Method for detecting cracked furnace tube and method for manufacturing base material for optical fiber
By increasing internal pressure and using chlorine gas detection, the method accurately identifies cracks and pinholes in the reactor core tube, preventing defective optical fiber preform production.
Patent Information
- Application Number
- JP2023079196
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-12
- Publication Date
- 2024-11-22
AI Technical Summary
Existing methods for detecting cracks and pinholes in the reactor core tube of a sintering furnace for optical fiber preforms are inaccurate, particularly when using helium gas, and minute cracks are difficult to detect due to low gas leakage, leading to potential defects in the optical fiber transmission characteristics.
A method that increases the internal pressure of the reactor core tube with a detection gas present, detecting the gas flowing into the furnace body to accurately identify cracks and pinholes, utilizing chlorine gas for cost-effective detection and helium leak detection as a secondary verification.
Accurate detection of cracks and pinholes in the reactor core tube is achieved, preventing the production of defective optical fiber preforms by stopping production when defects are found, thus ensuring high-quality fiber production.
Smart Images

Figure 2024163508000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for detecting cracks in a core tube of a sintering furnace for an optical fiber preform and a method for manufacturing an optical fiber preform. [Background technology]
[0002] If cracks or pinholes occur in the core tube in a sintering furnace for optical fiber preforms, the transmission characteristics of the optical fiber obtained from the manufactured optical fiber preforms deteriorate. For this reason, methods for detecting cracks and pinholes occurring in the core tube have been studied. Patent Document 1 discloses an optical fiber preform manufacturing device equipped with a halogen-based gas detector having a sensor installed in the middle of the sealing gas flow passage of a heating furnace. Patent Document 2 discloses a method for detecting cracks in the core tube using a helium leak detector. Patent Document 3 discloses a method for supplying a detection gas into the core tube and detecting the detection gas that has flowed into the furnace body. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 5-78140 [Patent Document 2] Japanese Patent Application Publication No. 11-1337 [Patent Document 3] JP 2004-231482 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, when helium gas is used as the detection gas, there is a possibility that helium leaking from the exhaust port will be detected even if there are no cracks or pinholes in the core tube. Also, in the case of a method of supplying detection gas for detection, if the cracks are minute, the amount of detection gas flowing out from the core tube is small, making it difficult to accurately detect cracks or pinholes.
[0005] An object of the present disclosure is to provide a method for detecting cracks in a core tube that can accurately detect cracks and pinholes in a core tube in a sintering furnace for optical fiber preforms, and a method for manufacturing optical fiber preforms. [Means for solving the problem]
[0006] The method for detecting a crack in a furnace core tube according to the present disclosure includes increasing an internal pressure of the furnace core tube while a detection gas is contained in the furnace core tube; The detection gas that has flowed into the furnace body located outside the furnace tube in conjunction with an increase in the internal pressure of the furnace tube is detected.
[0007] The present disclosure relates to a method for producing an optical fiber preform, comprising inserting an optical fiber porous preform into a furnace tube and heating and making the preform transparent, the method comprising the steps of: performing a method for detecting cracks in a core tube according to an embodiment of the present disclosure during a period from when the porous optical fiber preform is inserted into the core tube until when the optical fiber preform is removed from the core tube; When a core tube crack is detected by the core tube crack detection method, The optical fiber preform is judged to be defective, or production using the furnace tube is stopped until it is confirmed that the transmission loss of the optical fiber produced from the optical fiber preform is satisfactory. Effect of the Invention
[0008] According to the present disclosure, it is possible to provide a method for detecting cracks in a core tube that can accurately detect cracks or pinholes in a core tube in a sintering furnace for an optical fiber preform, and a method for manufacturing an optical fiber preform. [Brief description of the drawings]
[0009] [Figure 1] FIG. 2 is a cross-sectional view showing an example of a sintering furnace for an optical fiber preform. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] [Description of the embodiments of the present disclosure] First, the embodiments of the present disclosure will be listed and described. (1) increasing the internal pressure of a furnace tube while the detection gas is contained within the furnace tube; This is a method for detecting cracks in a core tube in a sintering furnace for optical fiber preform, which detects the detection gas that has flowed into a furnace body located outside the core tube in conjunction with an increase in the internal pressure of the core tube.
[0011] According to the method for detecting a crack in the core tube of this embodiment, a change in the concentration of the detection gas linked to an increase in pressure is detected, so that a crack in the core tube can be accurately detected.
[0012] (2) In the above (1), the detection gas may be chlorine gas.
[0013] In the method for detecting cracks in a furnace tube according to the present embodiment, an inexpensive chlorine gas detector can be used, so that a gas detector can be installed for each furnace body at low cost, and the presence or absence of cracks in the furnace tube can be inspected every time sintering is performed.
[0014] (3) In the above (2), when the detection gas is detected, the presence or absence of helium gas flowing into the furnace body may be checked using a helium leak detector while supplying helium gas into the furnace tube.
[0015] According to the core tube crack detection method of this embodiment, an additional inspection is performed using a portable helium leak detector only if chlorine gas is detected, making it possible to detect core tube cracks more accurately without incurring significant costs.
[0016] A method for producing an optical fiber preform according to an embodiment of the present disclosure includes: (4) A method for manufacturing an optical fiber preform, comprising inserting an optical fiber porous preform into a furnace tube and heating and making the preform transparent, Implementing the method for detecting cracks in a core tube according to any one of (1) to (3) above during the period from when the porous optical fiber preform is inserted into the core tube until when the optical fiber preform is removed from the core tube; When a core tube crack is detected by the core tube crack detection method, The optical fiber preform is judged to be defective, or production using the furnace tube is stopped until it is confirmed that the transmission loss of the optical fiber produced from the optical fiber preform is satisfactory.
[0017] According to the manufacturing method of the optical fiber preform of this embodiment, if a core tube crack is detected, the manufactured optical fiber preform is either deemed defective, or manufacturing is not continued until it is confirmed that the transmission loss is good, thereby avoiding the continued manufacturing of defective optical fiber preforms.
[0018] (5) In the above (4), the method for producing the optical fiber preform includes a dehydration step and a clarification step, The dehydration step is a step of supplying a gas containing chlorine gas into the furnace tube while maintaining the inside of the furnace tube at a negative pressure relative to the internal pressure of the furnace body, The transparentizing step is a step of maintaining an inside of the furnace tube at a positive pressure with respect to an internal pressure of the furnace body, At the timing of switching from the dehydration process to the transparentization process, the presence or absence of a crack in the core tube may be checked by the core tube crack detection method described in (2) above.
[0019] According to the manufacturing method for optical fiber preform of this embodiment, crack detection is performed using chlorine gas as the detection gas at the timing of switching from the dehydration process to the transparency process, so that cracks in the core tube can be detected without supplying additional detection gas or increasing the pressure for crack detection.
[0020] [Details of the embodiment of the present disclosure] Specific examples of the core tube crack detection method of the present disclosure will be described below with reference to the drawings. Note that the present invention is not limited to these examples, but is defined by the claims, and is intended to include all modifications within the meaning and scope of the claims.
[0021] (Sintering furnace) First, the configuration of a sintering furnace for carrying out the core tube crack detection method or the optical fiber preform manufacturing method of the present disclosure will be described. Fig. 1 is a cross-sectional view showing an example of a sintering furnace 1 for manufacturing an optical fiber preform. The sintering furnace 1 has a cylindrical core tube 11 made of quartz glass, a heater 13 arranged to surround the core tube 11, a furnace body 12 formed to cover the heater 13, and a lid 14 covering the upper part of the core tube 11.
[0022] A gas supply port 15 is provided at the bottom of the furnace core tube 11, and is configured so that helium gas, chlorine gas, and the like used in the manufacturing process of the optical fiber preform can be supplied into the furnace core tube 11 from the direction of the arrow in the figure. In addition, the lid 14 is provided with a gas exhaust port (not shown).
[0023] The furnace body 12 is also provided with a gas supply port and a gas exhaust port (not shown), and is configured to be able to supply an inert gas such as nitrogen gas into the furnace body 12. A gas detector 16 is also connected to the furnace body 12, and is able to detect the gas contained in the furnace body 12. The gas types detected by the gas detector 16 are gases supplied into the furnace tube 11 in the manufacturing process of the optical fiber preform, and examples of such gases include helium gas, chlorine gas, silicon tetrachloride gas, and fluorine tetrachloride gas. In addition to the heater 13, a heat insulating material (not shown) made of a material such as carbon is arranged inside the furnace body 12.
[0024] 1 shows a porous base material 2 inserted from above into a furnace tube 11. The porous base material 2 is supported by a support rod 3, and can be moved in the vertical direction via the support rod 3.
[0025] (Manufacturing process of optical fiber base material) Next, the manufacturing process of the optical fiber preform will be explained. The optical fiber preform is obtained by dehydrating and sintering the optical fiber porous preform produced by the VAD method, OVD method, etc. to make it transparent. The manufacturing process of the optical fiber preform includes a dehydration process and a transparentization process.
[0026] In the dehydration process, the porous base material 2 is first inserted from above into the core tube 11, and the lower end of the porous base material is adjusted to a position (heat zone) where it is heated by the heater 13. Next, a gas having a dehydrating effect is supplied from the gas supply port 15 to the core tube 11, and heating by the heater 13 is started. After that, the porous base material 2 is gradually moved downward to dehydrate the entire porous base material 2. The gas having a dehydrating effect may be a halogen gas or a halogen compound gas, and may be chlorine gas in particular. Usually, in the dehydration process, an inert gas is supplied into the core tube 11 together with the gas having a dehydrating effect. Examples of the inert gas include helium gas, nitrogen gas, and argon gas. In the dehydration process, the pressure in the core tube 11 is made smaller than the pressure in the furnace body 12, that is, the core tube 11 is made negative pressure. After the entire porous base material 2 has been dehydrated, the supply of the gas having a dehydrating effect is stopped, and the porous base material 2 is moved upward to return to the position at the start of the dehydration process.
[0027] Next, a transparentization process is performed in which the dehydrated porous base material 2 is sintered at a high temperature to make it transparent. In the transparentization process, the porous base material 2 is sintered using the heater 13 while helium gas is supplied into the furnace tube 11. In the transparentization process, like the dehydration process, heating is started from the lower end of the porous base material 2, and the porous base material 2 is gradually moved downward to make the entire porous base material 2 transparent. In the transparentization process, the pressure inside the furnace tube 11 is made higher than the pressure inside the furnace body 12, that is, the inside of the furnace tube 11 is made to be in a positive pressure state.
[0028] Incidentally, since sintering is performed at high temperatures in the clarification process, the portion of the furnace tube 11 made of quartz glass located near the heater 13 gradually crystallizes as the temperature repeatedly rises and falls. As a result, the crystallized portion of the furnace tube 11 may crack and cause pinholes. In addition, when an earthquake occurs, the shaking may cause tiny cracks or pinholes to form in the furnace tube 11. Even if no pinholes appear immediately after the earthquake, they may appear after a certain amount of time has passed.
[0029] If sintering is performed with a pinhole in the furnace tube 11, impurities contained in the heater 13, etc., will enter the furnace tube 11 through the pinhole from the furnace body 12 and be incorporated into the optical fiber preform. As a result, the transmission loss of the optical fiber obtained by drawing the optical fiber preform will worsen. Since it takes time from the production of the optical fiber preform to the measurement of the transmission loss of the optical fiber obtained by drawing the optical fiber preform, the production of the optical fiber preform will continue without noticing the presence of the pinhole in the furnace tube 11. As a result, there is a risk that all the optical fiber preforms produced during that time will be defective. To avoid such a situation, it is necessary to accurately detect cracks and pinholes in the furnace tube 11 before measuring the transmission loss of the optical fiber.
[0030] (Method of detecting core tube cracks) A method for detecting a crack in a core tube according to an embodiment of the present disclosure increases the internal pressure of the core tube 11 while the core tube 11 contains a detection gas, and detects the detection gas that has flowed into the furnace body 12 located outside the core tube 11 in conjunction with the increase in the internal pressure of the core tube 11. When the internal pressure of the core tube 11 increases, the amount of gas that flows from the core tube 11 into the furnace body 12 through cracks or pinholes increases. Therefore, when detection gas is detected in the furnace body 12 in conjunction with the increase in the internal pressure of the core tube 11, it can be determined that there is a high probability that a crack or pinhole has occurred in the core tube 11.
[0031] As the detection gas, it is preferable to use the gas used in the manufacturing process of the optical fiber preform. If the gas used in the manufacturing process is used, there is no need to supply a separate gas to detect the core tube crack. Examples of such detection gas include helium gas, chlorine gas, silicon tetrachloride gas, and fluorine tetrachloride gas. It is particularly preferable that the detection gas is chlorine gas. A chlorine gas detector is cheaper than, for example, a helium leak detector, and a gas detector 16 can be installed for each furnace body at low cost. In addition, when chlorine gas is supplied into the core tube 11 in the dehydration process, the pressure in the core tube 11 is increased during the transition from the dehydration process to the transparentization process, so that the chlorine gas in the furnace body 12 can be detected in conjunction with the pressure increase at that time to detect the core tube crack. According to this embodiment, the presence or absence of a crack in the core tube can be inspected in each dehydration sintering process without adding a new process.
[0032] In the above-mentioned method, when chlorine gas flowing into the furnace body 12 is detected, it is preferable to use a helium leak detector to check for the presence or absence of helium gas flowing into the furnace body 12 while supplying helium gas into the furnace core tube. Helium leak detectors have high detection sensitivity but are expensive, so it is difficult from a cost perspective to install one for each furnace body. By performing additional inspection using a portable helium leak detector only when chlorine gas is detected, it is possible to detect core tube cracks more accurately without incurring large costs.
[0033] (Method of manufacturing optical fiber base material) The method for manufacturing an optical fiber preform according to an embodiment of the present disclosure is a method for manufacturing an optical fiber preform by inserting a porous optical fiber preform into a core tube and heating and making it transparent, and a method for detecting a crack in a core tube according to an embodiment of the present disclosure is carried out between the time when the porous optical fiber preform is inserted into the core tube 11 and the time when the optical fiber preform is removed from the core tube 11. Furthermore, in the method for manufacturing an optical fiber preform according to the present embodiment, when a crack in the core tube is detected by the method for detecting a crack in the core tube, the optical fiber preform is judged to be defective, or manufacturing using the core tube 11 is stopped until it is confirmed that the transmission loss of the optical fiber manufactured by drawing the optical fiber preform is good.
[0034] According to the manufacturing method of the optical fiber preform according to the present embodiment, the presence or absence of a crack in the core tube can be checked every time the porous preform 2 is inserted into the core tube 11 and the optical fiber preform is removed from the core tube, so that it is possible to quickly and easily determine whether the optical fiber preform is defective. Alternatively, the manufacturing using the core tube 11 is stopped until it is confirmed that the transmission loss of the optical fiber manufactured by drawing the optical fiber preform is satisfactory, so that it is possible to avoid continuing to manufacture optical fiber preforms with defective transmission loss.
[0035] The manufacturing method for an optical fiber preform according to this embodiment includes a dehydration step and a transparentizing step, in which the dehydration step is a step of supplying a gas containing chlorine gas into the core tube 11 while maintaining the inside of the core tube 11 at a negative pressure relative to the internal pressure of the furnace body 12, and the transparentizing step is a step of maintaining the inside of the core tube 11 at a positive pressure relative to the internal pressure of the furnace body 12, and at the timing of switching from the dehydration step to the transparentizing step, the chlorine gas that has flowed into the furnace body 12 may be detected to check for the presence or absence of cracks in the core tube 11. According to this embodiment, crack detection is performed using chlorine gas as a detection gas at the timing of switching from the dehydration step to the transparentizing step, so that cracks in the core tube can be detected without supplying additional detection gas or increasing the pressure for crack detection. [Explanation of symbols]
[0036] 1 Sintering furnace 11. Core tube 12 Furnace body 13 Heater 14 Lid 15 Gas supply port 16 Gas detector 2 Porous base material 3 Support rod
Claims
1. In a state where the detection gas is contained in the furnace tube, the internal pressure of the furnace tube is increased; A method for detecting cracks in a core tube of a sintering furnace for optical fiber preform, comprising detecting the detection gas flowing into a furnace body located outside the core tube in conjunction with an increase in the internal pressure of the core tube.
2. 2. The method for detecting a crack in a furnace core tube according to claim 1, wherein the detection gas is chlorine gas.
3. 3. The method for detecting a crack in a furnace core tube according to claim 2, further comprising the steps of: supplying helium gas into the furnace core tube when the detection gas is detected; and detecting the presence or absence of helium gas flowing into the furnace body using a helium leak detector.
4. A method for manufacturing an optical fiber preform, comprising inserting an optical fiber porous preform into a furnace tube and heating and making the preform transparent, comprising the steps of: a furnace tube crack detection method according to any one of claims 1 to 3 being carried out during a period from when the porous optical fiber preform is inserted into the furnace tube until when the optical fiber preform is removed from the furnace tube; When a core tube crack is detected by the core tube crack detection method, a manufacturing method for an optical fiber preform, the manufacturing method using the furnace tube being stopped until the optical fiber preform is judged to be defective or until it is confirmed that the transmission loss of the optical fiber manufactured from the optical fiber preform is satisfactory.
5. The method for producing the optical fiber preform includes a dehydration step and a clarification step, The dehydration step is a step of supplying a gas containing chlorine gas into the furnace tube while maintaining the inside of the furnace tube at a negative pressure relative to the internal pressure of the furnace body, The transparentizing step is a step of maintaining an inside of the furnace tube at a positive pressure with respect to an internal pressure of the furnace body, At the timing of switching from the dehydration process to the transparentization process, the presence or absence of a crack in the core tube is checked by the core tube crack detection method according to claim 2. The method for producing the optical fiber preform according to claim 4 .
Citation Information
Patent Citations
Device for producing optical fiber preform
JP1993078140A
Detection of cracking of oven core tube in process for sintering optical fiber base material and production of optical fiber base material
JP1999001337A
Method of detecting abnormality of core tube, and heating furnace
JP2004231482A