Resin composition
A resin composition combining aluminum nitride and alumina fillers with specific properties addresses the challenges of thermal conductivity and fluidity in multilayer printed wiring boards, enhancing heat dissipation and reliability in high-density electronic devices.
Patent Information
- Application Number
- JP2023142107
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-12
- Filing Date
- 2023-09-01
- Publication Date
- 2024-11-22
AI Technical Summary
Existing resin compositions for multilayer printed wiring boards and component-embedded substrates face limitations in achieving high thermal conductivity, fluidity, and low linear expansion, making it difficult to meet the demands of high-density electronic devices that generate significant heat.
A resin composition combining aluminum nitride filler with a specific particle size distribution and alumina filler, along with a balanced ratio of epoxy resins, is used to enhance thermal conductivity and fluidity while reducing linear expansion.
The resin composition achieves high thermal conductivity, low linear expansion, and excellent fluidity, enabling efficient production of multilayer printed wiring boards and component-embedded boards with improved heat dissipation and reliability.
Smart Images

Figure 2024163831000001 
Figure 2024163831000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition. [Background technology]
[0002] As electronic devices become more powerful and smaller, the wiring in multilayer printed wiring boards is becoming finer and denser. As a manufacturing technique for multilayer printed wiring boards, a manufacturing method using a build-up method in which insulating layers and conductor layers are alternately stacked is known. The insulating layer can be efficiently formed by using a film-like resin composition (resin composition film). As the resin composition film, a resin composition containing a thermosetting epoxy resin and silica is generally used (Patent Document 1). The insulating layer of a multilayer printed wiring board is generally formed by stacking a resin composition film on a conductor layer, and then heat-curing the resin composition while adhering the conductor layer and the resin composition with a vacuum laminator or a heat press, thereby laminating and bonding the resin composition. Therefore, the resin composition film is required to have high fluidity under lamination conditions to follow the shape of the conductor layer, and for this reason, it is common to use a solid epoxy resin and a liquid epoxy resin in combination as the epoxy resin. In addition, since the linear expansion due to heat of the insulating layer and the conductor layer (copper wiring) is significantly different, there is also a reliability issue such as the occurrence of cracks in thermal cycles, etc., and the insulating layer is also required to have low linear expansion. For this reason, resin composition films are generally highly filled with silica in order to reduce the linear expansion coefficient.
[0003] Also, as a method of high-density mounting, electronic component embedded board technology, in which electronic components that have been mounted on the surface of a board are embedded inside the board with an encapsulating resin, is attracting attention. A cavity is formed in the core of a resin board or a copper board, electronic components such as ICs and capacitors are placed in the cavity, and then a thermosetting resin is embedded in the cavity to encapsulate and embed the electronic components. The resin composition film used in the above-mentioned multilayer printed wiring board can also be used for this encapsulating resin. The resin composition film is superimposed on the core on which the electronic components are placed, the resin composition is embedded in the cavity by a heat press, and the resin composition is thermally cured to encapsulate. Even when used in a component embedded board, high fluidity and low linear expansion are required for cavity embedding.
[0004] As a higher density mounting form, a module is also used in which a multi-layer wiring layer is formed by the semi-additive method on the surface of a component-embedded substrate that has electronic components built into it, and further electronic components are mounted on the surface.
[0005] Furthermore, in recent years, with the miniaturization and high performance of electronic devices, the density and mounting of semiconductor elements in multilayer printed wiring boards and component-embedded boards are increasing. Accordingly, the amount of heat generated by semiconductor elements is also increasing, and it is important to efficiently dissipate the heat from the board. Therefore, in order to address such issues, it has been proposed to use a resin composition with high thermal conductivity using aluminum nitride, which has a higher thermal conductivity than silica, as a resin composition film in the manufacture of multilayer printed wiring boards by the build-up method (Patent Document 2). Specifically, Patent Document 2 proposes a resin composition containing aluminum nitride or silicon nitride treated with a silane compound, an epoxy resin, and a curing agent, and in the examples, a resin composition showing a maximum thermal conductivity of 2.8 W / m·K is disclosed. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2011-132507 A [Patent Document 2] WO2014 / 208352 Summary of the Invention [Problem to be solved by the invention]
[0007] As described above, a resin composition with high thermal conductivity is required, and a resin composition for a film with a maximum thermal conductivity of 2.8 W / m·K is known, as in Patent Document 2. However, in consideration of the recent trend toward higher density and higher mounting of electronic devices, a higher thermal conductivity is required. However, since resin composition films used in multilayer printed wiring boards and component-embedded boards are required to have not only thermal conductivity but also high fluidity and low linear expansion, there are limitations on the resin composition / filler composition, and the conventional technology has a limit to achieving high thermal conductivity with a resin composition that can be used as a resin composition film used in the manufacture of multilayer printed wiring boards and component-embedded boards. Therefore, the present invention aims to provide a resin composition that has high fluidity and a cured product with a low linear expansion coefficient and high thermal conductivity. [Means for solving the problem]
[0008] The present inventors have conducted extensive research to achieve the above object, and as a result have found that by using a combination of an aluminum nitride filler having a specific particle size distribution and an alumina filler having a specific particle size, it is possible to obtain a resin composition having the properties required for a resin composition film used in the manufacture of a multilayer printed wiring board or a component-embedded board, and a cured product thereof having high thermal conductivity.
[0009] That is, the present invention is a resin composition comprising (A) an epoxy resin, (B) an aluminum nitride filler, and (C) an alumina filler, wherein the total amount of the aluminum nitride filler (B) and the alumina filler (C) is 800 to 1500 parts by mass per 100 parts by mass of the epoxy resin (A), the epoxy resin (A) comprises (A-1) a solid epoxy resin and (A-2) a liquid epoxy resin, the aluminum nitride filler (B) has an average particle size D50 of 0.2 to 3 μm and a maximum particle size Dmax of 5 μm or less, and the alumina filler (C) has an average particle size D50 of 0.05 to 1.5 μm.
[0010] The aluminum nitride filler (B) has a specific surface area of 0.5 to 10 m 2 / g, and the (C) alumina filler has a specific surface area of 1 to 50 m 2 / g, and the ratio S2 / S1 of the total surface area S1 of the aluminum nitride filler (B) to the total surface area S2 of the alumina filler (C) is preferably 0.5 to 2.2. Also, a film made of the resin composition can be given as a preferred embodiment. Effect of the Invention
[0011] The present invention provides a resin composition having high fluidity and a cured product having low linear expansion and high thermal conductivity. By forming such a resin composition into a film, it becomes possible to efficiently produce multilayer printed wiring boards and component-embedded boards having excellent heat dissipation performance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] An example of an embodiment of the present invention will be described in detail below. However, the present invention is not limited to the embodiment described below, and can be modified as desired without departing from the gist of the present invention.
[0013] (A) Epoxy resin An epoxy resin is used as the resin of the resin composition of the present invention. The epoxy resin preferably contains a compound containing one or more epoxy groups in the molecule (hereinafter, sometimes referred to as "reactive epoxy resin"). Such a reactive epoxy resin may be a low molecular compound having an epoxy group. The reactive epoxy resin more preferably contains two or more epoxy resins in the molecule. The reactive epoxy resin is preferably contained in an amount of 50 mass% or more based on the total amount of epoxy resin. When the epoxy resin contains a reactive epoxy resin, in a scene where the resin composition of the present invention is used as a resin composition film for manufacturing a multilayer printed wiring board or a component-embedded board, the epoxy resin softens and has excellent fluidity, making it easy to follow the shape of the conductor layer of the multilayer printed wiring board, the cavity of the component-embedded board, and the shape of the electronic component, and after changing into a desired shape, it is heat-cured to have high strength and heat resistance, so that it is easy to improve the reliability of these boards. There is no particular upper limit on the blending ratio of the reactive epoxy resin to the total amount of epoxy resin, and the total amount of epoxy resin may be a reactive epoxy resin.
[0014] The epoxy resin includes both (A-1) solid epoxy resin and (A-2) liquid epoxy resin. In the present invention, an epoxy resin that is solid at a temperature of 25°C is referred to as (A-1) solid epoxy resin, and an epoxy resin that is liquid at 25°C is referred to as (A-2) liquid epoxy resin.
[0015] By including the (A) epoxy resin in the (A-1) solid epoxy resin, the strength and heat resistance of the resin composition after heat curing can be improved. On the other hand, most solid epoxy resins have high melt viscosity, and considering that the resin composition of the present invention is used as a resin composition film in the manufacture of a multilayer printed wiring board or a component-embedded board, it is necessary to increase the fluidity so that it can conform to the desired board shape, and therefore a liquid epoxy resin with high fluidity is used in combination with a solid epoxy resin with high heat resistance.
[0016] As the solid epoxy resin, tetrafunctional naphthalene type epoxy resin, trifunctional naphthalene type epoxy resin, trisphenolmethane type epoxy resin, phenol novolac type epoxy resin, cresol novolac type epoxy resin, bisphenol A novolac type epoxy resin, naphthol novolac type epoxy resin, naphthol cresol novolac type epoxy resin, dicyclopentadiene type epoxy resin, biphenyl aralkyl type epoxy resin, bixylenol type epoxy resin, naphthylene ether type epoxy resin or fluorene type epoxy resin is preferred, and tetrafunctional naphthalene type epoxy resin, biphenyl aralkyl type epoxy resin, trisphenolmethane type epoxy resin, bixylenol type epoxy resin, naphthylene ether type epoxy resin or fluorene type epoxy resin is more preferred. Specific examples of solid epoxy resins include "HP-4700", "HP-4710" (tetrafunctional naphthalene type epoxy resins), "N-690", "N-695" (cresol novolac type epoxy resins), "HP-7200", "HP-7200L", "HP-7200H" (dicyclopentadiene type epoxy resins), "HP6000", "HP-6000H" (naphthylene ether type epoxy resins) manufactured by DIC Corporation, and "EPPN-501H", "EPPN-501HY", "EPPN-502H" (trisphenolmethane type epoxy resins), "NC7000L", and "NC-7000H" manufactured by Nippon Kayaku Co., Ltd. , "NC-7300L" (naphthol cresol novolac epoxy resin), "NC-3000H", "NC-3000", "NC-3000L", "NC-3100", "NC-3500" (biphenyl aralkyl type epoxy resin), "ESN475" (naphthol novolac type epoxy resin) and "ESN485" (naphthol novolac type epoxy resin) manufactured by Nippon Steel Chemical Co., Ltd., "YX4000H", "YL6121" (biphenyl type epoxy resin), "YX4000HK" (bixylenol type epoxy resin), "YL7800" (fluorene type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd., and the like. These may be used alone or in combination of two or more types.
[0017] By including the (A) epoxy resin in the (A-2) liquid epoxy resin, the melt viscosity of the resin composition can be reduced and the flowability can be improved, which makes it possible for the resin composition of the present invention to have excellent flowability and conform to the shape of the conductor layer or cavity when subjected to heat and pressure molding when used as a resin composition film in the manufacture of a multilayer printed wiring board or a component-embedded board.
[0018] As the liquid epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, phenol novolac type epoxy resin, or naphthalene type epoxy resin is preferred, and bisphenol A type epoxy resin and bisphenol F type epoxy resin are more preferred. Specific examples of liquid epoxy resins include "jER828", "jER828EL", "jER828US" (bisphenol A type epoxy resin), "jER806", "jER806H", "jER807" (bisphenol F type epoxy resin), and "jER152" (phenol novolac type epoxy resin) manufactured by Mitsubishi Chemical Corporation, "ZX1059" (mixture of bisphenol A type epoxy resin and bisphenol F type epoxy resin) manufactured by Nippon Steel Chemical Co., Ltd., and "HP4032", "HP4032D", and "HP4032SS" (naphthalene type epoxy resin) manufactured by DIC Corporation. These may be used alone or in combination of two or more types.
[0019] The viscosity of the (A-2) liquid epoxy resin at 25° C. is preferably 500 poise or less, more preferably 10 to 300 poise, and even more preferably 20 to 200 poise. By setting it within this range, the melt viscosity of the resin composition can be kept low, and high fluidity can be obtained.
[0020] The blending ratio of the solid epoxy resin (A-1) and the liquid epoxy resin (A-2) (solid epoxy resin:liquid epoxy resin) is preferably in the range of 9:1 to 1:9 by mass, more preferably in the range of 4:1 to 1:4, further preferably in the range of 3:1 to 1:3, and particularly preferably in the range of 2:1 to 1:2. By setting the blending ratio of the solid epoxy resin and the liquid epoxy resin in the above range, it becomes easy to achieve both high fluidity and heat resistance.
[0021] The epoxy equivalent of the (A) epoxy resin is preferably 50 to 4500, more preferably 50 to 3000, even more preferably 80 to 2000, and even more preferably 100 to 1000. By setting it within this range, the crosslink density of the cured product of the resin composition becomes sufficient, and it becomes easy to bring about sufficient heat resistance and mechanical strength when used as a resin composition film. The epoxy equivalent can be measured according to JIS K7236, and is the mass of the resin per equivalent of epoxy group.
[0022] (B) Aluminum nitride filler The resin composition of the present invention is blended with an aluminum nitride filler having an average particle size D50 of 0.2 to 3 μm and a maximum particle size Dmax of 5 μm or less. By blending an aluminum nitride filler, it becomes possible for the cured product of the resin composition to have high thermal conductivity. Furthermore, by making the average particle size 0.2 to 3 μm, the resin composition can be easily molded into a film of about 10 μm to several hundred μm in order to be used as a film, and high thermal conductivity can be easily obtained at that thickness. Furthermore, by making the maximum particle size Dmax 5 μm or less, the melt viscosity of the resin composition is reduced, and in the case of using the resin composition in the manufacture of a multilayer printed wiring board or a component-embedded board, the resin composition has good conformability to the shape of a conductor layer or a cavity when heated and pressurized.
[0023] The average particle size of the (B) aluminum nitride filler is preferably 0.3 to 2 μm, more preferably 0.5 to 1.5 μm, and the maximum particle size is preferably 4.5 μm or less, more preferably 4 μm or less.
[0024] In the present invention, the average particle size D50 is the particle size at which the cumulative 50% value is reached on a volume basis in the particle size distribution measured by a laser diffraction scattering method, and the maximum particle size Dmax is the maximum value of the measured particle size.
[0025] The method for producing the aluminum nitride filler (B) is not particularly limited, and aluminum nitride filler produced by a known method can be used. Examples of the method for producing aluminum nitride include direct nitridation, reduction nitridation, and gas phase synthesis. Specific examples of aluminum nitride fillers that can be used include aluminum nitride filler HF-01D (manufactured by Tokuyama Corporation). It is also possible to use commercially available aluminum nitride powder by adjusting the particle size distribution using a sieve or a classifier so that the average particle size and maximum particle size are satisfied.
[0026] (B) The specific surface area of the aluminum nitride filler is not particularly limited, but is preferably 0.5 to 10 m 2 / g, and 0.8 to 7m 2 / g is more preferable, and 1.0 to 5m 2 By having the specific surface area in the above range, dispersibility in the epoxy resin is improved, and when the resin composition is used as a film, the melt viscosity of the resin composition is low and can be easily set in the optimal range.
[0027] (B) The aluminum nitride filler may contain impurities such as alkaline earth elements and rare earth elements, which are derived from the raw materials or intentionally added during the synthesis process, up to about 5 parts by mass. However, an amount of impurities that significantly reduces the crystallinity of aluminum nitride is not preferable because it causes a decrease in thermal conductivity. The aluminum nitride content in the aluminum nitride filler is preferably 95% by mass or more, and more preferably 99% by mass or more.
[0028] (B) The aluminum nitride filler may be a filler that has been surface-treated with a surface treatment agent. By performing the surface treatment, the water resistance of the aluminum nitride is improved, and the affinity with the epoxy resin is improved, so that the filling property of the aluminum nitride filler is improved, and it becomes easy to improve the flowability of the resin composition. As the surface treatment agent, for example, a known treatment agent such as a silane compound, an aluminate coupling agent, a titanate coupling agent, etc. can be used without any particular limitation. Among these, a silane compound that can react at a particularly high reaction rate can be preferably used.
[0029] Specific examples of the silane compound used as the surface treatment agent include silane compounds having a reactive functional group, such as 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-acryloxypropyltrimethoxysilane, 3-acryloxypropylmethyldimethoxysilane, 3-acryloxypropylmethyldiethoxysilane, 3-acryloxypropyltrimethoxysilane, 3-acryloxypropyltrimethoxysilane, 3-acryloxypropyltriethoxy ...trimethoxysilane, 3-acryloxypropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, 3-acryloxypropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, 3-acryloxypropyltriethoxysilane, 3-acryloxypropyltriethoxysilane, 3-acryloxypropyltriethoxysilane, 3-acryloxypropyltriethoxysilane, 3-acryloxypropyltriethoxysilane, 3-acryloxypropyltriethoxysilane, 3-acryloxypropyltriethoxysilane, 3-acryloxypropyltriethoxysilane, 3-acryloxypropyltriethoxysilane, 3-acryloxy alkoxysilanes such as N-mercaptopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 2-aminoethyl-3-aminopropyltrimethoxysilane, 2-aminoethyl-3-aminopropylmethyldimethoxysilane, 3-dimethylaminopropyltrimethoxysilane, 3-diethylaminopropyltrimethoxysilane, 3-triethoxysilyl-N-(1,3-dimethylbutylidene)propylamine, N-phenyl-3-aminopropyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, p-styryltrimethoxysilane, and allyltrimethoxysilane.
[0030] Examples of silane compounds having a non-reactive functional group include methyltrimethoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, trimethylmethoxysilane, ethyltrimethoxysilane, n-propyltrimethoxysilane, isobutyltrimethoxysilane, isobutyltriethoxysilane, n-hexyltrimethoxysilane, n-hexyltriethoxysilane, cyclohexyltrimethoxysilane, cyclohexylmethyldimethoxysilane, n-octyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, diphenyldimethoxysilane, diphenyldiethoxysilane, trifluoropropyltrimethoxysilane, and trifluoropropylmethyldimethoxysilane.
[0031] Other usable silane compounds include chlorosilanes such as vinyltrichlorosilane, methyltrichlorosilane, dimethyldichlorosilane, trichloromethylsilane, ethyldimethylchlorosilane, propyldimethylchlorosilane, phenyltrichlorosilane, trifluoropropyltrichlorosilane, and isopropyldiethylchlorosilane.
[0032] Among silane compounds, those with high affinity to epoxy resins are preferred, and examples of silane compounds with high affinity include silane compounds having functional groups that can react with epoxy groups, such as glycidoxy groups and amino groups. Although they are not reactive with epoxy groups, functional groups such as methacryloxy groups, acryloxy groups, phenyl groups, vinyl groups, and styryl groups also have high affinity with epoxy resins, and silane compounds having these functional groups are also suitable. When the surface treatment agent is used, the amount of the surface treatment agent is 0.1 to 5 parts by mass, preferably 0.5 to 4 parts by mass, based on 100 parts by mass of the raw powder before surface treatment.
[0033] The surface treatment method may be any known method without particular limitation, and may be either a dry surface treatment or a wet surface treatment. Dry surface treatment is a method of dry mixing without using a large amount of solvent when mixing the raw material powder and the surface treatment agent, and examples of such methods include a method of gasifying the surface treatment agent and mixing it with the raw material powder, a method of spraying or dropping a liquid surface treatment agent and mixing it with the raw material powder, and a method of diluting the surface treatment agent with a small amount of organic solvent to increase the amount of liquid, and then spraying or dropping it. Wet surface treatment is a method of mixing the raw material powder and the surface treatment agent with a solvent, and examples of such methods include a method of mixing the raw material powder, the surface treatment agent, and a solvent, and then removing the solvent by drying or the like.
[0034] (C) Alumina filler The resin composition of the present invention contains an alumina filler having an average particle size D50 of 0.05 to 1.5 μm. By thus containing an alumina filler having a particle size smaller than that of the aluminum nitride filler (B), the alumina particles enter the gaps between the aluminum nitride particles in the resin composition, and the contact area of the thermally conductive particles is increased while maintaining the high fluidity of the resin composition, thereby improving the thermal conductivity.
[0035] The average particle size D50 of the (C) alumina filler is preferably 0.1 to 1 μm, and more preferably 0.15 to 0.8 μm. The maximum particle size Dmax of the alumina filler is preferably 5 μm or less, more preferably 4 μm or less, and even more preferably 3 μm or less.
[0036] (C) The specific surface area of the alumina filler is not particularly limited, but is preferably 1 to 50 m 2 / g, and 1.5 to 30m 2 / g is more preferable, and 2 to 20m 2 With a specific surface area in the above range, when the aluminum nitride filler (B) is combined with the epoxy resin and mixed therewith, the dispersibility in the epoxy resin is improved, and it becomes easy to lower the melt viscosity of the resin composition.
[0037] The crystallinity of the (C) alumina filler is not particularly limited, but the higher the crystallinity, the more preferable, and the higher the proportion of alpha crystals in the crystal system, the more preferable. The higher the crystallinity of the alumina filler, the easier it is to obtain a resin composition with high thermal conductivity as a cured product. The crystallinity of the alumina filler can be confirmed by X-ray diffraction.
[0038] The relationship between the particle size of the (C) alumina filler and the particle size of the (B) aluminum nitride filler is not particularly limited, but the ratio of D50 of the alumina filler to D50 of the aluminum nitride filler is preferably 0.02 to 0.9, more preferably 0.05 to 0.8, and even more preferably 0.10 to 0.7. When the particle size ratio is within the above range, the fillability of the aluminum nitride filler and the alumina filler in the resin is improved, and it becomes easy to lower the melt viscosity of the resin composition.
[0039] (C) Alumina filler may be used without surface treatment, or may be a filler that has been surface-treated with a surface treatment agent. When using a surface-treated alumina filler, the surface treatment method may be any known method without particular limitation, and may be any of dry surface treatment and wet surface treatment. As the surface treatment agent, for example, known treatment agents such as silane compounds, aluminate coupling agents, titanate coupling agents, etc. may be used without particular limitation. Among these, the silane compounds described above are preferably used. When the surface treatment agent is used, the amount of the surface treatment agent is 0.1 to 5 parts by mass, preferably 0.5 to 4 parts by mass, based on 100 parts by mass of the raw powder before surface treatment.
[0040] In the resin composition of the present invention, the total amount of the aluminum nitride filler (B) and the alumina filler (C) is 800 to 1500 parts by mass per 100 parts by mass of the epoxy resin (A). This allows the flowability, low linear expansion, and high thermal conductivity of the resin composition to be improved in a well-balanced manner. The total amount of the aluminum nitride filler (B) and the alumina filler (C) is preferably 900 to 1400 parts by mass, more preferably 1000 to 1300 parts by mass per 100 parts by mass of the epoxy resin (A).
[0041] The ratio of the amount of the aluminum nitride filler (B) and the alumina filler (C) is not particularly limited, but it is preferable that the ratio S2 / S1 of the total surface area S1 of the aluminum nitride filler (B) to the total surface area S2 of the alumina filler (C) is 0.5 to 2.2. By setting the value of S2 / S1 in the above range, the thermal conductivity of the resin composition can be made higher. Although the reason is not clear, it is presumed that the balance of the interaction between the epoxy resin and each filler improves the adhesion between the epoxy resin and the filler interface, thereby improving the filling property of the filler. The value of S2 / S1 is more preferably 0.8 to 2.1, even more preferably 1.0 to 1.8, and particularly preferably 1.1 to 1.5. The total surface area S1 of the aluminum nitride filler (B) can be calculated by the product of the specific surface area of the aluminum nitride filler and the amount of the aluminum nitride filler. Similarly, the total surface area S2 of the alumina filler (C) can be calculated by multiplying the specific surface area of the alumina filler by the amount of the alumina filler blended.
[0042] Other Ingredients The resin composition of the present invention may contain components other than the (A) epoxy resin, (B) aluminum nitride filler, and (C) alumina filler, so long as the effects of the present invention are not impaired. Examples of the other components include a curing agent for the epoxy resin, a curing accelerator, other resins other than the epoxy resin, other fillers, a flame retardant, rubber particles, a thickener, a defoaming agent, a leveling agent, an adhesion imparting agent, an antioxidant, an ultraviolet degradation inhibitor, and a colorant.
[0043] The epoxy resin curing agent has a function of reacting with the epoxy resin and curing when the (A) epoxy resin contains a reactive epoxy resin. By including a curing agent for the epoxy resin in the resin composition of the present invention, it becomes easy to obtain a cured product having high strength and heat resistance when the resin composition of the present invention is thermally cured. The epoxy resin curing agent is not particularly limited, and a known curing agent can be used. For example, phenol-based curing agents, naphthol-based curing agents, active ester-based curing agents, cyanate ester-based curing agents, benzoxazine-based curing agents, acid anhydride-based curing agents, etc. are mentioned, and from the viewpoint of moldability of the resin composition into a film and heat resistance of the cured product, etc., phenol-based curing agents, naphthol-based curing agents, and active ester-based curing agents are preferred. The curing agent may be used alone or in combination of two or more.
[0044] Of the phenol-based and naphthol-based hardeners, taking into consideration the heat resistance and water resistance of the cured product, phenol-based hardeners and naphthol-based hardeners having a novolac structure are preferred. As phenol-based hardeners, phenol novolac, cresol novolac, bisphenol A type novolac, phenol aralkyl novolac, biphenyl aralkyl novolac, amino triazine novolac (phenol novolac containing a triazine structure), triphenyl methane novolac, cyclopentadiene phenol novolac, etc. are preferred. As naphthol-based hardeners, naphthol aralkyl type phenol novolac, aralkyl type naphthol-phenol novolac, naphthol-cresol type novolac are preferred.
[0045] Specific examples of phenol-based curing agents and naphthol-based curing agents include "GPH-103", "GPH-65", and "TKG-105" manufactured by Nippon Kayaku Co., Ltd.; "TD-2093", "TD-2090", "LF-6161", "LF-4871", "LA-7052", "LA-7054", "LA-1536", and "LA-1356" manufactured by DIC Corporation; "ZX-798" and "SN485" manufactured by Nippon Steel Chemical Co., Ltd.; "TPM-100" and "GPNX" manufactured by Gun-ei Chemical Co., Ltd.; and "S-TPM" and "J-DDP" manufactured by JFE Chemical Corporation.
[0046] The reactive group equivalent (hydroxyl group equivalent) of the phenol-based curing agent and naphthol-based curing agent is not particularly limited, but from the viewpoints of moldability of the resin composition into a film and heat resistance of the cured product, it is preferably 20 to 4000, more preferably 50 to 2000, and even more preferably 50 to 1000. The hydroxyl group equivalent is the mass of the resin per equivalent of hydroxyl group.
[0047] Examples of the active ester curing agent include an active ester curing agent having a dicyclopentadiene structure, an active ester curing agent having a naphthalene structure, an active ester curing agent containing an acetylated product of phenol novolac, and an active ester curing agent containing a benzoylated product of phenol novolac. Taking into consideration the heat resistance and water resistance of the cured product, an active ester curing agent having a dicyclopentadiene structure and an active ester curing agent having a naphthalene structure are more preferred. Specific examples of the active ester curing agent include "HPC-8000-65T" (an active ester curing agent having a dicyclopentadiene structure) and "HPC-8150-62T" (an active ester curing agent having a naphthalene structure) manufactured by DIC Corporation.
[0048] The reactive group equivalent (active ester group equivalent) of the active ester curing agent is not particularly limited, but from the viewpoints of moldability of the resin composition into a film and heat resistance of the cured product, it is preferably 50 to 2000, more preferably 50 to 1000, and even more preferably 100 to 500. The active ester group equivalent is the mass of the resin per equivalent of active ester group.
[0049] The amount of the curing agent in the resin composition of the present invention is not particularly limited, but considering the heat resistance and mechanical strength of the cured product, the amount of the curing agent is preferably 50 to 200, more preferably 65 to 150, and even more preferably 75 to 125 parts by mass per 100 parts by mass of the epoxy resin (A). The total number of reactive groups such as hydroxyl groups and active ester groups of the curing agent is not particularly limited, but is preferably 0.5 to 2, more preferably 0.6 to 1.5, and even more preferably 0.65 to 1.25, relative to the total number of epoxy groups of the epoxy resin (A). Here, the total number of epoxy groups of the epoxy resin (A) is the value obtained by dividing the mass of each epoxy resin by the epoxy equivalent, and the total number of reactive groups of the curing agent is the value obtained by dividing the mass of each curing agent by the reactive group equivalent.
[0050] The curing accelerator has a function of promoting the reaction between the epoxy group of the epoxy resin (A) and the reactive group of the curing agent or the polymerization of the epoxy group. When the resin composition of the present invention contains the curing accelerator for the epoxy resin, when the epoxy resin (A) contains a reactive epoxy resin, the resin composition of the present invention can be easily cured during thermal curing, and high strength can be easily obtained after curing. When the resin composition of the present invention contains the curing agent for the epoxy resin, the blending amount of the curing accelerator is preferably 0.01 to 5 parts by mass, more preferably 0.05 to 3 parts by mass, and even more preferably 0.1 to 2 parts by mass relative to 100 parts by mass of the epoxy resin (A).
[0051] As the curing accelerator for the epoxy resin, known substances can be used without any particular limitation, and examples thereof include amine-based curing accelerators, imidazole-based curing accelerators, phosphorus-based curing accelerators, guanidine-based curing accelerators, etc., with amine-based curing accelerators and imidazole-based curing accelerators being preferred. The curing accelerators may be used alone or in combination of two or more.
[0052] Examples of the amine curing accelerator include trialkylamines such as triethylamine and tributylamine, 4-dimethylaminopyridine, benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, and 1,8-diazabicyclo(5,4,0)-undecene.
[0053] Examples of the imidazole-based curing accelerator include 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, and 1-benzyl-2-methylimidazole. Phenylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazolium trimellitate, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl -(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct imidazole compounds such as 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5 hydroxymethylimidazole, 2,3-dihydro-1H-pyrrolo[1,2-a]benzimidazole, 1-dodecyl-2-methyl-3-benzylimidazolium chloride, 2-methylimidazoline, and 2-phenylimidazoline, as well as adducts of imidazole compounds and epoxy resins.
[0054] Examples of phosphorus-based curing accelerators include triphenylphosphine, phosphonium borate compounds, tetraphenylphosphonium tetraphenylborate, n-butylphosphonium tetraphenylborate, tetrabutylphosphonium decanoate, (4-methylphenyl)triphenylphosphonium thiocyanate, tetraphenylphosphonium thiocyanate, and butyltriphenylphosphonium thiocyanate.
[0055] Examples of the guanidine curing accelerator include dicyandiamide, 1-methylguanidine, 1-ethylguanidine, 1-cyclohexylguanidine, 1-phenylguanidine, 1-(o-tolyl)guanidine, dimethylguanidine, diphenylguanidine, trimethylguanidine, tetramethylguanidine, pentamethylguanidine, 1,5,7-triazabicyclo[4.4.0]dec-5-ene, 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene, 1-methylbiguanide, 1-ethylbiguanide, 1-n-butylbiguanide, 1-n-octadecylbiguanide, 1,1-dimethylbiguanide, 1,1-diethylbiguanide, 1-cyclohexylbiguanide, 1-allylbiguanide, 1-phenylbiguanide, and 1-(o-tolyl)biguanide.
[0056] By including other resins in the resin composition of the present invention, the flexibility of the resin composition can be imparted. This improves the coating property when forming a resin composition film, resulting in a uniform film, and the film becomes flexible, improving the winding property, and also making it easier to improve the impact resistance of the cured product and make it less likely to crack. Examples of other resins include thermoplastic resins such as phenoxy resins, polyvinyl acetal resins, polyolefin resins, polybutadiene resins, polyimide resins, polyamideimide resins, polyethersulfone resins, polyphenylene ether resins, and polysulfone resins. Among these, phenoxy resins having a structure similar to that of epoxy resins are preferred because of their good compatibility with epoxy resins. These thermoplastic resins may be used alone or in combination of two or more.
[0057] Examples of the phenoxy resin include phenoxy resins having one or more skeletons selected from the group consisting of bisphenol A skeleton, bisphenol F skeleton, bisphenol S skeleton, bisphenol acetophenone skeleton, novolac skeleton, biphenyl skeleton, fluorene skeleton, dicyclopentadiene skeleton, norbornene skeleton, naphthalene skeleton, anthracene skeleton, adamantane skeleton, terpene skeleton, trimethylcyclohexane skeleton, and the like. The terminal of the phenoxy resin may be any terminal structure such as a phenolic hydroxyl group or an epoxy group. The phenoxy resin may be used alone or in combination of two or more kinds. Specific examples of the phenoxy resin include "YX6954BH30" (phenoxy resin containing bisphenol acetophenone skeleton), "YX8100BH30" (phenoxy resin containing bisphenol S skeleton), and "YX7553BH30" manufactured by Mitsubishi Chemical Corporation. The weight average molecular weight of the phenoxy resin is preferably 5000 to 10000. The weight average molecular weight is a polystyrene-equivalent weight average molecular weight measured by gel permeation chromatography.
[0058] When the resin composition of the present invention contains a phenoxy resin, the amount of the phenoxy resin is preferably 0.1 to 50 parts by mass, more preferably 0.5 to 30 parts by mass, and even more preferably 1 to 20 parts by mass, per 100 parts by mass of the epoxy resin (A).
[0059] The other fillers are fillers made of materials other than aluminum nitride and alumina, and may include, for example, silica, zinc oxide, magnesium oxide, titanium oxide, silicon nitride, boron nitride, aluminum hydroxide, magnesium hydroxide, silicon carbide, calcium carbonate, barium sulfate, talc, diamond, etc.
[0060] The amount of the other filler is preferably 10% by mass or less, more preferably 5% by mass or less, even more preferably 1% by mass or less, and particularly preferably none, based on the total amount of the aluminum nitride filler (B) and the alumina filler (C). The particle size of the other filler is preferably smaller than that of the aluminum nitride filler (B), more preferably an average particle size of less than 2 μm, even more preferably less than 1.5 μm. The maximum particle size is also preferably smaller than that of the aluminum nitride filler (B), more preferably a maximum particle size of less than 4.5 μm, even more preferably less than 4 μm.
[0061] The resin composition of the present invention may contain a flame retardant or rubber particles as other components. The flame retardant is a compound that imparts flame retardancy when the resin composition of the present invention is used in a semiconductor product, and examples of the flame retardant include organic phosphorus flame retardants, organic nitrogen-containing phosphorus compounds, nitrogen compounds, silicone flame retardants, and metal hydroxides. These flame retardants may be used alone or in combination of two or more. In addition, by including rubber particles, the internal stress when the resin composition is thermally cured can be alleviated to reduce warping of the cured product, and impact resistance can also be imparted. Examples of rubber particles include fine particles such as core-shell type rubber particles, cross-linked acrylonitrile butadiene rubber particles, cross-linked styrene butadiene rubber particles, and acrylic rubber particles, and the average particle size is preferably 1 μm or less, and more preferably 0.8 μm or less. Furthermore, the resin composition of the present invention may contain additives such as thickeners, defoamers, leveling agents, adhesion imparting agents, antioxidants, ultraviolet degradation inhibitors, and colorants, as necessary.
[0062] The resin composition of the present invention is characterized by having high fluidity, and the cured product thereof has a low linear expansion coefficient and high thermal conductivity.
[0063] Since the resin composition has high fluidity, when used as a resin composition film, it is easy to improve adhesion by following the shape of the conductor layer of a multilayer printed wiring board, the cavity of a component-embedded board, and the electronic components. The resin composition of the present invention preferably has a minimum melt viscosity of 13,000 poise or less in the range of 90 to 140 ° C., more preferably 9,000 poise or less. In the manufacture of a multilayer printed wiring board using a resin composition film, the heat press condition is often performed by selecting an appropriate temperature in the range of 90 to 140 ° C. If the minimum melt viscosity of the resin composition in the range of 90 to 140 ° C. is 13,000 poise or less, the resin composition can be handled under conditions with high fluidity by selecting a temperature around the minimum value as the condition during heat and pressure molding in the manufacture of a multilayer printed wiring board or a component-embedded board. The minimum melt viscosity of the resin composition in the range of 90 to 140 ° C. is preferably 300 poise or more, more preferably 500 poise or more, from the viewpoint of handleability. The melt viscosity can be determined as a complex viscosity by measuring the temperature dispersion of dynamic viscoelasticity using a viscoelasticity measuring device (rotational rheometer).
[0064] The linear expansion coefficient of the cured product of the resin composition of the present invention is preferably 25 ppm / ° C. or less, and more preferably 22 ppm / ° C. or less. It is generally considered better to approach the linear expansion coefficient of copper, which is the conductor layer, of 17 ppm / ° C. The linear expansion coefficient can be measured using a thermomechanical analyzer and can be determined from the slope of the change in linear expansion coefficient up to the glass transition temperature.
[0065] The relative density of the resin composition of the present invention is preferably 0.90 or more, more preferably 0.95 or more, and even more preferably 0.97 or more. The relative density is expressed as the ratio of the density of a cured sample of the resin composition to the density (theoretical density) calculated from the density and compounding ratio of each material used, and is 1 when the theoretical density and the sample density are the same. A high relative density indicates that the filling of the filler into the resin is high, there are few defects such as voids in the resin composition, and the adhesion of the interface between each component is excellent, which tends to improve the fluidity, thermal conductivity, strength, durability, etc. of the resin composition. The upper limit of the relative density is not particularly limited, but is usually 1.0 or less. The density of the cured resin composition can be measured by the Archimedes method.
[0066] The thermal conductivity of the cured product of the resin composition of the present invention is preferably 3.5 W / m·K or more, more preferably 4.0 W / m·K or more, even more preferably 4.5 W / m·K or more, and particularly preferably 5.0 W / m·K or more. By using a resin composition having a high thermal conductivity of the cured product as a resin composition film, the heat dissipation of multilayer printed wiring boards and component-embedded boards can be improved. The higher the thermal conductivity, the better, but it is generally 30 W / m·K or less. The thermal conductivity can be measured by temperature wave thermal analysis (i-phase method).
[0067] The method for producing the resin composition of the present invention is not particularly limited, and the resin composition can be produced by mixing the resin, the filler, and other components as necessary by a known method using a blender, a mixer, or the like. When mixing, each component may be added to a mixer or the like at the same time and mixed, or each component may be added to a mixer or the like sequentially and mixed. The order of addition in this case is not particularly limited. Furthermore, the mixing may be performed under heating as necessary, or may be performed under an adjusted atmosphere such as an inert gas atmosphere.
[0068] The resin composition of the present invention has high fluidity, and the cured product thereof has high thermal conductivity and low linear expansion, so that it can be suitably used as the insulating layer of the multilayer printed wiring board or the sealing resin of the component-embedded board. In addition to these uses, it can be widely used in various uses requiring heat dissipation, such as adhesive films, insulating layers of metal-clad laminates, insulating resin sheets such as prepregs, underfill materials, die bonding materials, semiconductor sealing materials, hole filling resins, etc. When the resin composition of the present invention is used for the above-mentioned uses, it is generally suitable for industrial use to use it as a resin composition film formed into a film-like form.
[0069] The resin composition film of the present invention is obtained by molding the resin composition of the present invention into a film, and its thickness is preferably from 5 to 250 μm, more preferably from 10 to 200 μm, and further preferably from 20 to 150 μm.
[0070] The method for producing the resin composition film of the present invention is not particularly limited, and can be made into a film by a conventionally known method.Among them, a preferred method includes, for example, dissolving and mixing the resin composition in an organic solvent to prepare a varnish of the resin composition, applying the varnish of the resin composition on a support using a die coater or the like, and then drying the organic solvent by heating or blowing hot air or the like to produce a resin composition film.
[0071] Examples of the organic solvent include acetone, methanol, ethanol, butanol, 2-propanol, 2-methoxyethanol, 2-ethoxyethanol, 1-methoxy-2-propanol, 2-acetoxy-1-methoxypropane, toluene, xylene, methyl ethyl ketone, N,N-dimethylformamide, methyl isobutyl ketone, N-methyl-pyrrolidone, n-hexane, cyclohexane, cyclohexanone, and a mixture such as solvent naphtha, etc. These organic solvents may be used alone or in combination of two or more.
[0072] The boiling point of the organic solvent is preferably 200° C. or lower, and more preferably 180° C. or lower, since the organic solvent can be easily removed during drying. The content of the organic solvent in the varnish of the resin composition is not particularly limited, and may be appropriately adjusted in consideration of the coatability onto the support, etc.
[0073] The drying conditions are not particularly limited, but it is preferable to dry the resin composition film so that the content of the organic solvent in the resin composition film is preferably 10 mass % or less, more preferably 5 mass % or less. Although this varies depending on the boiling point of the organic solvent used in the resin composition varnish, for example, by heating and drying at 60°C to 150°C for 1 to 5 minutes, a resin composition film can be obtained to the extent that the thermal curing of the resin composition does not proceed too much.
[0074] The resin composition film of the present invention is preferably in a partially cured state, and is a so-called B-stage film. Since it is in a partially cured state and is not completely cured, it can easily conform to the shape of the conductor layer during the manufacturing process of a multilayer printed wiring board or a component-embedded board, and further curing can be progressed thereafter to improve strength and durability.
[0075] As the support, various plastic films can be suitably used. Examples of the plastic film include polyester films such as polyethylene terephthalate film, polybutylene terephthalate film, and polyethylene naphthalate, olefin films such as polyethylene film and polypropylene film, and polyimide film. Among them, polyethylene terephthalate film, which has excellent smoothness and heat resistance and is inexpensive, is more preferable. Taking into consideration wettability when coating the resin composition film and releasability when manufacturing various semiconductor substrates, the coated surface of the plastic film of the support may be subjected to release treatment, matte treatment, corona discharge treatment, etc. In addition, metal foils such as copper foil and aluminum foil can also be used as the support. As the copper foil, rolled copper foil, electrolytic copper foil, etc. can be suitably used. By using a metal foil as the support, the process of laminating metal foils in the manufacture of various substrates can be omitted, and the adhesive strength can be increased. The thickness of the support is not particularly limited, but is preferably in the range of 5 μm to 150 μm, more preferably in the range of 10 μm to 100 μm, and even more preferably in the range of 10 to 60 μm.
[0076] In the resin composition film, a protective film equivalent to the support may be further laminated on the surface not in contact with the support. The thickness of the protective film is not particularly limited, but is, for example, 5 μm to 40 μm. By laminating the protective film, it is possible to prevent adhesion of dust and the like to the surface of the resin composition film and damage. By laminating the protective film, it is also possible to wind the resin composition film in a roll. When manufacturing a multilayer printed wiring board, a component-embedded board, or other semiconductor materials, the protective film is peeled off before use.
[0077] The resin composition film has high fluidity and embeddability, and has a high thermal conductivity and a low linear expansion coefficient after curing, and therefore can be suitably used for forming an insulating layer of a multilayer printed wiring board or as a sealing resin for a component-embedded board. It can also be used in a wide range of applications requiring heat dissipation, such as adhesive films, insulating layers of metal-clad laminates, insulating resin sheets such as prepregs, underfill materials, die bonding materials, semiconductor sealing materials, and hole-filling resins. EXAMPLES
[0078] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. Various materials used and physical property measurement conditions are described below.
[0079] <Epoxy resin> (A-1) The following solid epoxy resin was used: NC-3000 (biphenyl aralkyl type epoxy resin manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent 276, softening point 58°C) EPPN-501HY (Trisphenolmethane type epoxy resin manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent 166, softening point 60°C) HP-4700 (DIC Corporation 4-functional naphthalene type epoxy resin, epoxy equivalent 163, softening point 92°C) Each of the above solid epoxy resins was dissolved in methyl ethyl ketone, and used as a 50 mass % epoxy resin solution for preparing a resin composition. (A-2) As the liquid epoxy resin, jER828 (a bisphenol A type epoxy resin manufactured by Mitsubishi Chemical Corporation, epoxy equivalent 189, viscosity (25°C) 135 poise) was used.
[0080] <Aluminum nitride filler> (B) The following aluminum nitride filler was used: B-1: HF-01D (Tokuyama Corp.) surface-treated with N-phenyl-3-aminopropyltrimethoxysilane (KBM-573, Shin-Etsu Chemical Co., Ltd.) according to the following method. Average particle size: 0.9 μm, maximum particle size: 3.3 μm, specific surface area: 2.8 m 2 / g. B-2: HF-01D (Tokuyama Corp.) surface-treated with 3-methacryloxypropyltriethoxysilane (KBM-503, Shin-Etsu Chemical Co., Ltd.) according to the following method. Average particle size: 0.9 μm, maximum particle size: 3.4 μm, specific surface area: 2.6 m 2 / g. B-3: Aluminum nitride powder H grade (Tokuyama Corp.) surface-treated with N-phenyl-3-aminopropyltrimethoxysilane (KBM-573, Shin-Etsu Chemical Co., Ltd.) according to the following method. Average particle size 1.1 μm, maximum particle size 6.5 μm, specific surface area 2.6 m 2 / g. The surface treatment was performed by placing 600 g of the raw material powder, 5 g of the surface treatment agent, and 1,200 g of isopropyl alcohol in a glass recovery flask, stirring for 30 minutes with a fluororesin stirring blade, and then removing the isopropyl alcohol under reduced pressure at 50°C using a rotary evaporator, followed by drying under reduced pressure at 100°C.
[0081] <Alumina filler> (C) The following alumina filler was used: ·AA-03F (manufactured by Sumitomo Chemical Co., Ltd., average particle size 0.28μm, specific surface area 6.4m) 2 / g) ·NXA-150 (manufactured by Sumitomo Chemical Co., Ltd., average particle size 0.20 μm, specific surface area 9.7 m 2 / g) AHPA-0.5AF (Sasol, average particle size 0.44μm, specific surface area 8.0m 2 / g) ·AA-1.5 (manufactured by Sumitomo Chemical Co., Ltd., average particle size 1.7 μm, specific surface area 1.3 m 2 / g)
[0082] <Hardening agent> The following epoxy resin hardeners were used: HPC-8000-65T (DIC Corporation active ester-based curing agent with dicyclopentadiene structure, active ester group equivalent weight 223, non-volatile content 65% by mass in toluene solution) GPH-103 (biphenyl aralkylphenol novolac manufactured by Nippon Kayaku Co., Ltd., hydroxyl equivalent 230, softening point 103°C) Solid GPH-103 was dissolved in methyl ethyl ketone and used as a 50% by mass solution for preparing the resin composition.
[0083] <Curing accelerator> The curing accelerator used was 4-dimethylaminopyridine (DMAP, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.).
[0084] <Phenoxy resin> The phenoxy resin used was YX6954BH30 (a phenoxy resin containing a bisphenol acetophenone skeleton, manufactured by Mitsubishi Chemical Corporation, with a weight average molecular weight of 40670 and a cyclohexanone / methyl ethyl ketone (1 / 1) solution with a non-volatile content of 30% by mass).
[0085] <Measurement of average and maximum particle size of filler> Aluminum nitride filler or alumina filler was dispersed in ethanol in the case of aluminum nitride filler, or in water in the case of alumina filler, at a concentration of 0.2 mass%, and the dispersed samples were irradiated with ultrasonic waves at about 200 W for 2 minutes to measure particle size distribution using a laser diffraction scattering type particle size distribution meter (MICROTRACK-MT3300EXII, manufactured by Microtrack Bell Co., Ltd.). In the volume frequency distribution of particle sizes obtained (particle size distribution), the volume frequency was accumulated from the smallest particle size, and the particle size D50 at which the accumulated value reached 50% was defined as the average particle size, and the maximum value Dmax of the measured particle sizes was defined as the maximum particle size.
[0086] <Measurement of the specific surface area of filler> The specific surface area of the aluminum nitride filler and the alumina filler was determined by the BET method (single-point nitrogen adsorption method) using a flow-type automatic specific surface area measuring device (Shimadzu Corporation: Flowsorb II-2300). For the measurement, 2 g of powder sample was used, which was previously dried at 100°C for 1 hour in a nitrogen gas flow.
[0087] <Measurement of minimum melt viscosity> The resin composition films prepared in the examples and comparative examples were peeled off from the polyethylene terephthalate film support, and the melt viscosity was measured using a viscoelasticity measuring device (rotational rheometer) (Anton Paar: MCR302e). A parallel plate with a diameter of 10 mm was used for the geometry, and dynamic viscoelasticity was measured at a gap of 1 mm, a temperature range of 60°C to 180°C, a frequency of 1 Hz, and a strain of 10%, and the minimum value of the complex viscosity in the range of 90 to 140°C was taken as the minimum melt viscosity.
[0088] <Measurement of linear expansion coefficient> The resin composition films prepared in the examples and comparative examples were cut into strips with a width of 5 mm and heat-treated at 180°C for 90 minutes to be thermally cured. The obtained cured products were measured twice consecutively by the tensile load method using a thermomechanical analyzer (NETZSCH: TMA4000SE) with a sample length (between chucks) of 20 mm, a load of 1 g, and a heating rate of 5°C / min from 30°C to 220°C. The linear expansion coefficient was calculated from the slope of the change in linear expansion coefficient from 30°C to the glass transition temperature (the temperature at which the slope of the TMA curve changes) in the second measurement result.
[0089] <Measurement of thermal conductivity> The resin composition films prepared in the examples and comparative examples were heat-cured at 180°C for 90 minutes. The thermal conductivity (W / m K) of the obtained cured products was 2 / sec) x density (kg / m 3) × specific heat (J / kg K). Thermal diffusivity was measured by temperature wave thermal analysis (ai-Phase Mobile 1u, ISO22007-3, manufactured by Ai-Phase Corporation). The same test piece was measured 12 times and the average value was used. Density was measured using the Archimedes method (XS204V, manufactured by Mettler Toledo Corporation), and specific heat was measured using a differential scanning calorimeter (DSC) method (Thermo Plus Evo DSC8230, manufactured by Rigaku Corporation).
[0090] <Relative density measurement> The relative density of the cured product was calculated as the ratio of the actual density measured above to the theoretical density calculated by calculation, i.e., actual value / theoretical value. Here, the theoretical density was calculated by assuming the density of the aluminum nitride filler, alumina filler, and the remaining components excluding the filler component to be 3.26 g / m 3 , 3.98g / m 3 , 1.17g / m 3 was calculated from the blending ratio of each component.
[0091] Example 1 (A-2) 50 parts by mass of liquid epoxy resin jER828, 135 parts by mass of hardener HPC-8000-65T (87.8 parts by mass as non-volatile content), 33 parts by mass of phenoxy resin YL6954BH30 (9.9 parts by mass as non-volatile content), 0.8 parts by mass of hardening accelerator DMAP, and 430 parts by mass of (C) alumina filler AA-03F were stirred and mixed. Thereto, 50 parts by mass of (A-1) solid epoxy resin NC3000 as non-volatile content (100 parts by mass as adjusted methyl ethyl ketone solution), 740 parts by mass of (B) aluminum nitride filler B-1, and 300 parts by mass of methyl ethyl ketone were added and stirred for 30 minutes using a homodisper, and then kneaded using a three-roll mill. Furthermore, methyl ethyl ketone was appropriately added to adjust the viscosity, and then filtered and defoamed to prepare a varnish of the resin composition. Next, the resin composition varnish obtained above was uniformly applied to the release-treated surface of a support (release-treated polyethylene terephthalate film (Higashiyama Film Co., Ltd., HY-NS80, thickness 38 μm)) so that the thickness after drying would be 80 μm, and dried at 80° C. for 3 minutes to produce a resin composition film (B stage). The composition of the resin composition film and the evaluation results are shown in Table 1.
[0092] [Examples 2 to 19, Comparative Examples 1 to 8] A resin composition film was produced in the same manner as in Example 1, except that the composition of the resin composition film was changed as shown in Tables 1 and 2. The composition and evaluation results of the resin composition film are shown in Tables 1 and 2.
[0093] [Table 1]
[0094] [Table 2]
[0095] In the resin compositions of Examples 1 to 19, which use a combination of aluminum nitride filler and alumina filler, it was confirmed that the filling and dispersibility of the filler are good, the melt viscosity and linear expansion coefficient of the film are low, and the thermal conductivity and relative density are high. In particular, in Examples 1 to 4, 6, 8, 10, and 12 to 19, in which the ratio S2 / S1 of the total surface area of the aluminum nitride filler to the alumina filler is in the range of 0.5 to 2.2, a resin composition film with high thermal conductivity is obtained.
[0096] If the total amount of aluminum nitride filler and alumina filler is too large (Comparative Example 2), the filling property of the filler decreases, so the melt viscosity increases and the relative density also decreases. As a result, the thermal conductivity also starts to decrease. If the total amount of the filler is too small (Comparative Example 1), the melt viscosity decreases, but the thermal conductivity is insufficient and the linear expansion coefficient also increases. If only aluminum nitride filler is used without blending alumina filler (Comparative Examples 3 to 6), the filling property of the filler decreases, so the melt viscosity increases, and the relative density and thermal conductivity also decrease. In the case of aluminum nitride filler with a large maximum particle size Dmax (Comparative Examples 3, 5, and 7), the melt viscosity increases. If the average particle size of the alumina filler is large (Comparative Example 8), the melt viscosity increases and the thermal conductivity decreases.
Claims
1. (A) an epoxy resin, (B) an aluminum nitride filler, and (C) an alumina filler, the total amount of the aluminum nitride filler (B) and the alumina filler (C) is 800 to 1500 parts by mass relative to 100 parts by mass of the epoxy resin (A); The epoxy resin (A) includes a solid epoxy resin (A-1) and a liquid epoxy resin (A-2), The aluminum nitride filler (B) has an average particle size D50 of 0.2 to 3 μm and a maximum particle size Dmax of 5 μm or less, The (C) alumina filler has an average particle size D50 of 0.05 to 1.5 μm. Resin composition.
2. The aluminum nitride filler (B) has a specific surface area of 0.5 to 10 m 2 / g, The alumina filler (C) has a specific surface area of 1 to 50 m 2 / g, a ratio S2 / S1 of a total surface area S1 of the aluminum nitride filler (B) to a total surface area S2 of the alumina filler (C) is 0.5 to 2.2; The resin composition according to claim 1.
3. A resin composition film comprising the resin composition according to claim 1 or 2.
4. A multilayer printed wiring board comprising the resin composition according to claim 1 or 2 or a cured product thereof.
5. A component-embedded substrate comprising the resin composition according to claim 1 or 2 or a cured product thereof.
Citation Information
Patent Citations
Epoxy resin composition
JP2011132507A
Resin composition
WO2014208352A1