The adhesive tape with controlled shear modulus and peel strength, combined with specific acrylic polymers, addresses adhesion and peeling issues in semiconductor manufacturing, enhancing the transfer and retransfer of micro LED chips by ensuring effective adhesion and minimizing residue.

JP2024163338APending Publication Date: 2024-11-21SEKISUI CHEMICAL CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024160036
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-12-28
Filing Date
2024-09-17
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Conventional adhesive tapes used as carrier materials for chip components in semiconductor manufacturing, such as micro LED displays, face issues with poor adhesion, improper peeling, and adhesive residue during the transfer process, leading to inefficient transfer and retransfer of micro LED chips.

Method used

An adhesive tape with a shear storage modulus G' of 1 MPa or less at 10 Hz and -20°C, surface peel strength of 0.5 MPa or less, and an acrylic adhesive layer containing specific (meth)acrylic polymers with controlled glass transition temperatures and molecular structures, ensuring effective adhesion and peeling performance.

Benefits of technology

The adhesive tape effectively adheres chip components during reception and exhibits excellent peeling performance during retransfer, minimizing adhesive residue, thereby improving the transfer and retransfer efficiency of micro LED chips.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024163338000001_ABST
    Figure 2024163338000001_ABST
Patent Text Reader

Abstract

To provide a pressure-sensitive adhesive tape that can have chip components suitably pasted thereto when receiving the chip components, that exhibits excellent detachment performance when re-transferring the chip components, and that can prevent an adhesive from being left on the chip components.SOLUTION: A pressure-sensitive adhesive tape has at least one layer of a base material and at least one layer of a pressure sensitive adhesive layer. The pressure sensitive adhesive layer has a shear storage modulus G' of 1 MPa or less at a frequency of 10 Hz at -20°C. The pressure-sensitive adhesive tape exhibits a surface detachment strength of 0.5 MPa or less with respect to SUS in an attachment area of 10 mm×10 mm.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an adhesive tape. [Background technology]

[0002] In the manufacturing process of semiconductor devices, a large number of chip components arranged on an adhesive layer are often transferred onto a drive circuit board. For example, a micro LED display is a display device in which each chip that makes up a pixel is a tiny light emitting diode (LED, Light Emitting Diode) chip, and these micro LED chips emit light to display images. Micro LED displays have high contrast, a fast response speed, and can be made thin because they do not require the color filters used in liquid crystal displays, organic electroluminescence displays, etc., and are therefore attracting attention as next-generation display devices. In a micro LED display, many micro LED chips are densely packed in a flat surface.

[0003] In the manufacturing process of semiconductor devices such as micro LED displays, for example, a transfer laminate having a large number of chip components arranged on an adhesive layer is placed opposite a drive circuit board, and the chip components are peeled off from the transfer laminate to make an electrical connection with the drive circuit board (transfer process).

[0004] The transfer step may be performed multiple times. That is, before the chip components are finally transferred onto the drive circuit board, the chip components are once transferred onto a carrier material for transportation or processing, and then the chip components are retransferred from the carrier material to another carrier material or onto the drive circuit board. For example, Patent Document 1 describes a transfer substrate having at least a base material and an impact absorbing layer as a carrier material. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2019 / 065441 Summary of the Invention [Problem to be solved by the invention]

[0006] Since the carrier material is also required to have the ability to temporarily hold the chip components, the use of an adhesive tape having an adhesive layer is also being considered. However, when a conventional adhesive tape is used as a carrier material, the chip components do not adhere to the adhesive tape when they are received, and transfer cannot be performed satisfactorily. In addition, when the chip components are transferred again to another carrier material or a drive circuit board after being received, there are problems such as poor peeling of the chip components, and even if the chip components can be peeled off, residue of the adhesive layer adheres to the chip components.

[0007] To provide an adhesive tape which can adhere a chip component well when receiving the chip component, exhibits excellent peeling performance when retransferring the chip component, and can suppress adhesive residue on the chip component. [Means for solving the problem]

[0008] Disclosure 1 relates to an adhesive tape having at least one layer of substrate and at least one layer of adhesive layer, wherein the adhesive layer has a shear storage modulus G' of 1 MPa or less at a frequency of 10 Hz and at -20°C, and the adhesive tape has a surface peel strength against SUS of 0.5 MPa or less in an application area of ​​10 mm x 10 mm. Disclosure 2 is the pressure-sensitive adhesive tape of Disclosure 1, wherein the pressure-sensitive adhesive layer has a shear storage modulus G' at a frequency of 10 Hz and at -20°C of 0.3 MPa or less. The present disclosure 3 is the pressure-sensitive adhesive tape according to the present disclosure 1 or 2, wherein the pressure-sensitive adhesive layer has a shear storage modulus G' at a frequency of 10 Hz and 23° C. of 0.04 MPa or less. The present disclosure 4 is the pressure-sensitive adhesive tape of the present disclosure 1, 2, or 3, wherein the pressure-sensitive adhesive layer has a thickness of 40 μm or more. The present disclosure 5 is a pressure-sensitive adhesive tape according to the present disclosure 1, 2, 3, or 4, which has a surface peel strength to SUS of 0.01 MPa or more in an application area of ​​10 mm×10 mm. The present disclosure 6 is a pressure-sensitive adhesive tape according to the present disclosure 1, 2, 3, 4, or 5, which has a surface peel strength to SUS of 0.2 MPa or less in an application area of ​​10 mm×10 mm. The present disclosure 7 is the pressure-sensitive adhesive tape of the present disclosure 1, 2, 3, 4, 5, or 6, wherein the pressure-sensitive adhesive layer is an acrylic pressure-sensitive adhesive layer containing a (meth)acrylic polymer. The present disclosure 8 is the pressure-sensitive adhesive tape of the present disclosure 7, wherein the (meth)acrylic polymer has a hydroxyl value of 45 mgKOH / g or less. The present disclosure 9 is a pressure-sensitive adhesive tape according to the present disclosure 7 or 8, wherein the (meth)acrylic polymer contains 80% by weight or more of a structural unit derived from a (meth)acrylic acid ester (a) having a glass transition temperature (Tg) of 0°C or lower when made into a homopolymer. The present disclosure 10 is the pressure-sensitive adhesive tape of the present disclosure 9, wherein the (meth)acrylic polymer contains 40% by weight or more of structural units derived from a (meth)acrylic acid ester (a-1) having an alkyl group having 12 or more carbon atoms and having a glass transition temperature (Tg) of 0°C or lower when made into a homopolymer. The present disclosure 11 is the pressure-sensitive adhesive tape of the present disclosure 10, wherein the (meth)acrylic acid ester (a-1) having an alkyl group having 12 or more carbon atoms and having a glass transition temperature (Tg) of 0°C or lower when made into a homopolymer contains lauryl (meth)acrylate. The present disclosure 12 is the pressure-sensitive adhesive tape of the present disclosure 9, wherein the (meth)acrylic polymer contains 90% by weight or more of a structural unit derived from a (meth)acrylic acid ester (a) having a glass transition temperature (Tg) of 0°C or lower when made into the homopolymer. The present disclosure 13 is the pressure-sensitive adhesive tape of the present disclosure 7, 8, 9, 10, 11, or 12, wherein the (meth)acrylic polymer contains a structure derived from a hydroxyl group-containing monomer. The present disclosure 14 is the pressure-sensitive adhesive tape of the present disclosure 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, or 13, wherein the pressure-sensitive adhesive layer is a photocurable pressure-sensitive adhesive layer. A fifteenth aspect of the present disclosure is the pressure-sensitive adhesive tape of any one of the seventh, eighth, nineth, tenth, eleventh, twelfth, and thirteenth aspects of the present disclosure, wherein the (meth)acrylic polymer contains a carbon-carbon double bond in a side chain. A sixteenth aspect of the present disclosure is the pressure-sensitive adhesive tape of the fifteenth aspect of the present disclosure, wherein the (meth)acrylic polymer has a carbon-carbon double bond equivalent of 0.5 meq / g or less. Disclosure 17 is an adhesive tape according to Disclosure 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, or 16, which is used to receive a component in a process of transferring the component. Disclosure 18 is the adhesive tape of Disclosure 17, wherein the component is a semiconductor device. The present invention will be described in detail below.

[0009] The present inventors have found that, in an adhesive tape having at least one substrate and at least one adhesive layer, by adjusting the shear storage modulus G' at low temperature of the adhesive layer and the surface peel strength measured by a specific method to be equal to or less than a certain value, an adhesive tape useful as a carrier material can be obtained. That is, the present inventors have found that such an adhesive tape can adhere chip components well when receiving the chip components, exhibits excellent peeling performance when retransferring the chip components, and can suppress adhesive residue on the chip components, and have completed the present invention.

[0010] FIG. 1 is a cross-sectional view showing a schematic example of a process for transferring a chip component arranged on an adhesive layer onto an adhesive tape. 1, chip components 1 are disposed on an adhesive layer 4 laminated on a substrate 5, and the chip components 1 are peeled off from the adhesive layer 4, for example, by a method such as irradiation with laser light. An adhesive tape 8 receives the chip components 1 peeled off from the adhesive layer 4, and serves as a carrier material for subsequently retransferring the chip components 1 onto another carrier material or a drive circuit board. The adhesive tape 8 has a substrate 3 and an adhesive layer 2. The laminate 9 of the substrate 5 and the adhesive layer 4 may be, for example, a single-sided adhesive tape in which the substrate 5 is a substrate such as a resin film and the adhesive layer 4 is composed only of an adhesive layer, or a laminate of a support and a double-sided adhesive tape in which the substrate 5 is a support such as a glass substrate and the adhesive layer 4 is a double-sided adhesive tape (which may have a substrate).

[0011] The pressure-sensitive adhesive tape of the present invention is a pressure-sensitive adhesive tape having at least one layer of a substrate and at least one layer of a pressure-sensitive adhesive layer. By having the above-mentioned base material, the adhesive tape of the present invention has appropriate stiffness and excellent handleability, and is an adhesive tape useful as a carrier material capable of receiving and retransferring chip components.

[0012] The substrate is not particularly limited, and examples of the substrate material include polyethylene terephthalate, polyethylene naphthalate, polyacetal, polyamide, polycarbonate, polyphenylene ether, polybutylene terephthalate, ultra-high molecular weight polyethylene, syndiotactic polystyrene, polyarylate, polysulfone, polyethersulfone, polyphenylene sulfide, polyetheretherketone, polyimide, polyetherimide, fluororesin, liquid crystal polymer, etc. Among these, polyethylene terephthalate and polyethylene naphthalate are preferred because of their excellent heat resistance.

[0013] The thickness of the substrate is not particularly limited, but the preferred lower limit is 4 μm, and the preferred upper limit is 188 μm. By making the thickness of the substrate within the above range, the adhesive tape can have a suitable stiffness and excellent handling properties. The more preferred lower limit of the thickness of the substrate is 50 μm, the more preferred upper limit is 125 μm, the even more preferred lower limit is 75 μm, and the even more preferred upper limit is 100 μm.

[0014] The pressure-sensitive adhesive layer has an upper limit of a shear storage modulus G' at a frequency of 10 Hz and at -20°C of 1 MPa. The adhesive tape is usually used to receive chip components at high speed. The shear storage modulus G' when a force is applied at such high speed is highly related to the shear storage modulus G' at low temperature based on the temperature-velocity conversion rule, so the inventors have studied the shear storage modulus G' of the adhesive layer at low temperature. If the shear storage modulus G' at a frequency of 10 Hz and -20°C is 1 MPa or less, the cushioning properties of the adhesive layer when receiving the chip components are improved, and the adhesive tape can favorably attach the chip components when receiving them. The upper limit of the shear storage modulus G' at a frequency of 10 Hz and -20°C is preferably 0.8 MPa, more preferably 0.5 MPa, and even more preferably 0.3 MPa. The lower limit of the shear storage modulus G' at a frequency of 10 Hz and -20°C is not particularly limited, but from the viewpoint of further improving the peeling performance when retransferring chip components, a preferable lower limit is 0.05 MPa, and a more preferable lower limit is 0.1 MPa.

[0015] The shear storage modulus G' of the pressure-sensitive adhesive layer at room temperature is not particularly limited, but a preferred upper limit of the shear storage modulus G' at a frequency of 10 Hz and 23° C. is 0.1 MPa. If the shear storage modulus G' at a frequency of 10 Hz and 23° C. is 0.1 MPa or less, the pressure-sensitive adhesive tape can better attach chip components when receiving the chip components. A more preferred upper limit of the shear storage modulus G' at a frequency of 10 Hz and 23° C. is 0.04 MPa. The lower limit of the shear storage modulus G' at a frequency of 10 Hz and 23° C. is not particularly limited, but from the viewpoint of further improving the peeling performance when retransferring chip components, a preferable lower limit is 0.01 MPa, and a more preferable lower limit is 0.015 MPa.

[0016] The shear storage modulus G' of the pressure-sensitive adhesive layer at a frequency of 10 Hz at -20°C and 23°C can be obtained as the storage modulus at each temperature when a dynamic viscoelasticity spectrum is measured from -40 to 140°C under conditions of a heating rate of 5°C / min and 10 Hz in a simple heating mode using, for example, a viscoelasticity spectrometer (DVA-200, manufactured by IT Measurement & Control Co., Ltd.). When the pressure-sensitive adhesive layer is a curable pressure-sensitive adhesive layer, the shear storage modulus G' of the pressure-sensitive adhesive layer means the shear storage modulus G' measured for the pressure-sensitive adhesive layer before curing. When the thickness of the pressure-sensitive adhesive layer is less than 100 μm, the pressure-sensitive adhesive layers are laminated to form a pressure-sensitive adhesive layer for measurement having a thickness of 100 μm or more. The shear storage modulus G' of the obtained pressure-sensitive adhesive layer for measurement is measured as described above.

[0017] The above pressure-sensitive adhesive tape has an upper limit of surface peel strength against SUS when applied in an area of ​​10 mm x 10 mm of 0.5 MPa. If the surface peel strength is 0.5 MPa or less, the adhesive strength of the adhesive tape is not too high, and therefore excellent peeling performance can be exhibited when retransferring chip components, and adhesive residue on the chip components can be suppressed. The upper limit of the surface peel strength is preferably 0.4 MPa, and more preferably 0.2 MPa. There is no particular restriction on the lower limit of the surface peel strength, but from the viewpoint of further improving the retention performance of the chip components, a preferable lower limit is 0.005 MPa, and a more preferable lower limit is 0.01 MPa.

[0018] FIG. 2 is a diagram showing a schematic diagram of a method for measuring the surface peel strength of an adhesive tape. First, the adhesive tape 8 is cut to 10 mm x 10 mm. The adhesive layer of the cut adhesive tape 8 is attached to a SUS jig 12 (SUS304) and pressed at 0.3 MPa for 10 seconds. One side of a double-sided adhesive tape for measurement 11 (manufactured by Sekisui Chemical Co., Ltd., product name #560, or an equivalent product) is attached to the back surface of the adhesive tape 8 attached to the SUS jig 12. The other side of the double-sided adhesive tape for measurement 11 is attached to a glass plate 10 with a thickness of 5 mm. Thereafter, when the adhesive layer of the adhesive tape 8 is a curing type adhesive layer, for example, a UV lamp with a wavelength of 365 nm is used to illuminate the adhesive layer with an intensity of 10 mW / cm. 2 , irradiation amount 2500mJ / cm 2 The adhesive layer is cured by irradiating ultraviolet light from the glass plate 10 side under the above conditions. That is, when the adhesive layer is a curable adhesive layer, the surface peel strength of the adhesive tape means the surface peel strength measured on the adhesive tape after the adhesive layer is cured. Then, the glass plate 10 is fixed to a tensile tester (Shimadzu Corporation, AGS-X, or equivalent). A tensile test is performed in which the SUS jig 12 is pulled in the vertical direction (in the direction of the arrow in the figure) at a peel speed of 200 mm / min using a tensile tester (Shimadzu Corporation, AGS-X, or equivalent) under an environment of room temperature of 23°C and relative humidity of 50%, and the surface peel strength is measured. The surface peel strength means the maximum peel strength. In addition, when the adhesive tape is a double-sided adhesive tape, the surface peel strength is measured by a tensile tester in the same manner, except that the adhesive layer on the side opposite to the side on which the surface peel strength is measured is attached and fixed to a glass plate. At this time, the adhesive layer on the side opposite to the side on which the surface peel strength of the adhesive tape is measured may be directly attached and fixed to the glass plate, or may be fixed via a double-sided adhesive tape 11 for measurement.

[0019] The thickness of the adhesive layer is not particularly limited, but the preferred lower limit is 30 μm, and the preferred upper limit is 200 μm. If the thickness is within the above range, the cushioning properties of the adhesive layer when receiving the chip component are further improved, and the adhesive tape can better attach the chip component when receiving the chip component. The more preferred lower limit of the thickness is 40 μm, the more preferred upper limit is 150 μm, the even more preferred lower limit is 70 μm, and the even more preferred upper limit is 100 μm.

[0020] The method for adjusting the shear storage modulus G' of the pressure-sensitive adhesive layer and the surface peel strength of the pressure-sensitive adhesive tape to be within the above range is not particularly limited, and examples include a method for adjusting the composition, molecular weight (weight average molecular weight (Mw)), hydroxyl value, double bond equivalent, etc. of the base polymer contained in the pressure-sensitive adhesive layer, a method for adjusting the degree of crosslinking (gel fraction) of the pressure-sensitive adhesive layer, etc.

[0021] The pressure-sensitive adhesive layer is not particularly limited, and examples thereof include an acrylic pressure-sensitive adhesive layer, a rubber-based pressure-sensitive adhesive layer, a urethane pressure-sensitive adhesive layer, a silicone-based pressure-sensitive adhesive layer, etc. Among these, an acrylic pressure-sensitive adhesive layer containing a (meth)acrylic polymer is preferred from the viewpoints of easy adjustment of the molecular weight, degree of crosslinking, etc., and excellent heat resistance, weather resistance, cost, etc.

[0022] The (meth)acrylic polymer is a polymer containing structural units derived from a (meth)acrylic monomer. The (meth)acrylic monomer is not particularly limited, and examples thereof include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, lauryl (meth)acrylate, isomyristyl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, etc. These (meth)acrylic monomers may be used alone, or two or more of them may be used in combination.

[0023] Among them, a (meth)acrylic acid ester (a) (hereinafter, also simply referred to as "(meth)acrylic acid ester (a)") having a glass transition temperature (Tg) of 0° C. or less when made into a homopolymer is preferred. That is, the (meth)acrylic polymer preferably contains a structural unit derived from the (meth)acrylic acid ester (a). By containing such a relatively flexible structural unit in the (meth)acrylic polymer, the shear storage modulus G' of the pressure-sensitive adhesive layer and the surface peel strength of the pressure-sensitive adhesive tape can be easily adjusted to the above range, and the pressure-sensitive adhesive tape has higher peel performance when retransferring chip components, allowing the chip components to be better attached when receiving them. In particular, by containing such a relatively flexible structural unit in the (meth)acrylic polymer and adjusting the degree of crosslinking (gel fraction) of the pressure-sensitive adhesive layer to an appropriate range, the shear storage modulus G' of the pressure-sensitive adhesive layer and the surface peel strength of the pressure-sensitive adhesive tape can be easily adjusted to a more preferred range.

[0024] The glass transition temperature (Tg) of the (meth)acrylic acid ester (a) is not particularly limited as long as it is 0° C. or lower, but since the peeling performance when the chip component is retransferred is further improved and the chip component can be more satisfactorily attached when the chip component is received, the preferred lower limit is −80° C. and the preferred upper limit is −5° C. The more preferred lower limit of the glass transition temperature (Tg) is −70° C. and the more preferred upper limit is −10° C. The glass transition temperature (Tg) of a homopolymer can be measured, for example, by differential scanning calorimetry (manufactured by TA Instruments) for a homopolymer having a weight average molecular weight (Mw) of about 5,000 to 1,000,000 or a degree of polymerization of about 500,000 to 10,000.

[0025] The (meth)acrylic acid ester (a) preferably contains a (meth)acrylic acid ester (a-1) (hereinafter also simply referred to as "(meth)acrylic acid ester (a-1)") having an alkyl group with 12 or more carbon atoms and having a glass transition temperature (Tg) of 0° C. or lower when made into a homopolymer. The (meth)acrylic acid ester (a) also preferably contains a (meth)acrylic acid ester (a-2) (hereinafter also simply referred to as "(meth)acrylic acid ester (a-2)") having an alkyl group with 7 or more and less than 12 carbon atoms and having a glass transition temperature (Tg) of 0° C. or lower when made into a homopolymer. When the (meth)acrylic polymer contains structural units having an alkyl group with a relatively long carbon chain, the shear storage modulus G' of the pressure-sensitive adhesive layer and the surface peel strength of the pressure-sensitive adhesive tape can be more easily adjusted to fall within preferred ranges. In particular, since the shear storage modulus G' of the pressure-sensitive adhesive layer and the surface peel strength of the pressure-sensitive adhesive tape can be more easily adjusted to be within a preferred range, it is more preferable that the (meth)acrylic acid ester (a) contains both the (meth)acrylic acid ester (a-1) and the (meth)acrylic acid ester (a-2).

[0026] The (meth)acrylic acid ester (a-1) is not particularly limited, and examples of the (meth)acrylic monomers mentioned above include lauryl acrylate (Tg of -23°C when homopolymerized), lauryl methacrylate (Tg of -65°C when homopolymerized), etc. Further examples include isomyristyl acrylate (Tg of -56°C when homopolymerized), isostearyl acrylate (Tg of -18°C when homopolymerized), etc. Among them, at least one selected from the group consisting of lauryl acrylate, lauryl methacrylate, and isostearyl acrylate is preferred, since it makes it easier to adjust the shear storage modulus G' of the pressure-sensitive adhesive layer and the surface peel strength of the pressure-sensitive adhesive tape to a more preferred range. Furthermore, lauryl (meth)acrylate is more preferred, and lauryl acrylate is even more preferred.

[0027] The (meth)acrylic acid ester (a-2) is not particularly limited, and examples thereof include heptyl acrylate (Tg of -68°C when homopolymerized), 2-ethylhexyl acrylate (Tg of -70°C when homopolymerized), and octyl acrylate (Tg of -65°C when homopolymerized). Further examples thereof include isononyl acrylate (Tg of -58°C when homopolymerized), and isodecyl acrylate (Tg of -62°C when homopolymerized). Among these, at least one selected from the group consisting of heptyl acrylate and 2-ethylhexyl acrylate is preferred, and 2-ethylhexyl acrylate is more preferred, since the shear storage modulus G' of the pressure-sensitive adhesive layer and the surface peel strength of the pressure-sensitive adhesive tape are more easily adjusted to a preferred range.

[0028] When the (meth)acrylic polymer contains the (meth)acrylic acid ester (a), the content of the structural unit derived from the (meth)acrylic acid ester (a) in the (meth)acrylic polymer is not particularly limited, but the preferred lower limit is 40% by weight. If the content of the structural unit is 40% by weight or more, the shear storage modulus G' of the pressure-sensitive adhesive layer and the surface peel strength of the pressure-sensitive adhesive tape are easily adjusted to a more preferred range, and the pressure-sensitive adhesive tape has higher peel performance when retransferring chip components, allowing the chip components to be attached better when receiving the chip components. The more preferred lower limit of the content of the structural unit is 45% by weight, the even more preferred lower limit is 80% by weight, and the even more preferred lower limit is 90% by weight. There are no particular limitations on the upper limit of the content of the above structural units, but the upper limit is preferably 98% by weight, and more preferably 95% by weight.

[0029] Furthermore, when the (meth)acrylic acid ester (a) contains the (meth)acrylic acid ester (a-1), the content of the structural unit derived from the (meth)acrylic acid ester (a-1) in the (meth)acrylic polymer is not particularly limited, but the preferred lower limit is 40% by weight. If the content of the structural unit is 40% by weight or more, the shear storage modulus G' of the pressure-sensitive adhesive layer and the surface peel strength of the pressure-sensitive adhesive tape are easily adjusted to a more preferred range, and the pressure-sensitive adhesive tape has higher peel performance when retransferring chip components, allowing the chip components to be attached better when receiving them. The more preferred lower limit of the content of the structural unit is 45% by weight. Although there is no particular upper limit to the content of the above structural units, if the content is too large, alkyl groups having long carbon chains (alkyl groups having 12 or more carbon atoms) present in the side chains crystallize at low temperatures, and the shear storage modulus G' at a frequency of 10 Hz and -20°C becomes too high, so that the upper limit is preferably 80% by weight, and more preferably 70% by weight.

[0030] The (meth)acrylic polymer preferably further contains a structure derived from a crosslinkable functional group-containing monomer. The (meth)acrylic polymer contains a structure derived from the crosslinkable functional group-containing monomer, so that the cohesive strength of the adhesive layer can be adjusted by crosslinking the crosslinkable functional group, and the adhesive strength and shear storage modulus G' of the adhesive layer can be easily adjusted. This makes it easier to adjust the shear storage modulus G' of the adhesive layer and the surface peel strength of the adhesive tape to a more preferred range, so that the adhesive tape has higher peeling performance when retransferring chip components, and can better attach chip components when receiving the chip components. The crosslinkable functional group may or may not be crosslinked, but is more preferably crosslinked. However, even if the structure is not crosslinked, the cohesive strength of the adhesive layer is increased due to the interaction between the functional groups.

[0031] Examples of the crosslinkable functional group-containing monomer include monomers containing a carboxyl group, a hydroxyl group, an epoxy group, a double bond, a triple bond, an amino group, an amide group, a nitrile group, etc. These crosslinkable functional group-containing monomers may be used alone or in combination of two or more. Among them, at least one selected from the group consisting of a carboxyl group-containing monomer and a hydroxyl group-containing monomer is preferred. Hydroxyl group-containing monomers are more preferred because the shear storage modulus G' of the pressure-sensitive adhesive layer is easily adjusted by crosslinking with an isocyanate-based crosslinking agent. The crosslinkable functional group-containing monomer may further contain an alkyl group, an ether group, a carbonyl group, an ester group, a carbonate group, an amide group, a urethane group, or the like.

[0032] The carboxyl group-containing monomer includes (meth)acrylic acid-based monomers such as (meth)acrylic acid. The hydroxyl group-containing monomer includes 4-hydroxybutyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, etc. The epoxy group-containing monomer includes glycidyl (meth)acrylate, etc. The double bond-containing monomer includes allyl (meth)acrylate, hexanediol di(meth)acrylate, etc. The triple bond-containing monomer includes propargyl (meth)acrylate, etc. The amide group-containing monomer includes (meth)acrylamide, etc. Among them, 4-hydroxybutyl acrylate is more preferable because it is easy to adjust the shear storage modulus G' of the pressure-sensitive adhesive layer to the above range.

[0033] In the (meth)acrylic polymer, the content of the structure derived from the monomer having the crosslinkable functional group is not particularly limited, but from the viewpoint of adjusting the adhesive strength and shear storage modulus G' of the pressure-sensitive adhesive layer, the preferred lower limit of the content of the structure is 0.1% by weight, and the preferred upper limit is 30% by weight. The more preferred lower limit of the content of the structure is 0.5% by weight, and the more preferred upper limit is 25% by weight. In addition, the content of the structure derived from the hydroxyl group-containing monomer in the (meth)acrylic polymer is not particularly limited, but from the viewpoint of adjusting the adhesive strength and shear storage modulus G' of the pressure-sensitive adhesive layer, the preferred lower limit of the content of the structure is 1 wt %, and the preferred upper limit is 20 wt %. The more preferred lower limit of the content of the structure is 3 wt %, and the more preferred upper limit is 10 wt %.

[0034] The (meth)acrylic polymer may contain a carbon-carbon double bond in a side chain. The side chain means a branched structure extending from the main chain, where the longest chain in the polymer is the main chain. By containing a carbon-carbon double bond in the side chain of the (meth)acrylic polymer, the pressure-sensitive adhesive layer can be made into a curable pressure-sensitive adhesive layer that is cured by, for example, heating, light irradiation, etc., and has a significantly reduced adhesive strength. In such a case, the shear storage modulus G' of the pressure-sensitive adhesive layer and the surface peel strength of the pressure-sensitive adhesive tape can be easily adjusted to a more preferred range, and the pressure-sensitive adhesive tape has higher peeling performance when retransferring chip components, allowing the chip components to be attached better when receiving them. Examples of the curable pressure-sensitive adhesive layer include a heat-curable pressure-sensitive adhesive layer and a photocurable pressure-sensitive adhesive layer. From the viewpoint of storage stability, a photocurable pressure-sensitive adhesive layer is preferred.

[0035] The (meth)acrylic polymer can be obtained by copolymerizing a monomer mixture containing the (meth)acrylic monomer, the crosslinkable functional group-containing monomer, and the like by radical reaction in the presence of a polymerization initiator. When the acrylic polymer contains a carbon-carbon double bond in the side chain, the carbon-carbon double bond can be introduced into the side chain of the acrylic polymer by, for example, copolymerizing the double bond-containing monomer as the crosslinkable functional group-containing monomer. In addition, after copolymerizing, for example, the carboxyl group-containing monomer, the hydroxyl group-containing monomer, etc. as the crosslinkable functional group-containing monomer, the resulting polymer may be reacted with a compound containing a double bond and a functional group capable of reacting with a carboxyl group, a hydroxyl group, etc. in the polymer (hereinafter, also referred to as a "functional group-containing unsaturated compound"). The functional group-containing unsaturated compound is not particularly limited, and examples thereof include isocyanate group-containing unsaturated compounds such as 2-methacryloyloxyethyl isocyanate (MOI). As a method for subjecting the monomer mixture to a radical reaction, i.e., a polymerization method, a conventionally known method is used, and examples thereof include solution polymerization (boiling point polymerization or constant temperature polymerization), emulsion polymerization, suspension polymerization, bulk polymerization, and the like.

[0036] The hydroxyl value of the (meth)acrylic polymer is not particularly limited, but a preferred upper limit is 45 mgKOH / g. If the hydroxyl value is 45 mgKOH / g or less, the adhesive strength and shear storage modulus G' of the adhesive layer can be easily adjusted. This makes it easier to adjust the shear storage modulus G' of the adhesive layer and the surface peel strength of the adhesive tape to a more preferred range, and the adhesive tape has higher peeling performance when retransferring chip components, allowing the chip components to be attached more satisfactorily when receiving the chip components. A more preferred upper limit of the hydroxyl value is 20 mgKOH / g. The lower limit of the hydroxyl value is not particularly limited, but from the viewpoint of adjusting the adhesive strength of the pressure-sensitive adhesive layer and the shear storage modulus G' of the pressure-sensitive adhesive tape, a preferable lower limit is 1 mgKOH / g. The hydroxyl value of a (meth)acrylic polymer is an index that indicates the amount of hydroxyl groups (hydroxy groups) contained in a certain amount of sample. The hydroxyl value of a (meth)acrylic polymer is the amount of potassium hydroxide required in mg to neutralize the acetic acid bonded to the hydroxyl groups by neutralization titration after acetylating 1 g of the (meth)acrylic polymer, and can be calculated by measuring based on the potentiometric titration method specified in JIS K 0070:1992.

[0037] The carbon-carbon double bond equivalent of the (meth)acrylic polymer is not particularly limited, but if it is too high, the shear storage modulus G' at a frequency of 10 Hz and -20°C becomes too high, so the preferred upper limit is 0.5 meq / g. If the carbon-carbon double bond equivalent is 0.5 meq / g or less, the shear storage modulus G' of the pressure-sensitive adhesive layer and the surface peel strength of the pressure-sensitive adhesive tape are easily adjusted to a more preferred range, and the pressure-sensitive adhesive tape has higher peeling performance when retransferring chip components, allowing the chip components to be attached more satisfactorily when receiving the chip components. The more preferred upper limit of the carbon-carbon double bond equivalent is 0.3 meq / g. The lower limit of the carbon-carbon double bond equivalent is not particularly limited, and may be 0 meq / g. The carbon-carbon double bond equivalent of the (meth)acrylic polymer is the milliequivalent (meq / g) of the carbon-carbon double bond of the unsaturated compound having a double bond per 1 g of the (meth)acrylic polymer, and is a calculated value calculated from the amount of the raw material charged. Specifically, the carbon-carbon double bond equivalent E (meq / g) can be calculated from the mass Wa (g) of the (meth)acrylic polymer, the substance amount nb (mol) of the unsaturated compound having a double bond contained in the (meth)acrylic polymer, and the number N (pieces) of the carbon-carbon double bonds contained in one molecule of the unsaturated compound having a double bond, using the following formula. E=nb×N×1000 / Wa

[0038] The weight average molecular weight (Mw) of the (meth)acrylic polymer is not particularly limited, but a preferred upper limit is 1 million. If the weight average molecular weight (Mw) is 1 million or less, the shear storage modulus G' and surface peel strength can be easily adjusted to a more preferred range, and the adhesive tape has higher peeling performance when retransferring chip components, allowing the chip components to be attached better when receiving them. A more preferred upper limit of the weight average molecular weight (Mw) is 950,000, and an even more preferred upper limit is 900,000. The lower limit of the weight average molecular weight (Mw) is not particularly limited, but from the viewpoints of adhesive strength, shape retention, etc. of the pressure-sensitive adhesive layer, the lower limit is preferably 400,000, and more preferably 500,000. The weight average molecular weight of the (meth)acrylic polymer can be determined, for example, by GPC (Gel Permeation Chromatography) in terms of standard polystyrene. More specifically, for example, the weight average molecular weight can be measured using a Waters "2690 Separations Module" as a measuring device, a Showa Denko "GPC KF-806L" as a column, ethyl acetate as a solvent, a sample flow rate of 1 mL / min, and a column temperature of 40°C.

[0039] The pressure-sensitive adhesive layer may contain a tackifier resin. Examples of the tackifier resin include rosin ester resins, hydrogenated rosin resins, terpene resins, terpene phenol resins, coumarone-indene resins, alicyclic saturated hydrocarbon resins, C5 petroleum resins, C9 petroleum resins, C5-C9 copolymer petroleum resins, etc. These tackifier resins may be used alone or in combination of two or more.

[0040] The content of the tackifier resin is not particularly limited, but from the viewpoint of further improving the peeling performance when retransferring chip components, it is preferable that the tackifier resin is not contained. When the tackifier resin is contained, the preferred upper limit is 10 parts by weight per 100 parts by weight of the resin (e.g., (meth)acrylic polymer) that is the main component of the adhesive layer. When the content of the tackifier resin is 10 parts by weight or less, the adhesive layer has higher peeling performance when retransferring chip components.

[0041] The pressure-sensitive adhesive layer preferably contains a crosslinking agent to form a crosslinked structure between the main chains of the resin constituting the pressure-sensitive adhesive layer (e.g., the (meth)acrylic polymer, the tackifier resin, etc.). The crosslinking agent is not particularly limited, and examples thereof include isocyanate-based crosslinking agents, aziridine-based crosslinking agents, epoxy-based crosslinking agents, metal chelate-type crosslinking agents, etc. Among them, when the (meth)acrylic polymer contains a structural unit derived from the hydroxyl group-containing monomer, an isocyanate-based crosslinking agent is preferred because the shear storage modulus G' of the pressure-sensitive adhesive layer is easily adjusted by crosslinking with the hydroxyl group. The content of the crosslinking agent is preferably 0.01 to 10 parts by weight, and more preferably 0.1 to 7 parts by weight, based on 100 parts by weight of the resin (for example, the (meth)acrylic polymer) that is the main component of the pressure-sensitive adhesive layer.

[0042] When the pressure-sensitive adhesive layer is a curable pressure-sensitive adhesive layer, it may further contain a polymerization initiator such as a thermal polymerization initiator or a photopolymerization initiator. The content of the polymerization initiator is not particularly limited, but is preferably 0.01 to 5 parts by weight, more preferably 0.1 to 3 parts by weight, per 100 parts by weight of the (meth)acrylic polymer.

[0043] The pressure-sensitive adhesive layer may further contain an inorganic filler such as fumed silica, etc. By incorporating the inorganic filler, the cohesive strength of the pressure-sensitive adhesive layer can be increased.

[0044] The pressure-sensitive adhesive layer may further contain known additives such as plasticizers, resins, surfactants, waxes, fine particle fillers, etc. These additives may be used alone or in combination of two or more kinds.

[0045] The gel fraction of the pressure-sensitive adhesive layer is not particularly limited, but the preferred lower limit is 50% by weight, and the preferred upper limit is 95% by weight. If the gel fraction is 50% by weight or more, the adhesive strength of the pressure-sensitive adhesive layer is adjusted to a relatively low range, and the surface peel strength of the pressure-sensitive adhesive tape is easily adjusted. As a result, the pressure-sensitive adhesive tape has higher peel performance when retransferring chip components. If the gel fraction is 95% by weight or less, the shear storage modulus G' of the pressure-sensitive adhesive layer is easily adjusted. As a result, the pressure-sensitive adhesive tape can better attach chip components when receiving them. The more preferred lower limit of the gel fraction is 80% by weight, the more preferred upper limit is 94% by weight, the even more preferred lower limit is 85% by weight, and the even more preferred upper limit is 93% by weight. The gel fraction of the pressure-sensitive adhesive layer can be measured by the following method. 0.1 g of only the adhesive layer (adhesive composition) is taken out from the adhesive tape, immersed in 50 mL of ethyl acetate, and shaken in a shaker at 23°C and 200 rpm for 24 hours. After shaking, the ethyl acetate and the adhesive composition that has absorbed and swollen with the ethyl acetate are separated using a metal mesh (mesh size #200). The separated adhesive composition is dried at 110°C for 1 hour. The weight of the adhesive composition containing the dried metal mesh is measured, and the gel fraction of the adhesive layer is calculated using the following formula. When the adhesive layer is a curable adhesive layer, the gel fraction of the adhesive layer means the gel fraction measured for the adhesive layer before curing. Gel fraction (wt%) = 100 × (W1-W2) / W0 (W0: initial weight of adhesive composition, W1: weight of adhesive composition including metal mesh after drying, W2: initial weight of metal mesh) However, if the pressure-sensitive adhesive composition is not completely dissolved in ethyl acetate, a solvent such as toluene, hexane, water, etc. is used instead of ethyl acetate. Specifically, if the pressure-sensitive adhesive composition contains, for example, a styrene-based elastomer, toluene or hexane is used, and if it contains polyvinyl alcohol, hot water at 90°C is used.

[0046] The pressure-sensitive adhesive tape of the present invention may be a single-sided pressure-sensitive adhesive tape having a pressure-sensitive adhesive layer on only one side of a substrate, or a double-sided pressure-sensitive adhesive tape having pressure-sensitive adhesive layers on both sides of a substrate. In addition, since the adhesive tape of the present invention is attached to a support to improve the handling property, the adhesive tape of the present invention is preferably a double-sided adhesive tape, and more preferably a double-sided adhesive tape having an adhesive layer on both sides of a substrate. The support is not particularly limited, and examples thereof include glass, a quartz substrate, a metal plate, etc. When the pressure-sensitive adhesive tape of the present invention is a double-sided pressure-sensitive adhesive tape having pressure-sensitive adhesive layers on both sides of a substrate, the pressure-sensitive adhesive layers on both sides may be the pressure-sensitive adhesive layers described above, or one side may be the pressure-sensitive adhesive layer described above, and the other side (the side in contact with a support or the like) may be another pressure-sensitive adhesive layer. The other pressure-sensitive adhesive layer is not particularly limited, and a conventionally known pressure-sensitive adhesive layer may be used.

[0047] The use of the pressure-sensitive adhesive tape of the present invention is not particularly limited, but it is preferably used to receive a component in a process of transferring the component. The above-mentioned component is not particularly limited, but is preferably a semiconductor device. Examples of the semiconductor device include chip components such as a micro LED chip and an optical chip of an image sensor. Among them, a micro LED chip is preferable. The adhesive tape of the present invention is particularly suitable for use as an adhesive tape for receiving chip components in a step of transferring chip components arranged on an adhesive layer as shown in Fig. 1 onto an adhesive tape. The method for transferring chip components onto the adhesive tape of the present invention is not particularly limited, and for example, a method of irradiating laser light or the like can be adopted. The method for retransferring chip components from the adhesive tape of the present invention onto another carrier material or a drive circuit board is not particularly limited, and for example, a method of directly laminating another carrier material having adhesiveness and peeling it off to transfer, or a method of irradiating laser light or the like can be used. Effect of the Invention

[0048] According to the present invention, it is possible to provide an adhesive tape that can adhere chip components well when receiving the chip components, exhibits excellent peeling performance when retransferring the chip components, and can suppress adhesive residue on the chip components. [Brief description of the drawings]

[0049] [Figure 1] 1A to 1C are cross-sectional views that diagrammatically show an example of a process for transferring a chip component disposed on an adhesive layer onto an adhesive tape. [Diagram 2] FIG. 2 is a diagram showing a schematic diagram of a method for measuring surface peel strength of an adhesive tape. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0050] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0051] Example 1 (1) Preparation of (meth)acrylic polymer 52 parts by weight of ethyl acetate was put into a reactor equipped with a thermometer, a stirrer, and a cooling tube, and after replacing with nitrogen, the reactor was heated to start reflux. 30 minutes after the ethyl acetate boiled, 0.08 parts by weight of azobisisobutyronitrile was put in as a polymerization initiator. 94.7 parts by weight of 2-ethylhexyl acrylate, 5 parts by weight of 2-hydroxyethyl acrylate, and 0.3 parts by weight of acrylic acid were added dropwise evenly and gradually over 1 hour and 30 minutes to react. 30 minutes after the dropwise addition, 0.1 parts by weight of azobisisobutyronitrile was added, and the polymerization reaction was continued for another 5 hours. Ethyl acetate was added to the reactor to dilute it and cool it, thereby obtaining a solution of a (meth)acrylic polymer (hydroxyl value 24.2 mgKOH / g, double bond equivalent 0 meq / g). The weight average molecular weight of the obtained (meth)acrylic polymer was measured using a Waters 2690 Separations Module as a measuring device, a Showa Denko GPC KF-806L column, ethyl acetate as a solvent, at a sample flow rate of 1 mL / min and a column temperature of 40° C. The weight average molecular weight was 800,000.

[0052] (2) Manufacture of adhesive tapes To the obtained (meth)acrylic polymer solution, an isocyanate crosslinking agent, Coronate L-45 (manufactured by Tosoh Corporation), was added so that the solid content was 1.8 parts by weight per 100 parts by weight of the (meth)acrylic polymer, and the mixture was further thoroughly stirred to obtain an adhesive solution. The obtained adhesive solution was applied to a 100 μm thick polyethylene terephthalate (PET) film as a substrate using an applicator so that the dried film had a thickness of 40 μm, and dried at 110° C. for 3 minutes to obtain an adhesive tape.

[0053] (3) Measurement of gel fraction 0.1 g of only the adhesive layer (adhesive composition) was taken out from the adhesive tape, immersed in 50 mL of ethyl acetate, and shaken in a shaker at 23°C and 200 rpm for 24 hours. After shaking, ethyl acetate and the adhesive composition swollen by absorbing the ethyl acetate were separated using a metal mesh (mesh size #200). The separated adhesive composition was dried at 110°C for 1 hour. The weight of the adhesive composition containing the dried metal mesh was measured, and the gel fraction of the adhesive layer was calculated using the following formula. When the adhesive layer is a curable adhesive layer, the gel fraction of the adhesive layer means the gel fraction measured for the adhesive layer before curing. Gel fraction (wt%) = 100 × (W1-W2) / W0 (W0: initial weight of adhesive composition, W1: weight of adhesive composition including metal mesh after drying, W2: initial weight of metal mesh)

[0054] (4) Measurement of shear storage modulus G' The dynamic viscoelasticity spectrum of the adhesive layer was measured from -40 to 140°C using a viscoelasticity spectrometer (IT Measurement and Control Co., Ltd., DVA-200) under conditions of a heating rate of 5°C / min and 10 Hz in a simple heating mode. The shear storage modulus G' at -20°C and 23°C and a frequency of 10 Hz was determined. When the adhesive layer is a curable adhesive layer, the shear storage modulus G' of the adhesive layer means the shear storage modulus G' measured for the adhesive layer before curing.

[0055] (5) Measurement of surface peel strength (adhesive area 10mm x 10mm, against SUS) FIG. 2 is a diagram showing a schematic diagram of a method for measuring the surface peel strength of an adhesive tape. First, the adhesive tape 8 was cut to 10 mm x 10 mm. The adhesive layer of the cut adhesive tape 8 was attached to a SUS jig 12 (SUS304) and pressed at 0.3 MPa for 10 seconds. One side of a double-sided adhesive tape 11 for measurement (manufactured by Sekisui Chemical Co., Ltd., product name #560) was attached to the back side of the adhesive tape 8 attached to the SUS jig 12. The other side of the double-sided adhesive tape 11 for measurement was attached to a glass plate 10 with a thickness of 5 mm. Thereafter, the glass plate 10 was fixed to a tensile tester (manufactured by Shimadzu Corporation, AGS-X). In addition, when measuring the surface peel strength after ultraviolet irradiation of the adhesive tape 8, a UV lamp with a wavelength of 365 nm was used to measure the peel strength of the adhesive tape 8 using an intensity of 10 mW / cm before fixing the glass plate 10 to the tensile tester. 2 , irradiation amount 2500mJ / cm 2 The adhesive layer of the adhesive tape 8 was cured by irradiating the adhesive layer from the glass plate 10 side with ultraviolet light under the above conditions. A tensile test was performed in an environment of room temperature 23°C and relative humidity 50%, in which a SUS jig 12 was pulled in the vertical direction (arrow direction in the figure) at a peeling speed of 200 mm / min using a tensile tester (Shimadzu Corporation, AGS-X), to measure the surface peel strength of the adhesive tape. The surface peel strength means the maximum peel strength.

[0056] (Examples 2 to 9, 13 to 16, Comparative Examples 1 to 3, 5) An adhesive tape was obtained in the same manner as in Example 1, except that the composition and weight average molecular weight of the (meth)acrylic polymer, the type and amount of the crosslinking agent, the thickness of the adhesive layer, etc. were changed as shown in Tables 1 and 2. As the crosslinking agent, an isocyanate-based crosslinking agent, Coronate HX (manufactured by Tosoh Corporation), and an epoxy-based crosslinking agent, Tetrad C (manufactured by Mitsubishi Gas Chemical Co., Inc.), were also used.

[0057] (Examples 10 to 12, Comparative Examples 4, 6, and 7) A (meth)acrylic polymer solution was obtained in the same manner as in Example 1, except that the composition and weight average molecular weight of the (meth)acrylic polymer were changed as shown in Tables 1 and 2. 2-methacryloyloxyethyl isocyanate (MOI) was added as an isocyanate group-containing unsaturated compound in the amounts shown in Tables 1 and 2 relative to 100 parts by weight of the resin solid content of the obtained solution containing the (meth)acrylic polymer, and an addition reaction was carried out at 60°C for 2 hours to obtain a solution of a (meth)acrylic polymer containing a carbon-carbon double bond in the side chain. Thereafter, the type and amount of crosslinking agent, the thickness of the adhesive layer, etc. were changed as shown in Tables 1-2, and an adhesive tape was obtained in the same manner as in Example 1, except that the photopolymerization initiator omnirad651 (manufactured by IGM Resins BV) was added in the amount shown in Tables 1-2.

[0058] <Evaluation> The pressure-sensitive adhesive tapes obtained in the Examples and Comparative Examples were evaluated as follows, and the results are shown in Tables 1 and 2.

[0059] (1) Evaluation of chip component transfer performance (chip component adhesion) Separately from the obtained adhesive tape, a single-sided adhesive tape for testing was prepared. A single-sided adhesive tape for testing was attached to the surface of a wafer on which 10 Si chips (500 μm × 500 μm square, 50 μm thick) were arranged.The wafer was then peeled off to place the Si chips on the single-sided adhesive tape for testing. The single-sided adhesive tape on which the Si chips were placed was placed opposite the adhesive tape obtained in the examples or comparative examples, and a semiconductor solid-state laser was used to irradiate each Si chip from the substrate side of the single-sided adhesive tape for testing with a laser beam of 365 nm wavelength with an output of 4 W and 4 KHz, to peel off the Si chips and transfer them onto the adhesive tape. When the adhesive tape received the Si chips, the transfer performance of the chip components was evaluated as follows: "◎" if 10 Si chips were attached to the adhesive tape, "◯" if 8 to 9 Si chips were attached, and "×" if 7 or less Si chips were attached.

[0060] (2) Retransfer performance and adhesive residue during retransfer The obtained adhesive tape was attached to the Si chip side of a wafer on which 10 Si chips (500 μm × 500 μm square, 50 μm thick) were arranged. The wafer was then peeled off to place the Si chips on the adhesive tape. In Examples 10 to 12 and Comparative Examples 4, 6, and 7, in which the adhesive layer was a curable adhesive layer (photocurable adhesive layer), a UV lamp with a wavelength of 365 nm was used, and the intensity was 10 mW / cm. 2 , irradiation amount 2500mJ / cm 2 The adhesive layer was cured by irradiating the substrate with ultraviolet light under the above conditions. The adhesive tape with the Si chips placed on it was placed against the adhesive surface of a protect tape (6312C, Sekisui Chemical Co., Ltd.), and the Si chips were pressed onto the protect tape by pressing them with a 2 kg roller at a speed of 300 mm / min, and then the protect tape was peeled off to peel off the Si chips from the adhesive tape and transfer them onto the protect tape. The retransfer performance was evaluated as follows: when 10 Si chips could be placed on the protect tape from the adhesive tape, it was marked as "◎", when 8 to 9 Si chips could be placed, it was marked as "◯", and when 7 or fewer Si chips could be placed, it was marked as "×". In addition, the surface of the Si chip peeled off from the adhesive tape was observed under a microscope, and the adhesive residue was evaluated as "good" if no adhesive residue was observed, and "poor" if adhesive residue was observed.

[0061] [Table 1]

[0062] [Table 2]

[0063] BA: Butyl acrylate HPA: Heptyl acrylate 2-EHA: 2-Ethylhexyl acrylate LA: Lauryl acrylate 2-HEA: 2-hydroxyethyl acrylate 4-HBA: 4-hydroxybutyl acrylate AAc: acrylic acid AAm: Acrylamide [Industrial Applicability]

[0064] According to the present invention, it is possible to provide an adhesive tape that can adhere chip components well when receiving the chip components, exhibits excellent peeling performance when retransferring the chip components, and can suppress adhesive residue on the chip components. [Explanation of symbols]

[0065] 1 Chip components 2 Adhesive layer 3 Base material 4 Adhesive layer 5 Base material 8. Adhesive Tape 9. Laminate of substrate and pressure-sensitive adhesive layer 10 Glass Plate 11 Double-sided adhesive tape for measurement 12 SUS jig

Claims

1. An adhesive tape having at least one layer of a substrate and at least one layer of an adhesive layer, the pressure-sensitive adhesive layer has a shear storage modulus G' of 1 MPa or less at a frequency of 10 Hz and -20°C; The pressure-sensitive adhesive tape has a surface peel strength against SUS of 0.5 MPa or less when the tape is applied in an area of ​​10 mm x 10 mm. An adhesive tape characterized by:

2. 2. The pressure-sensitive adhesive tape according to claim 1, wherein the pressure-sensitive adhesive layer has a shear storage modulus G' of 0.3 MPa or less at a frequency of 10 Hz and -20°C.

3. 3. The pressure-sensitive adhesive tape according to claim 1, wherein the pressure-sensitive adhesive layer has a shear storage modulus G' of 0.04 MPa or less at a frequency of 10 Hz and 23°C.

4. 4. The adhesive tape according to claim 1, wherein the adhesive layer has a thickness of 40 [mu]m or more.

5. 5. The pressure-sensitive adhesive tape according to claim 1, 2, 3 or 4, which has a surface peel strength against SUS (SUS) of 0.01 MPa or more in an application area of ​​10 mm x 10 mm.

6. 6. The pressure-sensitive adhesive tape according to claim 1, 2, 3, 4 or 5, which has a surface peel strength against SUS (SUS) of 0.2 MPa or less in an application area of ​​10 mm x 10 mm.

7. 7. The pressure-sensitive adhesive tape according to claim 1, wherein the pressure-sensitive adhesive layer is an acrylic pressure-sensitive adhesive layer containing a (meth)acrylic polymer.

8. 8. The pressure-sensitive adhesive tape according to claim 7, wherein the (meth)acrylic polymer has a hydroxyl value of 45 mgKOH / g or less.

9. The pressure-sensitive adhesive tape according to claim 7 or 8, characterized in that the (meth)acrylic polymer contains 80% by weight or more of a structural unit derived from a (meth)acrylic acid ester (a) having a glass transition temperature (Tg) of 0°C or lower when formed into a homopolymer.

10. The pressure-sensitive adhesive tape according to claim 9, characterized in that the (meth)acrylic polymer contains 40% by weight or more of structural units derived from a (meth)acrylic acid ester (a-1) which has an alkyl group having 12 or more carbon atoms and has a glass transition temperature (Tg) of 0°C or lower when made into a homopolymer.

11. The pressure-sensitive adhesive tape according to claim 10, characterized in that the (meth)acrylic acid ester (a-1) having an alkyl group having 12 or more carbon atoms and having a glass transition temperature (Tg) of 0°C or lower when made into a homopolymer contains lauryl (meth)acrylate.

12. The pressure-sensitive adhesive tape according to claim 9, characterized in that the (meth)acrylic polymer contains 90% by weight or more of structural units derived from a (meth)acrylic acid ester (a) having a glass transition temperature (Tg) of 0°C or lower when formed into the homopolymer.

13. 13. The pressure-sensitive adhesive tape according to claim 7, 8, 9, 10, 11 or 12, wherein the (meth)acrylic polymer contains a structure derived from a hydroxyl group-containing monomer.

14. 14. The adhesive tape according to claim 1, wherein the adhesive layer is a photocurable adhesive layer.

15. 14. The pressure-sensitive adhesive tape according to claim 7, wherein the (meth)acrylic polymer contains a carbon-carbon double bond in a side chain.

16. 16. The pressure-sensitive adhesive tape according to claim 15, wherein the (meth)acrylic polymer has a carbon-carbon double bond equivalent of 0.5 meq / g or less.

17. 17. The adhesive tape according to claim 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15 or 16, which is used to receive a component in a process of transferring the component.

18. 18. The adhesive tape according to claim 17, wherein the part is a semiconductor device.

Citation Information

Patent Citations

  • Transfer substrate and transfer method

    WO2019065441A1