Multilayer electronic component

By integrating gallium into the dielectric material and side margin sections of multilayer ceramic capacitors, the issues of pore formation and moisture penetration are mitigated, enhancing reliability and electrical performance.

JP2024163851APending Publication Date: 2024-11-22SAMSUNG ELECTRO MECHANICS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024039923
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-08-22
Filing Date
2024-03-14
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing multilayer ceramic capacitors face issues with reduced reliability due to pore formation, moisture penetration, and electric field concentration, which affect dielectric breakdown voltage and moisture resistance, especially when manufactured with side margin parts using conventional ceramic materials.

Method used

Incorporating gallium (Ga) into the dielectric material and side margin sections of multilayer electronic components, along with controlled firing processes, to suppress pore formation and enhance moisture resistance and electrical properties.

Benefits of technology

The addition of gallium improves moisture resistance reliability and electrical characteristics by reducing pore formation and electric field concentration, allowing for effective operation at lower temperatures and improved dielectric density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024163851000001_ABST
    Figure 2024163851000001_ABST
Patent Text Reader

Abstract

To provide a multilayer electronic component which has high moisture resistance reliability and can alleviate an electrical field concentration phenomenon, even when sintered at a low temperature.SOLUTION: A multilayer electronic component includes: a body 110 including a capacitance forming portion Ac that includes a dielectric layer 11 and an internal electrode (121 and 122) alternately disposed with the dielectric layer in a first direction, and cover portions 112 and 113 that are disposed on both end-surfaces of the capacitance forming portion in the first direction, respectively, and also including a first surface and a second surface opposing each other in the first direction, a third surface and a fourth surface connected to the first surface and the second surface and opposing each other in a second direction, and a fifth surface and a sixth surface connected to the first to fourth surfaces and opposing each other in a third direction; external electrodes disposed on the third and fourth surfaces of the body, respectively; and side margin portions 114 and 115 disposed on the fifth and sixth surfaces of the body, respectively. At least one of the capacitance forming portion, the cover portions, and the side margin portions includes a secondary phase including gallium (Ga).SELECTED DRAWING: Figure 6
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a multilayer electronic component. [Background technology]

[0002] Multi-Layered Ceramic Capacitor (MLCC), a type of multi-layered electronic component, is a chip-type capacitor that is mounted on the printed circuit boards of various electronic products such as visual devices such as liquid crystal displays (LCDs) and plasma display panels (PDPs), computers, smartphones, and mobile phones to charge and discharge electricity.

[0003] Such multilayer ceramic capacitors have the advantages of being small yet high capacitance and easy to mount, and can be used as components of various electronic devices. As various electronic devices such as computers and mobile devices become smaller and have higher output, there is an increasing demand for multilayer ceramic capacitors to be smaller and have higher capacitance.

[0004] In order to miniaturize and increase the capacity of multilayer ceramic capacitors, it is necessary to maximize the effective electrode area (increase the effective volume fraction required to achieve capacity). In order to realize a small-sized and high-capacity multilayer ceramic capacitor as described above, when manufacturing a multilayer ceramic capacitor, the internal electrodes are exposed in the width direction of the body, thereby maximizing the area of ​​the internal electrodes in the width direction through a margin-free design. In this case, a ceramic green sheet for the side margin is separately attached to the electrode exposed surface in the width direction of the body before firing after the body is manufactured, and then sintered.

[0005] By forming the side margin by separately attaching a ceramic green sheet for the side margin, the capacitance per unit volume of the capacitor can be improved. However, problems such as shortened chip life and defects can occur due to the penetration of moisture from the outside through the interfacial bond between the main body and the side margin, or the penetration of plating solution during the plating process. Development to solve these problems is required.

[0006] More specifically, during the process of forming the side margin, many pores are generated at the interface where the main body and the side margin come into contact, which may reduce reliability, and the pores may cause electric field concentration, which may result in a problem of a lower breakdown voltage (BDV).In addition, as an interface bond occurs at the boundary between the main body and the side margin, the bonding strength may decrease and the moisture resistance reliability may decrease, or the pores may reduce the sintering density, which may reduce moisture resistance reliability. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Japanese Patent Publication No. 2022-068525 [Patent Document 2] Japanese Patent Publication No. 2006-062937 Summary of the Invention [Problem to be solved by the invention]

[0008] One of the various problems that the present invention aims to solve is to provide a multilayer electronic component having a dielectric material with excellent density even when fired at a low temperature.

[0009] One of the various problems that the present invention aims to solve is to provide a multilayer electronic component having a reduced number of pores and improved moisture resistance reliability.

[0010] One of the various problems to be solved by the present invention is to provide a multilayer electronic component with improved electrical characteristics by reducing the size of dielectric crystal grains and alleviating the electric field concentration phenomenon.

[0011] However, the various problems to be solved by the present invention are not limited to the above-described content, and can be more easily understood in the process of explaining specific embodiments of the present invention.

Means for Solving the Problems

[0012] A multilayer electronic component according to an embodiment of the present invention includes a dielectric layer, a capacitance forming portion including internal electrodes alternately arranged with the dielectric layer in a first direction, and cover portions arranged on both end surfaces in the first direction of the capacitance forming portion, and includes a main body including a first surface and a second surface facing each other in the first direction, a third surface and a fourth surface facing each other in a second direction connected to the first surface and the second surface, a fifth surface and a sixth surface facing each other in a third direction connected from the first surface to the fourth surface, external electrodes arranged on the third surface and the fourth surface of the main body, and side margin portions arranged on the fifth surface and the sixth surface of the main body, and at least one of the capacitance forming portion, the cover portion, and the side margin portion can include a secondary phase containing gallium (Ga).

[0013] A multilayer electronic component according to an embodiment of the present invention includes a dielectric layer, a capacitance forming portion including internal electrodes alternately arranged with the dielectric layer in a first direction, a main body including a first surface and a second surface facing each other in the first direction, a third surface and a fourth surface facing each other in a second direction connected to the first surface and the second surface, a fifth surface and a sixth surface facing each other in a third direction connected from the first surface to the fourth surface, external electrodes arranged on the third surface and the fourth surface of the main body, and side margin portions arranged on the fifth surface and the sixth surface of the main body. When the number of moles of gallium (Ga) with respect to 100 moles of titanium (Ti) contained in the side margin portion is defined as MG, and the number of moles of gallium (Ga) with respect to 100 moles of titanium (Ti) contained in the capacitance forming portion is defined as AG, 0 < MG and 0 ≤ AG ≤ MG can be satisfied. Effect of the Invention

[0014] One of the effects of the present invention is that the multilayer electronic component has excellent density even when fired at a low temperature.

[0015] One of the advantages of the present invention is that the number of pores in the multilayer electronic component is reduced, improving the moisture resistance reliability.

[0016] One of the advantages of the present invention is that the size of the dielectric crystal grains is small, thereby alleviating the electric field concentration phenomenon and improving the electrical characteristics of the multilayer electronic component.

[0017] However, the various yet significant advantages and effects of the present invention are not limited to the above, and can be more easily understood in the course of describing specific embodiments of the present invention. [Brief description of the drawings]

[0018] [Figure 1] 1 is a schematic perspective view of a multilayer electronic component according to an embodiment of the present invention; [Diagram 2] 2 is a schematic perspective view of the multilayer electronic component of FIG. 1 with external electrodes removed. [Diagram 3] 2 is a schematic perspective view of the multilayer electronic component of FIG. 1 with external electrodes and side margins removed. [Figure 4] 2 is a schematic exploded perspective view showing a laminated structure of internal electrodes; FIG. [Diagram 5] 2 is a schematic cross-sectional view taken along line II' of FIG. 1. [Figure 6] 2 is a schematic cross-sectional view taken along line II-II' in FIG. 1. [Figure 7] 1 is a schematic representation of a dielectric microstructure. [Figure 8](a) is an image of the side margin taken with a transmission electron microscope (TEM) in HAADF mode, (b) is an image of the same area analyzed by EDS for silicon (Si) and gallium (Ga), and (c) is an image of the same area analyzed by EDS for gallium (Ga). [Figure 9] (a) and (b) are images taken by SEM of region M in Fig. 6. Specifically, (a) is an image taken by SEM of the capacitance forming portion and side margin portion of the comparative example, and (b) is an image taken by SEM of the capacitance forming portion and side margin portion of the example. [Figure 10] 13A is a graph showing the moisture resistance reliability evaluation of the comparative example, and FIG. 13B is a graph showing the moisture resistance reliability evaluation of the example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] Hereinafter, the embodiments of the present invention will be described with reference to specific embodiments and the accompanying drawings. However, the embodiments of the present invention can be modified into several other forms, and the scope of the present invention is not limited to the embodiments described below. Furthermore, the embodiments of the present invention are provided to more completely explain the present invention to those skilled in the art. Therefore, the shapes and sizes of elements in the drawings may be enlarged or reduced (or highlighted or simplified) for clearer explanation, and elements indicated by the same reference numerals in the drawings are the same elements.

[0020] In addition, in the drawings, parts that are not relevant to the description are omitted in order to clearly explain the present invention, and the size and thickness of each component shown in the drawings are arbitrarily shown for convenience of explanation, so the present invention is not necessarily limited by the drawings. Furthermore, components having the same function within the same concept may be described using the same reference numerals. Furthermore, throughout the specification, when a part "includes" a certain component, it does not mean that the part excludes other components, but that the part may further include other components, unless otherwise specified to the contrary.

[0021] In the drawings, the first direction can be defined as the stacking direction or thickness (T) direction, the second direction can be defined as the length (L) direction, and the third direction can be defined as the width (W) direction.

[0022] Multilayer Electronic Components FIG. 1 is a schematic perspective view of a multilayer electronic component according to one embodiment of the present invention, FIG. 2 is a schematic perspective view of the multilayer electronic component of FIG. 1 excluding external electrodes, FIG. 3 is a schematic perspective view of the multilayer electronic component of FIG. 1 excluding external electrodes and side margin portions, FIG. 4 is a schematic separated perspective view showing the laminated structure of internal electrodes, FIG. 5 is a schematic cross-sectional view taken along line I-I' in FIG. 1, FIG. 6 is a schematic cross-sectional view taken along line II-II' in FIG. 1, and FIG. 7 is a schematic view of a dielectric microstructure.

[0023] Hereinafter, a multilayer electronic component according to an embodiment of the present invention will be described in detail with reference to Figures 1 to 7. Although a multilayer ceramic capacitor will be described as an example of a multilayer electronic component, the present invention can also be applied to various electronic products that use a dielectric composition, such as an inductor, a piezoelectric element, a varistor, or a thermistor.

[0024] A stacked electronic component 100 according to an embodiment of the present invention includes a dielectric layer 111, a capacitance forming portion Ac including internal electrodes 121 and 122 alternately arranged with the dielectric layer 111 in a first direction, and cover portions 112 and 113 arranged on both end - surfaces in the first direction of the capacitance forming portion Ac. It includes a main body 110 having a first surface 1 and a second surface 2 facing each other in the first direction, a third surface 3 and a fourth surface 4 facing each other in a second direction and connected to the first surface 1 and the second surface 2, and a fifth surface 5 and a sixth surface 6 facing each other in a third direction and connected to the first surface 1, the second surface 2, the third surface 3, and the fourth surface 4, external electrodes 131 and 132 arranged on the third surface 3 and the fourth surface 4 of the main body 110, and side margin portions 114 and 115 arranged on the fifth surface 5 and the sixth surface 6 of the main body 110. At least one of the capacitance forming portion Ac, the cover portions 112 and 113, and the side margin portions 114 and 115 can include a secondary phase 20 containing gallium (Ga).

[0025] A stacked electronic component 100 according to another embodiment of the present invention includes a dielectric layer 111, a capacitance forming portion Ac including internal electrodes 121 and 122 alternately arranged with the dielectric layer 111 in a first direction, a main body 110 having a first surface 1 and a second surface 2 facing each other in the first direction, a third surface 3 and a fourth surface 4 facing each other in a second direction and connected to the first surface 1 and the second surface 2, and a fifth surface 5 and a sixth surface 6 facing each other in a third direction and connected to the first surface 1, the second surface 2, the third surface 3, and the fourth surface 4, external electrodes 131 and 132 arranged on the third surface 3 and the fourth surface 4 of the main body 110, and side margin portions 114 and 115 arranged on the fifth surface 5 and the sixth surface 6 of the main body 110. When the number of moles of gallium (Ga) per 100 moles of titanium (Ti) contained in the side margin portions 114 and 115 is defined as MG, and the number of moles of gallium (Ga) per 100 moles of titanium (Ti) contained in the capacitance forming portion Ac is defined as AG, 0 < MG and 0 ≤ AG ≤ MG can be satisfied.

[0026] In the main body 110, the dielectric layer 111 and the internal electrodes 121 and 122 can be alternately laminated.

[0027] More specifically, the main body 110 may include a capacitance forming portion Ac disposed inside the main body 110 and including a dielectric layer 111 and a first internal electrode 121 and a second internal electrode 122 alternately arranged facing each other across the dielectric layer 111 to form a capacitance.

[0028] Although there is no particular limitation on the specific shape of the body 110, the body 110 may be hexahedral or a similar shape as shown in the drawing. Due to shrinkage of ceramic particles contained in the body 110 during the firing process, the body 110 may not be a hexahedral shape with perfectly straight lines, but may be substantially hexahedral.

[0029] The main body 110 may have a first surface 1 and a second surface 2 facing each other in a first direction, a third surface 3 and a fourth surface 4 connected to the first surface 1 and the second surface 2 and facing each other in the second direction, and a fifth surface 5 and a sixth surface 6 connected to the first surface 1, the second surface 2, the third surface 3, and the fourth surface 4 and facing each other in the third direction.

[0030] The multiple dielectric layers 111 forming the body 110 are in a fired state, and the boundaries between adjacent dielectric layers 111 can be integrated to such an extent that they are difficult to see without the use of a scanning electron microscope (SEM).

[0031] The raw material for forming the dielectric layer 111 is not limited as long as a sufficient electrostatic capacitance can be obtained. In general, a perovskite (ABO3)-based material can be used, such as a barium titanate-based material, a lead complex perovskite-based material, or a strontium titanate-based material. The barium titanate-based material can include BaTiO3-based ceramic particles, and examples of the ceramic particles include BaTiO3, BaTiO3 partially solid-dissolved with Ca (calcium), Zr (zirconium), etc. 1-x Ca x )TiO3(0 <x<1)、Ba(Ti 1-y Ca y )O3(0 <y<1)、(Ba 1-x Cax )(Ti 1-y Zr y )O3 (0 < x < 1, 0 < y < 1) or Ba(Ti 1-y Zr y )O3 (0 < y < 1), etc. can be mentioned.

[0032] In addition, as raw materials for forming the dielectric layer 111, various ceramic additives, organic solvents, binders, dispersants, etc. can be added to particles such as barium titanate (BaTiO3) according to the purpose of the present invention.

[0033] In addition, since the dielectric layer 111 can be formed using a dielectric material such as barium titanate (BaTiO3), it can include a dielectric microstructure after firing. The dielectric microstructure includes a plurality of crystal grains 11 and grain boundaries 12 disposed between adjacent crystal grains 11, and can include a plurality of triple points 13 at which three or more grain boundaries 12 meet.

[0034] The thickness td of the dielectric layer 111 does not particularly need to be limited.

[0035] However, in order to more easily achieve miniaturization and high capacitance of the multilayer electronic component, the thickness of the dielectric layer 111 can be 0.6 μm or less, and more preferably 0.4 μm or less.

[0036] Here, the thickness td of the dielectric layer 111 can mean the thickness td of the dielectric layer 111 disposed between the first internal electrode 121 and the second internal electrode 122.

[0037] On the other hand, the thickness td of the dielectric layer 111 can mean the size of the dielectric layer 111 in the first direction. Also, the thickness td of the dielectric layer 111 can mean the average thickness td of the dielectric layer 111 and can mean the average size of the dielectric layer 111 in the first direction.

[0038] The average size in the first direction of the dielectric layer 111 may be measured by scanning an image of a cross-section in the first and second directions of the body 110 with a scanning electron microscope (SEM) at a magnification of 10,000. More specifically, the average size in the first direction of one dielectric layer 111 may mean an average value calculated by measuring the size in the first direction at 30 equally spaced points in the second direction of one dielectric layer 111 from the scanned image. The 30 equally spaced points may be designated as the capacitance forming portion Ac. Furthermore, if such an average value measurement is extended to 10 dielectric layers 111 to measure the average value, the average size in the first direction of the dielectric layer 111 may be further generalized.

[0039] The internal electrodes 121 and 122 may be laminated alternately with the dielectric layers 111 .

[0040] The internal electrodes 121, 122 may include a first internal electrode 121 and a second internal electrode 122, and the first internal electrode 121 and the second internal electrode 122 are alternately arranged to face each other across the dielectric layer 111 that constitutes the main body 110, and may be exposed to the third surface 3 and the fourth surface 4 of the main body 110, respectively.

[0041] More specifically, the first internal electrode 121 may be spaced apart from the fourth surface 4 and exposed through the third surface 3, and the second internal electrode 122 may be spaced apart from the third surface 3 and exposed through the fourth surface 4. A first external electrode 131 may be disposed on the third surface 3 of the body 110 and connected to the first internal electrode 121, and a second external electrode 132 may be disposed on the fourth surface 4 of the body 110 and connected to the second internal electrode 122.

[0042] That is, the first internal electrode 121 may be connected to the first external electrode 131 without being connected to the second external electrode 132, and the second internal electrode 122 may be connected to the second external electrode 132 without being connected to the first external electrode 131. In this case, the first internal electrode 121 and the second internal electrode 122 may be electrically isolated from each other by the dielectric layer 111 disposed therebetween.

[0043] Meanwhile, the body 110 may be formed by alternately stacking ceramic green sheets on which the first internal electrodes 121 are printed and ceramic green sheets on which the second internal electrodes 122 are printed, and then firing the stacked ceramic green sheets.

[0044] There are no particular limitations on the material forming the internal electrodes 121 and 122, and any material having excellent electrical conductivity can be used. For example, the internal electrodes 121 and 122 may include one or more of nickel (Ni), copper (Cu), palladium (Pd), silver (Ag), gold (Au), platinum (Pt), tin (Sn), tungsten (W), titanium (Ti), and alloys thereof.

[0045] The internal electrodes 121 and 122 may be formed by printing a conductive paste for internal electrodes, which contains at least one of nickel (Ni), copper (Cu), palladium (Pd), silver (Ag), gold (Au), platinum (Pt), tin (Sn), tungsten (W), titanium (Ti), and alloys thereof, on a ceramic green sheet. The method for printing the conductive paste for internal electrodes may be a screen printing method or a gravure printing method, but the present invention is not limited thereto.

[0046] On the other hand, the thickness te of the internal electrodes 121 and 122 does not need to be particularly limited.

[0047] However, in order to more easily achieve miniaturization and high capacity of the multilayer electronic component, the thickness of the internal electrodes 121, 122 can be 0.6 μm or less, and more preferably 0.4 μm or less.

[0048] Here, the thickness te of the internal electrodes 121, 122 may refer to the size of the internal electrodes 121, 122 in the first direction. In addition, the thickness te of the internal electrodes 121, 122 may refer to the average thickness te of the internal electrodes 121, 122, or may refer to the average size of the internal electrodes 121, 122 in the first direction.

[0049] The average size of the internal electrodes 121, 122 in the first direction may be measured by scanning an image of a cross-section of the body 110 in the first and second directions with a scanning electron microscope (SEM) at a magnification of 10,000. More specifically, the average size of one internal electrode in the first direction may be an average value calculated by measuring the size of one internal electrode in the first direction at 30 equally spaced points in the second direction from the scanned image. The 30 equally spaced points may be designated as the capacitance forming portion Ac. Furthermore, if such an average value measurement is extended to 10 internal electrodes 121, 122 to measure the average value, the average size of the internal electrodes 121, 122 in the first direction may be further generalized.

[0050] Meanwhile, the body 110 may include cover portions 112 and 113 disposed on both end surfaces in the first direction of the capacitance forming portion Ac.

[0051] More specifically, it may include an upper cover part 112 disposed on an upper part of the capacitance forming part Ac in the first direction, and a lower cover part 113 disposed on a lower part of the capacitance forming part Ac in the first direction.

[0052] The upper cover part 112 and the lower cover part 113 may be formed by stacking a single dielectric layer or two or more dielectric layers in a first direction on the upper and lower surfaces of the capacitance forming part Ac, respectively, and may basically serve to prevent damage to the internal electrodes 121, 122 due to physical or chemical stress.

[0053] The upper cover part 112 and the lower cover part 113 do not include the internal electrodes 121, 122 and may include the same material as the dielectric layer 111 of the capacitance forming part Ac, but may have a different composition from that of the dielectric layer 111 of the capacitance forming part Ac. That is, the upper cover part 112 and the lower cover part 113 may include a ceramic material, for example, a barium titanate (BaTiO3)-based ceramic material.

[0054] In addition, the cover portions 112, 113 may be formed using a dielectric material such as barium titanate (BaTiO3), and may include a dielectric microstructure after firing. The dielectric microstructure may include a plurality of crystal grains 11 and crystal grain boundaries 12 disposed between adjacent crystal grains 11, and may include a triple point 13, which is a point where three or more crystal grain boundaries 12 meet.

[0055] On the other hand, the thickness tc of the covers 112 and 113 does not need to be particularly limited.

[0056] However, in order to more easily achieve miniaturization and high capacity of the multilayer electronic component, the thickness tc of the cover parts 112, 113 can be 100 μm or less, preferably 30 μm or less, and more preferably 20 μm or less for ultra-small products.

[0057] Here, the thickness tc of the cover parts 112, 113 may refer to the size of the cover parts 112, 113 in the first direction. In addition, the thickness tc of the cover parts 112, 113 may refer to the average thickness tc of the cover parts 112, 113, or may refer to the average size of the cover parts 112, 113 in the first direction.

[0058] The average size in the first direction of the covers 112 and 113 may be measured by scanning an image of a cross section in the first and second directions of the body 110 with a scanning electron microscope (SEM) at a magnification of 10,000. More specifically, the average size in the first direction may be calculated by measuring the size in the first direction at 30 points equally spaced in the second direction from an image obtained by scanning one cover.

[0059] In addition, the average size of the cover portion in the first direction measured by the above-mentioned method may be substantially the same as the average size of the cover portion in the first direction in cross-sections of the body 110 in the first and third directions.

[0060] Meanwhile, side margin parts 114 and 115 may be disposed on both end surfaces of the body 110 in the third direction.

[0061] More specifically, the side margin portions 114, 115 may include a first side margin portion 114 disposed on the fifth surface 5 of the main body 110 and a second side margin portion 115 disposed on the sixth surface 6. That is, the side margin portions 114, 115 may be disposed on both end surfaces of the main body 110 in the third direction.

[0062] As shown in the figure, the side margin portions 114, 115 may refer to the areas between both ends of the first internal electrode 121 and the second internal electrode 122 in the third direction and the boundary surface of the body 110, based on the cross-sections in the first and third directions of the body 110.

[0063] The side margins 114 and 115 essentially serve to prevent damage to the internal electrodes 121 and 122 due to physical or chemical stress.

[0064] The side margin portions 114, 115 can also be formed by forming internal electrodes 121, 122 by applying a conductive paste to the ceramic green sheet except for the areas where the side margin portions 114, 115 are to be formed, and then cutting the laminated internal electrodes 121, 122 so that they are exposed on the fifth surface 5 and the sixth surface 6 of the main body 110 in order to suppress steps caused by the internal electrodes 121, 122, and then stacking a single dielectric layer 111 or two or more dielectric layers 111 in the third direction on both end surfaces in the third direction of the capacitance forming portion Ac.

[0065] The first side margin portion 114 and the second side margin portion 115 do not include the internal electrodes 121, 122 and may include the same material as the dielectric layer 111 of the capacitance forming portion Ac, but may have a different composition from that of the dielectric layer 111 of the capacitance forming portion Ac. That is, the first side margin portion 114 and the second side margin portion 115 may include a ceramic material, for example, a barium titanate (BaTiO3)-based ceramic material.

[0066] In addition, the side margins 114, 115 may be formed using a dielectric material such as barium titanate (BaTiO3), and may include a dielectric microstructure after firing. The dielectric microstructure may include a plurality of crystal grains 11 and crystal grain boundaries 12 disposed between adjacent crystal grains 11, and may include a triple point 13, which is a point where three or more crystal grain boundaries 12 meet.

[0067] On the other hand, the width wm of the first side margin portion 114 and the second side margin portion 115 does not need to be particularly limited.

[0068] However, in order to more easily achieve miniaturization and high capacity of the laminated electronic component 100, the width wm of the first side margin portion 114 and the second side margin portion 115 can be 100 μm or less, preferably 30 μm or less, and for ultra-small products, more preferably 20 μm or less.

[0069] Here, the width wm of the side margin portions 114, 115 may refer to the size in the third direction of each of the side margin portions 114, 115. In addition, the width wm of the side margin portions 114, 115 may refer to the average width wm of the side margin portions 114, 115, or may refer to the average size in the third direction of the side margin portions 114, 115.

[0070] The average size in the third direction of the side margin portions 114, 115 may be measured by scanning an image of a cross-section in the first and third directions of the multilayer electronic component 100 with a scanning electron microscope (SEM) at a magnification of 10,000. More specifically, it may refer to an average value calculated by measuring the size in the third direction at 10 points equally spaced in the first direction from an image obtained by scanning one side margin portion.

[0071] Meanwhile, in order to miniaturize and increase the capacity of a multilayer ceramic capacitor, it is necessary to maximize the effective area of ​​the electrodes (increase the effective volume fraction required to realize the capacity). In order to realize a small-sized and high-capacity multilayer ceramic capacitor as described above, in manufacturing a multilayer ceramic capacitor, the internal electrodes are exposed in the width direction of the body, and the area of ​​the internal electrodes in the width direction is maximized by a margin-free design. In this case, a ceramic green sheet for the side margin is separately attached to the electrode exposed surface in the width direction of the body before firing after the body is manufactured, and then sintered.

[0072] Although the capacitance per unit volume of the capacitor can be improved by forming the side margin by separately attaching a ceramic green sheet for the side margin, problems such as shortened chip life and defects can occur due to the penetration of moisture from the outside through the interface joint between the body and the side margin or the penetration of plating solution during the plating process. Therefore, development to solve these problems is required.

[0073] More specifically, during the process of forming the side margin, many pores may be generated at the interface where the main body and the side margin come into contact, which may reduce reliability, and the pores may cause electric field concentration, which may result in a problem of a lower breakdown voltage (BDV).In addition, as an interface bond occurs at the boundary between the main body and the side margin, the bonding strength may decrease and the moisture resistance reliability may decrease, and the pores may reduce the sintering density, which may result in a decrease in moisture resistance reliability.

[0074] Development is underway to improve the density of the side margins in order to improve the reliability of multilayer electronic components, and the ceramic material currently used for the side margins, barium titanate (BaTiO3) containing tin (Sn), has the effect of reducing the grain size, alleviating electric field concentration and improving electrical characteristics, but it has the problem of increasing pores, which reduces reliability. To solve this problem, research has been conducted to improve the reliability of multilayer electronic components by using low-temperature sintering materials, which are known to lower the sintering temperature of dielectric ceramics, to suppress the generation of pores.

[0075] However, low-temperature sintering materials have low melting points but also low boiling points and are highly volatile. Therefore, during the high-temperature sintering process of electronic components such as MLCCs that are mainly made of ceramics, gasification may occur, causing a side effect of polluting the sintering furnace. In addition, it may be difficult to optimize the process conditions, and the generation of pores may be further promoted.

[0076] Therefore, the multilayer electronic component according to one embodiment of the present invention has an effect of preventing the above-mentioned side effects from occurring even in a low-temperature firing process by including gallium (Ga) in the dielectric material, composition, and dielectric microstructure of crystal grains, etc., used in the multilayer electronic component. In addition, the addition of gallium (Ga) can suppress pore generation, improve moisture resistance reliability, and improve electrical properties or mechanical properties.

[0077] The present invention can be applied to any microstructure in a multilayer electronic component, and is described as an example of a dielectric microstructure, but is not limited thereto. Specifically, the present invention can be applied to the dielectric layer 111 of the body 110, the internal electrodes 121 and 122, and the capacitance forming portion Ac including the margin portion (no reference numeral) in the second direction (length direction) of the end region of the internal electrode not connected to the external electrode, the cover portions 112 and 113, or the side margin portions 114 and 115.

[0078] The capacitance-forming portion Ac described in the present invention does not strictly mean only the area that forms capacitance, but can mean a concept including a longitudinal margin portion (no drawing symbol) of the end area of ​​the internal electrode that is not connected to the external electrode.

[0079] In the multilayer electronic component 100 according to one embodiment of the present invention, at least one of the capacitance forming portion Ac, the cover portions 112, 113, and the side margin portions 114, 115 may include a secondary phase 20 containing gallium (Ga).

[0080] Since at least one of the capacitance forming portion Ac, the cover portions 112, 113, and the side margin portions 114, 115 contains a secondary phase 20 containing gallium (Ga), the generation of pores in the dielectric microstructure contained in at least one of the capacitance forming portion Ac, the cover portions 112, 113, and the side margin portions 114, 115 is suppressed, and the moisture resistance reliability can be improved, or the electrical and mechanical properties can be improved.

[0081] Furthermore, as described above, at least one of the dielectric layer 111, the capacitance forming portion Ac, the cover portions 112, 113, and the side margin portions 114, 115 includes a plurality of crystal grains 11 and crystal grain boundaries 12 arranged between adjacent crystal grains, and at least one of the crystal grains 11 can include gallium (Ga), and at least one of the crystal grain boundaries 12 can include gallium (Ga).

[0082] In the present invention, the term "secondary-phase" may refer to particles or segregation having a different composition from the perovskite-based (ABO3) dielectric particles. Specifically, the atomic percentage (at%) of barium (Ba) in the secondary phase particles may be 30.0 at% or less, the atomic percentage (at%) of titanium (Ti) in the secondary phase particles may be 30.0 at% or less, the atomic percentage (at%) of silicon (Si) in the secondary phase particles may be 15.0 at% or less, the atomic percentage (at%) of aluminum (Al) in the secondary phase particles may be 15.0 at% or less, or the atomic percentage (at%) of gallium (Ga) in the secondary phase particles may be 0.2 at% or more. In addition, the term may refer to particles that satisfy all of the above conditions of the atomic percentages (at%) of barium (Ba), titanium (Ti), silicon (Si), aluminum (Al) and gallium (Ga).

[0083] More specifically, the atomic percentage (at%) of gallium (Ga) contained in the secondary phase 20 may be 0.2 at% or more.

[0084] When the atomic percentage (at%) of gallium (Ga) contained in the secondary phase 20 is 0.2 at% or more, pore generation in the dielectric microstructure is suppressed, and moisture resistance reliability can be improved.

[0085] The upper limit of the atomic percentage (at%) of gallium (Ga) contained in the secondary phase 20 is not particularly limited as long as it is for improving the moisture resistance reliability, but in order to prevent side effects due to the excessive addition of gallium (Ga), it may be preferably 1.0 at% or less, more preferably 0.7 at% or less.

[0086] If the atomic percentage (at%) of gallium (Ga) contained in the secondary phase 20 is less than 0.2 at%, it may not be possible to clearly distinguish it from noise during EDS analysis, or the effect of suppressing pore generation may be slight, resulting in an insufficient effect on improving moisture resistance reliability.

[0087] In the present invention, as a more specific example of a method for measuring the content of elements contained in each component of the multilayer electronic component 100, in the case of a destructive method, the components inside the dielectric crystal grains at the center of the chip can be analyzed using SEM-EDS, TEM-EDS, or STEM-EDS. First, an analysis sample is prepared by thinning a region including a dielectric microstructure in a cross section of a body where sintering is completed using a focused ion beam (FIB) device. Then, the thinned sample is subjected to argon (Ar) ion milling to remove a damaged layer on the surface, and then each component is mapped from an image obtained using SEM-EDS, TEM-EDS, or STEM-EDS to perform qualitative / quantitative analysis. In this case, the qualitative / quantitative analysis graph of each component can be expressed by converting each element into mass percentage (wt%), atomic percentage (at%), or molar percentage (mol%).

[0088] As another method, the chip can be crushed to select the area containing the dielectric microstructure, and the components of the area containing the dielectric microstructure can be analyzed using devices such as an inductively coupled plasma optical emission spectrometer (ICP-OES) or an inductively coupled plasma mass spectrometer (ICP-MS).

[0089] Alternatively, the secondary phase 20 may comprise glass, for example, silicon (Si) based glass, or may comprise aluminum (Al)-silicon (Si) based glass.

[0090] By including glass in the secondary phase 20, the secondary phase 20 can be more easily formed from glass, and elements other than gallium (Ga) can be included in the secondary phase 20 without being dissolved in the barium titanate (BaTiO3)-based dielectric material.

[0091] More specifically, the secondary phase 20 may further include other elements besides gallium (Ga).

[0092] For example, the low-temperature sintering aid may further include at least one of lithium (Li), sodium (Na), potassium (K), rubidium (Rb) and cesium (Cs) in addition to gallium (Ga). Low-temperature sintering aids other than gallium (Ga) are highly volatile and may not be easily detected in the final product, and may contaminate the sintering furnace during the manufacturing process. However, the above-mentioned problems can be minimized by controlling the sintering atmosphere and temperature conditions, and they can be detected using X-ray diffraction (XRD) analysis equipment, so at least one of lithium (Li), sodium (Na), potassium (K), rubidium (Rb) and cesium (Cs) may be further added as necessary.

[0093] Furthermore, when the secondary phase 20 is a glassy secondary phase, it may further contain silicon (Si) or may further contain aluminum (Al).

[0094] When the secondary phase 20 contains silicon (Si), the atomic percentage (at%) of silicon (Si) contained in the secondary phase 20 may be 15.0 at% or less, and preferably 13.4 at% or less.

[0095] In the case where the secondary phase 20 contains aluminum (Al), the atomic percentage (at%) of aluminum (Al) contained in the secondary phase 20 may be 15.0 at% or less, and preferably 11.2 at% or less.

[0096] In addition, other minor components may be further included, including, but not limited to, at least one of tin (Sn), magnesium (Mg), vanadium (V), manganese (Mn), zirconium (Zr), titanium (Ti), barium (Ba), and rare earth elements.

[0097] Here, the rare earth elements can be at least one of lanthanum (La), yttrium (Y), actinium (Ac), cerium (Ce), praseodymium (Pr), neodymium (Nd), promethium (Pm), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), and ruthenium (Lu).

[0098] More specifically, the ratio of the atomic percentage (at%) of gallium (Ga) to the atomic percentage (at%) of silicon (Si) contained in the secondary phase 20 may be 3.94% or more.

[0099] By satisfying the ratio of the atomic percentage (at%) of gallium (Ga) to the atomic percentage (at%) of silicon (Si) contained in the secondary phase 20 being 3.94% or more, the generation of pores in the dielectric microstructure is suppressed, and the moisture resistance reliability can be improved.

[0100] The upper limit of the ratio of the atomic percentage (at%) of gallium (Ga) to the atomic percentage (at%) of silicon (Si) contained in the secondary phase 20 is not particularly limited, but may be 8.00% or less, and preferably 7.21% or less.

[0101] If the ratio of the atomic percentage (at%) of gallium (Ga) to the atomic percentage (at%) of silicon (Si) contained in the secondary phase 20 is less than 3.94%, the effect of suppressing pore formation is slight, and the effect of improving moisture resistance reliability may not be excellent.

[0102] Also, as mentioned above, the secondary phase 20 can include tin (Sn).

[0103] At this time, the atomic percentage (at%) of tin (Sn) contained in the secondary phase 20 may be 0.3 at% or less.

[0104] When the atomic percentage (at%) of tin (Sn) contained in the secondary phase 20 is 0.3 at% or less, it is easy to control the size of the crystal grains 11, and the reduction in the size of the crystal grains 11 reduces electric field concentration, improving electrical characteristics and / or mechanical characteristics.

[0105] If the atomic percentage (at%) of tin (Sn) contained in the secondary phase 20 exceeds 0.3 at%, excessive pores may be generated, resulting in a decrease in moisture resistance reliability.

[0106] In one embodiment of the present invention, a secondary phase 20 may be located at at least one triple point 13 .

[0107] However, the secondary phase 20 is not limited to being located at the at least one triple point 13, but may also be located at the at least one grain boundary 12 or at least one grain 11.

[0108] In one embodiment of the present invention, the side margins 114, 115 may include gallium (Ga).

[0109] This does not only mean that the secondary phase 20 contained in the side margin portions 114, 115 contains gallium (Ga), but can mean that the dielectric microstructure of the side margin portions 114, 115, for example, at least one crystal grain 11, at least one crystal grain boundary 12, or at least one triple point 13, contains gallium (Ga).

[0110] More specifically, the number of moles of gallium (Ga) per 100 moles of titanium (Ti) contained in the side margin portions 114 and 115 may be 0.1 moles or more.

[0111] When the number of moles of gallium (Ga) per 100 moles of titanium (Ti) contained in the side margin portions 114 and 115 is 0.1 moles or more, the generation of pores in the dielectric microstructure contained in the side margin portions 114 and 115 can be suppressed, thereby improving the moisture resistance reliability.

[0112] The upper limit of the number of moles of gallium (Ga) per 100 moles of titanium (Ti) contained in the side margin portions 114 and 115 is not particularly limited as long as it is for the purpose of improving moisture resistance reliability, but in order to prevent side effects such as a decrease in dielectric breakdown voltage (BDV) due to the excessive addition of gallium (Ga), the upper limit of the number of moles of gallium (Ga) may be 3.0 moles or less, and preferably 2.0 moles or less.

[0113] If the mole number of gallium (Ga) per 100 moles of titanium (Ti) contained in the side margin portions 114, 115 is less than 0.1 moles, the effect of suppressing pore formation may be slight, and the effect of improving moisture resistance reliability may not be excellent.

[0114] The side margins 114, 115 may further contain elements other than gallium (Ga).

[0115] For example, the low-temperature sintering aid may further include at least one of lithium (Li), sodium (Na), potassium (K), rubidium (Rb), and cesium (Cs) in addition to gallium (Ga). Low-temperature sintering aids other than gallium (Ga) are highly volatile and may not be easily detected in the final product, and may contaminate the sintering furnace during the manufacturing process. However, the above-mentioned problems can be minimized by controlling the sintering atmosphere and temperature conditions, and they can be detected using EDS analysis or X-ray diffraction (XRD) analysis equipment, so at least one low-temperature sintering aid of lithium (Li), sodium (Na), potassium (K), rubidium (Rb), and cesium (Cs) may be further added as necessary.

[0116] The side margins 114 and 115 may further include silicon (Si) or aluminum (Al), and may further include other minor components including, but not limited to, at least one of tin (Sn), magnesium (Mg), vanadium (V), manganese (Mn), zirconium (Zr), titanium (Ti), barium (Ba), and rare earth elements.

[0117] Here, the rare earth elements can be at least one of lanthanum (La), yttrium (Y), actinium (Ac), cerium (Ce), praseodymium (Pr), neodymium (Nd), promethium (Pm), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), and ruthenium (Lu), and preferably can be one of yttrium (Y), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), and ytterbium (Yb).

[0118] As mentioned above, the side margins 114, 115 may include tin (Sn).

[0119] At this time, the number of moles of tin (Sn) per 100 moles of titanium (Ti) contained in the side margin portions 114 and 115 may be 0.1 moles or more and 5.0 moles or less.

[0120] By satisfying the ratio of moles of tin (Sn) to 100 moles of titanium (Ti) contained in the side margin portions 114, 115 being 0.1 moles or more and 5.0 moles or less, it is easy to control the size of the crystal grains 11, and the size of the crystal grains 11 can be small and the size distribution can be narrowed, so that the moisture resistance reliability can be improved, electrical properties such as the dielectric breakdown voltage (BDV) can be improved, and mechanical properties such as impact resistance or crack resistance can be improved.

[0121] When the number of moles of tin (Sn) relative to 100 moles of titanium (Ti) contained in the side margin portions 114 and 115 is less than 0.1 mole, the effect of improving moisture resistance reliability, electrical characteristics, or mechanical characteristics may be slight. When the number of moles of tin (Sn) exceeds 5.0 moles, sintering of the dielectric powder particles may not proceed due to excessive sintering suppression, and it may be difficult to realize a fine dielectric structure, or the size of the dielectric crystal grains may be small, and there is a risk of deterioration in moisture resistance reliability or mechanical characteristics.

[0122] In the multilayer electronic component 100 according to an embodiment of the present invention, when the number of moles of gallium (Ga) relative to 100 moles of titanium (Ti) contained in the side margin portions 114 and 115 is MG, and the number of moles of gallium (Ga) relative to 100 moles of titanium (Ti) contained in the capacitance forming portion Ac is AG, 0 < MG and 0 ≦ AG ≦ MG can be satisfied.

[0123] Here, the capacitance forming portion Ac can be a concept including the dielectric layer 111, the internal electrodes 121 and 122, and the margin portion (not shown in the drawing code) in the second direction (length direction) of the end region of the internal electrode not connected to the external electrode.

[0124] By adding gallium (Ga) to the side margin portions 114 and 115 (0 < MG), pore generation can be suppressed, and moisture resistance reliability can be improved.

[0125] On the other hand, even if gallium (Ga) is not added to the capacitance forming portion Ac (AG = 0), by adding gallium (Ga) to the side margin portions 114 and 115, penetration of moisture or plating solution from the outside can be effectively prevented.

[0126] Also, when adding gallium (Ga) to the capacitance forming portion Ac (0 < AG), it is obvious that moisture and plating solution penetration from the outside can be more effectively prevented. However, by ensuring that the number of moles of gallium (Ga) relative to 100 moles of titanium (Ti) contained in the capacitance forming portion Ac does not exceed the number of moles of gallium (Ga) relative to 100 moles of titanium (Ti) contained in the side margin portions 114 and 115 (AG ≦ MG), it is possible to prevent unexpected deterioration of the electrical or mechanical characteristics of the capacitance forming portion Ac, thereby effectively preventing moisture and plating solution penetration from the outside.

[0127] This is because by attaching separate side margin portions 114 and 115 to the fifth surface 5 and the sixth surface 6 of the main body 110, the boundary surface between the main body 110 and the side margin portions 114 and 115 may become brittle due to moisture and plating solution penetration from the outside. However, by adding gallium (Ga) to the side margin portions 114 and 115 (0 < MG), the moisture resistance reliability can be further improved. As the gallium (Ga) contained in the side margin portions 114 and 115 diffuses into the capacitance forming portion Ac during the firing process, the moisture resistance reliability at the boundary surface between the main body 110 and the side margin portions 114 and 115 can be further improved. Here, the boundary surface between the main body 110 and the side margin portions 114 and 115 can include the boundary surface between the capacitance forming portion Ac and the side margin portions 114 and 115.

[0128] Even when the number of moles of gallium (Ga) relative to 100 moles of titanium (Ti) contained in the capacitance forming portion Ac is more than the number of moles of gallium (Ga) relative to 100 moles of titanium (Ti) contained in the side margin portions 114 and 115 (MG < AG), the moisture resistance reliability at the boundary surface between the main body 110 and the side margin portions 114 and 115 can be further improved as the gallium (Ga) contained in the main body 110 diffuses into the side margin portions 114 and 115 during the firing process. However, when the gallium (Ga) content in the side margin portions 114 and 115 is low, it may be difficult to effectively prevent moisture and plating solution penetration from the outside.

[0129] In other words, by satisfying 0 < MG and 0 ≤ AG ≤ MG, the generation of pores in the fine structure can be further suppressed, and the moisture resistance reliability can be improved.

[0130] When the number of moles of gallium (Ga) relative to 100 moles of titanium (Ti) contained in the dielectric layer 111 of the laminated electronic component 100 according to an embodiment of the present invention is defined as DG, 0 < MG and 0 ≤ DG ≤ MG can be satisfied.

[0131] On the other hand, even if gallium (Ga) is not added to the dielectric layer 111 (DG = 0), by adding gallium (Ga) to the side margin portions 114 and 115, it is possible to effectively prevent moisture and plating solution penetration from the outside.

[0132] Also, when a small amount of gallium (Ga) is added to the dielectric layer 111 (0 < DG), it is obvious that moisture and plating solution penetration from the outside can be more effectively prevented. However, by ensuring that the number of moles of gallium (Ga) relative to 100 moles of titanium (Ti) contained in the dielectric layer 111 does not exceed the number of moles of gallium (Ga) relative to 100 moles of titanium (Ti) contained in the side margin portions 114 and 115 (DG ≤ MG), it is possible to prevent unexpected deterioration of the electrical or mechanical properties of the dielectric layer 111, and effectively prevent moisture and plating solution penetration from the outside.

[0133] By attaching separate side margin portions 114 and 115 to the fifth surface 5 and the sixth surface 6 of the main body 110 including the dielectric layer 111, the interface between the dielectric layer 111 and the side margin portions 114 and 115 may become brittle due to moisture and plating solution penetration from the outside. However, by adding gallium (Ga) to the side margin portions 114 and 115 (0 < MG), the moisture resistance reliability can be further improved. As the gallium (Ga) contained in the side margin portions 114 and 115 diffuses into the dielectric layer 111 during the firing process, the moisture resistance reliability at the interface between the dielectric layer 111 and the side margin portions 114 and 115 can be further improved. Here, the interface between the main body 110 and the side margin portions 114 and 115 can include the interface between the dielectric layer 111 and the side margin portions 114 and 115.

[0134] Even when the number of moles of gallium (Ga) with respect to 100 moles of titanium (Ti) contained in the dielectric layer 111 is larger than the number of moles of gallium (Ga) with respect to 100 moles of titanium (Ti) contained in the side margin portions 114 and 115 (MG < DG), as the gallium (Ga) contained in the dielectric layer 111 diffuses into the side margin portions 114 and 115 during the firing process, the moisture resistance reliability at the interface between the main body 110 and the side margin portions 114 and 115 can be further improved. However, when the gallium (Ga) content in the side margin portions 114 and 115 is low, it may be difficult to effectively prevent moisture and plating solution penetration from the outside.

[0135] In other words, by satisfying 0 < MG and 0 ≦ DG ≦ MG, the generation of pores in the fine structure can be further suppressed, and the moisture resistance reliability can be improved.

[0136] When defining the number of moles of gallium (Ga) with respect to 100 moles of titanium (Ti) contained in the cover portions 112 and 113 as CG in the multilayer electronic component 100 according to an embodiment of the present invention, 0 < MG and 0 ≦ CG ≦ MG can be satisfied.

[0137] On the one hand, even if gallium (Ga) is not added to the cover parts 112 and 113 (CG = 0), by adding gallium (Ga) to the side margin parts 114 and 115 (0 < MG), it is possible to effectively prevent moisture and plating solution penetration from the outside.

[0138] Also, it is obvious that when a small amount of gallium (Ga) is added to the cover parts 112 and 113 (0 < CG), it is possible to more effectively prevent moisture and plating solution penetration from the outside.

[0139] However, by ensuring that the number of moles of gallium (Ga) relative to 100 moles of titanium (Ti) contained in the cover parts 112 and 113 does not exceed the number of moles of gallium (Ga) relative to 100 moles of titanium (Ti) contained in the side margin parts 114 and 115 (CG ≤ MG), it is possible to prevent unexpected defects in the electrical or mechanical properties of the cover parts 112 and 113, and effectively prevent moisture and plating solution penetration from the outside.

[0140] This is because by attaching separate side margin parts 114 and 115 to the fifth surface 5 and the sixth surface 6 of the main body 110 including the cover parts 112 and 113, the interface between the cover parts 112 and 113 and the side margin parts 114 and 115 may become vulnerable due to moisture and plating solution penetration from the outside. However, by adding gallium (Ga) to the side margin parts 114 and 115 (0 < MG), the moisture resistance reliability can be further improved. As the gallium (Ga) contained in the side margin parts 114 and 115 diffuses into the cover parts 112 and 113 during the firing process, the moisture resistance reliability at the interface between the cover parts 112 and 113 and the side margin parts 114 and 115 can be further improved.

[0141] Even when the number of moles of gallium (Ga) per 100 moles of titanium (Ti) contained in the cover portions 112 and 113 is greater than the number of moles of gallium (Ga) per 100 moles of titanium (Ti) contained in the side margin portions 114 and 115 (MG < CG), as the gallium (Ga) contained in the cover portions 112 and 113 diffuses into the side margin portions 114 and 115 during the firing process, the moisture resistance reliability at the interface between the cover portions 112 and 113 and the side margin portions 114 and 115 can be further improved. However, when the gallium (Ga) content in the side margin portions 114 and 115 is low, it may be difficult to effectively prevent external moisture and plating solution penetration into the interface between the main body 110 and the side margin portions 114 and 115. This may be because the third-direction ends of the internal electrodes 121 and 122 are in contact with or located near the side margin portions 114 and 115, and thus it is easier for external moisture and plating solution to penetrate into the side margin portions 114 and 115 than into the cover portions 112 and 113.

[0142] In other words, by satisfying 0 < MG and 0 ≦ CG ≦ MG, the generation of pores in the microstructure can be further suppressed, and the moisture resistance reliability can be improved.

[0143] On the other hand, in the multilayer electronic component 100 according to an embodiment of the present invention, based on the cross-section of the side margin portions 114 and 115 in the first direction and the second direction (thickness and length directions), the side margin portions 114 and 115 are in contact with the external electrodes 131 and 132, respectively, and a region within 10 μm in the direction of the side margin portions 114 and 115 from the interface where the side margin portions 114 and 115 are in contact with the external electrodes 131 and 132 can contain gallium (Ga).

[0144] The interfaces between the side margins 114, 115 and the external electrodes 131, 132 can serve as paths through which moisture from the outside or plating solution can penetrate, which can lead to problems with reduced moisture resistance reliability. However, by including gallium (Ga) in a region within 10 μm in the direction of the side margins 114, 115 from the interfaces where the side margins 114, 115 and the external electrodes 131, 132 contact, it is possible to more effectively suppress the generation of pores and more effectively improve the moisture resistance reliability of the regions that serve as paths through which moisture from the outside or plating solution can penetrate.

[0145] In this case, the inclusion of gallium (Ga) in a region within 10 μm in the direction of the side margin portions 114, 115 from the interface where the side margin portions 114, 115 and the external electrodes 131, 132 contact can mean that the microstructure contains gallium (Ga), and that the crystal grains 11, crystal grain boundaries 12, triple points 13, secondary phases 20, etc. that may be arranged in the corresponding region contain gallium (Ga), thereby suppressing the generation of pores and improving the moisture resistance reliability.

[0146] Meanwhile, in the present invention, the side margins 114 and 115 contain gallium (Ga) to suppress the generation of pores. This is not particularly limited to the above, but it is preferable that the side margins 114 and 115 have a unit area of ​​150 μm 2 By "pores" it can mean 30 or less, preferably 25 or less, and more preferably 21 or less pores per unit area.

[0147] Unit area 150μm 2 By satisfying the requirement that the number of pores per unit area be 30 or less, the moisture resistance reliability can be improved.

[0148] As an example of one embodiment of the present invention, FIG. 9(b) shows a unit area of ​​150 μm 2In other words, when an image of a region including an end of an internal electrode and one side margin portion is taken with a scanning electron microscope (SEM) based on a cross-section in the first and third directions at the center of the second direction of the multilayer electronic component 100, a 150 μm 2 In this case, 150 μm 2 The area is not particularly limited to this, but may correspond to an area whose third direction size×first direction size is (7.5 μm×20 μm).

[0149] In one embodiment of the present invention, the ceramic electronic component 100 has a structure having two external electrodes 131, 132. However, the number and shapes of the external electrodes 131, 132 may vary depending on the shape of the internal electrodes 121, 122 and other purposes.

[0150] The external electrodes 131 and 132 may be disposed on the body 110 and connected to the internal electrodes 121 and 122 .

[0151] More specifically, the external electrodes 131, 132 may include a first external electrode 131 and a second external electrode 132 disposed on a third surface 3 and a fourth surface 4 of the body 110, respectively, and connected to the first internal electrode 121 and the second internal electrode 122, respectively. That is, the first external electrode 131 may be disposed on the third surface 3 of the body and connected to the first internal electrode 121, and the second external electrode 132 may be disposed on the fourth surface 4 of the body and connected to the second internal electrode 122.

[0152] Furthermore, the external electrodes 131, 132 may be arranged to extend on a portion of the first surface 1 and the second surface 2 of the main body 110, or may be arranged to extend on a portion of the fifth surface 5 and the sixth surface 6 of the main body 110. That is, the first external electrode 131 may be arranged on a portion of the first surface 1, the second surface 2, the fifth surface 5, the sixth surface 6 of the main body 110, and the third surface 3 of the main body 110, and the second external electrode 132 may be arranged on a portion of the first surface 1, the second surface 2, the fifth surface 5, the sixth surface 6 of the main body 110, and the third surface 3 of the main body 110.

[0153] The external electrodes 131, 132 may be formed using any material that has electrical conductivity, such as a metal, and the specific material may be determined taking into consideration electrical characteristics, structural stability, etc., and may further have a multi-layer structure.

[0154] For example, the external electrodes 131, 132 may include electrode layers 131a, 132a disposed on the body 110 and plating layers 131b, 132b disposed on the electrode layers 131a, 132a.

[0155] As a more specific example of the electrode layers 131a and 132a, the electrode layers 131a and 132a may be fired electrodes containing a conductive metal and glass, or resin-based electrodes containing a conductive metal and resin.

[0156] Also, the electrode layers 131a and 132a may be in a form in which a fired electrode and a resin-based electrode are sequentially formed on the body 110.

[0157] In addition, the electrode layers 131a and 132a may be formed by transferring a sheet containing a conductive metal onto the body 110, or may be formed by transferring a sheet containing a conductive metal onto a fired electrode.

[0158] The conductive metal used for the electrode layers 131a and 132a is not particularly limited as long as it can be electrically connected to the internal electrodes 121 and 122 to form capacitance, and may include, for example, at least one selected from the group consisting of nickel (Ni), copper (Cu), palladium (Pd), silver (Ag), gold (Au), platinum (Pt), tin (Sn), tungsten (W), titanium (Ti), and alloys thereof. The electrode layers 131a and 132a may be formed by applying a conductive paste prepared by adding glass frit to the conductive metal particles, and then firing the paste.

[0159] The plating layers 131b and 132b can serve to improve mounting characteristics.

[0160] The type of plating layers 131b, 132b is not particularly limited, and may be a single layer plating layer 131b, 132b containing one or more of nickel (Ni), tin (Sn), palladium (Pd), and alloys thereof, or may be formed of multiple layers.

[0161] As a more specific example of the plating layers 131b, 132b, the plating layers 131b, 132b may be Ni plating layers or Sn plating layers, and may be in a form in which a Ni plating layer and a Sn plating layer are sequentially formed on the electrode layers 131a, 132a, or in a form in which a Sn plating layer, a Ni plating layer and a Sn plating layer are sequentially formed. The plating layers 131b, 132b may also include a plurality of Ni plating layers and / or a plurality of Sn plating layers.

[0162] The size of the multilayer electronic component 100 does not need to be particularly limited.

[0163] However, in order to simultaneously achieve miniaturization and high capacity, the thickness of the dielectric layers and internal electrodes must be reduced and the number of layers must be increased, so the effects of the present invention may be more pronounced in a multilayer electronic component 100 having a size of 1005 (length x width: 1.0 mm x 0.5 mm) or less.

[0164] The present invention will be described in more detail below with reference to examples. However, these examples are provided to aid in the specific understanding of the invention, and the scope of the present invention is not limited to these examples.

[0165] (Example) In Comparative Example 1, a multilayer electronic component was manufactured to which a side margin portion to which gallium (Ga) was not added was applied.

[0166] Example 1 was produced as a multilayer electronic component having a side margin portion to which 0.3 moles of gallium (Ga) was added to 100 moles of titanium (Ti). The side margin portion was produced under the same conditions as Comparative Example 1, except that 0.3 moles of gallium (Ga) was added to 100 moles of titanium (Ti).

[0167] The following Table 1 shows the firing density (g / cm) of sample chips taken out at 25°C intervals from 1050°C to 1150°C during the firing process of Comparative Example 1 and Example 1. 3 ) were measured and shown as approximate values.

[0168] [Table 1]

[0169] In the case of Comparative Example 1, the firing density at 1050°C was about 4.20 g / cm 3 , the firing density at 1075℃ is about 4.60g / cm 3 , the firing density at 1100℃ is about 5.10g / cm 3 , the firing density at 1125℃ is about 5.70g / cm 3 , the firing density at 1150℃ is about 5.90g / cm 3 In the case of Example 1, the firing density at 1050°C was about 4.60 g / cm 3 , the firing density at 1075℃ is about 5.00g / cm 3 , the firing density at 1100℃ is about 5.85g / cm 3 , the firing density at 1125℃ is about 5.90g / cm 3 , the firing density at 1150℃ is about 5.95g / cm 3It was confirmed that the sintering temperature was lowered by adding gallium (Ga). In the case of Comparative Example 1 where no gallium (Ga) was added, sintering was almost completed at about 1150°C, whereas in the case of Example 1 where gallium (Ga) was added, sintering was almost completed at about 1100°C. This suggests that the addition of gallium (Ga) lowered the sintering temperature. In addition, in light of the results of Examples 2 to 4 described below, it can be predicted that there is an effect of improving the density and moisture resistance reliability of the dielectric microstructure, and it can be seen that the lower the sintering temperature, the easier it is to control the firing process.

[0170] Next, the atomic percentages (at %) of various elements contained in the secondary phase of Example 2 were measured.

[0171] Specifically, in Example 2, a multilayer electronic component was fabricated to which a side margin portion was applied in which 0.3 moles of gallium (Ga) was added to 100 moles of titanium (Ti), and the multilayer electronic component was fabricated under the same conditions as Example 1.

[0172] The cross-sections of the side margin portion of Example 2 in the first and third directions were analyzed by TEM-EDS, and gallium (Ga) and silicon (Si) were mapped and observed. The analysis images can be seen in (a) to (c) of FIG. 8.

[0173] More specifically, Figure 8(a) is an image of a cross section of the side margin taken using a transmission electron microscope (TEM) in high-angle annular dark-field (HAADF) mode, Figure 8(b) is an image of the same area analyzed by EDS for silicon (Si) and gallium (Ga), and Figure 8(c) is an image of the same area analyzed by EDS for gallium (Ga).

[0174] In addition, as shown in FIG. 8(b), it was confirmed that secondary phases containing gallium (Ga) and silicon (Si) were located at triple junctions included in the side margin portion. EDS analysis was performed on the regions (points) 1.spx to 9.spx shown in the nine secondary phases, and the results are shown in Table 2 below.

[0175] Table 2 shows the atomic percentages (at%) of titanium (Ti), tin (Sn), gallium (Ga), and silicon (Si) measured by TEM-EDS for each secondary phase region (point) detected in the image. The atomic percentages (at%) of gallium (Ga) relative to the atomic percentage (at%) of silicon (Si) contained in the secondary phase are expressed as a percentage (%).

[0176] On the other hand, the secondary phase was analyzed to contain at least one of magnesium (Mg), aluminum (Al), vanadium (V), manganese (Mn), zirconium (Zr), barium (Ba), and dysprosium (Dy), but the specific atomic percentage (at%) values ​​of each element were not listed in Table 2.

[0177] [Table 2]

[0178] In Example 2, which was fabricated under the same conditions as Example 1, it can be confirmed that the ratio (Ga / Si) of the atomic percentage (at%) of gallium (Ga) to the atomic percentage (at%) of silicon (Si) contained in the secondary phase is 3.94% or more and 7.21% or less. With reference to Examples 1, 3 and 4, it can be predicted that when the elements contained in the secondary phase are in the atomic percentage (at%) range of Table 2, the generation of pores in the dielectric microstructure is suppressed and the moisture resistance reliability is improved.

[0179] Next, the number of pores in the side margin portion for Comparative Example 2 and Example 3 was compared.

[0180] Comparative Example 2 was manufactured under the same conditions as Comparative Example 1 using a multilayer electronic component to which a side margin portion to which gallium (Ga) was not added was applied.

[0181] Example 3 was produced using a multilayer electronic component having a side margin portion in which 0.3 moles of gallium (Ga) was added to 100 moles of titanium (Ti), and was produced under the same conditions as Example 1 or Example 2.

[0182] 9(a) and 9(b) are images taken with a scanning electron microscope (SEM) of an area including an end of an internal electrode and one side margin portion based on a cross-section in the first and third directions at the center in the second direction of the multilayer electronic component 100.

[0183] More specifically, (a) of Figure 9 is an image taken with a scanning electron microscope (SEM) of the capacitance formation portion and side margin portion of Comparative Example 2, and (b) of Figure 9 is an image taken with a scanning electron microscope (SEM) of the capacitance formation portion and side margin portion of Example 3.

[0184] The unit area of ​​150 μm corresponds to the rectangular region of the side margin portion in Comparative Example 2 and Example 3. 2 The number of pores was observed, and in the case of Comparative Example 2, the number of pores was 45, and in the case of Example 3, the number of pores was 21.

[0185] From this, it can be confirmed that in the case of Example 3 in which gallium (Ga) is added, the generation of pores is suppressed more than in the case of Comparative Example 2 in which no gallium (Ga) is added.

[0186] Next, the moisture resistance reliability evaluation for Comparative Example 3 and Example 4 was compared.

[0187] In Comparative Example 3, a multilayer electronic component was manufactured using a side margin portion to which no gallium (Ga) was added, and was manufactured under the same conditions as in Comparative Example 1 or Comparative Example 2.

[0188] Example 4 was produced using a multilayer electronic component having a side margin portion in which 0.3 moles of gallium (Ga) was added to 100 moles of titanium (Ti), and was produced under the same conditions as Examples 1 to 3.

[0189] Forty sample chips each having the conditions of Comparative Example 3 and Example 4 were fabricated, and moisture resistance reliability evaluation was carried out.

[0190] The moisture resistance reliability evaluation was performed for 8 hours under the conditions of temperature 85°C, relative humidity 85%, and voltage condition 1.2Vr. Of the 40 sample chips, the insulation resistance (IR) value was 10 4 Sample chips that dropped below Ω were counted as defective and are listed in Table 3.

[0191] [Table 3]

[0192] Fig. 10(a) is a graph of the moisture resistance reliability evaluation of Comparative Example 3, and Fig. 10(b) is a graph of the moisture resistance reliability evaluation of Example 4. It was confirmed that in the case of Comparative Example 3, two chips were defective, whereas in the case of Example 4, the number of chips that were defective corresponds to zero. From this, it can be confirmed that in the case of Example 4 in which gallium (Ga) was added, the moisture resistance reliability was improved compared to Comparative Example 3 in which gallium (Ga) was not added.

[0193] Next, comparative examples and examples were manufactured by varying the number of moles of gallium (Ga) per 100 moles of titanium (Ti) contained in the side margin portion, and 30 pieces of each were manufactured using 0603 (length x width: 0.6 mm x 0.3 mm) size chips. The dissipation factor (DF), capacitance (μF), breakdown voltage (BDV), and short rate (%) were measured and evaluated, and the results are shown in Table 4.

[0194] [Table 4]

[0195] When comparing DF (%), capacitance (μF), BDV (V), and short (%) of Comparative Example 4 and Comparative Example 5, in which gallium (Ga) is not added to the side margin portion, with Examples 5 to 13, in which gallium (Ga) is added to the side margin portion, it can be confirmed that the addition of gallium (Ga) improves one or more of the characteristics of DF, capacitance, BDV, and short. This is expected to be because the addition of gallium (Ga) increases the dielectric grain size of the side margin portion and the region adjacent to the side margin portion among the capacitance forming portion. However, since the BDV characteristic decreases as the content of gallium (Ga) increases, it is expected that the appropriate content of gallium (Ga) for 100 moles of titanium (Ti) contained in the side margin portion is up to 3.0 moles in order to achieve the target characteristic.

[0196] Although the embodiments of the present invention have been described in detail above, the present invention is not limited to the above-described embodiments and the accompanying drawings, but is limited by the scope of the accompanying claims. Therefore, various substitutions, modifications, and changes can be made by a person having ordinary knowledge in the art within the scope of the technical idea of ​​the present invention described in the claims, and these also belong to the scope of the present invention.

[0197] In addition, the expression "one embodiment" used in this specification does not mean the same embodiment, but is provided to emphasize and describe each unique feature that is different from the others. However, the above-mentioned one embodiment does not exclude being realized in combination with the features of another embodiment. For example, even if a matter described in a specific embodiment is not described in another embodiment, it can be understood as a description related to the other embodiment, unless there is a description that is opposite or contradictory to the matter in the other embodiment.

[0198] The terms used in this specification are merely used to describe one embodiment and are not intended to limit the present disclosure. In this case, the singular expression includes the plural expression unless otherwise clearly indicated in the context. [Explanation of symbols]

[0199] 11 Crystal grains 12 Grain Boundaries 13 Triple Point 20 Secondary phase 100 Multilayer electronic components 110 Main unit 111 Dielectric layer 112, 113 Cover part 114, 115 Side margin 121, 122 Internal electrode 131, 132 External electrode

Claims

1. a capacitance forming portion including a dielectric layer and internal electrodes alternately disposed with the dielectric layer in a first direction, and a cover portion disposed on both end surfaces of the capacitance forming portion in the first direction, the body including a first surface and a second surface facing each other in the first direction, a third surface and a fourth surface connected to the first surface and the second surface and facing each other in the second direction, and a fifth surface and a sixth surface connected to the first surface and the fourth surface and facing each other in the third direction; external electrodes disposed on the third surface and the fourth surface of the body; and a side margin portion disposed on the fifth surface and the sixth surface of the main body, At least one of the capacitance forming portion, the cover portion, and the side margin portion includes a secondary phase containing gallium (Ga).

2. The laminated electronic component according to claim 1 , wherein the secondary phase further comprises silicon (Si).

3. 2. The multilayer electronic component according to claim 1, wherein at least one of the dielectric layer, the capacitance forming portion, the cover portion, and the side margin portion includes a plurality of crystal grains and crystal grain boundaries disposed between adjacent crystal grains, and when a point where three or more crystal grain boundaries meet is defined as a triple junction, the secondary phase is disposed at at least one triple junction.

4. The multilayer electronic component according to claim 3 , wherein at least one of the crystal grains contains gallium (Ga).

5. 4. The multilayer electronic component according to claim 3, wherein at least one of the crystal grain boundaries contains gallium (Ga).

6. 2. The multilayer electronic component according to claim 1, wherein an atomic percentage (at%) of gallium (Ga) contained in the secondary phase is 0.2 at% or more.

7. 3. The multilayer electronic component according to claim 2, wherein the ratio of an atomic percentage (at%) of gallium (Ga) to an atomic percentage (at%) of silicon (Si) contained in the secondary phase is 3.94% or more.

8. 2. The multilayer electronic component according to claim 1, wherein the number of moles of gallium (Ga) per 100 moles of titanium (Ti) contained in said side margin portion is 0.1 moles or more.

9. 9. The multilayer electronic component according to claim 8, wherein the number of moles of gallium (Ga) per 100 moles of titanium (Ti) contained in the side margin portion is 3.0 moles or less.

10. The laminated electronic component according to claim 1 , wherein the secondary phase further comprises tin (Sn).

11. The multilayer electronic component according to claim 10 , wherein the atomic percentage (at %) of tin (Sn) contained in the secondary phase is 0.3 at % or less.

12. The multilayer electronic component according to claim 1 , wherein the side margin portion further contains tin (Sn).

13. 13. The multilayer electronic component according to claim 12, wherein the number of moles of tin (Sn) per 100 moles of titanium (Ti) contained in the side margin portion is 0.1 moles or more and 5.0 moles or less.

14. 2. The multilayer electronic component according to claim 1, wherein MG is the number of moles of gallium (Ga) per 100 moles of titanium (Ti) contained in the side margin portion, and AG is the number of moles of gallium (Ga) per 100 moles of titanium (Ti) contained in the capacitance forming portion, and 0<MG and 0≦AG≦MG are satisfied.

15. 2. The multilayer electronic component according to claim 1, wherein MG is the number of moles of gallium (Ga) per 100 moles of titanium (Ti) contained in the side margin portion, and DG is the number of moles of gallium (Ga) per 100 moles of titanium (Ti) contained in the dielectric layer, and 0<MG and 0≦AG≦MG are satisfied.

16. 2. The multilayer electronic component according to claim 1, wherein, when the number of moles of gallium (Ga) per 100 moles of titanium (Ti) contained in the side margin portion is defined as MG, and the number of moles of gallium (Ga) per 100 moles of titanium (Ti) contained in the cover portion is defined as CG, 0<MG and 0≦CG≦MG are satisfied.

17. 2. The multilayer electronic component according to claim 1, wherein, based on a cross-section of the side margin portion in the first direction and the second direction, the side margin portion is in contact with the external electrode, and a region within 10 μm in the direction of the side margin portion from an interface where the side margin portion and the external electrode are in contact contains gallium (Ga).

18. the side margin portion includes a first side margin portion disposed on the fifth surface of the main body and a second side margin portion disposed on the sixth surface of the main body, 2 . The multilayer electronic component according to claim 1 , wherein at least one of the first side margin portion and the second side margin portion has an average size in the third direction of 20 μm or less.

19. The unit area of ​​the side margin is 150 μm 2 2. The multilayer electronic component according to claim 1, wherein the number of pores per unit area is 30 or less.

20. The multilayer electronic component according to claim 1 , wherein the secondary phase further contains at least one of lithium (Li), sodium (Na), potassium (K), rubidium (Rb), and cesium (Cs).

21. 20. The multilayer electronic component according to claim 1, wherein the secondary phase further contains at least one of magnesium (Mg), aluminum (Al), vanadium (V), manganese (Mn), zirconium (Zr), barium (Ba), and a rare earth element.

22. a capacitance forming part including a dielectric layer and internal electrodes arranged alternately with the dielectric layer in a first direction; a body including a first surface and a second surface facing each other in the first direction, a third surface and a fourth surface connected to the first surface and the second surface and facing each other in the second direction, and a fifth surface and a sixth surface connected from the first surface to the fourth surface and facing each other in the third direction; external electrodes disposed on the third surface and the fourth surface of the body; and a side margin portion disposed on the fifth surface and the sixth surface of the main body, A multilayer electronic component, in which 0<MG and 0≦AG≦MG are satisfied, where MG is the number of moles of gallium (Ga) per 100 moles of titanium (Ti) contained in the side margin portion, and AG is the number of moles of gallium (Ga) per 100 moles of titanium (Ti) contained in the capacitance forming portion.

23. 23. The multilayer electronic component according to claim 22, further comprising cover portions disposed on both end surfaces of the capacitance forming portion in the first direction.

24. 24. The multilayer electronic component according to claim 23, wherein at least one of the capacitance forming portion, the cover portion, and the side margin portion includes a secondary phase containing gallium (Ga).

25. 25. The laminated electronic component of claim 24, wherein the secondary phase further comprises silicon (Si).

26. 25. The multilayer electronic component according to claim 24, wherein at least one of the capacitance forming portion, the cover portion, and the side margin portion includes a plurality of crystal grains and crystal grain boundaries disposed between adjacent crystal grains, and when a point where three or more crystal grain boundaries meet is defined as a triple junction, the secondary phase is disposed at at least one triple junction.

27. 27. The laminated electronic component according to claim 26, wherein at least one of the crystal grains comprises gallium (Ga).

28. 27. The laminated electronic component of claim 26, wherein at least one of the grain boundaries comprises gallium (Ga).

29. 25. The multilayer electronic component according to claim 24, wherein the atomic percentage (at%) of gallium (Ga) contained in the secondary phase is 0.2 at% or more.

30. 26. The multilayer electronic component according to claim 25, wherein the ratio of the atomic percentage (at%) of gallium (Ga) to the atomic percentage (at%) of silicon (Si) contained in the secondary phase is 3.94% or more.

31. 23. The multilayer electronic component according to claim 22, wherein the number of moles of gallium (Ga) per 100 moles of titanium (Ti) contained in the side margin portion is 0.1 moles or more.

32. 32. The multilayer electronic component according to claim 31, wherein the number of moles of gallium (Ga) per 100 moles of titanium (Ti) contained in the side margin portion is 3.0 moles or less.

33. 25. The laminated electronic component according to claim 24, wherein the secondary phase further comprises tin (Sn).

34. The multilayer electronic component according to claim 33, wherein the atomic percentage (at%) of tin (Sn) contained in the secondary phase is 0.3 at% or less.

35. The multilayer electronic component according to claim 22 , wherein the side margin portion further contains tin (Sn).

36. 36. The multilayer electronic component according to claim 35, wherein the number of moles of tin (Sn) per 100 moles of titanium (Ti) contained in the side margin portion is 0.1 moles or more and 5.0 moles or less.

37. 23. The multilayer electronic component according to claim 22, wherein when the number of moles of gallium (Ga) per 100 moles of titanium (Ti) contained in the dielectric layer is taken as DG, 0<MG and 0≦DG≦MG are satisfied.

38. 24. The multilayer electronic component according to claim 23, wherein CG is the number of moles of gallium (Ga) per 100 moles of titanium (Ti) contained in the cover portion, and 0<MG and 0≦CG≦MG are satisfied.

39. 39. The multilayer electronic component according to claim 22, wherein, based on a cross-section of the side margin in the first direction and the second direction, the side margin is in contact with the external electrode, and a region within 10 μm in the direction of the side margin from an interface where the side margin and the external electrode are in contact contains gallium (Ga).

40. the side margin portion includes a first side margin portion disposed on the fifth surface of the main body and a second side margin portion disposed on the sixth surface of the main body, 39. The multilayer electronic component according to claim 22, wherein at least one of the first side margin portion and the second side margin portion has an average size in the third direction of 20 μm or less.

41. The unit area of ​​the side margin is 150 μm 2 39. The multilayer electronic component according to claim 22, wherein the number of pores per unit area is 30 or less.

42. 25. The laminated electronic component of claim 24, wherein the secondary phase further comprises at least one of lithium (Li), sodium (Na), potassium (K), rubidium (Rb), and cesium (Cs).

43. 25. The laminated electronic component of claim 24, wherein the secondary phase further comprises at least one of magnesium (Mg), aluminum (Al), vanadium (V), manganese (Mn), zirconium (Zr), barium (Ba), and rare earth elements.

Citation Information

Patent Citations

  • Dielectric porcelain composition and electronic parts

    JP2006062937A

  • Multi-layer ceramic electronic component

    JP2022068525A