etc. The porosity P (volume %) of the inorganic filler is defined as the volume-based ratio of the total volume of one or more voids present inside the particle to the total volume of the particle based on the outer surface of the particle (total volume of voids / volume of particle), and is, for example, a measured value D of the actual density of the inorganic filler. M (g / cm 3 ), and the theoretical value of the material density of the material forming the inorganic filler D T (g / cm 3 ) is used to calculate the following formula (1):

[0108]

number

[0109] (E) The actual density of the inorganic filler can be measured, for example, by using a true density measuring device. Examples of the true density measuring device include ULTRAPYCNOMETER 1000 manufactured by QUANTACHROME. For example, nitrogen is used as the measurement gas.

[0110] (E) Inorganic filler may be a commercially available product. (E) Inorganic filler commercially available products include, for example, "SP60-05" and "SP507-05" manufactured by Nippon Steel Chemical & Material Co., Ltd.; "YC100C", "YA050C", "YA050C-MJE", "YA010C", "SC2500SQ", "SO-C4", "SO-C2", and "SO-C1" manufactured by Admatechs Co., Ltd.; "UFP-30", "DAW-03", and "FB-105FD" manufactured by Denka Co., Ltd.; "Silfil NSS-3N", "Silfil NSS-4N", and "Silfil NSS-5N" manufactured by Tokuyama Corporation; "Cellfiers" and "MGH-005" manufactured by Taiheiyo Cement Corporation; and "LPH-208" manufactured by Ube Exsymo Co., Ltd.

[0111] (E) The inorganic filler is preferably treated with a surface treatment agent from the viewpoint of improving moisture resistance and dispersibility. Examples of the surface treatment agent include fluorine-containing silane coupling agents, aminosilane coupling agents, epoxysilane coupling agents, mercaptosilane coupling agents, silane coupling agents, alkoxysilanes, organosilazane compounds, titanate coupling agents, etc. Furthermore, the surface treatment agent may be used alone or in any combination of two or more types.

[0112] Examples of commercially available surface treatment agents include Shin-Etsu Chemical Co., Ltd.'s "KBM403" (3-glycidoxypropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM803" (3-mercaptopropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBE903" (3-aminopropyltriethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM573" (N-phenyl-3-aminopropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "SZ-31" (hexamethyldisilazane), Shin-Etsu Chemical Co., Ltd.'s "KBM103" (phenyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM-4803" (long-chain epoxy-type silane coupling agent), and Shin-Etsu Chemical Co., Ltd.'s "KBM-7103" (3,3,3-trifluoropropyltrimethoxysilane).

[0113] From the viewpoint of improving the dispersibility of the inorganic filler, the degree of surface treatment with the surface treatment agent is preferably within a predetermined range. Specifically, 100% by mass of the inorganic filler is preferably surface-treated with 0.2% to 5% by mass of the surface treatment agent, more preferably 0.2% to 3% by mass, and even more preferably 0.3% to 2% by mass.

[0114] The degree of surface treatment with the surface treatment agent can be evaluated by the amount of carbon per unit surface area of ​​the inorganic filler. From the viewpoint of improving the dispersibility of the inorganic filler, the amount of carbon per unit surface area of ​​the inorganic filler is set to 0.02 mg / m 2 More than 0.1 mg / m is preferable. 2 More preferably, 0.2 mg / m or more 2 On the other hand, from the viewpoint of preventing an increase in the melt viscosity of the resin composition or the melt viscosity in the form of a sheet, it is more preferable that the melt viscosity is 1.0 mg / m 2 Less than 0.8 mg / m is preferred. 2 Less than 0.5 mg / m is more preferable. 2 The following is even more preferred:

[0115] (E) The amount of carbon per unit surface area of ​​the inorganic filler can be measured after the surface-treated inorganic filler is washed with a solvent (e.g., methyl ethyl ketone (MEK)). Specifically, a sufficient amount of MEK as a solvent is added to the inorganic filler that has been surface-treated with a surface treatment agent, and ultrasonic cleaning is performed at 25°C for 5 minutes. After removing the supernatant and drying the solid content, the amount of carbon per unit surface area of ​​the inorganic filler can be measured using a carbon analyzer. As the carbon analyzer, the "EMIA-320V" manufactured by Horiba, Ltd., or the like can be used.

[0116] From the viewpoint of significantly obtaining the effects of the present invention, the content of the (E) inorganic filler, when the non-volatile components in the resin composition are taken as 100 mass%, is preferably 55 mass% or more, more preferably 60 mass% or more, even more preferably 65 mass% or more, or 70 mass% or more, and is preferably 85 mass% or less, more preferably 80 mass% or less, and even more preferably 75 mass% or less.

[0117] <(F) Curing accelerator> In addition to the above-mentioned components, the resin composition may further contain a curing accelerator as an optional component (F). The curing accelerator (F) as the component (F) does not include those corresponding to the above-mentioned components (A) to (D). By including the component (F), it becomes possible to further accelerate the curing of the component (A). The component (F) may be used alone or in combination of two or more kinds.

[0118] Examples of the component (F) include phosphorus-based curing accelerators, urea-based curing accelerators, guanidine-based curing accelerators, imidazole-based curing accelerators, metal-based curing accelerators, amine-based curing accelerators, etc. Among these, curing accelerators selected from amine-based curing accelerators and metal-based curing accelerators are preferred, and amine-based curing accelerators are particularly preferred.

[0119] Examples of the phosphorus-based curing accelerator include aliphatic phosphonium salts such as tetrabutyl phosphonium bromide, tetrabutyl phosphonium chloride, tetrabutyl phosphonium acetate, tetrabutyl phosphonium decanoate, tetrabutyl phosphonium laurate, bis(tetrabutyl phosphonium)pyromellitate, tetrabutyl phosphonium hydrogenhexahydrophthalate, tetrabutyl phosphonium 2,6-bis[(2-hydroxy-5-methylphenyl)methyl]-4-methylphenolate, and di-tert-butyldimethylphosphonium tetraphenylborate; methyl triphenyl phosphonium bromide, ethyl triphenyl phosphonium bromide, propyl triphenyl phosphonium bromide, butyl triphenyl phosphonium bromide, benzyl triphenyl phosphonium chloride, tetraphenyl phosphonium bromide, p-tolyl triphenyl phosphonium tetra-p-tolylborate, tetraphenyl phosphonium bromide, and the like. aromatic phosphonium salts such as tetraphenylborate, tetraphenylphosphonium tetra-p-tolylborate, triphenylethylphosphonium tetraphenylborate, tris(3-methylphenyl)ethylphosphonium tetraphenylborate, tris(2-methoxyphenyl)ethylphosphonium tetraphenylborate, (4-methylphenyl)triphenylphosphonium thiocyanate, tetraphenylphosphonium thiocyanate, and butyltriphenylphosphonium thiocyanate; aromatic phosphine-borane complexes such as triphenylphosphine-triphenylborane; aromatic phosphine-quinone adducts such as triphenylphosphine-p-benzoquinone adduct; aliphatic phosphines such as tributylphosphine, tri-tert-butylphosphine, trioctylphosphine, di-tert-butyl(2-butenyl)phosphine, di-tert-butyl(3-methyl-2-butenyl)phosphine, and tricyclohexylphosphine;Dibutylphenylphosphine, di-tert-butylphenylphosphine, methyldiphenylphosphine, ethyldiphenylphosphine, butyldiphenylphosphine, diphenylcyclohexylphosphine, triphenylphosphine, tri-o-tolylphosphine, tri-m-tolylphosphine, tri-p-tolylphosphine, tris(4-ethylphenyl)phosphine, tris(4-propylphenyl)phosphine, tris(4-isopropylphenyl)phosphine, tris(4-butylphenyl)phosphine, tris(4-tert-butylphenyl)phosphine, tris(2,4-dimethylphenyl)phosphine, tris(2,5-dimethylphenyl)phosphine, tris(2,6-dimethylphenyl)phosphine Examples of aromatic phosphines include tris(3,5-dimethylphenyl)phosphine, tris(2,4,6-trimethylphenyl)phosphine, tris(2,6-dimethyl-4-ethoxyphenyl)phosphine, tris(2-methoxyphenyl)phosphine, tris(4-methoxyphenyl)phosphine, tris(4-ethoxyphenyl)phosphine, tris(4-tert-butoxyphenyl)phosphine, diphenyl-2-pyridylphosphine, 1,2-bis(diphenylphosphino)ethane, 1,3-bis(diphenylphosphino)propane, 1,4-bis(diphenylphosphino)butane, 1,2-bis(diphenylphosphino)acetylene, and 2,2'-bis(diphenylphosphino)diphenyl ether.

[0120] Examples of the urea-based curing accelerator include 1,1-dimethylurea; aliphatic dimethylureas such as 1,1,3-trimethylurea, 3-ethyl-1,1-dimethylurea, 3-cyclohexyl-1,1-dimethylurea, and 3-cyclooctyl-1,1-dimethylurea; 3-phenyl-1,1-dimethylurea, 3-(4-chlorophenyl)-1,1-dimethylurea, 3-(3,4-dichlorophenyl)-1,1-dimethylurea, 3-(3-chloro-4-methylphenyl)-1,1-dimethylurea, 3-(2-methylphenyl)-1,1-dimethylurea, 3-(4-methylphenyl)-1,1-dimethylurea, and 3-(3,4-dimethylphenyl)-1,1-dimethylurea. aromatic dimethylureas such as butylurea, 3-(4-isopropylphenyl)-1,1-dimethylurea, 3-(4-methoxyphenyl)-1,1-dimethylurea, 3-(4-nitrophenyl)-1,1-dimethylurea, 3-[4-(4-methoxyphenoxy)phenyl]-1,1-dimethylurea, 3-[4-(4-chlorophenoxy)phenyl]-1,1-dimethylurea, 3-[3-(trifluoromethyl)phenyl]-1,1-dimethylurea, N,N-(1,4-phenylene)bis(N',N'-dimethylurea), and N,N-(4-methyl-1,3-phenylene)bis(N',N'-dimethylurea) [toluene bisdimethylurea].

[0121] Examples of the guanidine curing accelerator include dicyandiamide, 1-methylguanidine, 1-ethylguanidine, 1-cyclohexylguanidine, 1-phenylguanidine, 1-(o-tolyl)guanidine, dimethylguanidine, diphenylguanidine, trimethylguanidine, tetramethylguanidine, pentamethylguanidine, 1,5,7-triazabicyclo[4.4.0]dec-5-ene, 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene, 1-methylbiguanide, 1-ethylbiguanide, 1-n-butylbiguanide, 1-n-octadecylbiguanide, 1,1-dimethylbiguanide, 1,1-diethylbiguanide, 1-cyclohexylbiguanide, 1-allylbiguanide, 1-phenylbiguanide, and 1-(o-tolyl)biguanide.

[0122] Examples of the imidazole-based curing accelerator include 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, and 1-benzyl-2-methylimidazole. Phenylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazolium trimellitate, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl -(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct imidazole compounds such as 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2,3-dihydro-1H-pyrrolo[1,2-a]benzimidazole, 1-dodecyl-2-methyl-3-benzylimidazolium chloride, 2-methylimidazoline, and 2-phenylimidazoline, as well as adducts of imidazole compounds and epoxy resins.

[0123] As the imidazole-based curing accelerator, commercially available products may be used, for example, "1B2PZ", "2MZA-PW", "2PHZ-PW", and "C11Z-A" manufactured by Shikoku Chemical Industry Co., Ltd., and "P200-H50" manufactured by Mitsubishi Chemical Corporation.

[0124] Examples of metal-based curing accelerators include organometallic complexes or organometallic salts of metals such as cobalt, copper, zinc, iron, nickel, manganese, and tin. Specific examples of organometallic complexes include organocobalt complexes such as cobalt(II) acetylacetonate and cobalt(III) acetylacetonate, organocopper complexes such as copper(II) acetylacetonate, organozinc complexes such as zinc(II) acetylacetonate, organoiron complexes such as iron(III) acetylacetonate, organonickel complexes such as nickel(II) acetylacetonate, and organomanganese complexes such as manganese(II) acetylacetonate. Examples of organometallic salts include zinc octylate, tin octylate, zinc naphthenate, cobalt naphthenate, tin stearate, and zinc stearate.

[0125] Examples of the amine curing accelerator include trialkylamines such as triethylamine and tributylamine, 4-dimethylaminopyridine, benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, and 1,8-diazabicyclo(5,4,0)-undecene.

[0126] As the amine-based curing accelerator, a commercially available product may be used, for example, "MY-25" manufactured by Ajinomoto Fine-Techno Co., Ltd.

[0127] From the viewpoint of significantly obtaining the desired effects of the present invention, the content of the (F) component, relative to 100 mass% of the non-volatile components in the resin composition, is preferably 0.01 mass% or more, more preferably 0.05 mass% or more, even more preferably 0.1 mass% or more, and is preferably 1 mass% or less, more preferably 0.8 mass% or less, even more preferably 0.5 mass% or less.

[0128] <(G) Other Additives> The resin composition may further contain other additives as optional components in addition to the above-mentioned components. Examples of the (G) other additives include radical polymerizable compounds (excluding those corresponding to component (C)); thermoplastic resins; elastomers; polymerization initiators; organometallic compounds such as organocopper compounds, organozinc compounds, and organocobalt compounds; colorants such as phthalocyanine blue, phthalocyanine green, iodine green, diazo yellow, crystal violet, titanium oxide, and carbon black; polymerization inhibitors such as hydroquinone, catechol, pyrogallol, and phenothiazine; leveling agents such as silicone-based leveling agents and acrylic polymer-based leveling agents; thickeners such as bentone and montmorillonite; defoamers such as silicone-based defoamers, acrylic defoamers, fluorine-based defoamers, and vinyl resin-based defoamers; ultraviolet absorbers such as benzotriazole-based ultraviolet absorbers; adhesion improvers such as urea silane; density enhancers such as triazole-based adhesion imparting agents, tetrazole-based adhesion imparting agents, and triazine-based adhesion imparting agents. adhesion imparting agents; antioxidants such as hindered phenol-based antioxidants; fluorescent brightening agents such as stilbene derivatives; surfactants such as fluorine-based surfactants and silicone-based surfactants; flame retardants such as phosphorus-based flame retardants (e.g., phosphate ester compounds, phosphazene compounds, phosphinic acid compounds, red phosphorus), nitrogen-based flame retardants (e.g., melamine sulfate), halogen-based flame retardants, and inorganic flame retardants (e.g., antimony trioxide); dispersants such as phosphate ester-based dispersants, polyoxyalkylene-based dispersants, acetylene-based dispersants, silicone-based dispersants, anionic dispersants, and cationic dispersants; stabilizers such as borate-based stabilizers, titanate-based stabilizers, aluminate-based stabilizers, zirconate-based stabilizers, isocyanate-based stabilizers, carboxylic acid-based stabilizers, and carboxylic anhydride-based stabilizers; photopolymerization initiation assistants such as tertiary amines; and photosensitizers such as pyrarizones, anthracenes, coumarins, xanthones, and thioxanthones. (G) Other additives may be used alone or in combination of two or more.

[0129] <(H) Solvent> The resin composition may further contain an arbitrary solvent as a volatile component in addition to the non-volatile components described above. As the (H) solvent, a known solvent can be appropriately used, and the type is not particularly limited, and it is preferable that the solvent is an organic solvent. As the (H) solvent, for example, ketone-based solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, etc.; ester-based solvents such as methyl acetate, ethyl acetate, butyl acetate, isobutyl acetate, isoamyl acetate, methyl propionate, ethyl propionate, γ-butyrolactone, etc.; ether-based solvents such as tetrahydropyran, tetrahydrofuran, 1,4-dioxane, diethyl ether, diisopropyl ether, dibutyl ether, diphenyl ether, anisole, etc.; alcohol-based solvents such as methanol, ethanol, propanol, butanol, ethylene glycol, etc.; 2-ethoxyethyl acetate, propylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, ethyl diglycol acetate, γ-butyrolactone, methyl methoxypropionate, etc. Examples of the solvent include ether ester solvents such as ethyl acetate, ester alcohol solvents such as methyl lactate, ethyl lactate, and methyl 2-hydroxyisobutyrate, ether alcohol solvents such as 2-methoxypropanol, 2-methoxyethanol, 2-ethoxyethanol, propylene glycol monomethyl ether, and diethylene glycol monobutyl ether (butylcarbitol), amide solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone, sulfoxide solvents such as dimethyl sulfoxide, nitrile solvents such as acetonitrile and propionitrile, aliphatic hydrocarbon solvents such as hexane, cyclopentane, cyclohexane, and methylcyclohexane, and aromatic hydrocarbon solvents such as benzene, toluene, xylene, ethylbenzene, and trimethylbenzene. The (H) solvent may be used alone or in combination of two or more in any ratio.

[0130] From the viewpoint of obtaining the effect of the present invention significantly, the resin composition preferably contains 0.5% by mass or more and 3% by mass or less of the (H) solvent, based on 100% by mass of all the components of the resin composition. Specifically, the (H) solvent is preferably contained in an amount of 3% by mass or less, more preferably 2% by mass or less, and even more preferably 1.5% by mass or less, based on 100% by mass of all the components of the resin composition, and is preferably contained in an amount of 0.5% by mass or more, more preferably 0.8% by mass or more, and even more preferably 1% by mass or more.

[0131] The method for preparing the resin composition of the present invention is not particularly limited, and examples thereof include a method in which the blending components are mixed and dispersed using a rotary mixer or the like, with the addition of a solvent or the like as necessary.

[0132] <Physical properties and applications of resin compositions> The resin composition contains component (A), component (B), and a predetermined amount of component (C). This makes it possible to obtain a cured product with excellent bending resistance and to suppress the amount of resin seepage. Furthermore, it becomes possible to obtain a cured product with low dielectric tangent and dielectric constant.

[0133] The resin composition contains a combination of the (B) component and a predetermined amount of the (C) component, and therefore exhibits the characteristic of suppressing the amount of resin seepage. Specifically, a resin composition layer of a resin sheet is laminated on a glass cloth-based epoxy resin double-sided copper-clad laminate having a copper foil thickness of 18 μm, and then heat-cured at 130° C. for 30 minutes and then at 170° C. for 30 minutes to form an insulating layer. During lamination, the resin composition flows, and the amount of resin composition seeping out from the support is measured by measuring the distance from the end of the support to the end of the resin that has seeped out. The distance at that time is the amount of resin seepage, and the amount of resin seepage is preferably 5 mm or less. There is no particular limit to the lower limit, but it may be 0 mm or more, 0.01 mm or more, etc. The amount of resin seepage can be measured according to the method described in the examples described below.

[0134] Since the resin composition contains a combination of the (B) component and a predetermined amount of the (C) component, the cured product obtained by thermally curing the resin composition at 190° C. for 90 minutes exhibits the property of excellent bending resistance. Thus, the cured product provides an insulating layer with excellent bending resistance. The bending resistance is measured using an MIT test device under the measurement conditions of a load of 2.5 N, a bending angle of 90 degrees, a bending radius of 1.0 mm, and a bending speed of 175 times / min. The number of times the cured product is bent under the above conditions is preferably 300 times or more, more preferably 380 times or more, and even more preferably 400 times or more, 450 times or more. There is no particular upper limit, but it may be 10,000 times or less. The bending resistance can be measured according to the method described in the examples described below.

[0135] A cured product obtained by thermally curing a resin composition at 190°C for 90 minutes usually exhibits the characteristic of a low dielectric loss tangent. Thus, the cured product provides an insulating layer with a low dielectric loss tangent. The dielectric loss tangent is preferably 0.005 or less, more preferably 0.004 or less, and even more preferably 0.003 or less. The lower limit of the dielectric loss tangent may be 0.0001 or more. The dielectric loss tangent can be measured according to the method described in the examples below.

[0136] A cured product obtained by thermally curing a resin composition at 190°C for 90 minutes usually exhibits the characteristic of a low dielectric constant. Thus, the cured product provides an insulating layer with a low dielectric constant. The dielectric constant is preferably 4 or less, more preferably 3.8 or less, and even more preferably 3.5 or less. The lower limit of the dielectric constant may be 0.001 or more. The dielectric constant can be measured according to the method described in the examples below.

[0137] The resin composition of the present invention can obtain a cured product having excellent bending resistance, and can suppress the amount of resin seepage. Furthermore, it is possible to obtain a cured product having a low dielectric tangent and dielectric constant. Therefore, the resin composition of the present invention can be suitably used as a resin composition for insulation purposes. Specifically, it can be suitably used as a resin composition for forming an insulating layer (resin composition for forming an insulating layer) for forming a conductor layer (including a rewiring layer) formed on an insulating layer.

[0138] Furthermore, in the multilayer printed wiring board described below, the resin composition can be suitably used as a resin composition for forming an insulating layer of a multilayer printed wiring board (resin composition for forming an insulating layer of a multilayer printed wiring board) and a resin composition for forming an interlayer insulating layer of a printed wiring board (resin composition for forming an interlayer insulating layer of a printed wiring board).

[0139] In addition, for example, when a semiconductor chip package is manufactured through the following steps (1) to (6), the resin composition of the present invention can be suitably used as a resin composition for a rewiring formation layer (resin composition for forming a rewiring formation layer) as an insulating layer for forming a rewiring layer, and as a resin composition for sealing a semiconductor chip (resin composition for sealing a semiconductor chip). When a semiconductor chip package is manufactured, a rewiring layer may be further formed on the sealing layer. (1) A step of laminating a temporary fixing film onto a substrate; (2) a step of temporarily fixing a semiconductor chip on a temporary fixing film; (3) forming an encapsulation layer on the semiconductor chip; (4) peeling the substrate and the temporary fixing film from the semiconductor chip; (5) forming a rewiring formation layer as an insulating layer on the surface of the semiconductor chip from which the base material and the temporary fixing film have been peeled off; and (6) A process of forming a rewiring layer as a conductor layer on the rewiring formation layer.

[0140] [Resin sheet] The resin sheet of the present invention includes a support and a resin composition layer formed from the resin composition of the present invention provided on the support.

[0141] The thickness of the resin composition layer is preferably 100 μm or less, more preferably 80 μm or less, and even more preferably 50 μm or less, from the viewpoint of making the printed wiring board thinner and being able to provide a cured product with excellent insulation even if the cured product of the resin composition is a thin film. The lower limit of the thickness of the resin composition layer is not particularly limited, but can usually be 5 μm or more.

[0142] Examples of the support include films made of plastic materials, metal foils, and release papers, with films made of plastic materials and metal foils being preferred.

[0143] When a film made of a plastic material is used as the support, examples of the plastic material include polyesters such as polyethylene terephthalate (hereinafter sometimes abbreviated as "PET") and polyethylene naphthalate (hereinafter sometimes abbreviated as "PEN"), polycarbonate (hereinafter sometimes abbreviated as "PC"), acrylics such as polymethyl methacrylate (PMMA), cyclic polyolefins, triacetyl cellulose (TAC), polyether sulfide (PES), polyether ketone, polyimide, etc. Among these, polyethylene terephthalate and polyethylene naphthalate are preferred, and inexpensive polyethylene terephthalate is particularly preferred.

[0144] When a metal foil is used as the support, examples of the metal foil include copper foil, aluminum foil, etc., and copper foil is preferred. As the copper foil, a foil made of a single metal, copper, or an alloy of copper and another metal (e.g., tin, chromium, silver, magnesium, nickel, zirconium, silicon, titanium, etc.) may be used.

[0145] The surface of the support to be bonded to the resin composition layer may be subjected to a matte treatment, a corona treatment, or an antistatic treatment.

[0146] In addition, as the support, a support with a release layer having a release layer on the surface to be bonded to the resin composition layer may be used. The release agent used in the release layer of the support with a release layer may be, for example, one or more release agents selected from the group consisting of alkyd resins, polyolefin resins, urethane resins, and silicone resins. The support with a release layer may be a commercially available product, for example, "SK-1", "AL-5", and "AL-7" manufactured by Lintec Corporation, "Lumirror T60" manufactured by Toray Industries, Inc., "Purex" manufactured by Teijin Limited, and "Unipeel" manufactured by Unitika Limited, which are PET films having a release layer mainly composed of an alkyd resin-based release agent.

[0147] The thickness of the support is not particularly limited, but is preferably in the range of 5 μm to 75 μm, and more preferably in the range of 10 μm to 60 μm. When a support with a release layer is used, it is preferable that the total thickness of the support with a release layer is in the above range.

[0148] In one embodiment, the resin sheet may further include other layers as necessary. Examples of such other layers include a protective film equivalent to the support provided on the surface of the resin composition layer that is not bonded to the support (i.e., the surface opposite to the support). The thickness of the protective film is not particularly limited, but is, for example, 1 μm to 40 μm. By laminating the protective film, adhesion of dirt and the like to the surface of the resin composition layer and scratches can be suppressed.

[0149] The resin sheet can be produced, for example, by preparing a resin varnish by dissolving the resin composition in a solvent, applying the resin varnish onto a support using a die coater or the like, and then drying the varnish to form a resin composition layer. The solvent is as described above.

[0150] Drying may be performed by a known method such as heating or hot air blowing. Drying conditions are not particularly limited, but drying is performed so that the content of the solvent in the resin composition layer becomes 10 mass % or less, preferably 5 mass % or less. Although it varies depending on the boiling point of the solvent in the resin varnish, for example, when a resin varnish containing 30 mass % to 60 mass % of the solvent is used, the resin composition layer can be formed by drying at 50°C to 150°C for 3 minutes to 10 minutes.

[0151] The resin sheet can be stored in a rolled state. When the resin sheet has a protective film, it can be used by peeling off the protective film.

[0152] [Printed wiring board] The printed wiring board of the present invention includes an insulating layer formed from a cured product of the resin composition of the present invention.

[0153] The printed wiring board can be produced, for example, by using the above-mentioned resin sheet by a method including the following steps (I) and (II). (I) A step of laminating a resin sheet on an inner layer substrate so that a resin composition layer of the resin sheet is bonded to the inner layer substrate. (II) A step of thermally curing the resin composition layer to form an insulating layer

[0154] The "inner layer substrate" used in step (I) is a member that becomes the substrate of a printed wiring board, and examples thereof include a glass epoxy substrate, a metal substrate, a polyester substrate, a polyimide substrate, a BT resin substrate, and a thermosetting polyphenylene ether substrate. The substrate may have a conductor layer on one or both sides, and the conductor layer may be patterned. An inner layer substrate having a conductor layer (circuit) formed on one or both sides of the substrate may be called an "inner layer circuit substrate". In addition, an intermediate product on which an insulating layer and / or a conductor layer is to be further formed during the manufacture of a printed wiring board is also included in the "inner layer substrate" of the present invention. When the printed wiring board is a circuit board with built-in components, an inner layer substrate with built-in components may be used.

[0155] The lamination of the inner layer substrate and the resin sheet can be carried out, for example, by thermocompression bonding the resin sheet to the inner layer substrate from the support side. Examples of the member for thermocompression bonding the resin sheet to the inner layer substrate (hereinafter also referred to as the "thermocompression bonding member") include a heated metal plate (such as a SUS plate) or a metal roll (SUS roll). It is preferable to press the thermocompression member not directly onto the resin sheet, but via an elastic material such as heat-resistant rubber so that the resin sheet can sufficiently follow the surface irregularities of the inner layer substrate.

[0156] The lamination of the inner layer substrate and the resin sheet may be performed by a vacuum lamination method. In the vacuum lamination method, the thermocompression temperature is preferably in the range of 60°C to 160°C, more preferably in the range of 80°C to 140°C, the thermocompression pressure is preferably in the range of 0.098MPa to 1.77MPa, more preferably in the range of 0.29MPa to 1.47MPa, and the thermocompression time is preferably in the range of 20 seconds to 400 seconds, more preferably in the range of 30 seconds to 300 seconds. The lamination is preferably performed under reduced pressure conditions of 26.7hPa or less.

[0157] The lamination can be performed by a commercially available vacuum laminator, such as a vacuum pressure laminator manufactured by Meiki Seisakusho Co., Ltd., a vacuum applicator manufactured by Nikko Materials Co., Ltd., or a batch type vacuum pressure laminator.

[0158] After lamination, the laminated resin sheet may be smoothed under normal pressure (atmospheric pressure), for example, by pressing a thermocompression member from the support side. The pressing conditions for the smoothing treatment may be the same as the thermocompression conditions for the lamination. The smoothing treatment may be performed using a commercially available laminator. The lamination and smoothing treatment may be performed consecutively using the commercially available vacuum laminator.

[0159] The support may be removed between step (I) and step (II) or after step (II).

[0160] In step (II), the resin composition layer is thermally cured to form an insulating layer. The conditions for thermally curing the resin composition layer are not particularly limited, and conditions that are usually employed when forming an insulating layer for a printed wiring board may be used.

[0161] For example, the thermal curing conditions for the resin composition layer vary depending on the type of resin composition, etc., but the curing temperature is preferably 120° C. to 240° C., more preferably 150° C. to 220° C., and even more preferably 170° C. to 210° C. The curing time is preferably 5 minutes to 120 minutes, more preferably 10 minutes to 100 minutes, and even more preferably 15 minutes to 100 minutes.

[0162] Before the resin composition layer is thermally cured, the resin composition layer may be preheated at a temperature lower than the curing temperature. For example, prior to thermally curing the resin composition layer, the resin composition layer may be preheated at a temperature of 50° C. or more and less than 120° C. (preferably 60° C. or more and 115° C. or less, more preferably 70° C. or more and 110° C. or less) for 5 minutes or more (preferably 5 minutes to 150 minutes, more preferably 15 minutes to 120 minutes, and even more preferably 15 minutes to 100 minutes).

[0163] In manufacturing a printed wiring board, the steps of (III) drilling holes in the insulating layer, (IV) roughening the insulating layer, and (V) forming a conductor layer may be further carried out. These steps (III) to (V) may be carried out according to various methods known to those skilled in the art for use in manufacturing printed wiring boards. When the support is removed after step (II), the support may be removed between step (II) and step (III), between step (III) and step (IV), or between step (IV) and step (V). In addition, the formation of the insulating layer and the conductor layer in steps (II) to (V) may be repeated to form a multilayer wiring board, as necessary.

[0164] Step (III) is a step of drilling holes in the insulating layer, which allows holes such as via holes and through holes to be formed in the insulating layer. Step (III) may be performed using, for example, a drill, a laser, plasma, etc., depending on the composition of the resin composition used to form the insulating layer. The dimensions and shape of the holes may be appropriately determined depending on the design of the printed wiring board.

[0165] Step (IV) is a step of roughening the insulating layer. Usually, in this step (IV), smears are also removed. The procedure and conditions of the roughening treatment are not particularly limited, and known procedures and conditions that are usually used when forming an insulating layer of a printed wiring board can be adopted. For example, the insulating layer can be roughened by performing a swelling treatment with a swelling liquid, a roughening treatment with an oxidizing agent, and a neutralization treatment with a neutralizing liquid in this order. The swelling liquid used in the roughening treatment is not particularly limited, but includes an alkaline solution, a surfactant solution, and the like, and is preferably an alkaline solution, and as the alkaline solution, a sodium hydroxide solution and a potassium hydroxide solution are more preferable. Examples of commercially available swelling liquids include "Swelling Dip Securigans P", "Swelling Dip Securigans SBU", and "Swelling Dip Securigant P" manufactured by Atotech Japan. The swelling treatment using a swelling liquid is not particularly limited, but can be performed, for example, by immersing the insulating layer in a swelling liquid at 30°C to 90°C for 1 to 20 minutes. From the viewpoint of suppressing the swelling of the resin of the insulating layer to an appropriate level, it is preferable to immerse the insulating layer in a swelling liquid at 40°C to 80°C for 5 to 15 minutes. The oxidizing agent used in the roughening treatment is not particularly limited, but examples thereof include an alkaline permanganate solution in which potassium permanganate or sodium permanganate is dissolved in an aqueous solution of sodium hydroxide. The roughening treatment using an oxidizing agent such as an alkaline permanganate solution is preferably performed by immersing the insulating layer in an oxidizing agent solution heated to 60°C to 100°C for 10 to 30 minutes. In addition, the concentration of permanganate in the alkaline permanganate solution is preferably 5% by mass to 10% by mass. Examples of commercially available oxidizing agents include alkaline permanganate solutions such as "Concentrate Compact CP" and "Dosing Solution Securiganth P" manufactured by Atotech Japan. The neutralizing solution used in the roughening treatment is preferably an acidic aqueous solution, and a commercially available product is, for example, "Reduction Solution Securiganth P" manufactured by Atotech Japan. Treatment with a neutralizing solution can be performed by immersing the surface that has been roughened with an oxidizing agent in the neutralizing solution at 30°C to 80°C for 1 to 30 minutes.From the viewpoint of workability etc., a method in which the object that has been subjected to roughening treatment with an oxidizing agent is immersed in a neutralizing solution at 40° C. to 70° C. for 5 minutes to 20 minutes is preferred.

[0166] In one embodiment, the arithmetic mean roughness (Ra) of the insulating layer surface after the roughening treatment is preferably 300 nm or less, more preferably 250 nm or less, and even more preferably 200 nm or less. There is no particular limit to the lower limit, but it is preferably 30 nm or more, more preferably 40 nm or more, and even more preferably 50 nm or more. The arithmetic mean roughness (Ra) of the insulating layer surface can be measured using a non-contact surface roughness meter.

[0167] Step (V) is a step of forming a conductor layer, and the conductor layer is formed on the insulating layer. The conductor material used for the conductor layer is not particularly limited. In a preferred embodiment, the conductor layer contains one or more metals selected from the group consisting of gold, platinum, palladium, silver, copper, aluminum, cobalt, chromium, zinc, nickel, titanium, tungsten, iron, tin and indium. The conductor layer may be a single metal layer or an alloy layer, and examples of the alloy layer include layers formed from alloys of two or more metals selected from the above group (e.g., nickel-chromium alloy, copper-nickel alloy and copper-titanium alloy). Among these, from the viewpoints of versatility in forming the conductor layer, cost, ease of patterning, and the like, a single metal layer of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver, or copper, or an alloy layer of a nickel-chromium alloy, a copper-nickel alloy, or a copper-titanium alloy is preferred, a single metal layer of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver, or copper, or an alloy layer of a nickel-chromium alloy is more preferred, and a single metal layer of copper is even more preferred.

[0168] The conductor layer may be a single-layer structure or a multi-layer structure in which two or more single metal layers or alloy layers made of different kinds of metals or alloys are laminated. When the conductor layer has a multi-layer structure, the layer in contact with the insulating layer is preferably a single metal layer of chromium, zinc or titanium, or an alloy layer of a nickel-chromium alloy.

[0169] The thickness of the conductor layer depends on the desired design of the printed wiring board, but is generally 3 μm to 35 μm, and preferably 5 μm to 30 μm.

[0170] In one embodiment, the conductor layer may be formed by plating. For example, a conductor layer having a desired wiring pattern can be formed by plating the surface of the insulating layer by a conventionally known technique such as a semi-additive method or a full-additive method, and from the viewpoint of ease of production, it is preferable to form the conductor layer by the semi-additive method. An example of forming the conductor layer by the semi-additive method will be described below.

[0171] First, a plating seed layer is formed on the surface of an insulating layer by electroless plating. Next, a mask pattern is formed on the formed plating seed layer to expose a part of the plating seed layer corresponding to a desired wiring pattern. After a metal layer is formed on the exposed plating seed layer by electrolytic plating, the mask pattern is removed. Thereafter, unnecessary plating seed layer is removed by etching or the like to form a conductor layer having a desired wiring pattern.

[0172] [Semiconductor Devices] The semiconductor device of the present invention includes the printed wiring board of the present invention. The semiconductor device of the present invention can be manufactured by using the printed wiring board of the present invention.

[0173] Examples of the semiconductor device include various semiconductor devices used in electric appliances (for example, computers, mobile phones, digital cameras, and televisions) and vehicles (for example, motorcycles, automobiles, trains, ships, and aircraft).

[0174] The semiconductor device of the present invention can be manufactured by mounting a component (semiconductor chip) on a conductive portion of a printed wiring board. The "conductive portion" refers to a portion of a printed wiring board that transmits an electric signal, and the portion may be either on the surface or embedded. The semiconductor chip is not particularly limited as long as it is an electric circuit element made of semiconductor material.

[0175] The method of mounting a semiconductor chip when manufacturing a semiconductor device is not particularly limited as long as the semiconductor chip functions effectively, but specific examples include a wire bonding mounting method, a flip chip mounting method, a bumpless buildup layer (BBUL) mounting method, an anisotropic conductive film (ACF) mounting method, a non-conductive film (NCF) mounting method, etc. Here, the "bumpless buildup layer (BBUL) mounting method" refers to "a mounting method in which a semiconductor chip is directly embedded in a recess in a printed wiring board and the semiconductor chip is connected to the wiring on the printed wiring board." EXAMPLES

[0176] The present invention will be described in more detail below using examples, but the present invention is not limited to these examples. In the following description, unless otherwise specified, "parts" and "%" mean "parts by mass" and "% by mass", respectively.

[0177] <Synthesis Example 1: Synthesis of Active Ester Resin A> In a flask equipped with a thermometer, a dropping funnel, a cooling tube, a fractionating tube, and a stirrer, 165g of a polyaddition reaction resin of dicyclopentadiene and phenol (hydroxyl equivalent: 165g / eq., softening point 85°C), 134g (1.0 mol) of ortho-allylphenol, and 1200g of toluene were charged, and the system was purged with nitrogen under reduced pressure. Then, 203g (1.0 mol) of isophthalic acid chloride was charged, and the system was purged with nitrogen under reduced pressure. 0.6g of tetrabutylammonium bromide was added, and while performing a nitrogen gas purging treatment, the system was controlled to 60°C or less, and 412g of a 20% aqueous sodium hydroxide solution was dropped over 3 hours, and after the dropwise addition, the mixture was stirred for 1.0 hour. After the reaction was completed, the aqueous layer was removed by standing and separating. Water was further added to the obtained toluene layer and stirred for 15 minutes, and the aqueous layer was removed by standing and separating. This operation was repeated until the pH of the aqueous layer reached 7. The non-volatile content was adjusted to 70% by mass by heat drying, thereby obtaining an active ester resin A represented by the following formula. [ka]

[0178] In the above chemical formula, each s is independently an integer of 0 or 1 or more, and the average value of r calculated from the charge ratio is 1. The dashed line in the chemical formula is a structure obtained by reacting isophthalic acid chloride with a polyaddition reaction resin of phenol and / or ortho-allylphenol. The ester group equivalent of the obtained active ester resin A was calculated from the charge ratio and was 214 g / eq.

[0179] <Synthesis Example 2: Synthesis of Active Ester Resin B> A flask equipped with a thermometer, a dropping funnel, a cooling tube, a fractionating tube, and a stirrer was charged with 320 g of diallyl bisphenol A and 1500 g of toluene, and the contents were dissolved while the flask was purged with nitrogen under reduced pressure. Next, 240 g of benzoyl chloride and 102 g of isophthalic acid chloride were charged, and the contents were dissolved while the flask was purged with nitrogen under reduced pressure. 0.8 g of tetrabutylammonium bromide was further added and dissolved. While purging with nitrogen gas, the system was controlled to 60°C or less, and 412 g of 20% aqueous sodium hydroxide solution was dropped over 3 hours. After the dropwise addition, stirring was continued for 1.0 hour under the same conditions. After the reaction was completed, the reaction mixture was left to stand and separated, and the aqueous layer was removed. Water was added to the remaining toluene phase, and the mixture was stirred and mixed for about 15 minutes, and the mixture was left to stand and the aqueous layer was removed. This operation was repeated until the pH of the aqueous layer reached 7. Then, the non-volatile content was adjusted to 70% by mass by heating and drying, and an active ester resin B represented by the following formula was obtained. [ka]

[0180] In the above formula, the average value of m2 calculated from the charge ratio was 1. The ester group equivalent of the obtained active ester resin B was calculated from the charge ratio and was 245 g / eq.

[0181] <Example 1: Preparation of resin composition 1> Naphthalene type epoxy resin (DIC Corporation "HP-4032-SS", epoxy equivalent 144 g / eq.) 5 parts, naphthalene aralkyl type epoxy resin (Nippon Steel Chemical & Material Corporation "ESN-475V", epoxy equivalent 330 g / eq.) 10 parts, biphenyl aralkyl type epoxy resin (Nippon Kayaku Co., Ltd. "NC-3000L", epoxy equivalent 269 g / eq.) 5 parts, active ester resin A synthesized in Synthesis Example 1 30 parts, rubber particles (Dow Chemical Japan "EXL2655") 2 parts, other hardeners (phenolic hardener, DIC "LA-3018-50P", hydroxyl equivalent 151 g / eq., 1-methoxy-2-propanol solution with non-volatile content of 50% by mass), inorganic filler (spherical silica surface-treated with an amine-based alkoxysilane compound (Shin-Etsu Chemical Co., Ltd. "KBM573") (Admatechs Co., Ltd. "SO-C2", average particle size 0.5 μm, specific surface area 5.8 m) 2 Resin composition 1 was obtained by mixing 130 parts of cellulose acetate / g), 0.3 parts of a curing accelerator (manufactured by Shikoku Chemical Industry Co., Ltd., "1B2PZ"), 20 parts of MEK, and 10 parts of cyclohexanone and dispersing the mixture uniformly using a high-speed rotating mixer.

[0182] <Example 2: Preparation of resin composition 2> In Example 1, 30 parts of the active ester resin A synthesized in Synthesis Example 1 was changed to 30 parts of the active ester resin B synthesized in Synthesis Example 2. Resin composition 2 was obtained in the same manner as in Example 1 except for the above.

[0183] <Example 3: Preparation of resin composition 3> In Example 1, 2 parts of rubber particles (manufactured by Dow Chemical Japan, "EXL2655") were changed to 2 parts of rubber particles (manufactured by Aica Kogyo, "AC3816N"). Resin composition 3 was obtained in the same manner as in Example 1 except for the above.

[0184] <Example 4: Preparation of resin composition 4> In Example 1, 4 parts of a carbodiimide curing agent ("V-03" manufactured by Nisshinbo Chemical Inc., active group equivalent of about 216 / eq., toluene solution with non-volatile content of 50%) was used. Resin composition 4 was obtained in the same manner as in Example 1 except for the above.

[0185] <Example 5: Preparation of resin composition 5> In Example 4, 30 parts of the active ester resin A synthesized in Synthesis Example 1 was changed to 30 parts of the active ester resin B synthesized in Synthesis Example 2. Resin composition 5 was obtained in the same manner as in Example 4 except for the above.

[0186] <Example 6: Preparation of resin composition 6> In Example 1, the amount of rubber particles (Dow Chemical Japan's "EXL2655") was changed from 2 parts to 6 parts. Resin composition 6 was obtained in the same manner as in Example 1 except for the above.

[0187] <Example 7: Preparation of resin composition 7> In Example 1, 1) Spherical silica (Admatechs, "SO-C2", average particle size 0.5 μm, specific surface area 5.8 m) surface-treated with an inorganic filler (amine-based alkoxysilane compound (Shin-Etsu Chemical Co., Ltd., "KBM573"). 2 / g) from 130 parts to 65 parts, 2) 25 parts of an inorganic filler having hollow portions (spherical silica having hollow portions (average particle size 0.5 μm, porosity 50 vol%, Ube Exsymo's "LHP-208") surface-treated with an amine-based alkoxysilane compound (Shin-Etsu Chemical Co., Ltd.'s "KBM573")) was used. Resin composition 7 was obtained in the same manner as in Example 1 except for the above.

[0188] <Example 8: Preparation of resin composition 8> In Example 4, 5 parts of the other curing agent (phenol-based curing agent, "LA-3018-50P" manufactured by DIC Corporation, hydroxyl equivalent 151 g / eq., 1-methoxy-2-propanol solution with non-volatile content of 50 mass %) was changed to 5 parts of a 50 mass % MEK solution of the other curing agent (phenol-based curing agent, "KAYAHARD GPH103" manufactured by Nippon Kayaku Co., Ltd., hydroxyl equivalent 231 g / eq.). Resin composition 8 was obtained in the same manner as in Example 4 except for the above.

[0189] <Example 9: Preparation of resin composition 9> In Example 4, 1) The amount of active ester resin A synthesized in Synthesis Example 1 was changed from 30 parts to 20 parts. 2) In addition, 10.8 parts of an active ester curing agent (DIC Corporation's "HPC-8000-65T", active group equivalent 223 g / eq., toluene solution with non-volatile content of 65% by mass) was used. Resin composition 9 was obtained in the same manner as in Example 4 except for the above.

[0190] <Example 10: Preparation of resin composition 10> In Example 4, 1) The amount of active ester resin A synthesized in Synthesis Example 1 was changed from 30 parts to 10 parts. 2) In addition, 21.5 parts of an active ester curing agent (DIC Corporation's "HPC-8000-65T", active group equivalent 223 g / eq., toluene solution with non-volatile content of 65% by mass) was used. A resin composition 10 was obtained in the same manner as in Example 4 except for the above.

[0191] <Example 11: Preparation of resin composition 11> In Example 2, 1) The amount of active ester resin B synthesized in Synthesis Example 2 was changed from 30 parts to 15 parts. 2) In addition, 16.2 parts of an active ester curing agent (DIC Corporation's "HPC-8000-65T", active group equivalent 223 g / eq., toluene solution with non-volatile content of 65% by mass) was used. Resin composition 11 was obtained in the same manner as in Example 2 except for the above.

[0192] <Example 12: Preparation of resin composition 12> In Example 2, 30 parts of the active ester resin B synthesized in Synthesis Example 2 was changed to 30 parts of the active ester resin C shown below (wherein m, n≧0, toluene solution with 70 mass% nonvolatile content, functional group equivalent of 250 g / eq.). Resin composition 12 was obtained in the same manner as in Example 2 except for the above. [ka]

[0193] <Example 13: Preparation of resin composition 13> In Example 11, 15 parts of the active ester resin B synthesized in Synthesis Example 2 was changed to 15 parts of the active ester resin C. Resin composition 13 was obtained in the same manner as in Example 11 except for the above.

[0194] <Comparative Example 1: Preparation of Resin Composition 14> In Example 1, 2 parts of rubber particles ("EXL2655" manufactured by Dow Chemical Japan) were not used. Resin composition 14 was obtained in the same manner as in Example 1 except for the above points.

[0195] <Comparative Example 2: Preparation of Resin Composition 15> In Example 1, 30 parts of the active ester A resin synthesized in Synthesis Example 1 was changed to 32.3 parts of an active ester curing agent (DIC Corporation's "HPC-8000-65T", active group equivalent 223 g / eq., toluene solution with non-volatile content of 65% by mass). Resin composition 15 was obtained in the same manner as in Example 1 except for the above.

[0196] <Comparative Example 3: Preparation of resin composition 16> In Example 1, the amount of rubber particles (Dow Chemical Japan's "EXL2655") was changed from 2 parts to 12 parts. Resin composition 16 was obtained in the same manner as in Example 1 except for the above points.

[0197] <Measurement of the average particle size of inorganic fillers> 100 mg of inorganic filler, 0.1 g of dispersant (SAN NOPCO "SN9228"), and 10 g of methyl ethyl ketone were weighed into a vial and dispersed by ultrasonic waves for 20 minutes. Using a laser diffraction particle size distribution measuring device (Shimadzu Corporation "SALD-2200"), the particle size distribution was measured by the batch cell method, and the average particle size was calculated based on the median diameter.

[0198] <Preparation of resin sheet> As a support, a polyethylene terephthalate film ("Lumirror R80" manufactured by Toray Industries, Inc., thickness 38 μm, softening point 130° C.) that had been subjected to a release treatment with an alkyd resin-based release agent ("AL-5" manufactured by Lintec Corporation) was prepared.

[0199] Each of the resin compositions 1 to 16 was uniformly applied onto a support by a die coater so that the thickness of the resin composition layer after drying was 40 μm, and dried at 70° C. to 100° C. for 3 minutes to form a resin composition layer on the support. Next, the rough surface of a polypropylene film (Oji F-Tex Co., Ltd. "Alphan MA-411", thickness 15 μm) was attached as a protective film to the surface of the resin composition layer that was not bonded to the support. This resulted in a resin sheet having the support, the resin composition layer, and the protective film in this order.

[0200] <Test Example 1: Measurement of dielectric properties (dielectric constant, dielectric tangent)> The protective film was peeled off from the prepared resin sheet, and the resin composition layer was thermally cured by heating at 190°C for 90 minutes, and then the support was peeled off. This is called evaluation cured product C. The obtained evaluation cured product C was cut into a test piece having a width of 2 mm and a length of 80 mm. The dielectric constant and dielectric loss tangent of the test piece were measured at a measurement frequency of 5.8 GHz and a measurement temperature of 23°C by a cavity resonance perturbation method using an "HP8362B" manufactured by Agilent Technologies. Measurements were performed on three test pieces, and the average values ​​were calculated.

[0201] <Test Example 2: Measurement of MIT folding endurance> The cured product C for evaluation obtained in Test Example 1 was cut into test pieces measuring 15 mm in width and 110 mm in length, and a bending test was carried out using an MIT testing device (MIT folding fatigue tester "MIT-DA", manufactured by Toyo Seiki Seisakusho) under the measurement conditions of a load of 2.5 N, a bending angle of 90 degrees, a bending radius of 1.0 mm, and a bending speed of 175 times / min. The test pieces were evaluated according to the following criteria. ◯: The cured product C for evaluation was bent 300 times or more until it broke. ×: The number of times that the cured product C for evaluation was bent until it broke was less than 300.

[0202] <Test Example 3: Measurement of resin seepage amount (resin flow amount)> (1) Preparation of inner layer board Both sides of a glass cloth-based epoxy resin double-sided copper-clad laminate (copper foil thickness 18 μm, board thickness 0.4 mm, board size 340 mm × 255 mm, Panasonic "R1515A") with an inner layer circuit formed were etched 1 μm with a microetching agent (Mec "CZ8101") to roughen the copper surface.

[0203] (2) Lamination of resin sheet The protective film was peeled off from the prepared resin sheet (200 mm x 250 mm) to expose the resin composition layer. Using a batch-type vacuum pressure laminator (Nikko Materials Co., Ltd., 2-stage build-up laminator "CVP700"), the resin composition layer was laminated on both sides of the inner layer substrate so that it was in contact with the inner layer substrate. The lamination was performed by reducing the pressure for 30 seconds to adjust the air pressure to 13 hPa or less, and then pressing at 120°C and a pressure of 0.98 MPa for 30 seconds. Next, a heat press was performed at 120°C and a pressure of 0.54 MPa for 60 seconds.

[0204] (3) Thermal curing of the resin composition layer The inner layer substrate laminated with the resin sheet was then placed in a 130°C oven and heated for 30 minutes, and then transferred to a 170°C oven and heated for 30 minutes to thermally cure the resin composition layer and form an insulating layer.

[0205] (4) Observation of the amount of resin seeping out In the insulating layer, a resin exudation portion was formed on the outside of the support due to the flow of the resin composition during lamination. The amount of resin composition exuding from the support was determined by measuring the distance from the end of the support to the end of the exuded resin, and was evaluated according to the following criteria. ○: The amount of leakage is 5mm or less. ×: The amount of seepage is greater than 5 mm.

[0206] [Table 1] *In the table, the content of each component is the value when the non-volatile components in the resin composition are taken as 100 mass %.

Claims

1. (A) an epoxy resin, (B) an active ester resin having an allyl group, and (C) a resin composition containing an organic filler, A resin composition, wherein the content of component (C) is 6 mass% or less, when the total amount of non-volatile components in the resin composition is 100 mass%.

2. The resin composition according to claim 1 , further comprising (D) a curing agent.

3. 3. The resin composition according to claim 2, wherein the component (D) comprises one or more selected from the group consisting of a phenol-based curing agent, a naphthol-based curing agent, a carbodiimide-based curing agent, an active ester-based curing agent (excluding those corresponding to the component (B)), a benzoxazine-based curing agent, and a cyanate ester-based curing agent.

4. The resin composition according to claim 1 , further comprising (E) an inorganic filler.

5. The resin composition according to claim 1, wherein the component (B) includes any one of a compound represented by general formula (B-1), a compound represented by general formula (B-2), and a compound represented by general formula (B-3). 【Chemistry 1】 (In general formula (B-1), Ar 11 each independently represents a monovalent aromatic hydrocarbon group which may have a substituent; Ar 12 each independently represents a divalent aromatic hydrocarbon group which may have a substituent; Ar 13 each independently represents a divalent aromatic hydrocarbon group which may have a substituent, a divalent aliphatic hydrocarbon group which may have a substituent, an oxygen atom, a sulfur atom, or a divalent group consisting of a combination thereof; and n represents an integer of 0 to 10. 【Chemistry 2】 (In general formula (B-2), Ar 21 each independently represents a monovalent aromatic hydrocarbon group which may have a substituent; Ar 22 each independently represents a divalent hydrocarbon group which may have a substituent; Ar 23 each independently represents a divalent aromatic hydrocarbon group which may have a substituent; and m represents an integer of 0 to 10. 【Chemistry 3】 (In general formula (B-3), Ar 21 each independently represents a monovalent aromatic hydrocarbon group which may have a substituent; Ar 31 each independently represents a divalent aromatic hydrocarbon group which may have a substituent; Ar 13 each independently represents a divalent aromatic hydrocarbon group which may have a substituent, a divalent aliphatic hydrocarbon group which may have a substituent, an oxygen atom, a sulfur atom, or a divalent group consisting of a combination thereof; mb and nb each independently represent 0 or more.

6. The resin composition according to claim 1 , wherein the content of the component (B) is 1% by mass or more and 25% by mass or less, when the total amount of non-volatile components in the resin composition is 100% by mass.

7. The resin composition according to claim 1, wherein the component (C) comprises core-shell type particles.

8. A resin sheet comprising a support and a resin composition layer provided on the support, the resin composition layer comprising the resin composition according to any one of claims 1 to 7.

9. A printed wiring board comprising an insulating layer formed from a cured product of the resin composition according to any one of claims 1 to 7.

10. A semiconductor device comprising the printed wiring board according to claim 9.

Citation Information

Patent Citations

  • Resist composition, its curing method and use

    JP2005194504A

  • Resin composition

    JP2016156019A

  • Resin composition

    JP2018044040A

  • Resin composition

    JP2019108557A

  • Resin composition, cured product of resin composition, resin sheet, printed wiring board, and semiconductor device

    JP2021028368A

Cited By

  • Circuit board production method

    WO2026211305A1