Method for producing zeolite

By employing multiple zeolites with shared CBUs, the method addresses the synthesis challenges of low-silica CON-type zeolites, enabling efficient production and extended catalyst life for lower olefin synthesis.

JP2024163752APending Publication Date: 2024-11-22MITSUBISHI CHEM CORP +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023079616
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing methods struggle to produce zeolites, particularly low-silica CON-type zeolites, which are difficult to synthesize and have insufficient catalyst lifespan for producing lower olefins.

Method used

A method involving the use of two or more types of zeolites with the same composite building units (CBUs) as the target zeolite, specifically using Beta and MFI type zeolites, to facilitate the synthesis of CON-type zeolites with a high aluminum content, enhancing catalyst longevity.

Benefits of technology

This approach allows for the easy production of CON-type zeolites with improved catalyst life, maintaining high conversion rates for a longer period, suitable for producing lower olefins.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024163752000003
    Figure 2024163752000003
  • Figure 2024163752000004
    Figure 2024163752000004
  • Figure 2024163752000001
    Figure 2024163752000001
Patent Text Reader

Abstract

To provide a method for producing zeolite which can easily obtain types of zeolite that are conventionally difficult to produce.SOLUTION: There is provided a method for producing zeolite using a plurality of zeolites different from zeolite (X) to be synthesized as silicon sources, wherein at least one zeolite (A) of the plurality of zeolites has one or more CBUs constituting the zeolite (X) to be synthesized, the zeolite (B) as at least another one of the plurality of zeolites has one or more other CBUs constituting the zeolite (X) to be synthesized, and the zeolite (A) and the zeolite (B) are each contained in the silicon sources at 5 mass% or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a zeolite, and more particularly to a method for producing a CON-type zeolite. [Background technology]

[0002] Zeolites are widely used industrially as catalysts, adsorbents, ion exchange materials, molecular sieves, separation materials, etc. The basic unit of the zeolite structure is the TO4 unit, which is made up of silicon, aluminum, and oxygen atoms, and several TO4 units are linked together to form structural units called composite building units (hereinafter referred to as "CBU"). As a method for synthesizing a target zeolite, a synthesis method called zeolite conversion method is known in which a zeolite is used as a starting material and converted into the target zeolite. Specifically, a method has been reported in which a zeolite having a common CBU with the target zeolite is used as a synthesis raw material (Non-Patent Documents 1-3), but on the other hand, there is also a document (Non-Patent Document 4) that claims that the correlation between the starting material and the final product cannot be explained by the structural similarity of the CBU alone.

[0003] Meanwhile, one application of zeolites is as a catalyst for producing lower olefins. For example, as disclosed in Patent Document 1, propylene and butene can be produced in high yields by using methanol and / or dimethyl ether as a raw material and a catalyst containing a zeolite having a CON structure (CIT-1 zeolite) as an active component. However, the catalytic life of CON-type zeolites is not necessarily sufficient, and frequent switching between reaction gas and regeneration gas is required to regenerate the catalyst. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2013-245163 A [Non-patent literature]

[0005] [Non-Patent Document 1] J.Jpn.Petrol.Inst.,56,183-197(2013) [Non-Patent Document 2] J.Am.Chem.Soc.,134,11542-11549(2012) [Non-Patent Document 3] J.Nanosci.Nanotechnol.,13,3020-3026(2013) [Non-Patent Document 4] Nat. Mater.,18,1177-1181(2019) Summary of the Invention [Problem to be solved by the invention]

[0006] Although the above-mentioned methods are known as methods for producing zeolites, some types of zeolites are difficult to produce. For example, in the case of CON-type zeolites, it is known that it is difficult to synthesize low-silica CON-type zeolites that contain a lot of aluminum. In other words, an important issue is how to synthesize difficult-to-synthesize zeolites such as low-silica CON-type zeolites in a simple manner. The present invention is devised to solve the above problems, and has an object to provide a method for producing zeolite, which can easily produce zeolites that have been difficult to produce in the past. As described above, although CON-type zeolite is useful as a catalyst for producing lower olefins, it has a problem of insufficient catalyst life. Therefore, the present invention also aims to provide a method for producing CON-type zeolite with a long catalyst life that can be used as a catalyst for synthesizing lower olefins. [Means for solving the problem]

[0007] The present inventors have conducted research to solve the above problems, and have found that a zeolite that is difficult to synthesize can be synthesized by synthesizing the zeolite using two or more different zeolites having a common CBU with the zeolite to be synthesized as raw materials, and have completed the present invention. In the present invention, even if all of the constituent CBUs are not prepared, a desired single phase of zeolite can be easily obtained by using two or more zeolites containing one of them. For example, even in the case of a low-silica CON-type zeolite that is difficult to synthesize, even if all four of the constituent CBUs are not prepared, a substantially single phase of CON-type zeolite can be easily obtained by using two or more zeolites containing one of them, and a low-silica CON-type zeolite can be obtained. Furthermore, the present inventors have found that when a CON-type zeolite obtained by using, as seed crystals, a low-silica CON-type zeolite, which has been difficult to obtain in the past but which has become easily obtainable according to the present invention, is used as a catalyst, a high raw material conversion rate can be maintained for a long period of time.

[0008] The present invention includes the following gist. [1] A method for producing a zeolite using, as a silicon source, multiple zeolites different from a zeolite (X) to be synthesized, characterized in that at least one of the multiple zeolites, zeolite (A), has one or more CBUs that constitute the zeolite (X) to be synthesized, and at least one other of the multiple zeolites, zeolite (B), has one or more other CBUs that constitute the zeolite (X) to be synthesized, and zeolite (A) and zeolite (B) are each contained in an amount of 5 mass% or more in the silicon source. [2] The method for producing a zeolite according to the above [1], wherein the zeolite (X) to be synthesized is a CON-type zeolite. [3] The method for producing a zeolite according to the above [1] or [2], wherein the zeolite (A) is a zeolite having at least bea as a CBU, and the zeolite (B) is a zeolite having at least mel as a CBU. [4] The method for producing a zeolite according to any one of the above [1] to [3], wherein the zeolite (A) is a Beta zeolite having at least bea as a CBU, and the zeolite (B) is an MFI zeolite having at least mel as a CBU. [5] The method for producing a zeolite according to any one of the above [1] to [4], wherein the zeolite (X) to be synthesized has a molar ratio (Si / Al) of silicon (Si) to aluminum (Al) of 500 or less. [6] A method for producing a CON-type zeolite, comprising adding, as seed crystals, a CON-type zeolite having a Si / Al ratio of 50 or less in an amount of 1 mass% or more relative to a silicon source. Effect of the Invention

[0009] According to the present invention, it is possible to provide a method for producing a zeolite that can easily produce a zeolite that has been difficult to produce in the past, and a method for producing a CON-type zeolite with a long catalytic life that can be used as a catalyst for synthesizing lower olefins. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a diagram showing the results of powder X-ray diffraction of the zeolites synthesized in Example 1 and Comparative Examples 1 to 3. [Diagram 2] 1 is a graph showing the transition of methanol conversion and selectivity of each component in the production of lower olefins using the zeolites of Example 2 and Comparative Example 4 as catalysts. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present invention will be described in detail below, but it is believed that the present invention can be applied to any zeolite. In the following description, low-silica CON-type zeolite containing a large amount of aluminum will be described as a representative zeolite that is difficult to produce. In other words, the description of the constituent elements described below is one example (representative example) of an embodiment of the present invention, and the present invention is not limited to these contents, and can be implemented in various modified forms within the scope of its gist.

[0012] [Zeolite manufacturing method] Zeolite can be produced by preparing a mixture of crystal precursors (hereinafter sometimes referred to as "raw materials") containing (a) a silicon source, (b) an aluminum source, (c) an alkali metal element source and / or an alkaline earth metal element source, (d) an organic structure directing agent, (e) water, and, if necessary, a seed crystal, and subjecting the mixture to hydrothermal synthesis.

[0013] (Raw material ingredients) (a) Silicon Source The silicon source used in this embodiment is characterized by using multiple zeolites different from the zeolite (X) to be synthesized as the silicon source. When one of the multiple zeolites is zeolite (A), it is essential that one or more of the CBUs of the zeolite (A) are the same as the CBUs constituting the zeolite (X) to be synthesized, and when another of the multiple zeolites is zeolite (B), it is essential that one or more of the CBUs of the zeolite (B) are the same as the CBUs constituting the zeolite (X) to be synthesized. As mentioned above, CBU refers to the structural unit defined by the International Zeolite Association (IZA). As the zeolite (X), AFX type, Beta, CHA type, CON type, DDR type, ERI type, FAU type, FER type, KFI type, LEV type, LTA type, LTL type, MEL type, MFI type, MSE type, MTW type, MWW type, RHO type, and SZR type are preferred, CON type, CHA type, KFI type, MTW type, and MWW type are more preferred, and CON type is even more preferred.

[0014] For example, when the zeolite (X) is a CON type zeolite, the CBU of the CON type zeolite is bea, mel, bre, and lau, and specific examples of the zeolite (A) and the zeolite (B) include Beta, IFR type, MSE type, STT type, BOG type, BRE type, HEU type, IWR type, IWW type, RRO type, STI type, TER type, ASV type, ATO type, BCT type, DFO type, EZT type, ITH type, LAU type, MSO type, OSI type, -RON type, SAO type, TUN type, UOZ type, DON type, MEL type, MFI type, MWW type, and SFG type. Among them, Beta zeolite having bea, mtw, and mor as the CBU, and MFI zeolite having mfi, mel, mor, and cas as the CBU can be preferably used. Further, it is preferable that the zeolite (A) is a zeolite having at least bea as a CBU, and the zeolite (B) is a zeolite having at least mel as a CBU. More specifically, it is preferable that the zeolite (A) is a beta zeolite having at least bea as a CBU, and the zeolite (B) is an MFI type zeolite having mel as a CBU.

[0015] When the zeolite (X) is a CHA type zeolite, the CBU of the CHA type zeolite is d6r and cha, and specific examples of the zeolite (A) and the zeolite (B) include AEI type, AFT type, AFX type, EAB type, EMT type, ERI type, FAU type, GME type, KFI type, LEV type, LTL type, LTN type, MOZ type, MSO type, MWW type, OFF type, SAS type, SAT type, SAV type, SBS type, SBT type, SZR type, TSC type, and -WEN type. Among them, FAU type zeolite having d6r and sod as CBU and AFT type zeolite having d6r, gme, cha, and aft as CBU can be preferably used.

[0016] When the zeolite (X) is a KFI type zeolite, the CBU of the KFI type zeolite is d6r, pau and lta, and specific examples of the zeolite (A) and the zeolite (B) include AEI type, AFT type, AFX type, CHA type, -CLO type, EAB type, EMT type, ERI type, FAU type, GME type, LEV type, LTA type, LTL type, LTN type, MER type, MOZ type, MSO type, MWW type, OFF type, PAU type, RHO type, SAS type, SAT type, SAV type, SBS type, SBT type, SZR type, TSC type, UFI type, -WEN type. Among them, FAU type zeolite having d6r and sod as CBU, and LTA type zeolite having d4r, sod and lta as CBU can be preferably used.

[0017] When the zeolite (X) is an MWW type zeolite, the CBU of the MWW type zeolite is d6r and mel, and specific examples of the zeolite (A) and the zeolite (B) include AEI type, AFT type, AFX type, CHA type, CON type, DON type, EAB type, EMT type, ERI type, FAU type, GME type, ITH type, IWR type, IWW type, KFI type, LEV type, LTL type, LTN type, MEL type, MFI type, MOZ type, MSO type, MWW type, OFF type, SAS type, SAT type, SAV type, SBS type, SBT type, SFG type, SZR type, TSC type, and -WEN type. Among them, FAU type zeolite having d6r and sod as the CBU, and MFI type zeolite having mfi, mel, mor, and cas as the CBU can be preferably used.

[0018] When the zeolite (X) is an MTW type zeolite, the CBU of the MTW type zeolite is jbw, cas, bik and mtw, and specific examples of the zeolite (A) and the zeolite (B) include Beta, BEC type, BIK type, BOG type, CAS type, CFI type, EUO type, GON type, IHW type, ISV type, IWV type, JBW type, MFI type, MSE type, MTT type, MTW type, NES type, NSI type, SFE type, SFF type, SFH type, SFN type, SSY type, STF type, STT type, TER type, TON type, TUN type, UTL type, and VET type. Among them, Beta zeolite having bea, mtw and mor as the CBU, and MFI zeolite having mfi, mel, mor and cas as the CBU can be suitably used.

[0019] Note that Beta is a zeolite that was previously written as *BEA, but as described in Zeolite, 40(2)72-77(2023), due to the abolition of the asterisk-marked framework type code for zeolites, it is now written as Beta.

[0020] The content of the zeolite (A) and the zeolite (B) in the silicon source is preferably 5% by mass or more. The content of the zeolite (A) is more preferably 10% by mass or more, even more preferably 15% by mass or more, even more preferably 20% by mass or more, particularly preferably 25% by mass or more, and particularly preferably 30% by mass or more. The content of the zeolite (B) is more preferably 10% by mass or more, even more preferably 15% by mass or more, even more preferably 20% by mass or more, particularly preferably 25% by mass or more, and particularly preferably 30% by mass or more. When the content is more than the above, the desired zeolite (X) can be effectively obtained. The upper limit of the content of zeolite (A) is not particularly limited, but taking into account the contents of other components in the raw material, it is usually 90 mass % or less, may be 70 mass % or less, or may be 50 mass % or less. The upper limit of the content of zeolite (B) is not particularly limited, but taking into account the contents of other components in the raw material, it is usually 90 mass % or less, may be 70 mass % or less, or may be 50 mass % or less.

[0021] The particle size of the zeolite (A) and the zeolite (B) is not particularly limited, but the average primary particle size is usually 0.02 μm or more, preferably 0.04 μm or more, more preferably 0.06 μm or more, and usually 5 μm or less, preferably 2 μm or less, more preferably 1 μm or less, and further preferably 0.60 μm or less. By setting the average primary particle size of the zeolite (A) and the zeolite (B) within the above range, the solubility in the raw material is increased, the production of by-products is suppressed, and the crystallization can be efficiently promoted.

[0022] The zeolite (A) and the zeolite (B) may be either a zeolite containing a structure-directing agent that has not been calcined after hydrothermal synthesis, or a zeolite containing no structure-directing agent that has been calcined. The zeolite (A) and the zeolite (B) may be added to the raw material after being dispersed in a suitable solvent, such as water, or may be added directly without being dispersed.

[0023] In addition, the raw material may contain other silicon sources in addition to the above zeolite (A) and zeolite (B). The other silicon sources are not limited as long as they are usually used as silicon sources, and include, for example, silicates such as fine silica, silica sol, silica gel, fumed silica, and water glass, silicon alkoxides such as tetramethoxysilane and tetraethoxysilane, and silicon halides. In addition, zeolites other than the above zeolite (A) and zeolite (B), for example, silica-containing zeolites such as FAU type zeolite and CHA type zeolite, and silicoaluminophosphates may be used as silicon sources. These silicon sources need only have the above-mentioned zeolite (A) and zeolite (B), and the other silicon sources may be used alone or in combination of two or more.

[0024] Among these other silicon sources (i.e., silicon sources other than zeolite (A) or (B)), in terms of cost advantage and ease of handling, preferably, fine silica, silica sol, water glass, silica-containing zeolite, etc. are used, and more preferably, in terms of reactivity, silica sol, water glass, silica-containing zeolite are used. The content of the other silicon source in the silicon source is not particularly limited, but is usually 90 mass% or less, preferably 75 mass% or less, more preferably 60 mass% or less, even more preferably 50 mass% or less, and particularly preferably 40 mass% or less.

[0025] (b) an aluminum source As the aluminum source used in this embodiment, a zeolite mixture containing the above-mentioned zeolite (A) and zeolite (B) may be used as both a silicon source and an aluminum source. The raw material according to the present invention may contain an aluminum source other than the above-mentioned multiple zeolites, such as amorphous aluminum hydroxide, aluminum hydroxide having a gibbsite structure, aluminum hydroxide having a bayerite structure, aluminum nitrate, aluminum sulfate, aluminum oxide, sodium aluminate, boehmite, pseudo-boehmite, alumina sol, aluminum alkoxide, etc. Furthermore, aluminum-containing zeolites such as FAU-type zeolite and CHA-type zeolite, and aluminophosphates may be used as the aluminum source. These aluminum sources may be used alone or in combination of two or more.

[0026] Of these aluminum sources, amorphous aluminum hydroxide, aluminum hydroxide having a gibbsite structure, aluminum hydroxide having a Bayerite structure, aluminum sulfate, and aluminum-containing zeolite are preferably used in terms of cost advantage and ease of handling, and amorphous aluminum hydroxide, aluminum sulfate, and aluminum-containing zeolite are more preferably used in terms of reactivity. More preferably, the aluminum source is a compound that is both a silicon source and an aluminum source, and the compound accounts for 90 mass% or more of the aluminum source. More preferably, the compound used as the aluminum source is a compound that is also a silicon source, excluding inevitable impurities. More preferably, the aluminum source is entirely composed of zeolite (A), zeolite (B), and seed crystals, excluding inevitable impurities, and most preferably, the aluminum source is composed of zeolite (A) and zeolite (B), excluding inevitable impurities.

[0027] (c) a source of alkali metal elements and / or an alkaline earth metal element The alkali metal element and alkaline earth metal element contained in the raw material subjected to the hydrothermal synthesis of this embodiment are not particularly limited, and examples thereof include lithium, sodium, potassium, rubidium, cesium, beryllium, magnesium, calcium, strontium, barium, etc. Although one kind of these may be contained alone or two or more kinds may be contained, it is preferable to contain an alkali metal element in terms of the tendency of zeolite crystallization to occur when a highly alkaline and particularly soluble raw material is used.

[0028] Examples of the alkali metal element source and the alkaline earth metal element source include hydroxides, chlorides, bromides, iodides, hydrogen carbonates, carbonates, etc. Among these compounds, hydroxides, hydrogen carbonates, and carbonates are basic in an aqueous solution state. Specific examples include hydroxides such as lithium hydroxide, sodium hydroxide, potassium hydroxide, cesium hydroxide, calcium hydroxide, strontium hydroxide, and barium hydroxide; hydrogen carbonates such as lithium hydrogen carbonate, sodium hydrogen carbonate, potassium hydrogen carbonate, cesium hydrogen carbonate, calcium hydrogen carbonate, strontium hydrogen carbonate, and barium hydrogen carbonate; and carbonates such as lithium carbonate, sodium carbonate, potassium carbonate, cesium carbonate, calcium carbonate, strontium carbonate, and barium carbonate. Among these, hydroxides of alkali metal elements such as lithium hydroxide, sodium hydroxide, potassium hydroxide, and cesium hydroxide are preferred, because they are highly alkaline and have the effect of promoting dissolution of the raw materials and the subsequent crystallization of the zeolite, more preferably sodium hydroxide, potassium hydroxide, and cesium hydroxide, and even more preferably sodium hydroxide and potassium hydroxide. These alkali metal sources and alkaline earth metal sources may be used alone or in combination of two or more.

[0029] (d) Organic structure directing agent As the organic structure directing agent (also called "template." Hereinafter, the organic structure directing agent may be referred to as "OSDA" (Organic Structure Directing Agent), etc.), various known substances such as tetraethylammonium cation (TEA) and tetrapropylammonium cation (TPA) can be used. In addition, as a nitrogen-containing organic structure directing agent described in, for example, U.S. Patent No. 5,512,267, the N,N,N-trimethyl-(-)-cis-myrtanylammonium cation can be used. In addition, the N,N,N-trimethyl-(+)-cis-myrtanylammonium cation, N,N,N-trimethyl-8-ammonium tricyclo[5.2.1.0 2,6 ]-decane-ammonium cation, N,N,N-trimethyl-8-ammonium tricyclo[5.2.1.02,6 ]-decene-ammonium cation, hexamethonium cation, pentaethonium cation, trimethylbenzylammonium cation, and the like.

[0030] As the phosphorus-containing organic structure-directing agent, various known substances such as tetraethylphosphonium, tetrapropylphosphonium, tetrabutylphosphonium, and diphenyldimethylphosphonium can be used. However, since phosphorus compounds may generate the harmful substance diphosphorus pentoxide when the synthesized zeolite is calcined to remove the OSDA, nitrogen-containing organic structure-directing agents are more preferred. The above ammonium cation and phosphonium cation are accompanied by an anion that does not inhibit the formation of the preferred CON zeolite of this embodiment. The anion is not particularly limited, but specifically, Cl - , Br - , I - Examples of the ions that can be used include halogen ions, hydroxide ions, acetates, sulfates, carboxylates, etc. Among these, hydroxide ions are particularly preferably used. These organic structure-directing agents may be used alone or in combination of two or more.

[0031] (e) water As the water used as a raw material, ion-exchanged water is usually used.

[0032] (f) Seed crystal In this embodiment, seed crystals may be added to the raw material to be subjected to hydrothermal synthesis. In the present invention, the zeolite mixture containing zeolite (A) and zeolite (B) used as the silicon source (a) also plays the role of seed crystals. The seed crystals need only have the zeolite (A) and zeolite (B), and no further seed crystals are required, but other seed crystals may be present. As the other seed crystals, only one type may be used, or a combination of zeolites with different structures and compositions may be used. The composition of the zeolite used as the other seed crystals is not particularly limited as long as it does not significantly affect the composition of the mixture. For example, as a seed crystal in the production of a CON type zeolite, which is a preferred embodiment, a CON type zeolite may be used. The particle size of the zeolite used as the seed crystals is not particularly limited, but the average primary particle size is usually 0.02 μm or more, preferably 0.04 μm or more, more preferably 0.06 μm or more, and usually 5 μm or less, preferably 2 μm or less, more preferably 1 μm or less, and even more preferably 0.60 μm or less. By setting the average primary particle size of the seed crystals within the above range, the solubility of the seed crystals in the mixture is increased, the production of by-products is suppressed, and the crystallization of the CON type phase can be efficiently promoted.

[0033] The seed crystals may be either a zeolite containing a structure-directing agent that has not been calcined after hydrothermal synthesis, or a zeolite containing no structure-directing agent that has been calcined. The seed crystals may be added to the raw material either after being dispersed in a suitable solvent, such as water, or directly without being dispersed.

[0034] (g) Other sources of element M The zeolite (X) synthesized in this embodiment, for example, a CON-type zeolite, may contain, as constituent elements, silicon, oxygen, aluminum, an alkali metal element, an alkaline earth metal element, and at least one element M selected from boron, gallium, and iron (hereinafter simply referred to as "element M").

[0035] That is, the raw materials used in the hydrothermal synthesis may contain a source of element M. The source of element M is not particularly limited and is selected from, for example, sulfates, nitrates, hydroxides, oxides, alkoxides, and zeolites containing element M of these elements. Among these sources of element M, sulfates, nitrates, hydroxides and alkoxides are preferred in terms of reactivity, and sulfates, nitrates and hydroxides are more preferred in terms of cost and workability.

[0036] As the boron source, boric acid, sodium borate, boron oxide, boron-containing zeolite, etc. are usually used, with boric acid and sodium borate being preferred, and boric acid being more preferred. As the gallium source, typically, gallium sulfate, gallium nitrate, gallium oxide, gallium chloride, gallium phosphate, gallium hydroxide, gallium-containing zeolite, etc. are used, with gallium sulfate and gallium nitrate being preferred, and gallium sulfate being more preferred. As the iron source, typically, iron nitrate, iron sulfate, iron oxide, iron chloride, iron hydroxide, iron-containing zeolite, etc. are used, with iron sulfate and iron nitrate being preferred, and iron sulfate being more preferred.

[0037] These sources of element M may be used singly or in combination of two or more of the same element, or in combination of one or more of different elements. The raw materials may also contain sources of other metals (such as lead, germanium, titanium, zirconium, tin, chromium, and cobalt). These may be contained in the mixture alone or in combination of two or more kinds.

[0038] (Raw material composition) In this embodiment, the preferred composition of the raw material (slurry or gel) to be subjected to hydrothermal synthesis is as follows. In addition, when seed crystals are added, the following compositions are values ​​calculated including silicon and aluminum contained in the seed crystals.

[0039] The molar ratio of silicon atoms to aluminum atoms in the raw material (Si / Al) is not particularly limited, but is usually greater than 1, preferably 3 or more, more preferably 5 or more, even more preferably 8 or more, and particularly preferably 10 or more, and is usually 1000 or less, preferably 500 or less, more preferably 100 or less, even more preferably 50 or less, and particularly preferably 25 or less. By setting the molar ratio of silicon atoms to aluminum atoms in the above range, it becomes easier to aim for the CON type, and the synthesis yield is improved. In addition, when used as a catalyst, it is preferable because the organic compound raw material can be efficiently converted by the acid site derived from Al.

[0040] The molar ratio of the total of alkali metal atoms and alkaline earth metal atoms to silicon atoms in the raw material [(alkali metal atoms + alkaline earth metal atoms) / Si] is not particularly limited, but is usually 0 or more, preferably 0.05 or more, more preferably 0.075 or more, and even more preferably 0.10 or more, and is usually 0.60 or less, preferably 0.40 or less, more preferably 0.30 or less, even more preferably 0.20 or less, and especially preferably 0.15 or less. By setting the above ratio within the above range, the incorporation of aluminum into the CON-type zeolite framework is sufficient, and the synthesis yield is improved. In addition, it is preferable in that the generation of by-products can be suppressed and the crystallization rate into the CON phase can be increased.

[0041] The molar ratio of the sum of the alkali metal atoms and the alkaline earth metal atoms to the aluminum atoms in the raw material [(alkali metal atoms+alkaline earth metal atoms) / Al] is not particularly limited, but is usually at least 0.1, preferably at least 0.5, more preferably at least 1, and even more preferably at least 2, and is usually at most 20, preferably at most 15, more preferably at most 10, and even more preferably at most 5. By setting the above ratio within the above range, the interaction between the alkali metal and the alkaline earth metal and the aluminum during crystallization becomes effective, which is preferable in that a CON-type zeolite is easily obtained.

[0042] The ratio of the organic structure-directing agent in the raw material is not particularly limited, but the molar ratio of the organic structure-directing agent to silicon atoms (organic structure-directing agent / Si) is usually 0.01 or more, preferably 0.02 or more, more preferably 0.05 or more, even more preferably 0.10 or more, particularly preferably 0.15 or more, and usually 0.60 or less, preferably 0.50 or less, more preferably 0.40 or less, even more preferably 0.30 or less, particularly preferably 0.25 or less. By setting the organic structure-directing agent in the raw material within the above range, nucleation in the mixture is promoted, crystallization of CON type zeolite is promoted, and it is preferable in that it can be synthesized with a high yield. In addition, it is preferable in that the amount of expensive organic structure-directing agent used can be reduced, and the production cost of zeolite can be reduced.

[0043] The molar ratio of the total of the organic structure-directing agent, the alkali metal atom, and the alkaline earth metal atom to the aluminum atom in the raw material [(organic structure-directing agent+alkali metal+alkaline earth metal) / Al] is not particularly limited, but is usually 0.1 or more, preferably 1 or more, more preferably 2 or more, and even more preferably 4 or more, and usually 50 or less, preferably 30 or less, more preferably 20 or less, and even more preferably 10 or less. By setting the above ratio within the above range, the interaction between aluminum and the organic structure-directing agent, alkali metal, and alkaline earth metal during crystallization becomes effective, which is preferable in that a CON-type zeolite is easily obtained.

[0044] The organic structure directing agent in the raw material preferably contains N,N,N-trimethyl-(-)-cis-myrtanyl ammonium cation. The molar ratio of N,N,N-trimethyl-(-)-cis-myrtanyl ammonium cation (hereinafter referred to as "TMMA") in the total organic structure directing agent [TMMA / total organic structure directing agent (TMMA+others)] is not particularly limited, but is usually 0 or more, preferably 0.20 or more, more preferably 0.40 or more, even more preferably 0.60 or more, particularly preferably 0.80 or more, with the upper limit being 1.0. A higher ratio of TMMA is preferable in that the crystallization of the CON type structure is more likely to proceed.

[0045] The proportion of water in the raw material is not particularly limited, but the molar ratio of H2O to silicon (H2O / Si) is usually 6 or more, preferably 8 or more, more preferably 10 or more, and even more preferably 12 or more, and usually 50 or less, preferably 40 or less, more preferably 30 or less, and even more preferably 25 or less. By setting the proportion of water in the mixture within the above range, crystallization can be promoted. In addition, the productivity per reactor can be increased. It is preferable in that the deterioration of stirring and mixing due to the increase in viscosity during the reaction and the waste liquid treatment cost can be suppressed.

[0046] The amount of seed crystals added to the raw material is not particularly limited, but is usually 0.1% by mass or more, preferably 1% by mass or more, more preferably 2% by mass or more, and even more preferably 4% by mass or more, based on SiO2 when all silicon (Si) contained in the mixture other than the seed crystals added in this embodiment is SiO2. The upper limit is not particularly limited, but is usually 20% by mass or less, preferably 15% by mass or less, more preferably 10% by mass or less, and even more preferably 8% by mass or less. By setting the amount of seed crystals in the above range, the amount of precursors directing the CON type structure becomes sufficient, and crystallization can be promoted. In addition, the amount of components derived from the seed crystals contained in the product is suppressed, and productivity can be increased, so that production costs can be reduced.

[0047] (Preparation of raw materials before reaction) In the manufacturing method of this embodiment, the silicon source, aluminum source, alkali metal element source and / or alkaline earth metal element source, organic structure directing agent, and water are mixed together to obtain a raw material, which is then hydrothermally synthesized. The order of mixing the components in these raw materials is not particularly limited, but it is preferable to prepare an alkaline solution by mixing water, an alkali metal element source and / or an alkaline earth metal element source, and an organic structure directing agent, and then add the aluminum source, silicon source, and seed crystals, if necessary, in this order, and mix them, since the raw materials are more uniformly dissolved when the silicon source and aluminum source are added after the alkaline solution is prepared.

[0048] (Aging) The raw materials before reaction prepared as described above may be hydrothermally synthesized immediately after preparation, but may be aged for a certain period of time under a specified temperature condition in order to obtain a zeolite with high crystallinity. In particular, when scaling up, the stirring property is deteriorated and the raw materials are likely to be insufficiently mixed. Therefore, it is preferable to improve the reaction mixture to a more homogeneous state by aging the raw materials while stirring them for a certain period of time. The aging temperature is usually 100° C. or lower, preferably 95° C. or lower, more preferably 90° C. or lower, and although there is no particular lower limit, it is usually 0° C. or higher, preferably 10° C. or higher. The aging temperature may be constant during aging, or may be changed stepwise or continuously. The maturation time is not particularly limited, but is usually 2 hours or more, preferably 3 hours or more, more preferably 5 hours or more, and usually 14 days or less, preferably 7 days or less, and more preferably 3 days or less.

[0049] (Hydrothermal synthesis process) Zeolite (X), such as CON-type zeolite, can be produced by heating the above-mentioned raw materials in a reaction vessel (hydrothermal synthesis). The heating temperature (reaction temperature) is not particularly limited, and is usually 100°C or higher, preferably 125°C or higher, more preferably 150°C or higher, and even more preferably 170°C or higher, and is usually 220°C or lower, preferably 210°C or lower, more preferably 205°C or lower, and even more preferably 200°C or lower. By setting the reaction temperature within the above range, the crystallization time of the CON type zeolite can be shortened, and the yield of the zeolite can be improved. In addition, it is preferable in that the by-production of zeolite with a different structure can be suppressed. The reaction temperature may be constant during the reaction, or may be changed stepwise or continuously.

[0050] The time required to raise the temperature to the heating temperature (reaction temperature) is not particularly limited, but is usually 0.1 hours or more, preferably 0.5 hours or more, and more preferably 1 hour or more, and there is no particular upper limit to the time required for raising the temperature.

[0051] The heating time (reaction time) is usually 1 hour or more, preferably 5 hours or more, more preferably 10 hours or more, and the upper limit is usually 30 days or less, preferably 15 days or less, more preferably 10 days or less, and further preferably 7 days or less. By setting the reaction time within the above range, the yield of CON-type zeolite can be improved, and it is also preferable in that the by-production of zeolite with a different structure can be suppressed.

[0052] The pressure during the reaction is not particularly limited, and the autogenous pressure that arises when the mixture placed in a sealed container is heated to the above-mentioned temperature range is sufficient, but an inert gas such as nitrogen may be added as necessary.

[0053] [Use as zeolite seed crystals] As described above, the production method of the present invention can efficiently produce zeolites that have been difficult to produce in the past. Furthermore, the zeolite (X) produced by the production method of the present invention is useful as seed crystals for further producing zeolite (X). For example, in the case of CON-type zeolite, which is one embodiment of zeolite (X), the CON-type high aluminum zeolite can be easily produced by the production method of the present invention. The CON-type high aluminum zeolite produced in this manner is useful as seed crystals for the subsequent production of CON-type zeolite. In this manner, by using the zeolite produced by the production method of the present invention as seed crystals, a catalyst that maintains a high conversion rate for a longer period of time can be produced. More specifically, the CON-type high aluminum zeolite produced by the production method of the present invention has, for example, a Si / Al (molar ratio, hereinafter meaning a molar ratio unless otherwise specified) of 50 or less, and by adding this as seed crystals in an amount of 1 mass% or more to the silicon source, a CON-type zeolite can be obtained. The Si / Al of the CON-type high aluminum zeolite used as the seed crystals is more preferably 40 or less, and even more preferably 30 or less. The content of the CON-type high aluminum zeolite used as seed crystals is more preferably 2% by mass or more, and further preferably 5% by mass or more, based on the silicon source.

[0054] Hereinafter, a CON type zeolite that is suitable as an example to which the production method of the present invention can be applied will be described. [CON type zeolite] One embodiment of the present invention is a CON type zeolite. A CON type zeolite is a zeolite having a three-dimensional pore structure in which two 12-membered ring structures and one 10-membered ring structure intersect as its constituent units. The CON type zeolite having this 12-membered ring structure is advantageous in the diffusion of reaction products in the pores compared to CHA type zeolite consisting of only 8-membered ring structures and MFI type zeolite consisting of only 10-membered ring structures. In addition, the CON type zeolite has a structure in which the 12-membered ring structure and the 10-membered ring structure intersect in a zigzag manner, and the pores in three directions do not intersect at one point, so the intersection space is small, coke due to the reaction is unlikely to be generated, and it is thought that the reaction activity is unlikely to be significantly reduced, and the catalyst life is long.

[0055] In this embodiment, the CON-type zeolite is preferably, but not limited to, a crystalline metallosilicate. The elements constituting the metallosilicate are, but not limited to, one or more selected from aluminum (Al), boron (B), titanium (Ti), vanadium (V), iron (Fe), zinc (Zn), gallium (Ga), germanium (Ge), zirconium (Zr), and tin (Sn).

[0056] Specifically, crystalline aluminosilicates containing Al as a constituent element and crystalline gallosilicates containing Ga are preferred. These zeolites have excellent catalytic activity because Al and Ga in the zeolite framework become acid sites and act as active sites for catalytic reactions. In particular, aluminosilicates containing Al are more desirable from the viewpoint of catalytic activity.

[0057] In addition, since the CON-type zeolite can be easily obtained by adding a boron compound to the raw material gel described later, it may contain B (boron) as a constituent element. Examples of such zeolite include crystalline boroaluminosilicate containing Si, Al and B as constituent elements, and crystalline galloboroaluminosilicate further containing Ga.

[0058] In the case of the crystalline aluminosilicate and crystalline gallosilicate, the ratio of the constituent elements is not particularly limited, but the Si / Al molar ratio or the Si / Ga molar ratio is usually 1 or more, preferably 3 or more, more preferably 5 or more, even more preferably 8 or more, particularly preferably 10 or more, and especially preferably 15 or more, and is usually 1000 or less, preferably 500 or less, more preferably 200 or less, even more preferably 100 or less, particularly preferably 50 or less, and especially preferably 25 or less. By setting the Si / Al molar ratio or the Si / Ga molar ratio in such a range, a zeolite catalyst having sufficient catalytic activity and further improved catalyst life can be obtained.

[0059] Furthermore, when the CON type zeolite of this embodiment contains B (boron), the Si / B molar ratio is not particularly limited, but is usually 3 or more, preferably 5 or more, more preferably 8 or more, and even more preferably 10 or more, and the upper limit may be, for example, 100,000 or less, 50,000 or less, or 10,000 or less.

[0060] The contents of Si, Al, Ga, B, etc. in the CON type zeolite of this embodiment are usually values ​​measured for the produced CON type zeolite by inductively coupled plasma atomic emission spectrometry (ICP-AES) or the like, and are not the ratios of the raw material charges.

[0061] The ion exchange sites of the CON type zeolite of this embodiment are not particularly limited, and may be H type or may be exchanged with metal ions, specifically, alkali metal ions, alkaline earth metal ions, cerium, tungsten, manganese, iron, etc.

[0062] The BET specific surface area of ​​the CON type zeolite of this embodiment is not particularly limited and is usually 400 m 2 / g or more, preferably 450m 2 / g or more, more preferably 500m 2 / g or more, more preferably 550m 2 / g or more, usually 1000m 2 / g or less, preferably 800m 2 / g or less, more preferably 700m 2 / g or less.

[0063] The outer surface area of ​​the CON type zeolite of this embodiment is not particularly limited and is usually 10 m 2 / g or more, preferably 30m 2 / g or more, more preferably 50m 2 / g or more, more preferably 60m 2 / g or more, particularly preferably 70m 2 / g or more, particularly preferably 80m 2 / g or more, usually 400m 2 / g or less, preferably 300m 2 / g or less, more preferably 250m 2 / g or less.

[0064] The micropore volume of the CON type zeolite of this embodiment is not particularly limited, and is usually 0.10 ml / g or more, preferably 0.12 ml / g or more, more preferably 0.15 ml / g or more, further preferably 0.17 ml / g or more, particularly preferably 0.19 ml / g or more, and is usually 3 ml / g or less, preferably 2 ml / g or less. The BET specific surface area, external surface area, and micropore volume can be calculated from nitrogen adsorption / desorption measurements.

[0065] The average primary particle size of the CON type zeolite of the present embodiment is not particularly limited, and is usually 3 μm or less, preferably 2 μm or less, more preferably 1 μm or less, further preferably 700 nm or less, particularly preferably 500 nm or less, and is usually 20 nm or more, preferably 40 nm or more. Here, the average primary particle size of the CON type zeolite can be determined by a scanning electron microscope (SEM).

[0066] [Application] The zeolite (X) produced by the production method of the present invention is used for various applications. Hereinafter, a detailed description will be given of an example in which the CON-type zeolite produced by the production method of the present invention is used as a catalyst. However, the zeolite (X) produced by the production method of the present invention is not limited to catalytic applications.

[0067] <Catalyst> The CON type zeolite of the present embodiment can be used as a catalyst. In particular, the CON type zeolite of the present embodiment is useful as a catalyst used in a reaction for producing lower olefins, but the applications of the zeolite catalyst of the present embodiment are not limited to catalysts for producing lower olefins, and are also suitably used for the production of p-xylene, the production of ethylbenzene and cumene, the aromatization of light hydrocarbons, hydrocracking, hydrodewaxing, the isomerization of alkanes, and the purification of automobile exhaust gases.

[0068] The CON type zeolite of this embodiment may be used as it is in the reaction as a catalyst in the present invention, or may be used as a mixture with other substances inactive in the reaction, such as compounds containing alkaline earth metals or silicon, or may be granulated or molded using a binder and used in the reaction. Examples of the substances and binders inactive in the reaction include alumina or alumina sol, silica, silica gel, silicate, quartz, and mixtures thereof. Among these, silica is preferred because it is expected to have excellent strength and catalytic performance as an industrial catalyst. Mixing with these substances is also effective in reducing the cost of the entire catalyst, increasing the density of the catalyst, and increasing the catalyst strength.

[0069] In the method for producing lower olefins using a catalyst containing the CON-type zeolite of this embodiment, examples of raw materials include methanol and dimethyl ether, but are not limited to these, and can be appropriately selected depending on the type of target olefin.

[0070] The process for producing lower olefins using the above catalyst will be described below by taking as an example the case where the raw material is methanol and / or dimethyl ether.

[0071] <Production method of lower olefins> The method for producing lower olefins includes a step of contacting a raw material containing methanol and / or dimethyl ether with a catalyst containing the above-mentioned CON-type zeolite.

[0072] The origin of methanol and dimethyl ether used as raw materials is not particularly limited. For example, they can be obtained by hydrogenation reaction of hydrogen / CO mixed gas derived from coal and natural gas, and by-products in the steel industry, by reforming reaction of alcohols derived from plants, by fermentation, from organic substances such as recycled plastics and urban waste, and by methanol synthesis reaction using carbon dioxide as raw material. In this case, the mixture of compounds other than methanol and dimethyl ether resulting from each production method may be used as it is, or may be purified. As the reaction raw material, only methanol or only dimethyl ether may be used, or a mixture of these may be used. When a mixture of methanol and dimethyl ether is used, there is no limitation on the mixing ratio.

[0073] The reaction mode in this embodiment is not particularly limited as long as the methanol and / or dimethyl ether feedstock is in the gas phase in the reaction zone, and a known gas phase reaction process using a fluidized bed reactor, a moving bed reactor, or a fixed bed reactor can be applied. A fixed bed reactor is advantageous in terms of facility costs including auxiliary facilities, catalyst costs, and operation management. The process may be carried out in any of a batch, semi-continuous or continuous manner, but is preferably carried out in a continuous manner, and may be a process using a single reactor or a process using multiple reactors arranged in series or parallel.

[0074] When the fixed bed reactor is filled with the above-mentioned catalyst, in order to minimize the temperature distribution in the catalyst layer, granular materials inactive to the reaction, such as quartz sand, alumina, silica, and silica-alumina, may be mixed with the catalyst and filled. In this case, there is no particular restriction on the amount of granular materials inactive to the reaction, such as quartz sand, used. In addition, it is preferable that the granular materials have a particle size similar to that of the catalyst, from the viewpoint of uniform mixing with the catalyst. Furthermore, the reaction substrates (reaction raw materials) may be divided and fed to the reactor for the purpose of dispersing heat generated by the reaction.

[0075] Although there is no particular limitation on the total concentration (substrate concentration) of methanol and dimethyl ether in all the components fed to the reactor, the sum of methanol and dimethyl ether is preferably 90 mol % or less, more preferably 10 mol % or more and 70 mol % or less, in all the components fed.

[0076] In addition to methanol and / or dimethyl ether, the reactor may contain gases inert to the reaction (also referred to as diluents), such as helium, argon, nitrogen, carbon monoxide, carbon dioxide, hydrogen, water, paraffins, hydrocarbons such as methane, aromatic compounds, and mixtures thereof. Among these, the coexistence of water (water vapor) is preferred because it is easily separated. As such a diluent, impurities contained in the reaction raw materials may be used as they are, or a separately prepared diluent may be mixed with the reaction raw materials. The diluent may also be mixed with the reaction raw materials before being placed in the reactor, or may be supplied to the reactor separately from the reaction raw materials.

[0077] The lower limit of the reaction temperature is usually about 200°C or higher, preferably 250°C or higher, more preferably 300°C or higher, and particularly preferably 400°C or higher, and the upper limit of the reaction temperature is usually 750°C or lower, preferably 700°C or lower, and more preferably 600°C or lower. If the reaction temperature is too low, the reaction rate is low, and a large amount of unreacted raw materials tends to remain, and the yield of low olefins also decreases. On the other hand, if the reaction temperature is too high, it is difficult to obtain stable catalyst activity, and the yield of low olefins decreases significantly. Here, the reaction temperature refers to the temperature at the outlet of the catalyst layer.

[0078] The upper limit of the reaction pressure is usually 5 MPa (absolute pressure, the same below), preferably 2 MPa, more preferably 1 MPa, more preferably 0.7 MPa, and particularly preferably 0.4 MPa. The lower limit of the reaction pressure is not particularly limited, but is usually 0.1 kPa or more, preferably 7 kPa or more, and more preferably 50 kPa or more. If the reaction pressure is too high, the amount of undesirable by-products such as paraffins and aromatic compounds produced increases, and the yield of lower olefins tends to decrease. If the reaction pressure is too low, the reaction rate tends to be slow.

[0079] The reactor outlet gas (reactor effluent) is a mixed gas containing lower olefins as the reaction product, by-products and a diluent. The lower olefin concentration in the mixed gas is usually 5 to 95 mass %. Although the reaction product contains methanol and / or dimethyl ether as unreacted raw materials depending on the reaction conditions, it is preferable to carry out the reaction under reaction conditions that result in a 100% conversion of methanol and / or dimethyl ether, which makes it easy, and preferably unnecessary, to separate the reaction product from the unreacted raw materials. By-products include olefins having 5 or more carbon atoms, paraffins, aromatic compounds and water.

[0080] As a reactor outlet gas, a mixed gas containing a lower olefin as a reaction product, unreacted raw materials, by-products, and a diluent may be introduced into known separation and purification equipment, and recovery, purification, recycling, and discharge treatments may be performed according to each component.

[0081] [Method for Producing CON-Type Zeolite] In the present invention, as described above, it facilitates the production of zeolite, which was difficult to produce conventionally. In particular, in the method for producing a CON-type zeolite that has a long life when used as a catalyst, as shown in another aspect of the present invention, it is a useful invention. More specifically, it is a method for producing a CON-type zeolite, characterized in that a CON-type zeolite with Si / Al of 50 or less is added as a seed crystal in an amount of 1% by mass or more based on the silicon source. Here, Si / Al is 50 or less, more preferably 40 or less, still more preferably 30 or less, and particularly preferably 25 or less. By setting the molar ratio of silicon atoms to aluminum atoms within this range, a catalyst that can maintain a high conversion rate for a longer period can be produced. In addition, the content of the CON-type high-aluminum zeolite used as the seed crystal is 1% by mass or more, more preferably 2% by mass or more, still more preferably 4% by mass or more, and particularly preferably 5% by mass or more based on the silicon source. By setting the content of the seed crystal within this range, it becomes easier to direct to the CON type, the synthesis yield is improved, and a catalyst that can maintain a high conversion rate for a longer period can be produced.

Examples

[0082] Hereinafter, the present invention will be described in more detail by way of examples, but the scope of the present invention is not limited by the following examples. (Evaluation Method) (1) Physical Properties of Zeolite <Elemental Analysis> Elemental analysis was performed by inductively coupled plasma atomic emission spectrometry (ICP-AES). For the measurement of the zeolites in Examples 1 and 2 and Comparative Example 4, "ICPE-9000" manufactured by Shimadzu Corporation was used. <X-ray Diffraction Measurement> X-ray diffraction (XRD) measurements of the synthesized zeolites were carried out using Rigaku's "Ultima III." <Nitrogen adsorption / desorption measurement> Nitrogen adsorption and desorption measurements of the synthesized proton-type zeolite powder were performed using a Microtrack-Bell Belsorp-MAX. For the measurements, the zeolite was heated and dried at 350°C for 3 hours under vacuum, and then nitrogen adsorption and desorption measurements were performed at liquid nitrogen temperature. Data analysis was performed using Microtrack-Bell's analysis software BELMaster. The BET specific surface area was calculated by BET plotting the measurement data at relative pressures (P / P0) of 0.000002 to 0.12. The external surface area and micropore volume were calculated by t-plotting the data at relative pressures (P / P0) of 0.85 to 0.92.

[0083] (2) Response evaluation <Production of lower olefins> Using the zeolites obtained in Example 2 and Comparative Example 4, lower olefins were produced. A fixed-bed flow reactor was used for the reaction, and 50 mg of pre-sized proton-type zeolite powder (particle size: 1 to 0.6 mm) was packed into a quartz reaction tube with an inner diameter of 6 mm. A mixed gas of 50 mol % methanol and 50 mol % nitrogen was introduced at a weight hourly space velocity of methanol of 15 hr -1 The mixture was fed to the reactor so that the reaction was carried out at 500°C and 0.1 MPa (absolute pressure). The products were analyzed by gas chromatography every hour from the start of the reaction. Figure 2 shows a graph showing the changes in methanol conversion and the selectivity of each component. Table 2 shows the methanol conversion (%), ethylene selectivity (C-mol%), propylene selectivity (C-mol%), butene selectivity (C-mol%) and catalyst life (hr) two hours after the reaction. The catalyst life was defined as the time during which the methanol conversion was maintained at 90% or more.

[0084] [Example 1] 5.5337g of 30.9 mass% N,N,N-trimethyl-(-)-cis-myrtanylammonium hydroxide (referred to as "TMMAOH" in Table 1) aqueous solution, 0.6584g of 8M sodium hydroxide aqueous solution, and 17.3217g of demineralized water were mixed, to which 0.2509g of boric acid (H3BO3) was added and stirred, and then 0.8047g of Beta zeolite (CP814E, Si / Al=12.5, Zeolyst) as a silicon source, 0.8117g of MFI type zeolite (HSZ-820-NHA, Si / Al=11.5, Tosoh) and 0.9076g of fumed silica (Cab-O-sil M7D, CABOT) were added and stirred sufficiently to prepare a raw material gel.

[0085] The obtained raw material gel was placed in an autoclave and heated at 200°C for 7 days at 40 rpm to carry out hydrothermal synthesis. The product was filtered, washed with water, and then dried at 100°C to obtain a white powder. The X-ray diffraction (XRD) pattern of the product confirmed that the product was CON-type zeolite. In Table 1, there is no description of the aluminum source, but this is because the zeolite described as the silicon source is also the aluminum source.

[0086] [Comparative Example 1] 5.5154 g of a 30.9 mass% TMMAOH aqueous solution, 0.6282 g of an 8 M sodium hydroxide aqueous solution, and 17.3660 g of demineralized water were mixed, to which 0.2458 g of boric acid (H3BO3) was added and stirred, and then 1.6020 g of beta zeolite (CP814E, Si / Al=12.5, Zeolyst) and 0.9053 g of fumed silica (Cab-O-sil M7D, CABOT) were added as silicon sources and stirred thoroughly to prepare a raw gel.

[0087] The obtained raw gel was placed in an autoclave and heated at 200°C for 7 days at 40 rpm to carry out hydrothermal synthesis. The product was filtered, washed with water, and then dried at 100°C to obtain a white powder. From the X-ray diffraction (XRD) pattern of the product, it was confirmed that the obtained product was a mixture of CON-type zeolite and Beta zeolite.

[0088] [Comparative Example 2] 5.5254 g of a 30.9 mass% TMMAOH aqueous solution, 0.8270 g of an 8 M sodium hydroxide aqueous solution, and 17.3291 g of demineralized water were mixed, to which 0.2475 g of boric acid (H3BO3) was added and stirred, and then 1.6009 g of MFI type zeolite (HSZ-820-NHA, Si / Al=11.5, manufactured by Tosoh Corporation) and 0.9032 g of fumed silica (Cab-O-sil M7D, manufactured by CABOT Corporation) were added as silicon sources and stirred thoroughly to prepare a raw gel.

[0089] The obtained raw material gel was placed in an autoclave and heated at 170°C for 7 days at 40 rpm to carry out hydrothermal synthesis. The product was filtered, washed with water, and then dried at 100°C to obtain a white powder. From the X-ray diffraction (XRD) pattern of the product, it was confirmed that the obtained product was a mixture of CON-type zeolite and MFI-type zeolite.

[0090] [Comparative Example 3] 5.5227g of 30.9% by mass TMMAOH aqueous solution, 0.6198g of 8M sodium hydroxide aqueous solution, and 17.3179g of demineralized water were mixed, to which 0.2476g of boric acid (H3BO3) and 0.4018g of aluminum sulfate were added and stirred, after which 2.4008g of fumed silica (Cab-O-sil M7D, manufactured by CABOT) was added as a silicon source and thoroughly stirred. Furthermore, 0.0490g of CON-type zeolite (Si / Al=270) was added as seed crystals and stirred to prepare a raw gel.

[0091] The obtained raw gel was placed in an autoclave and heated at 170°C for 7 days at 40 rpm to carry out hydrothermal synthesis. The product was filtered, washed with water, and then dried at 100°C to obtain a white powder. The X-ray diffraction (XRD) pattern of the product confirmed that the product was amorphous.

[0092] [Table 1]

[0093] The synthesis conditions and synthesis results of Example 1 and Comparative Examples 1 to 3 are shown in Table 1. In the table, the column for silicon source indicates the mass ratio when the sum of the masses of the silicon sources is 1, and the column for Si / Al in the table indicates the molar ratio. In Example 1, in which Beta zeolite and MFI zeolite were used as silicon sources, CON zeolite with low Si / Al (high Al content) was obtained. On the other hand, in Comparative Examples 1 and 2, although CON zeolite was obtained, it was a mixture with Beta zeolite (Comparative Example 1) and a mixture with MFI zeolite (Comparative Example 2), respectively. In Comparative Example 3, an amorphous substance with no crystallinity was synthesized.

[0094] [Example 2] 5.5499 g of 30.9 mass% TMMAOH aqueous solution, 0.6569 g of 8 M sodium hydroxide aqueous solution, and 17.3027 g of demineralized water were mixed, to which 0.2470 g of boric acid (H3BO3) and 0.0256 g of aluminum sulfate were added and stirred, and then 2.4058 g of fumed silica (Cab-O-sil M7D, manufactured by CABOT) was added as a silicon source and stirred thoroughly, and then 0.0481 g of proton-type CON-type zeolite (Si / Al=20) was added as seed crystals and stirred to prepare a raw gel.

[0095] The obtained raw material gel was placed in an autoclave and heated at 170°C for 4 days at 40 rpm to carry out hydrothermal synthesis. The product was filtered, washed with water, and then dried at 100°C to obtain a white powder. From the X-ray diffraction (XRD) pattern of the product, it was confirmed that the obtained product was CON-type zeolite. After drying, it was calcined in an air atmosphere at 600°C for 6 hours to obtain a sodium-type zeolite powder.

[0096] The obtained powder was subjected to ion exchange in a 2.5N ammonium nitrate aqueous solution at 80°C for 2 hours, then filtered and dried. The dried powder was again subjected to ion exchange in a 2.5N ammonium nitrate aqueous solution at 80°C for 3 hours, then filtered and dried to obtain an ammonium type zeolite powder. The powder was then calcined in an air atmosphere at 600°C for 3 hours to obtain the proton type zeolite powder of Example 2.

[0097] [Comparative Example 4] 5.5253 g of a 30.9 mass% TMMAOH aqueous solution, 0.6235 g of an 8 M sodium hydroxide aqueous solution, and 17.3117 g of demineralized water were mixed, to which 0.2471 g of boric acid (H3BO3) and 0.0256 g of aluminum sulfate were added and stirred, and then 2.4031 g of fumed silica (Cab-O-sil M7D, manufactured by CABOT) was added as a silicon source and stirred thoroughly, and then 0.0481 g of CON-type zeolite (Si / Al=270) was added as seed crystals and stirred to prepare a raw gel.

[0098] The obtained raw material gel was placed in an autoclave and heated at 170°C for 7 days at 40 rpm to carry out hydrothermal synthesis. The product was filtered, washed with water, and then dried at 100°C to obtain a white powder. From the X-ray diffraction (XRD) pattern of the product, it was confirmed that the obtained product was CON-type zeolite. After drying, it was calcined in an air atmosphere at 600°C for 6 hours to obtain a sodium-type zeolite powder.

[0099] The obtained powder was subjected to ion exchange in a 2.5N ammonium nitrate aqueous solution at 80°C for 2 hours, then filtered and dried. The dried powder was again subjected to ion exchange in a 2.5N ammonium nitrate aqueous solution at 80°C for 3 hours, then filtered and dried to obtain an ammonium type zeolite powder. Then, the powder was calcined in an air atmosphere at 600°C for 3 hours to obtain a proton type zeolite powder of Comparative Example 4.

[0100] The above-mentioned reaction evaluation (production of lower olefins) was carried out for Example 2 and Comparative Example 4. The results are shown in Table 2. In the table, those without a unit mean molar ratio.

[0101] [Table 2]

[0102] It is seen that the zeolite of Example 2 has a larger external surface area than that of Comparative Example 4, and maintains a high raw material conversion rate for a long period of time. [Industrial Applicability]

[0103] According to the production method of the present invention, zeolites that have been difficult to produce in the past can be easily obtained. Zeolites have many industrial applications, such as catalysts, adsorbents, ion exchange materials, molecular sieves, and separation materials. Moreover, according to the present invention, zeolites that have been difficult to produce in the past can be easily produced, and various other applications using zeolites are expected. From the above points, the present invention is an industrially important technology and a technology that can contribute to industry.

Claims

1. A method for producing a zeolite using a plurality of zeolites different from a zeolite (X) to be synthesized as a silicon source, characterized in that zeolite (A), which is at least one of the plurality of zeolites, has one or more CBUs constituting the zeolite (X) to be synthesized, zeolite (B), which is at least one other of the plurality of zeolites, has one or more other CBUs constituting the zeolite (X) to be synthesized, and zeolite (A) and zeolite (B) are each contained in an amount of 5 mass% or more in the silicon source.

2. The method for producing a zeolite according to claim 1, wherein the zeolite (X) to be synthesized is a CON-type zeolite.

3. The method for producing a zeolite according to claim 2, wherein the zeolite (A) has at least bea as a CBU, and the zeolite (B) has at least mel as a CBU.

4. The method for producing a zeolite according to claim 3, wherein the zeolite (A) is a Beta zeolite having at least bea as a CBU, and the zeolite (B) is an MFI zeolite having mel as a CBU.

5. 2. The method for producing a zeolite according to claim 1, wherein the molar ratio (Si / Al) of silicon (Si) to aluminum (Al) in the zeolite (X) to be synthesized is 500 or less.

6. A method for producing CON-type zeolite, comprising adding, as seed crystals, CON-type zeolite having a Si / Al ratio of 50 or less in an amount of 1 mass% or more relative to a silicon source.

Citation Information

Patent Citations

  • Method for producing MTW-type zeolite

    JP2012153578A

  • Con zeolite catalyst, method for producing con zeolite catalyst, and catalyst and absorbent containing con zeolite catalyst

    JP2022003013A