Mold release sheet, manufacturing method thereof, and method for manufacturing ceramic component using mold release sheet

A boron nitride and cellulose nanofiber-based release sheet addresses uneven application and environmental concerns, offering thin, strong, and space-efficient mold release with controlled atmospheres for ceramic manufacturing.

JP2024163535AInactive Publication Date: 2024-11-22NATIONAL INSTITUTE OF ADVANCED INDUSTRIAL SCIENCE & TECHNOLOGY
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023079245
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing mold release materials using boron nitride (BN) particles face issues such as uneven application, environmental impact, and poor space utilization due to the use of resin-based binders, leading to thickness and handling challenges.

Method used

A release sheet composed of boron nitride particles and cellulose nanofibers (CNF) with optional carbon particles, formulated to have a specific volume ratio and thickness, is produced using an aqueous slurry and dried to form a thin, strong sheet.

Benefits of technology

The sheet provides sufficient shape-retaining strength with reduced environmental impact, improves space utilization, and allows for controlled reducing atmospheres during ceramic member manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024163535000001_ABST
    Figure 2024163535000001_ABST
Patent Text Reader

Abstract

To provide a mold release sheet which is thinner and has sufficient shape retention strength while reducing environmental load.SOLUTION: A mold release sheet has sufficient shape retention strength even if thickness is small by using cellulose nanofibers derived from natural raw materials and having a fibrous state having a large ratio of fiber length / particle diameter as binders for boron nitride particles. Further, by including carbon particles in the release sheet, reduction in the case of manufacturing a product in a reducing atmosphere can be further appropriately performed.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a release sheet, a method for producing the same, and a method for producing a ceramic member using the release sheet. [Background technology]

[0002] Mold release materials are used to prevent seizure between ceramic members or between a member and a jig when they are manufactured by firing, and to prevent pressed products, cast products, etc. from sticking to the surface of a mold. Boron nitride, which also functions as a solid lubricant, is often used as a mold release material. Boron nitride (BN) is a bulky, fluffy particle that is difficult to handle in a dry state. Therefore, when it is applied as a solid to components or dies, etc., there are problems such as the particles scattering, failure to form an even film, and low adhesion to the surface. Therefore, it is common to prevent seizure or sticking between components by adding a solvent to make it liquid and applying it to anti-seizure parts or sliding parts by spraying or brushing (see Patent Document 1), or forming it into a sheet and sandwiching it between pre-fired molded bodies or between pre-fired molded bodies and jigs (Patent Documents 2 and 3).

[0003] Patent Document 1 describes a method in which a lubricating release agent, in which BN particles are dispersed in a solvent, is applied to the inner surface of a mold, and then the mold is used for casting, thereby preventing the material from sticking to the mold surface (Claim 1).

[0004] Patent Document 2 describes a method of forming a release agent layer by sandwiching a release sheet, which is made by forming an aqueous solution containing BN particles and an organic binder (ethyl cellulose, corn starch, acrylic resin, etc.) into a sheet and drying the sheet, between preforms before firing (Claim 1, paragraphs

[0017] ,

[0028] ,

[0031] ).

[0005] Patent Document 3 describes a method in which an unfired ceramic compact is sandwiched between a pair of release sheets made of a slurry containing BN particles, a binder polyvinyl butyral (PVB), and a dispersion medium, and then hot-press fired to obtain an oriented ceramic sintered body (Claims 1, 3, 10, Experimental Examples 1 and 3).

[0006] On the other hand, cellulose nanofibers (CNFs) are naturally derived materials that have been considered for various applications due to their low environmental impact, light weight, high strength, low thermal expansion, etc. Patent Document 4 describes a heat dissipation material made of a composite material of BN particles and CNFs. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2009-297754 A [Patent Document 2] JP 2001-240476 A [Patent Document 3] Patent No. 6490881 [Patent Document 4] Patent No. 6470539 Summary of the Invention [Problem to be solved by the invention]

[0008] As described in Patent Document 1, when a liquid mixture of BN particles and a solvent is applied to a mold or the like, droplets from the spray and streaks from the brush coating are likely to form, causing unevenness that can be transferred to the product surface. Furthermore, when a liquid is applied to the surface of a porous member such as a ceramic molded body before firing, the liquid may seep into the porous interior, causing adverse effects. Furthermore, unevenness transferred to the surface may lead to warping of the product.

[0009] Patent Documents 2 and 3 describe the production of ceramic members using release sheets containing BN particles. However, the binders used in the examples for the BN particles are resin-based synthetic products such as polyvinyl butyral (PVB) and acrylic resin, and the release sheets are produced from a slurry using an organic dispersion medium, which goes against the demand for carbon neutrality and places a large burden on the environment. Furthermore, the sheet-like material needs to have strength to maintain its shape as a sheet and make it easy to handle (hereinafter referred to as "shape retention strength"). However, resin-based synthetic binders do not have a strong bond with the BN particles, so a large amount of binder is required to achieve the required shape retention strength. Therefore, it is difficult to obtain a thin sheet-like material, and the release sheet takes up a large volume in the manufacturing equipment, which has a limited capacity (poor space factor).

[0010] Paragraph

[0031] of Patent Document 2 and paragraph

[0013] of Patent Document 3 give examples of binders derived from natural raw materials such as ethyl cellulose and corn starch, and the use of these is expected to have a certain effect in reducing the environmental load. However, like resin-based synthetic binders, these binders also require a certain amount of content to ensure shape retention strength, so there is a problem that the thickness cannot be reduced and the space factor cannot be improved.

[0011] In view of the above problems, an object of the present invention is to provide a release sheet that is thinner and has sufficient shape-retaining strength while reducing the environmental impact. [Means for solving the problem]

[0012] As mentioned above, CNF is a material that has been considered for various applications due to its characteristics such as low environmental impact, light weight, high strength, and low thermal expansion, and the above-mentioned Patent Document 4 describes a heat dissipation material made of a composite material of BN particles and CNF. However, the Patent Document does not describe anything about a release sheet. The present inventors have found that the above problems can be solved by using CNF as a binder for the BN particles in the release sheet.

[0013] That is, in order to solve the above problems, the present invention employs the following means. [1] A release sheet comprising boron nitride particles and cellulose nanofibers. [2] The release sheet of [1] above, wherein the boron nitride particles are contained in an amount of 40% or more and 95% or less by volume excluding voids in the release sheet. [3] The release sheet according to [2] or [3] above, containing carbon particles in a volume ratio of 1% to 20% by volume excluding voids in the release sheet. [4] The release sheet according to any one of [1] to [3] above, which has a film thickness of 1 μm or more and 200 μm or less. [5] The release sheet of [1] above, which has a three-layer structure in which a layer containing boron nitride particles, carbon particles, and cellulose nanofibers is sandwiched between layers containing boron nitride particles and cellulose nanofibers but not carbon particles. [6] The release sheet according to any one of [1] to [5] above, used in the production of a ceramic member. [7] The release sheet according to [6] above, wherein the ceramic member is a non-oxide ceramic member. [8] A method for producing a release sheet containing boron nitride particles and cellulose nanofibers, comprising a step of removing water from an aqueous slurry containing boron nitride particles and cellulose nanofibers and forming the slurry into a sheet. [9] The method for producing a release sheet according to [8] above, wherein the aqueous slurry further contains carbon particles.

[10] The method for producing a release sheet according to [8] or [9] above, wherein the step of removing the moisture and forming the slurry into a sheet is a step of pouring the slurry onto a non-absorbent substrate and drying it.

[11] The method for producing a release sheet according to [8] or [9] above, wherein the step of removing the moisture and forming the slurry into a sheet is a step of pouring the slurry onto a water-absorbent substrate and drying it.

[12] The method for producing a release sheet according to [8] or [9] above, wherein the step of removing the moisture and forming the slurry into a sheet is a step of screening the slurry through a mesh and drying it.

[13] A method for producing a ceramic member, comprising the step of sandwiching the release sheet according to any one of [1] to [5] above between a jig and a ceramic green body, and / or between ceramic green bodies, and firing the resulting product.

[14] The method for producing a ceramic member according to

[13] above, wherein the firing step is carried out in an inert gas atmosphere or a reducing gas atmosphere.

[15] The method for producing a ceramic member according to

[14] above, wherein the ceramic member is a non-oxide ceramic member. Effect of the Invention

[0014] According to the present invention, CNF, which has a high ratio of CNF fiber length / BN particle diameter and is therefore highly effective at binding BN particles, and which is derived from natural raw materials, is used as a binder for BN particles, making it possible to provide a thin release sheet that has sufficient shape retention strength with a smaller amount of binder while reducing the environmental impact. Furthermore, according to the present invention, the release sheet further contains carbon particles, so that reduction can be more appropriately carried out when a product is manufactured in a reducing atmosphere. Furthermore, according to the present invention, the release sheet is produced by removing water from the aqueous slurry and forming it into a sheet, thereby further reducing the environmental load. In addition, according to the present invention, the thickness of the release sheet can be reduced, thereby improving the space factor within a manufacturing device for ceramic members and the like. [Brief description of the drawings]

[0015] [Figure 1] Photograph of the release sheet obtained in Example 1 [Diagram 2] Photograph of the release sheet obtained in Example 2 [Diagram 3] Photograph of the release sheet obtained in Example 3 DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] The present invention provides a release sheet containing boron nitride particles and cellulose nanofibers, a method for producing the same, and a method for producing a ceramic member using the release sheet. In the present invention, "mold release" is not limited to the release between a product and a mold (to prevent seizure, sticking, and fusion), but also means the release between products (same as above).

[0017] Hereinafter, the configuration and effects of the present invention will be described along with technical concepts in accordance with an embodiment of the present invention (hereinafter, referred to as "the present embodiment"). In addition, when a numerical range is expressed using "~", it means that the numerical values ​​stated as the lower limit and upper limit are also included.

[0018] <Boron nitride (BN) particles> BN particles are known as a material with excellent releasability and lubricity. The BN particles used as a release material in the release sheet according to this embodiment are preferably hexagonal boron nitride particles. If the BN particles are too fine, the viscosity of the aqueous slurry described below will increase, making it difficult to produce a sheet. 50 It is preferable that the thickness is 0.5 μm or more, and more preferable that the thickness is 1 μm or more. In addition, if the BN particles are too large, the bonding strength with the CNFs described below may decrease. Therefore, the average particle size D of the BN particles 50 It is preferable that the thickness is 30 μm or less, and more preferably 10 μm or less. Such BN particles are readily available as a commercial product.

[0019] <Cellulose nanofiber> Cellulose nanofibers (CNF) are made by chemically or mechanically breaking down cellulose, the main component of plant cell walls, into nano-level particles. They are extremely fine fibers with diameters ranging from a few nm to 100 nm and lengths ranging from 100 nm to a few μm, which is more than 100 times the diameter. CNF, which is derived from natural sources, is a material that has been attracting attention in recent years due to its low environmental impact, light weight, high strength, low thermal expansion, and other properties. In this embodiment, CNF is used as a binder to bind the BN particles contained in the release sheet. As mentioned above, CNF is an extremely fine fiber with a length that is more than 100 times its nano-order diameter, so a small amount of CNF can entangle a large number of BN particles, thereby increasing the bonding between the BN particles and improving the shape retention strength of the sheet.

[0020] <Carbon particles> The release sheet according to this embodiment may contain carbon (C) particles in addition to BN particles and CNF. C particles have a reducing effect. C particles have higher dispersibility in aqueous slurry than BN particles, so the average particle diameter D 50 may be smaller than BN, and is preferably 0.01 μm or more. On the other hand, in order to maintain the bonding strength with CNF, the average particle diameter D 50 It is preferable that the thickness is 30 μm or less, and more preferable that the thickness is 10 μm or less. Since the C particles function as a reducing agent, the use of a release sheet containing the C particles is effective in generating and maintaining a reducing atmosphere, particularly when non-oxide ceramic components are manufactured by firing them in an inert gas atmosphere or a reducing gas atmosphere.

[0021] However, if a release sheet containing C particles is placed in direct contact with a porous green body and then fired, the C component may migrate into the voids in the pores, which may adversely affect the composition of the produced ceramic member. In such a case, a release sheet having a three-layer structure can be used, which includes a layer containing BN particles, C particles, and CNF sandwiched between two layers containing BN particles and CNF and not containing C, and the influence on the composition of the ceramic member can be avoided.

[0022] <Volume ratio of BN particles, CNF, and C particles> The specific volume ratio [BN / (BN + CNF)] of the BN particles contained in the release sheet in this embodiment is preferably 40% or more, excluding the voids of the release sheet, in order to obtain a thin sheet thickness, more preferably 70% or more for improving releasability, and even more preferably 80% or more. Also, in order to maintain the shape retention strength, it is preferably 95% or less, and more preferably 90% or less. The specific volume ratio [C / (BN + CNF + C)] when C particles are contained in the release sheet is preferably 1% or more, excluding the voids of the release sheet, and more preferably 3% or more for generating and maintaining a reducing atmosphere. Also, in order not to reduce the volume ratio of the BN particles having releasability, it is preferably 20% or less, and more preferably 15% or less. The measurement of the voids of the release sheet can be obtained from the ratio between the density of the sheet obtained by dividing the sheet mass by the volume (= area × thickness) and the density of a dense body assumed from the mass and density of BN, CNF, and C contained in the sheet. Alternatively, it can be obtained by the Archimedes method from the dry mass, water-containing mass, and underwater mass of the release sheet. Note that the measurement is not limited to the above method, and other methods may be used.

[0023] <Thickness of the release sheet> The release sheet is preferably as thin as possible as long as it can maintain the shape retention strength during use. For example, when manufacturing a ceramic member, a release sheet is interposed between the inner wall of a firing furnace or a jig and a green compact, or between a plurality of stacked green compacts, and a firing process is performed. If the size of the firing furnace is the same, a thinner release sheet allows more green compacts to be accommodated in the furnace, and more ceramic parts can be manufactured. Also, when a release sheet is used to cover the inner surface of the mold, it is preferable that the release sheet be thin in order to accurately transfer the shape of the mold to the product. The thickness of the release sheet is preferably 200 μm or less, more preferably 100 μm or less, and even more preferably 50 μm or less, while in order to maintain the shape retention strength, the thickness is preferably 1 μm or more, more preferably 10 μm or more, and even more preferably 20 μm or more.

[0024] <Manufacturing method of release sheet> The method for producing a release sheet according to this embodiment includes a step of adding a dispersion medium to the solid components, BN particles and CNF, or BN particles, C particles and CNF, to prepare a slurry, and a step of removing the solvent from the prepared slurry. The dispersion medium is preferably water. By using water as the dispersion medium instead of an organic solvent, the preparation of the slurry and the removal of water can be easily performed, and the process can be made with less environmental impact. In order to improve the dispersibility of the solid content, a dispersant such as polycarboxylate ammonium salt, polyethyleneimine, or a commercially available dispersant may be further added, but the addition of a dispersant is not essential. Even if the dispersant is not essential, the process can be made environmentally friendly.

[0025] The process for removing water from the aqueous slurry and forming it into a sheet is not particularly limited, but examples thereof include a process for pouring the slurry onto a non-absorbent substrate and drying it, a process for pouring the slurry onto an absorbent substrate, allowing it to absorb water and semi-dry, and then peeling it off and completely drying it, and a process for papering the slurry through a mesh and drying it. Examples of non-water-absorbent substrates include plastic sheets and aluminum sheets. Examples of the water-absorbent substrate include a porous ceramic water-absorbent plate, and a combination of filter paper and a Buchner funnel. The mesh preferably has an opening size of about 10 to 50 μm.

[0026] <Method of manufacturing ceramic member> The method for producing a ceramic member according to this embodiment includes a step of firing a green compact using a release sheet containing BN particles and CNF, or containing BN particles, C particles, and CNF. The release sheet may be placed between the green body and a jig such as an inner wall of a sintering container for a ceramic member or a spacer, or may be placed between multiple green bodies when stacking and sintering multiple green bodies.

[0027] The ceramic member according to the present invention includes an oxide-based ceramic member and a non-oxide-based ceramic member. The oxide-based ceramic member refers to any ceramic member that is fired at 800°C or less in an oxidizing atmosphere. Examples include alumina, zirconia, magnesia, barium titanate, lead titanate, etc. These may contain sintering aids. In addition, examples include glass-based members such as glass, glass / alumina, and glass / zirconia. The non-oxide ceramic member refers to any ceramic member that must be fired in an inert gas atmosphere or a reducing gas atmosphere, avoiding firing in an oxidizing atmosphere. Examples of non-oxide ceramic members include silicon nitride, silicon carbide, aluminum nitride, tungsten carbide, and cermet. These may contain sintering aids. In addition, oxide ceramics having a metal conductive layer or a carbon conductive layer inside may also be used.

[0028] When a green molded body on which a release sheet containing BN particles and CNF is arranged is fired at 400 to 800 ° C. in an oxidizing atmosphere, an inert gas atmosphere, or a reducing gas atmosphere, the CNF decomposes and is burned away or remains as residue C. Therefore, by the above firing process, only BN particles having a releasing effect, or only C of the residue of BN particles and CNF remains between the ceramic member and the jig, or between the ceramic members. Furthermore, when a release sheet containing C particles is used, in addition to BN particles or C of the residue of BN particles and CNF, C of the residue of C particles may also remain. The amount of C remaining can be adjusted by the firing temperature, time, and gas atmosphere.

[0029] When firing an oxide-based ceramic member in an oxidizing atmosphere, the above firing steps are carried out because oxidation of BN particles occurs at temperatures above 800° C. This method makes it possible to obtain an oxide-based ceramic member with good demolding properties. When firing a non-oxide ceramic member, after the above firing step, firing is further performed in an inert gas atmosphere or a reducing gas atmosphere at 1200 to 2500° C. This method makes it possible to obtain a non-oxide ceramic member with good demolding properties.

[0030] In particular, when a non-oxide ceramic member is produced, it is preferable to use a release sheet containing BN particles, C particles and CNF. By including C particles in the release sheet, it is possible to satisfactorily adjust the reducing atmosphere required for firing the green body of non-oxide ceramic. However, in order to prevent the C component from migrating to the ceramic member, it is preferable not to bring the release sheet containing C particles into direct contact with the green molding, and it is preferable to use a release sheet with a three-layer structure in which a layer containing C particles is sandwiched between two layers not containing C particles, as described above. EXAMPLES

[0031] The present invention will be specifically described below based on examples and comparative examples. It should be noted that the examples are merely preferred examples of the present invention, and the present invention is not limited to the following examples.

[0032] (Example 1-1) BN particles (Denka GP) 1g (density 2.1g / cm 3 , equivalent volume is 0.48cm 3 ), CNF (Sugino Machine WFo-10005, concentration 5 wt%, fiber diameter 10-50 nm) 15 g (solid content 0.75 g, density 1.5, volume equivalent 0.5 cm 3 ) and 0.5 g of a dispersant (ammonium polycarboxylate) were dispersed in 30 g of water to prepare an aqueous slurry. The volume ratio of BN particles and CNF particles, which are solid contents in the aqueous slurry, was BN:CNF=0.48:0.5. The volume ratio of the BN particles in the aqueous slurry excluding the binder (CNF) (hereinafter referred to as "slurry concentration") is about 1.6%, since the ratio of BN to water is 0.48:30.

[0033] The water was removed from the aqueous slurry by the following methods (1) to (3), and the aqueous slurry was formed into a sheet. The release sheet according to Example 1-1 was produced, in which the volume ratio of BN particles was 0.48 / (0.48+0.5)=49 vol% (excluding the void volume of the release sheet; the same applies below). (1) The mixture was poured onto a non-absorbent plastic sheet and left to dry at room temperature. (2) The mixture was poured onto a porous ceramic absorbent plate, left for 2 hours to absorb moisture, and then semi-dried. After that, it was peeled off from the substrate and completely dried. (3) The mixture was lifted up through a mesh having an opening of about 30 μm to form a sheet, which was then dried.

[0034] FIG. 1 shows an example of a photograph of the release sheet (70 mm×60 mm×80 μm) according to Example 1-1 produced by method (2). The sheet in Figure 1 had a nearly uniform thickness, and no cracks or holes were found. In other words, it was a well-made sheet without any problems. It could also be easily picked up with tweezers, and there were no problems with handling. In addition, for the release sheets according to Example 1-1 produced by methods (1) and (3), sheets of the same size as the sheet produced by method (2) were successfully produced, no cracks or holes were found, and there were no problems with handling.

[0035] (Example 1-2: Study of non-use of dispersant) An aqueous slurry was prepared in the same manner as in Example 1-1 except that no dispersant (ammonium polycarboxylate) was used, and then a release sheet according to Example 1-2 was prepared using the method in (2). It was possible to produce good sheets without any problems even without a dispersant. As in Example 1, there was no problem with handling. This is presumably because the CNF fibers have the effect of incorporating and dispersing the BN particles into the CNF network structure.

[0036] (Examples 1-3 to 1-6: Examination of BN particle size) Average particle diameter (D 50 The release sheets according to Examples 1-3 to 1-6 were produced in the same manner as in the method of (2) of Example 1-1, except that the following four types of BN particles with different molecular weights were used. Example 1-3: Showa Denko UHP-S2(D 50 =0.7μm), Example 1-4: Denka HGP (D 50 = 5 μm) Example 1-5: Denka MGP (D 50 = 10 μm) Example 1-6: Denka SGP (D 50 = 18 μm)

[0037] Example 1-4 (D 50 = 5 μm), Example 1-5 (D 50 In Example 1-1 (D = 10 μm), 50 = 7 μm), a good release sheet could be produced without any problems, and the handling properties were also good. Example 1-3 (D 50 = 0.7 μm), D 50 The viscosity of the aqueous slurry produced was higher than in other Examples in which the viscosity was larger, making it somewhat difficult to handle; however, it was possible to produce a release sheet without holes or cracks, and the handleability was also good. Example 1-6 (D 50 = 18μm), there was no problem in producing the release sheet. 50 The diameter was lower than in the other smaller examples, and care had to be taken when lifting it with tweezers, but handling was possible.

[0038] The results are shown in Table 1 below together with those of Example 1-1. From Table 1, the particle size range of the BN particles suitable for the release sheet according to the present invention can be predicted.

[0039] [Table 1]

[0040] (Example 2: Examination of the volume ratio of BN particles) BN particles (Denka HGP) 1g (density 2.1g / cm 3 , equivalent volume is 0.48cm 3 ), CNF (Sugino Machine WFo-10005) 3g (volume equivalent: 0.1cm 3 ) and 0.5 g of a dispersant (ammonium polycarboxylate) were dispersed in 15 g of water to prepare an aqueous slurry. The volume ratio of BN particles and CNF, which are the solid contents in the aqueous slurry, is BN:CNF=0.48:0.1, and the slurry concentration of BN particles is BN:water=0.48:15, so is approximately 3.2%. The water was removed from the aqueous slurry in the same manner as in Example 1, and the aqueous slurry was formed into a sheet to prepare a release sheet according to Example 2. The volume ratio of the BN particles in the release sheet is 0.48 / (0.48+0.1)=83 vol %.

[0041] 2 is a photograph of a release sheet (50 mm×40 mm×120 μm) according to Example 2 produced by method (1) as an example. Even in Example 2, in which the volume ratio of BN was more than 80% and the volume ratio of the binder was less than 20%, there were no problems with the production and handling of the sheet.

[0042] (Example 3-1: Examination of the addition of C particles) BN particles (Denka HGP) 1g (density 2.1g / cm 3 , equivalent volume is 0.48cm 3 ), C particles (high purity chemical, particle size 5μm) 0.2g (density 2.1g / cm 3 , equivalent volume 0.09cm 3 ), CNF (Sugino Machine WFo-10005) 17g (volume equivalent: 0.57cm3 ) and 0.5 g of a dispersant, ammonium polycarboxylate, were dispersed in 40 g of water to prepare an aqueous slurry. The volume ratio of BN particles, C particles, and CNF was BN:C:CNF = 0.48:0.09:0.57, and the slurry concentration of BN particles was BN:water = 0.48:40, so approximately 1.2 vol%, and the slurry concentration of C particles was C:water = 0.09:40, so approximately 0.2%. The water-based slurry was subjected to removal of water by the same methods (1) to (3) as in Example 1, and formed into a sheet to produce a release sheet according to Example 3-1. The volume percentages of the BN particles and C particles in the release sheet are 0.48 / (0.48+0.09+0.57)=42 vol% and 0.09 / (0.48+0.09+0.57)=8 vol%, respectively.

[0043] 3 is a photograph of a release sheet (80 mm×60 mm×110 μm) according to Example 3-1 produced by method (2) as an example. Even in Example 3-1 using C particles, there were no problems with sheet production and handling, and sufficient shape retention strength was ensured.

[0044] (Examples 3-2 to 3-5: Examination of C particle size) Average particle diameter (D 50 Release sheets according to Examples 3-2 to 3-5 were produced in the same manner as in (2) of Example 3-1, except that the following four types of C particles with different molecular weights were used. Example 3-2: Sigma-Aldrich Carbon Black (D 50 =0.1μm) Example 3-3: High Purity Chemical Carbon (D 50 = 10 μm) Example 3-4: High Purity Chemical Carbon (D 50 = 20μm) Example 3-5: High Purity Chemical Carbon (D 50 = 50 μm) Examples 3-2 to 3-4 (D 50 =0.1 μm, 10 μm, 20 μm), Example 3-1 (D 50= 2 μm), a good release sheet could be produced without any problems, and the handling properties were also good. Example 3-5 (D 50 = 50 μm), sheets could be produced, but black spots (large C particles) were sometimes visible within the sheets.

[0045] The results are shown in Table 2 below together with those of Example 3-1. From Table 2, the particle size range of the C particles suitable for the release sheet according to the present invention can be predicted.

[0046] [Table 2]

[0047] (Example 4: Three-layer structure) A slurry containing BN particles and CNF was prepared in the same manner as in Example 1-4. A slurry containing BN particles, C particles, and CNF was prepared in the same manner as in Example 3-1. Next, the slurry containing BN particles and CNF was poured onto a porous ceramic absorbent plate, and the slurry was allowed to absorb water and become semi-dried. After that, the slurry containing BN particles, C particles, and CNF was poured onto the plate, and the slurry was allowed to absorb water and become semi-dried. Then, the slurry containing BN particles and CNF was poured onto the plate, and the slurry was allowed to absorb water and become semi-dried. After that, the slurry was peeled off from the absorbent plate and completely dried to produce a three-layered sheet of BN-CNF / BN-C-CNF / BN-CNF. This sheet had no problems in handling and had sufficient shape retention strength.

[0048] In the following Examples 5 to 7, the type of binder is examined by comparison with Comparative Examples 5a to 7a and Comparative Examples 5b to 7b, and the relationship between the proportion of BN particles and the thickness and shape retention strength of the release sheet that can be produced is examined.

[0049] (Example 5: 50 vol% BN particles; CNF) 1 g of BN particles (Denka HGP) and 14.4 g of CNF (Sugino Machine WFo-10005) were dispersed in 38 g of water to prepare an aqueous slurry with a BN particle concentration of 1.3 vol %. The aqueous slurry was applied onto a non-absorbent plastic sheet using an applicator with a gap of 400 μm at a film-forming speed of 10 mm / sec., and after drying, a release sheet having a thickness of 25 μm, a length of 20 mm and a width of 5 mm was cut out. In order to evaluate the shape retention strength of the release sheet, the release sheet was pulled in the film-forming direction (the direction of movement of the applicator) and the tensile strength was measured. The higher the tensile strength, the higher the shape retention strength.

[0050] (Comparative Example 5a: 50 vol% BN particles; PVB) 9g of BN particles (Denka HGP), 4.5g of polyvinyl butanol (PVB: Sekisui BM-1), and 2.3g of dioctyl phthalate, a plasticizer, were dispersed in a mixture of 2-propanol and 1-butanol (volume ratio 3:1) to prepare a slurry with a slurry concentration of 12 vol% (no dispersant was used). The slurry was formed into a film in the same manner as in Example 5, and a release sheet having a thickness of 65 μm was cut out, and the tensile strength in the film formation direction was measured.

[0051] (Comparative Example 5b: 50 vol% BN particles; starch paste) 10 g of BN particles (Denka HGP) and 8 g of starch paste were mixed, and water was added as a dispersion medium to prepare an aqueous slurry with a slurry concentration of 15 vol%. The aqueous slurry was formed into a film in the same manner as in Example 5, and a release sheet having a thickness of 80 μm was cut out, and the tensile strength in the film formation direction was measured.

[0052] The tensile strength of the release sheets according to Example 5 and Comparative Examples 5a and 5b is shown in Table 3 below.

[0053] [Table 3]

[0054] From Table 3, it can be seen that in Example 5, in which the volume ratio of BN particles in the release sheet is 50 vol%, a release sheet that is thin and has high shape retention strength can be produced using a low-viscosity slurry liquid dispersed in a large amount of water, in which the binder is CNF. In contrast, in Comparative Example 5a, in which the binder is PVB, or Comparative Example 5b, in which the binder is starch glue, a slurry concentration of about 10 times or more that of Example 4 is required to produce a release sheet, and the sheet thickness is inevitably greater than that of Example 5. In addition, the shape retention strength is also inferior to that of Example 5.

[0055] (Example 6, Comparative Examples 6a and 6b: BN particles 70 vol%) Release sheets according to Example 6 and Comparative Examples 6a and 6b were produced in the same manner as in Example 5 and Comparative Examples 5a and 5b, respectively, except that the volume ratio of the BN particles in the release sheet was set to 70 vol%. The results for Example 6 and Comparative Examples 6a and 6b are shown in Table 4 below.

[0056] [Table 4]

[0057] Table 4 shows almost the same tendency as Table 3, even when the volume fraction of BN particles is 70 vol%. That is, in Example 6 in which the binder is CNF, a release sheet having a thickness of 37 μm and a shape retention strength of 8 MPa was obtained, whereas in Comparative Example 6a in which the binder is PVB, the release sheet obtained by increasing the slurry concentration by about 10 times had a thickness of 86 μm, and the shape retention strength of the release sheet was not as good as that of Example 6. In Comparative Example 6b in which the binder is starch paste, a film could not be formed even when the slurry concentration was 19 vol%, and a release sheet could not be produced.

[0058] (Example 7, Comparative Examples 7a and 7b: BN particles 83 vol%) Release sheets according to Example 7 and Comparative Examples 7a and 7b were produced in the same manner as in Example 5 and Comparative Examples 5a and 5b, respectively, except that the volume ratio of the BN particles in the release sheet was 83 vol%. In Example 7, a release sheet having a thickness of 48 μm was obtained, but in Comparative Example 7a, the volume ratio of the binder relative to the volume ratio of the BN particles was too small, and a sheet could not be produced. In Comparative Example 7b, in which the binder was starch paste, the slurry was highly viscous and creamy, and it was not possible to prepare a slurry suitable for sheet production. The experimental results for Example 7 and Comparative Examples 7a and 7b are shown in Table 5 below.

[0059] [Table 5]

[0060] From Table 5, it can be seen that even when the volume fraction of BN particles is 83 vol%, in Example 7 where the binder is CNF, the slurry concentration and sheet thickness are greater than those of Examples 5 and 6, but the thickness can be made 50 μm or less, and the shape retention strength is sufficient to withstand a tensile force of 2 MPa. In contrast, in Comparative Example 7a, in which the binder was PVB, it was impossible to form a film even when the slurry concentration was 21 vol%, and in Comparative Example 7b, in which the binder was starch paste, it was impossible to even prepare a slurry. The above results demonstrate that by using CNF as a binder for BN particles, it is possible to provide a thin release sheet with excellent shape retention.

[0061] (Example 8: Application to the production of aluminum nitride ceramic components) The release sheets (40 mm×40 mm) according to Examples 1-1 and 2 were sandwiched between an aluminum nitride green compact (30 mm×30 mm×0.5 mm) and a jig, and between the green compacts themselves, and were degreased in a sintering furnace at 500° C. in air for 1 hour, and sintered at 1850° C. in nitrogen at 1 atmosphere for 2 hours. BN layers were formed between the aluminum nitride members and the jig, and between the aluminum nitride members, when the aluminum nitride members were removed, and no adhesion sites were observed.

[0062] (Example 9: Application to the manufacture of silicon nitride ceramic components) The release sheets (40 mm x 40 mm) according to Examples 1-1 and 2 were sandwiched between a silicon nitride green body (30 mm x 30 mm x 0.5 mm) and a jig, and between the green bodies themselves, and were degreased in a sintering furnace at 500°C in air for 1 hour, and sintered at 1800°C in nitrogen at 5 atmospheres for 2 hours. BN layers were formed between the removed silicon nitride members and the jig, and between the silicon nitride members, and no adhesion sites were observed.

[0063] (Example 10: Application of release sheet containing C particles to the manufacture of aluminum nitride ceramic components) The release sheet (40 mm x 40 mm) according to Example 3-1 was sandwiched between an aluminum nitride green compact (φ25 mm x 3 mm) and a jig, and in a firing furnace, it was degreased in air at 500°C for 1 hour, and fired in nitrogen at 1 atm for 2 hours at 1850°C. A BN layer was formed between the aluminum nitride member and the jig when it was removed, and no adhesion was observed. The thermal conductivity of the obtained aluminum nitride was 190 W / mK when measured by the laser flash method. The aluminum nitride member produced in the same manner as in Example 10 using the release sheet of Example 1 had a thermal conductivity of 160 W / mK. Therefore, it can be seen that the release sheet containing C particles exerts a stronger reducing effect, contributing to improved thermal conductivity.

[0064] (Example 11: Application of three-layered sheet to the manufacture of ceramic components) A release sheet having a three-layer structure was prepared by sandwiching a sheet containing BN particles, C particles, and CNF according to Example 3-1 between the outer layers as an intermediate layer, and a silicon nitride member was fired in the same manner as in Example 9. A BN layer was formed between the removed silicon nitride member and the jig, and between the silicon nitride members, and no adhesion sites were observed. [Industrial Applicability]

[0065] The release sheet according to the present invention uses CNF, which has high binding affinity with BN particles, as a binder, so that even if the ratio of BN particles is increased to enhance releasability, a thin release sheet with high shape retention strength can be provided. Therefore, the present invention can be used to minimize the space factor during the production of ceramic members, pressed products, cast products, etc., and to prevent sticking or seizing between products and production equipment or between products. In addition, the release sheet according to the present invention can be produced using a slurry containing CNF, which is derived from natural products, as a binder for the BN particles, and water as a dispersion medium. Therefore, the present invention can produce a release sheet with low environmental impact. The release sheet according to the present invention, particularly by adding C particles, can adjust the reducing atmosphere, and can therefore be used to prevent seizure between a member and a jig, or between members, during firing in the production of non-oxide ceramic members such as silicon nitride and aluminum nitride.

Claims

1. A release sheet comprising boron nitride particles and cellulose nanofibers.

2. 2. The release sheet according to claim 1, wherein the boron nitride particles are contained in an amount of 40% or more and 95% or less by volume, excluding voids in the release sheet.

3. 3. The release sheet according to claim 2, comprising carbon particles in a volume ratio of 1% to 20% by volume excluding voids in the release sheet.

4. 2. The release sheet according to claim 1, having a film thickness of 1 μm or more and 200 μm or less.

5. 2. The release sheet according to claim 1, which has a three-layer structure in which a layer containing boron nitride particles, carbon particles, and cellulose nanofibers is interposed between two layers containing boron nitride particles and cellulose nanofibers but not carbon particles.

6. The release sheet according to any one of claims 1 to 5, which is used in the production of a ceramic member.

7. The release sheet according to claim 6 , wherein the ceramic member is a non-oxide ceramic member.

8. A method for producing a release sheet containing boron nitride particles and cellulose nanofibers, comprising a step of removing water from an aqueous slurry containing boron nitride particles and cellulose nanofibers and forming the slurry into a sheet.

9. The method for producing a release sheet according to claim 8 , wherein the aqueous slurry further contains carbon particles.

10. The method for producing a release sheet according to claim 8 or 9, wherein the step of removing the moisture and forming into a sheet is a step of pouring the slurry onto a non-water-absorbent substrate and drying it.

11. The method for producing a release sheet according to claim 8 or 9, wherein the step of removing the moisture and forming the slurry into a sheet is a step of pouring the slurry onto a water-absorptive substrate and drying the slurry.

12. The method for producing a release sheet according to claim 8 or 9, wherein the step of removing the moisture and forming the slurry into a sheet is a step of sifting the slurry through a mesh and drying it.

13. A method for producing a ceramic member, comprising a step of sandwiching the release sheet according to any one of claims 1 to 5 between a jig and a ceramic green body, and / or between ceramic green bodies, and firing the resulting product.

14. The method for producing a ceramic member according to claim 13, wherein the firing step is carried out in an inert gas atmosphere or a reducing gas atmosphere.

15. The method for producing a ceramic member according to claim 14, wherein the ceramic member is a non-oxide ceramic member.

Citation Information

Patent Citations

  • Pneumatic tire

    JP1989070539A

  • Resin body structure for automobile

    JP1989090881A

  • Hot press method and manufacturing method of ceramic element

    JP2001240476A

  • Casting method for ferrous alloy in semi-melted or semi-solidified state and mold for casting

    JP2009297754A