Method for producing rubber vulcanizate

By employing specific silane coupling agents and basic compounds in the production process, the viscosity issues of silica-containing rubber compositions are addressed, resulting in rubber vulcanizates with improved fuel efficiency and grip for tire applications.

JP2024163968AInactive Publication Date: 2024-11-26OSAKA SODA CO LTD

Patent Information

Application Number
JP2021168528
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2021-10-14
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The increase in viscosity of silica-containing rubber compositions due to the use of silane coupling agents, which reduces the interaction between silicas and affects the performance of tires in terms of fuel efficiency and grip.

Method used

A method involving the use of specific silane coupling agents, such as protected mercapto-based organosilicon compounds and organosilicon compounds with amino acid skeletons, combined with a basic compound, to knead with rubber and inorganic fillers, followed by vulcanization, to produce a rubber vulcanizate with improved fuel efficiency and grip.

Benefits of technology

The resulting rubber vulcanizate exhibits enhanced fuel efficiency and grip properties by reducing the hysteresis loss, making it suitable for dynamic applications like tire tread parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024163968000001
    Figure 2024163968000001
  • Figure 2024163968000002
    Figure 2024163968000002
  • Figure 2024163968000003
    Figure 2024163968000003
Patent Text Reader

Abstract

To provide a method for producing a rubber vulcanizate that makes it possible to obtain tires excellent in lower fuel consumption and excellent grip.SOLUTION: A method for producing a rubber vulcanizate comprising: a step (A step) in which rubber (A), an inorganic filler (B), a silane coupling agent (C), and a basic compound (D) are kneaded to obtain a rubber composition (A step); and a step (B step) for adding a vulcanizate to the rubber composition obtained in the A step and vulcanizing to obtain the rubber vulcanizate, where the silane coupling agent (C) is a (protected) mercapto-based organosilicon compound, an amino acid, or an organosilicon compound having a skeleton of the derivative thereof, and a condensate thereof.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a rubber vulcanizate. [Background technology]

[0002] In recent years, various silica-containing rubber products, such as silica-containing tires with excellent fuel efficiency and braking performance, anti-vibration rubber, and various rubber rolls, are becoming more and more popular. However, silica-containing rubber compositions have a significant increase in compound viscosity, so a method of alleviating the increase in viscosity by compounding a silane coupling agent is generally used. In addition, it is known that the silane coupling agent reacts with the silanol on the silica surface to reduce the interaction between silica particles, thereby lowering the loss tangent and dynamic modulus of rubber.

[0003] Currently, among silane coupling agents, polysulfide-based coupling agents are widely used in fuel-efficient tires (see Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2000-103794 A Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present invention is to provide a method for producing a rubber vulcanizate which enables the production of a tire having better fuel economy and grip. [Means for solving the problem]

[0006] As a result of extensive research to solve the above problems, the present inventors have Item 1. A step (step A) of kneading a rubber (A), an inorganic filler (B), a silane coupling agent (C), and a basic compound (D) to obtain a rubber composition; The method for producing a rubber vulcanizate includes a step (step B) of adding a vulcanizing agent to the rubber composition obtained in the step A, and vulcanizing the rubber composition to obtain a rubber vulcanizate, The silane coupling agent (C) is at least one selected from the group consisting of (protected) mercapto-based organosilicon compounds, organosilicon compounds having a skeleton of an amino acid or a derivative thereof, and condensates thereof, and compounds represented by formula (X). (R 1 O) 3 Si-R 2 -SC(=O)-C 17 H 35 …(X) [In formula (X), R 1 are independently H or (C 1 ~C 8 ) alkyl, R 2 is a straight chain (C 1 ~C 8 ) double bonded hydrocarbon or branched chain (C 1 ~C 8 ) double bond hydrocarbons, saturated (C 1 ~C 8 ) double bond hydrocarbon or unsaturated (C 1 ~C 8 ) double bonded hydrocarbon, alkyl group C 17 H 35 is branched or linear] Item 2. In the above formula (X), R 1 is ethyl, and R 2 CH 2 CH 2 CH 2 and the alkyl group C 17 H 35 Item 2. The method for producing a rubber vulcanizate according to Item 1, wherein the silane coupling agent is a linear silane coupling agent. Item 3. The method for producing a rubber vulcanizate according to Item 1, wherein the organosilicon compound having a skeleton of an amino acid or a derivative thereof is an organosilicon compound represented by formula [Y-1] and / or an organosilicon compound represented by formula [Y-2], or a condensate thereof. (R 3 O) 3 Si-R 4 -SC(=O)-C(-R 5 )-NH-R6 …[Y-1] [In formula [Y-1], R 3 are independently H or (C 1 ~C 8 ) alkyl, R 4 is a straight chain (C 1 ~C 8 ) double bonded hydrocarbon or branched chain (C 1 ~C 8 ) double bond hydrocarbons, saturated (C 1 ~C 8 ) double bond hydrocarbon or unsaturated (C 1 ~C 8 ) double bonded hydrocarbon, R 5 is hydrogen or an organic group, R 6 is hydrogen or a protecting group for an amino group; or (R 7 O) 3 Si-R 8 -SC(=O)-R 9 -NH-R 10 …[Y-2] (In formula [Y-2], R 7 are independently H or (C 1 ~C 8 ) alkyl, R 8 is a straight chain (C 1 ~C 8 ) double bonded hydrocarbon or branched chain (C 1 ~C 8 ) double bond hydrocarbons, saturated (C 1 ~C 8 ) double bond hydrocarbon or unsaturated (C 1 ~C 8 ) double bonded hydrocarbon, R 9 is a divalent hydrocarbon group having 1 to 20 carbon atoms which may contain a substituted or unsubstituted aromatic ring, R 10 is hydrogen or a protecting group for an amino group. Item 4. The method for producing a rubber vulcanizate according to Item 1, wherein the (protected) mercapto-based organosilicon compound is a compound represented by the formula [Z]. R 11 n (R 12 ) 3-n -Si-R 13-S-CO-R 14 …[Z] (In formula [Z], R 11 are each independently a hydrocarbon group, R 12 each independently represents an alkoxy group; R 13 is a divalent hydrocarbon group, R 14 is a monovalent hydrocarbon having 1 to 18 carbon atoms. n is an integer of 0, 1, or 2. Item 5. The method for producing a rubber vulcanizate according to any one of Items 1 to 4, wherein the rubber (A) is one or more selected from natural rubber (NR), polyisoprene rubber (IR), styrene-butadiene copolymer rubber (SBR), polybutadiene rubber (BR), acrylonitrile-butadiene copolymer rubber (NBR), chloroprene rubber (CR), ethylene-propylene copolymer rubber (EPDM), and butyl rubber (IIR). Effect of the Invention

[0007] The present inventors add both a specific silane coupling agent (C) and a basic compound (D) in step A, knead the mixture to obtain a rubber composition, and then add a vulcanizing agent and vulcanize the mixture to obtain a rubber vulcanizate in step B. They have found that the rubber vulcanizate has excellent fuel efficiency and grip properties when used as a tire. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The present invention relates to a process for producing a rubber composition comprising: kneading a rubber (A), an inorganic filler (B), a silane coupling agent (C), and a basic compound (D) to obtain a rubber composition (step A); The method for producing a rubber vulcanizate includes a step (step B) of adding a vulcanizing agent to the rubber composition obtained in step A, and vulcanizing the rubber composition to obtain a rubber vulcanizate, The silane coupling agent (C) is at least one selected from the group consisting of (protected) mercapto-based organosilicon compounds, organosilicon compounds having a skeleton of an amino acid or a derivative thereof, and condensates thereof, and compounds represented by formula (X). (R 1 O) 3 Si-R 2-SC(=O)-C 17 H 35 …(X) [In formula (X), R 1 are independently H or (C 1 ~C 8 ) alkyl, R 2 is a straight chain (C 1 ~C 8 ) double bonded hydrocarbon or branched chain (C 1 ~C 8 ) double bond hydrocarbons, saturated (C 1 ~C 8 ) double bond hydrocarbon or unsaturated (C 1 ~C 8 ) double bonded hydrocarbon, alkyl group C 17 H 35 is branched or linear]

[0009] A process Step A in the method for producing a rubber vulcanizate of the present invention is a step of kneading rubber (A), an inorganic filler (B), a silane coupling agent (C), and a basic compound (D) to obtain a rubber composition.

[0010] Rubber composition The rubber composition in step A of the present invention contains a rubber (A), an inorganic filler (B), a silane coupling agent (C), and a basic compound (D).

[0011] Rubber (A) The rubber (A) used in the rubber composition in the step A is not particularly limited, and may be natural rubber or synthetic rubber. The synthetic rubber is also not particularly limited, and examples thereof include diene rubbers such as styrene-butadiene rubber (SBR), butadiene rubber (BR), isoprene rubber (IR), nitrile rubber (NBR), acrylonitrile-butadiene rubber (NBR), and chloroprene rubber (CR); olefin rubbers such as butyl rubber (IIR), ethylene-propylene rubber (EPDM), acrylic rubber (ACM), chlorosulfonated polyethylene rubber (CSM), and fluororubber (FKM); silicone rubber (Q); and urethane rubber (AU).

[0012] The rubber (A) may be produced by any polymerization method, and may be a rubber produced by emulsion polymerization or a rubber produced by solution polymerization. The rubber may also be a so-called terminal-modified rubber, in which the molecular terminals are modified.

[0013] The above rubbers (A) can be used alone or in combination of two or more kinds.

[0014] Among them, from the viewpoint of reactivity with the silane coupling agent (C), the rubber (A) is more preferably a diene rubber, and particularly preferably at least one selected from the group consisting of styrene-butadiene rubber (SBR), butadiene rubber (BR), natural rubber (NR), butyl rubber (IIR), and ethylene-propylene rubber (EPDM).

[0015] In the step A, the content of the rubber (A) used in the rubber composition is not particularly limited, but may be, for example, 20 to 80% by mass based on the total mass of the rubber composition.

[0016] Inorganic filler (B) The inorganic filler (B) used in the rubber composition in the step A of the present invention is not particularly limited as long as it is one that is usually added during the kneading of the rubber composition, but for example, at least one selected from the group consisting of wet silica, dry silica, and aluminum hydroxide can be suitably used. By using these inorganic fillers (B), it is possible to obtain an effect of further improving the reinforcing properties of the rubber. Among them, it is particularly preferable to use wet silica as the inorganic filler (B) from the viewpoint of reactivity with the silane coupling agent. In addition, the BET specific surface area of ​​the above-mentioned wet silica, dry silica, and aluminum hydroxide is 20 to 300 m 2 / g, and 50 to 250m 2 / g is more preferable, and 100 to 250m 2 It is more preferable that the BET specific surface area of ​​the inorganic filler (B) is 20 m 2 / g, when the inorganic filler (B) is mixed with the rubber (A), the rubber has excellent reinforcement properties and improves the abrasion resistance of the rubber. 2 / g or less, an increase in the viscosity of the rubber when the inorganic filler (B) and the rubber (A) are mixed can be suppressed, and the inorganic filler (B) and the rubber can be kneaded more uniformly.

[0017] In step A, the content of the inorganic filler (B) used in the rubber composition is not limited to this, but is preferably 10 to 150 parts by weight, more preferably 20 to 120 parts by weight, and even more preferably 60 to 120 parts by weight, per 100 parts by weight of the rubber (A).

[0018] Silane coupling agent (C) The silane coupling agent (C) used in the rubber composition in step A of the present invention is not particularly limited, but examples thereof include (protected) mercapto-based organosilicon compounds, organosilicon compounds having a skeleton of an amino acid or a derivative thereof, and condensates thereof, and compounds represented by formula (X). (R 1 O) 3 Si-R2 -SC(=O)-C 17 H 35 …(X) [In formula (X), R 1 are independently H or (C 1 ~C 8 ) alkyl, R 2 is a straight chain (C 1 ~C 8 ) double bonded hydrocarbon or branched chain (C 1 ~C 8 ) double bond hydrocarbons, saturated (C 1 ~C 8 ) double bond hydrocarbon or unsaturated (C 1 ~C 8 ) double bonded hydrocarbon, alkyl group C 17 H 35 is branched or linear]

[0019] A compound represented by formula (X) Examples of the compound represented by formula (X) include the following. (R 1 O) 3 Si-R 2 -SC(=O)-C 17 H 35 …[X] [In formula (X), R 1 are independently H or (C 1 ~C 8 ) alkyl, preferably methyl or ethyl; R 2 is a straight chain (C 1 ~C 8 ) double bonded hydrocarbon or branched chain (C 1 ~C 8 ) double bond hydrocarbons, saturated (C 1 ~C 8 ) double bond hydrocarbon or unsaturated (C 1 ~C 8 ) double bonded hydrocarbons, preferably CH 2 , C.H. 2 CH 2 , C.H. 2 CH 2 CH 2 , C.H. 2 CH 2 CH2 CH 2 , CH(CH 3 ), C.H. 2 CH(CH 3 ), C(CH 3 ) 2 , CH(C 2 H 5 ), C.H. 2 CH 2 CH(CH 3 ), C.H. 2 CH(CH 3 )CH 2 means an alkyl group C 17 H 35 is branched or linear]

[0020] In formula (X), R 1 may be ethyl, R 2 CH 2 CH 2 CH 2 and the alkyl group C 17 H 35 is a straight chain ((CH 2 ) 16 CH 3 ) may be.

[0021] Examples of the compound represented by formula (X) include the compounds shown below.

[0022] (CH 3 O) 3 Si-CH 2 -SC(=O)-C 17 H 35 , (CH 3 O) 3 Si-CH 2 CH 2 -SC(=O)-C 17 H 35 , (CH 3 O) 3 Si-CH 2 CH 2 CH 2 -SC(=O)-C 17 H 35 , (CH3 ABOUT) 3 Si-CH 2 CH 2 CH 2 CH 2 -SC(=O)-C 17 H 35 、 (CH 3 ABOUT) 3 Si-CH 2 CH 2 CH 2 CH 2 CH 2 -SC(=O)-C 17 H 35 、 (CH 3 CH 2 ABOUT) 3 Si-CH 2 -SC(=O)-C 17 H 35 、 (CH 3 CH 2 ABOUT) 3 Si-CH 2 CH 2 -SC(=O)-C 17 H 35 、 (CH 3 CH 2 ABOUT) 3 Si-CH 2 CH 2 CH 2 -SC(=O)-C 17 H 35 、 (CH 3 CH 2 ABOUT) 3 Si-CH 2 CH 2 CH 2 CH 2 -SC(=O)-C 17 H 35 、または、 (CH 3 CH 2 ABOUT) 3 Si-CH 2 CH 2 CH 2 CH 2 CH 2 -SC(=O)-C 17H 35 .

[0023] The compound represented by formula (X) can be reacted with a compound represented by formula (X-1) (R 1 O) 3 Si-R 2 The mercaptosilane corresponding to --SH can be prepared by reacting it with stearic acid chloride, filtering off the resulting solid residue and distilling off the solvent. [In formula (X-1), R 1 are independently H or (C 1 ~C 8 ) alkyl, preferably methyl or ethyl; R 2 is a straight chain (C 1 ~C 8 ) double bonded hydrocarbon or branched chain (C 1 ~C 8 ) double bond hydrocarbons, saturated (C 1 ~C 8 ) double bond hydrocarbon or unsaturated (C 1 ~C 8 ) double bonded hydrocarbons, preferably CH 2 , C.H. 2 CH 2 , C.H. 2 CH 2 CH 2 , C.H. 2 CH 2 CH 2 CH 2 , CH(CH 3 ), C.H. 2 CH(CH 3 ), C(CH 3 ) 2 , CH(C 2 H 5 ), C.H. 2 CH 2 CH(CH 3 ), C.H. 2 CH(CH 3 )CH 2 means.]

[0024] In formula (X-1), R 1 may be ethyl, R 2 CH 2 CH 2CH 2 and the alkyl group C 17 H 35 is a straight chain ((CH 2 ) 16 CH 3 ) may be.

[0025] The compound represented by formula (X-1) (R 1 O) 3 Si-R 2 Examples of the -SH mercaptosilane include the following compounds.

[0026] (CH 3 O) 3 Si-CH 2 -SH, (CH 3 O) 3 Si-CH 2 CH 2 -SH, (CH 3 O) 3 Si-CH 2 CH 2 CH 2 -SH, (CH 3 O) 3 Si-CH 2 CH 2 CH 2 CH 2 -SH, (CH 3 O) 3 Si-CH 2 CH 2 CH 2 CH 2 CH 2 -SH, (CH 3 CH 2 O) 3 Si-CH 2 -SH, (CH 3 CH 2 O) 3 Si-CH 2 CH 2 -SH, (CH 3 CH 2 O) 3Si-CH 2 CH 2 CH 2 -SH, (CH 3 CH 2 O) 3 Si-CH 2 CH 2 CH 2 CH 2 -SH, or (CH 3 CH 2 O) 3 Si-CH 2 CH 2 CH 2 CH 2 CH 2 -SH.

[0027] Triethylamine or another amine may be used as an auxiliary base for the production of the compound represented by formula (X). Examples of the solvent include aliphatic hydrocarbons such as pentane, hexane, heptane, and octane, alicyclic hydrocarbons such as cyclopentane and cyclohexane, aromatic hydrocarbons such as benzene, toluene, and xylene, chlorinated hydrocarbons such as dichloromethane, 1,2-dichloroethane, chloroform, monochlorobenzene, and dichlorobenzene, ether solvents such as diethyl ether, tetrahydrofuran (THF), dioxane, and 1,2-dimethoxyethane, amide solvents such as N,N-dimethylformamide (DMF), N,N-dimethylacetamide, and N-methylpyrrolidone, ester solvents such as methyl formate, ethyl formate, methyl acetate, ethyl acetate, isopropyl acetate, and butyl acetate, ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone, nitrile solvents such as acetonitrile and benzonitrile, and sulfone solvents such as dimethyl sulfoxide and sulfolane. The solvent may be one or more of these.

[0028] Organosilicon compounds having an amino acid or its derivative skeleton, and their condensation products Examples of the organosilicon compound having a skeleton of an amino acid or a derivative thereof include an organosilicon compound represented by the formula [Y-1] and / or an organosilicon compound represented by the formula [Y-2]. (R 3 O) 3 Si-R 4 -SC(=O)-C(-R 5 )-NH-R 6 …[Y-1] [In formula [Y-1], R 3 are independently H or (C 1 ~C 8 ) alkyl, R 4 is a straight chain (C 1 ~C 8 ) double bonded hydrocarbon or branched chain (C 1 ~C 8 ) double bond hydrocarbons, saturated (C 1 ~C 8 ) double bond hydrocarbon or unsaturated (C 1 ~C 8 ) double bonded hydrocarbon, R 5 is hydrogen or an organic group, R 6 is hydrogen or a protecting group for an amino group; or (R 7 O) 3 Si-R 8 -SC(=O)-R 9 -NH-R 10 …[Y-2] [In formula [Y-2], R 7 are independently H or (C 1 ~C 8 ) alkyl, R 8 is a straight chain (C 1 ~C 8 ) double bonded hydrocarbon or branched chain (C 1 ~C 8 ) double bond hydrocarbons, saturated (C 1 ~C 8 ) double bond hydrocarbon or unsaturated (C 1 ~C 8 ) double bonded hydrocarbon, R 9 is a divalent hydrocarbon group having 1 to 20 carbon atoms which may contain a substituted or unsubstituted aromatic ring, R 10 is hydrogen or a protecting group for an amino group.

[0029] An example of an organosilicon compound having a skeleton of an amino acid or a derivative thereof is an organosilicon compound represented by the formula [Y-1]. (R 3 O) 3 Si-R 4 -SC(=O)-C(-R 5 )-NH-R 6 …(Y-1) [In formula [Y-1], R 3 are independently H or (C 1 ~C 8 ) alkyl, R 4 is a straight chain (C 1 ~C 8 ) double bonded hydrocarbon or branched chain (C 1 ~C 8 ) double bond hydrocarbons, saturated (C 1 ~C 8 ) double bond hydrocarbon or unsaturated (C 1 ~C 8 ) double bonded hydrocarbon, R 5 is hydrogen or an organic group, R 6 is hydrogen or a protecting group for an amino group.

[0030] In the organosilicon compound represented by the formula [Y-1], R 5 is hydrogen or an organic group, and examples of the organic group include an amino acid side chain group and a group derived from an amino acid side chain group. The amino acid side chain group means a functional group located in the side chain derived from an amino acid, specifically, -(CH 2 ) 3 -NH-C(NH 2 )(=NH)(arginine side chain group), -(CH 2 ) 4 NH 2 (lysine side group), -CH 2 OH (serine side chain group), -CHOHCH 3 (threonine side chain group), -CH 2 -C 6 H 4 -OH (tyrosine side chain group), -CH 2 CONH 2 (asparagine side chain group), -CH 2COOH (aspartic acid side chain group), -(CH 2 ) 2 CONH 2 (glutamine side chain group), -(CH 2 ) 2 COOH (glutamic acid side chain group), -CH 2 SH (cysteine ​​side group), -H (glycine side group), -CH 3 (alanine side chain group), -CH 2 C(C=CH-N=CH-NH-) (histidine side chain group), -CH(CH 3 )CH 2 CH 3 (isoleucine side chain group), -CH 2 CH(CH 3 ) 2 (Leucine side chain group), -(CH 2 ) 2 SCH 3 (methionine side chain group), -CH 2 C 6 H 5 (phenylalanine side chain group), -CH 2 -C(C=CH-NH-Ph-) (tryptophan side chain group), -CH(CH 3 ) 2 (valine side chain group), etc. 5 is preferably hydrogen, a substituted or unsubstituted alkyl group, an alkyl group having a substituted or unsubstituted thioether (-S-), or a substituted or unsubstituted aromatic group, and more preferably hydrogen, a substituted or unsubstituted alkyl group having 1 to 5 carbon atoms, an alkyl group having 1 to 5 carbon atoms having a substituted or unsubstituted thioether (-S-), or a substituted or unsubstituted aromatic group having 6 to 10 carbon atoms.

[0031] In the organosilicon compound represented by the formula [Y-1], R 6is hydrogen or a protecting group for an amino group. The protecting group for an amino group is not particularly limited as long as it acts as a protecting group for an amino group, and examples thereof include a tert-butyloxycarbonyl group, a benzyloxycarbonyl group, a 9-fluorenylmethyloxycarbonyl group, an acetyl group, an octanoyl group, a benzoyl group, a benzyl group, a 4-dimethylaminoazobenzene-4'-sulfonyl group, a 5-dimethylaminonaphthalene-1-sulfonyl group, a 2,4-dinitrophenyl group, a 2-nitrophenylsulfenyl group, a chloroacetyl group, and a formyl group. R 6 is preferably a hydrogen atom, a tert-butyloxycarbonyl group, a benzyloxycarbonyl group, an acetyl group, or an octanoyl group.

[0032] In the organosilicon compound represented by the formula [Y-1], examples of the substituent that can be substituted include alkyl groups such as methyl, ethyl, and isopropyl, aryl groups such as phenyl, aralkyl groups such as benzyl, unsaturated hydrocarbon groups such as vinyl, halogeno groups such as fluoro, chloro, bromo, and iodo, amino groups, and nitro groups.

[0033] An example of an organosilicon compound having a skeleton of an amino acid or a derivative thereof is an organosilicon compound represented by the formula [Y-2]. (R 7 O) 3 Si-R 8 -SC(=O)-R 9 -NH-R 10 …[Y-2] [In formula [Y-2], R 7 are independently H or (C 1 ~C 8 ) alkyl, R 8 is a straight chain (C 1 ~C 8 ) double bonded hydrocarbon or branched chain (C 1 ~C 8 ) double bond hydrocarbons, saturated (C 1 ~C 8 ) double bond hydrocarbon or unsaturated (C 1 ~C 8 ) double bonded hydrocarbon, R 9is a divalent hydrocarbon group having 1 to 20 carbon atoms which may contain a substituted or unsubstituted aromatic ring, R 10 is hydrogen or a protecting group for an amino group.

[0034] In formula [Y-2], R 7 are independently H or (C 1 ~C 8 ) alkyl, R 8 is a straight chain (C 1 ~C 8 ) double bonded hydrocarbon or branched chain (C 1 ~C 8 ) double bond hydrocarbons, saturated (C 1 ~C 8 ) double bond hydrocarbon or unsaturated (C 1 ~C 8 ) double bonded hydrocarbon, R 9 is a divalent hydrocarbon group having 1 to 20 carbon atoms which may contain a substituted or unsubstituted aromatic ring, R 10 is hydrogen or a protecting group for an amino group.

[0035] In the organosilicon compound represented by the formula [Y-2], R 9 represents a divalent hydrocarbon group having 1 to 20 carbon atoms which may contain a substituted or unsubstituted aromatic ring, is preferably a divalent hydrocarbon group having 1 to 12 carbon atoms which may contain a substituted or unsubstituted aromatic ring, and is particularly preferably a substituted or unsubstituted alkylene group having 1 to 8 carbon atoms.

[0036] In the organosilicon compound represented by the formula [Y-2], R 10 is hydrogen or a protecting group for an amino group. The protecting group for an amino group is not particularly limited as long as it acts as a protecting group for an amino group, and examples thereof include a tert-butyloxycarbonyl group, a benzyloxycarbonyl group, a 9-fluorenylmethyloxycarbonyl group, an acetyl group, an octanoyl group, a benzoyl group, a benzyl group, a 4-dimethylaminoazobenzene-4'-sulfonyl group, a 5-dimethylaminonaphthalene-1-sulfonyl group, a 2,4-dinitrophenyl group, a 2-nitrophenylsulfenyl group, a chloroacetyl group, and a formyl group. R 10is preferably a hydrogen atom, a tert-butyloxycarbonyl group, a benzyloxycarbonyl group, an acetyl group, or an octanoyl group.

[0037] In the organosilicon compound represented by the formula [Y-2], examples of the substituent that can be substituted include alkyl groups such as methyl, ethyl, and isopropyl, aryl groups such as phenyl, aralkyl groups such as benzyl, unsaturated hydrocarbon groups such as vinyl, halogeno groups such as fluoro, chloro, bromo, and iodo, amino groups, and nitro groups.

[0038] The method for producing the organosilicon compound of the present invention is not particularly limited, but a specific example is a production method in which mercaptosilane is reacted with an N-protected amino acid or an N-protected aminocarboxylic acid in the presence of a carbodiimide condensing agent and a base.

[0039] An N-protected amino acid is an amino acid in which the amino group is protected with a known protecting group, for example, a protecting group described in paragraph "0031" etc., and specific examples include Boc-alanine, Boc-phenylalanine, Boc-methionine, Z-alanine, Z-phenylalanine, Z-methionine, Ac-alanine, Ac-phenylalanine, Ac-methionine, N-(octanoyl)alanine, N-(octanoyl)phenylalanine, N-(octanoyl)methionine and the like, but are not particularly limited to these.

[0040] The N-protected aminocarboxylic acid is an aminocarboxylic acid in which the amino group is protected with a known protecting group, for example, a protecting group described in paragraph "0036". Specific examples include 3-Boc-aminopropanoic acid, 3-Z-aminopropanoic acid, 3-Ac-aminopropanoic acid, 3-(octanoyl)aminopropanoic acid, 4-Boc-aminobutyric acid, 4-Z-aminobutyric acid, 4-Ac-aminobutyric acid, 4-(octanoyl)aminobutyric acid, 5-Boc-aminovaleric acid, 5-Z-aminovaleric acid, 5-Ac-aminovaleric acid, 5-(octanoyl)aminovaleric acid, 6-Boc-aminocaproic acid, 6-Z-aminocaproic acid, 6-Ac-aminocaproic acid, 6-(octanoyl)aminocaproic acid, 7-Boc-aminoheptanoic acid, 7-Z-aminoheptanoic acid, 7-Ac-aminoheptanoic acid, 7-(octanoyl)aminocaproic acid, 7-Boc ... undecanoic acid, 8-Boc-aminooctanoic acid, 8-Z-aminooctanoic acid, 8-Ac-aminooctanoic acid, 8-(octanoyl)aminooctanoic acid, 9-Boc-aminonananoic acid, 9-Z-aminonananoic acid, 9-Ac-aminonananoic acid, 9-(octanoyl)aminonananoic acid, 11-Boc-aminoundecanoic acid, 11-Z-aminoundecanoic acid, 11-Ac-aminoundecanoic acid, 11-( Examples of such amino acids include, but are not limited to, 12-Boc-aminododecanoic acid, 12-Z-aminododecanoic acid, 12-Ac-aminododecanoic acid, 12-(octanoyl)aminododecanoic acid, 13-Boc-aminotridecanoic acid, 13-Z-aminotridecanoic acid, 13-Ac-aminotridecanoic acid, and 13-(octanoyl)aminotridecanoic acid. Note that Boc is an abbreviation for tert-butyloxycarbonyl group, Z is an abbreviation for benzyloxycarbonyl group, and Ac is an abbreviation for acetyl group.

[0041] The silane coupling agent (C) of the present invention may be a condensate (oligomer) obtained by hydrolyzing an organosilicon compound represented by formula [Y-1] or [Y-2] and then subjecting it to a condensation reaction, or may be a condensate (oligomer) obtained by subjecting it to a condensation reaction with other components. Examples of other components include alkyl polyols having 1 to 60 carbon atoms and divalent or higher which may contain a nitrogen atom in the molecule and / or (poly)alkyl ether polyols having 2 to 60 carbon atoms and divalent or higher which may contain a nitrogen atom in the molecule, and alkyl polyols having 2 to 60 carbon atoms and / or (poly)alkyl ether polyols having 2 to 60 carbon atoms are preferred, and alkyl polyols having 2 to 30 carbon atoms and / or (poly)alkyl ether polyols having 2 to 30 carbon atoms are more preferred.

[0042] Examples of the divalent or higher alkyl polyol of the present invention, which has 1 to 60 carbon atoms and may contain a nitrogen atom in the molecule, include ethylene glycol, propylene glycol, 1,3-propanediol, 1,4-butanediol, 2-methyl-1,3-propanediol, glycerin, trimethylolpropane, pentaerythritol, sorbitol, diethanolamine, methyldiethanolamine, butyldiethanolamine, triethanolamine, etc. Examples of the divalent or higher (poly)alkyl ether polyol, which has 2 to 60 carbon atoms and may contain a nitrogen atom in the molecule, include diethylene glycol, polyethylene glycol, dipropylene glycol, polypropylene glycol, etc.

[0043] (Protected) Mercapto-based Organosilicon Compounds Examples of (protected) mercapto-based organosilicon compounds include mercapto-based organosilicon compounds having a mercapto group as a compound, such as 3-mercaptopropyltrimethoxysilane and 3-mercaptopropyltriethoxysilane, and protected mercapto-based organosilicon compounds which are organosilicon compounds having no mercapto group (wherein the mercapto group is protected), such as 3-octanoylthio-1-propyltriethoxysilane and 3-propionylthiopropyltrimethoxysilane, and which subsequently come to have a mercapto group by the application of heat, chemicals, etc.

[0044] The (protected) mercapto-based organosilicon compound is preferably a compound represented by the following formula [Z]. R 11 n (R 12 ) 3-n -Si-R 13 -S-CO-R 14 …[Z] (In formula [Z], R 11 are each independently a hydrocarbon group, R 12 each independently represents an alkoxy group; R 13 is a divalent hydrocarbon group, R 14 is a monovalent hydrocarbon having 1 to 18 carbon atoms. n is an integer of 0, 1, or 2. R 11 are each independently a hydrocarbon group, preferably an alkyl group having 1 to 6 carbon atoms, and more preferably an alkyl group having 1 to 3 carbon atoms. R 12 are each independently an alkoxy group, preferably an alkoxy group having 1 to 8 carbon atoms, and more preferably an alkoxy group having 1 to 3 carbon atoms. R 13 is a divalent hydrocarbon group, preferably a divalent hydrocarbon group having 1 to 18 carbon atoms, and preferably an alkylene group having 1 to 4 carbon atoms. R 14 is preferably a monovalent hydrocarbon group having 1 to 18 carbon atoms, and more preferably a monovalent hydrocarbon group having 8 to 18 carbon atoms. n is 0, 1 or 2.

[0045] Specific examples of the (protected) mercapto-based organosilicon compound include, but are not limited to, NXT and NXT-LowV represented by formula [1]. These compounds can be used alone or in combination. Commercially available products or products synthesized by a commonly known synthesis method can be used. [ka]

[0046] Among these, 3-octanoylthiopropyltriethoxysilane and 3-octadecanoylthiopropyltriethoxysilane are preferred as the silane coupling agent (C).

[0047] In step A, the content of the silane coupling agent (C) used in the rubber composition is preferably 1 to 30 parts by mass, more preferably 2 to 25 parts by mass, and particularly preferably 3 to 15 parts by mass, per 100 parts by mass of rubber.

[0048] Other silane coupling agents In addition to the above-mentioned silane coupling agent (C), the rubber composition of the present invention may be compounded in combination with a silane coupling agent that is usually compounded in rubber. As the other silane coupling agent, for example, at least one of vinyl-based organosilicon compounds, alkyl-based organosilicon compounds, epoxy-based organosilicon compounds, methacrylic-based organosilicon compounds, (poly)sulfide-based organosilicon compounds, and condensates thereof may be contained (hereinafter, these organosilicon compounds may be collectively referred to as "other organosilicon compounds").

[0049] In the rubber composition of the present invention, when other organosilicon compounds, i.e., at least one selected from vinyl-based organosilicon compounds, alkyl-based organosilicon compounds, epoxy-based organosilicon compounds, methacrylic-based organosilicon compounds, (poly)sulfide-based organosilicon compounds, and condensates thereof, are contained, it is preferable to compound 0.1 to 20 parts by mass, more preferably 0.5 to 15 parts by mass, even more preferably 0.5 to 10 parts by mass, and even more preferably 0.5 to 5.0 parts by mass, relative to 100 parts by mass of the inorganic filler.

[0050] Examples of the vinyl-based organosilicon compound of the present invention include vinyltrimethoxysilane, vinyltriethoxysilane, vinyltris(2-methoxyethoxy)silane, allyltrichlorosilane, allyltriethoxysilane, diethoxymethylvinylsilane, trichlorovinylsilane, trichlorovinylsilane, and the like.

[0051] Examples of the alkyl-based organosilicon compound of the present invention include methyltrimethoxysilane, dimethyldiethoxysilane, propyltriethoxysilane, hexyltrimethoxysilane, octyltriethoxysilane, and hexamethyldisilazane.

[0052] Examples of the epoxy-based organosilicon compound of the present invention include 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, and the like.

[0053] Examples of the methacrylic organosilicon compound of the present invention include 3-methacryloxypropyltriethoxysilane, 3-methacryloxypropyltrimethoxysilane, and the like.

[0054] The (poly)sulfide-based organosilicon compound of the present invention is exemplified by a polysulfide-based silane coupling agent represented by formula (2), with bis(3-triethoxysilylpropyl) disulfide and bis(3-triethoxysilylpropyl) tetrasulfide being particularly preferred. (R15 -O) 3-m (R 15 ) m -Si-R 16 -S l -R 16 -Si-(R 15 ) m (OR 15 ) 3-m··· (2) (In formula (2), R 15 are independently alkyl groups having 1 to 18 carbon atoms, C a H 2a+1 O-((CH 2 ) b O) c where a is 1 to 18, b is 1 to 6, and c is 1 to 18; R 16 is an alkylene group having 1 to 9 carbon atoms or a divalent phenyl group, l is an integer of 1 to 9, and m is an integer of 0, 1, or 2.

[0055] Specific examples of other organic silicon compounds that can be used in combination include, but are not limited to, Kabras 2 and Kabras 4 manufactured by Osaka Soda Co., Ltd., Si-75 corresponding to the Kabras-2 type, Si-69 corresponding to the Kabras-4 type, and Si-363 represented by the following formula (3), manufactured by Degussa Co., Ltd., A-1289 corresponding to the Kabras-4 type, manufactured by Momentive Co., Ltd., A-189 which is 3-mercaptopropyltrimethoxysilane, and KBE-846 manufactured by Shin-Etsu Chemical Co., Ltd., which corresponds to the Kabras-4 type, etc. These compounds can also be used alone or in combination.

[0056] [ka]

[0057] In addition, it is preferred that the total mass of at least one of the organosilicon compound of the present invention, vinyl organosilicon compounds, alkyl organosilicon compounds, epoxy organosilicon compounds, methacrylic organosilicon compounds, (poly)sulfide organosilicon compounds, and condensates thereof does not exceed 30 parts by mass per 100 parts by mass of the silica-based filler.

[0058] Basic Compounds (D) The basic compound (D) used in the rubber composition in step A is not particularly limited, but examples thereof include a primary amine compound (d-1), a secondary amine compound (d-2), and a tertiary amine compound (d-3).

[0059] Examples of the primary amine compound (d-1) include ethylamine, n-propylamine, isopropylamine, 1,2-dimethylpropylamine, n-butylamine, isobutylamine, sec-butylamine, tert-butylamine, isoamylamine, tert-amylamine, 3-pentylamine, n-amylamine, n-hexylamine, n-heptylamine, n-octylamine, 2-octylamine, tert-octylamine, 2-ethylhexylamine, n-nonylamine, n-aminodecane, n-aminoundecane, n-dodecylamine, and n- Examples of the alkylamines include alkylamines having a straight-chain or branched hydrocarbon group, such as tridecylamine, 2-tridecylamine, n-tetradecylamine, n-pentadecylamine, n-hexadecylamine, n-heptadecylamine, n-octadecylamine, n-oleylamine, benzylamine, 2-phenylethylamine, 3-phenylpropylamine, ethanolamine, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropylmethyldimethoxysilane, and 3-aminopropylmethyldiethoxysilane.

[0060] Other examples include alicyclic amines such as cyclopropylamine, cyclobutylamine, cyclopropylamine, cyclohexylamine, cycloheptylamine, and cyclooctylamine, and aromatic amines such as aniline, etc. Furthermore, other examples include ether amines such as 3-isopropoxypropylamine, isobutoxypropylamine, and morpholine.

[0061] Examples of the secondary amine compound (d-2) include N,N-dipropylamine, N,N-dibutylamine, N,N-dipentylamine, N,N-dihexylamine, N,N-dipeptylamine, N,N-dioctylamine, N,N-dinonylamine, N,N-didecylamine, N,N-diundecylamine, N,N-didodecylamine, N,N-distearylamine, N-methyl-N-propylamine, N-ethyl-N-propylamine, N-propyl-N-butylamine, bis(2-ethylhexyl)amine, N-methylaminopropyltrimethoxysilane, (3-(butylamino)propyl)trimethoxysilane, 3-(N-phenyl)aminopropyltrimethoxysilane, bis(3-(trimethoxysilyl)propyl)amine, and cyclic amines such as piperidine.

[0062] Examples of the tertiary amine compound (d-3) include triethylamine, tributylamine, trihexylamine, dimethyloctylamine, dimethyldecylamine, dimethyllaurylamine, dimethylmyristylamine, dimethylpalmitylamine, dimethylstearylamine, dilaurylmonomethylamine, quinuclidine, dimethylaminoethanol, pyridine, (3-(dimethylamino)propyl)trimethoxysilane, (3-(diethylamino)propyl)trimethoxysilane, and the like.

[0063] Furthermore, in the present invention, a diamine compound (d-4) having two amino groups in one compound can also be used. Examples of the diamine compound (d-4) include ethylenediamine, N,N-dimethylethylenediamine, N,N'-dimethylethylenediamine, N-ethylethylenediamine, N,N-diethylethylenediamine, N,N'-diethylethylenediamine, 1,3-propanediamine, 2,2-dimethyl-1,3-propanediamine, N,N-dimethyl-1,3-propanediamine, and N,N'-dimethyl-1,3-propanediamine. diamine, N,N-diethyl-1,3-propanediamine, N,N'-diethyl-1,3-propanediamine, 1,4-butanediamine, N,N-dimethyl-1,4-butanediamine, N,N'-dimethyl-1,4-butanediamine, N,N-diethyl-1,4-butanediamine, N,N'-diethyl-1,4-butanediamine, 1,5-pentanediamine, 1,5-diamino-2-methylpentane, 1,6 -hexanediamine, N,N-dimethyl-1,6-hexanediamine, N,N'-dimethyl-1,6-hexanediamine, 1,7-heptanediamine, 1,8-octanediamine, 2-(2-aminoethylamino)ethanol, imidazole, N,N-dimethylaminopyridine (DMAP), diazabicyclononene (DBN), diazabicycloundecene (DBU), 1,4-diazabicyclo[2.2.2]octane (DABCO), 1,8-bis(dimethylamino)naphthalene (proton sponge), N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, N-(6-aminohexyl)-3-aminopropyltrimethoxysilane, and the like can be exemplified.

[0064] In addition to the above, examples of the basic compound (D) of the present invention include diethylenetriamine, 1,3-diphenylguanidine, 1,3-di-o-tolylguanidine, 1,2,3-triphenylguanidine, triethylenetetramine, and hexamethylenetetramine.

[0065] In the rubber composition of the present invention, the basic compound (D) may be used alone or in combination of two or more of the above-mentioned compounds.

[0066] Among these, as the basic compound (D), 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, quinuclidine, diazabicycloundecene (DBU), 1,3-diphenylguanidine, 1,3-di-o-tolylguanidine, 1,2,3-triphenylguanidine, and hexamethylenetetramine are preferred, and 3-aminopropyltriethoxysilane and 1,3-diphenylguanidine are more preferred.

[0067] The amount of the basic compound in the rubber composition of the present invention may be 0.1 to 10 parts by mass, more preferably 0.1 to 5 parts by mass, particularly preferably 0.5 to 5 parts by mass, further preferably 0.5 to 3 parts by mass, and most preferably 0.5 to 1.5 parts by mass, based on 100 parts by mass of rubber.

[0068] Mixing conditions in process A In step A, rubber (A), an inorganic filler (B), a silane coupling agent (C), and a basic compound (D) are kneaded to obtain a rubber composition.

[0069] It is preferable that the step A is carried out before the step B in which a vulcanizing agent is added and vulcanized. That is, the step A is a step in which an inorganic filler (B), a silane coupling agent (C), and a basic compound (D) are kneaded with rubber before the vulcanizing agent is added, thereby obtaining a rubber composition.

[0070] In the step A, the rubber (A), the inorganic filler (B), the silane coupling agent (C) and the basic compound (D) are preferably kneaded at 80 to 250°C, more preferably at 80 to 200°C. By kneading the above components in this temperature range, the inorganic filler and the like can be uniformly dispersed without gelling or scorching the kneaded mixture, and each component can be kneaded suitably. In addition, since no vulcanizing agent is added in the step A, it is possible to knead at a relatively high temperature without worrying about the formation of crosslinks. The kneading time in the step A is not particularly limited, but is, for example, 1 minute to 1 hour.

[0071] For the kneading in the step A, various mixing machines usually used in the rubber industry, such as a roll, a pressure kneader, an intermixer, a Banbury mixer, etc., can be used.

[0072] In step A, the order in which the rubber (A), inorganic filler (B), silane coupling agent (C), and basic compound (D) are added is not particularly limited, but it is preferable to add only the rubber (A) first, pre-mix, and then add the other components in that order.

[0073] Usually, when obtaining a rubber vulcanizate, in step A, rubber (A), inorganic filler (B), and silane coupling agent (C) are kneaded to obtain a rubber composition, and then in step B, a basic compound (D), a vulcanizing agent, etc. are added and vulcanization is performed to obtain a rubber vulcanizate. However, the key point in the manufacturing method of the present invention is that in step A, in addition to rubber (A), inorganic filler (B), and silane coupling agent (C), a basic compound (D) is also added and kneaded to obtain a rubber composition, and then in step B, a vulcanizing agent, etc. are added and vulcanization is performed to obtain a rubber vulcanizate, thereby obtaining a rubber vulcanizate that enables the production of tires with low fuel consumption and excellent grip.

[0074] This is because in process A, in addition to the rubber (A), inorganic filler (B), and silane coupling agent (C), a basic compound (D) is also added and then kneaded, which promotes the decomposition of the thioester bond and generates more mercaptosilane.

[0075] B process Step B in the method for producing a rubber vulcanizate of the present invention is a step in which compounding agents normally used in the rubber industry are added to the rubber composition obtained in step A, and the mixture is vulcanized to obtain a rubber vulcanizate.

[0076] In step B, compounding agents that are usually used in the rubber industry can be used in the rubber composition obtained in step A, as long as they do not deviate from the spirit of the present invention. For example, vulcanizing agents, processing aids such as stearic acid, titanate coupling agents, antioxidants such as phenyl-α-naphthylamine and N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine, fillers such as carbon black and calcium carbonate, sulfenamide crosslinking accelerators, crosslinking accelerators (auxiliaries) such as zinc oxide (zinc oxide), reinforcing agents, softeners, plasticizers, tackifiers, scorch inhibitors, etc. can be used.

[0077] Such a vulcanizing agent is not particularly limited as long as it is one that is usually added during the kneading operation of a rubber composition, but it is more preferable that the vulcanizing agent is at least one selected from sulfur, selenium, an organic peroxide, morpholine disulfide, a thiuram compound, and an oxime compound.

[0078] The content of the vulcanizing agent contained in the rubber composition according to the present invention is not particularly limited, but is preferably 0.1 to 20 parts by weight, more preferably 0.2 to 15 parts by weight, and even more preferably 0.5 to 10 parts by weight, per 100 parts by weight of rubber.

[0079] The content of the vulcanizing agent is preferably 0.1 parts by weight or more per 100 parts by weight of rubber, since the rubber can be crosslinked appropriately, and the content of the vulcanizing agent is preferably 20 parts by weight or less per 100 parts by weight of rubber, since rubber-like elasticity can be maintained.

[0080] Examples of sulfenamide crosslinking accelerators include N-cyclohexyl-2-benzothiazyl sulfenamide, N,N-dicyclohexyl-2-benzothiazyl sulfenamide, N-oxydiethylene-2-benzothiazyl sulfenamide, N-tert-butyl-2-benzothiazyl sulfenamide, and N-tert-butyl-di(2-benzothiazole)sulfenimide.

[0081] The amount of the crosslinking accelerator (auxiliary agent) in the rubber composition is preferably 0.1 to 15 parts by mass, more preferably 1 to 10 parts by mass, and particularly preferably 3 to 9 parts by mass, relative to 100 parts by mass of rubber. The amount of the crosslinking accelerator (auxiliary agent) is the total amount of the crosslinking accelerator and the crosslinking accelerator auxiliary agent, and when both the crosslinking accelerator and the crosslinking accelerator auxiliary agent are used, it represents the total amount of them.

[0082] Examples of processing aids include higher fatty acids such as stearic acid, oleic acid, palmitic acid, and lauric acid; higher fatty acid amides such as stearic acid amide and oleic acid amide; higher fatty acid esters such as ethyl oleate; and higher aliphatic amines such as stearylamine and oleylamine.

[0083] The amount of the processing aid in the rubber composition is, for example, 300 parts by mass or less, preferably 100 parts by mass or less, more preferably 50 parts by mass or less, and particularly preferably 10 parts by mass or less, per 100 parts by mass of rubber.

[0084] Examples of the softening agent include petroleum waxes such as carnauba wax and ceresin wax; polyglycols such as ethylene glycol, glycerin and diethylene glycol; aliphatic hydrocarbons such as vaseline, paraffin and naphthene; and silicone oils.

[0085] The amount of the softener in the rubber composition is, for example, 300 parts by mass or less, preferably 100 parts by mass or less, more preferably 50 parts by mass or less, and particularly preferably 30 parts by mass or less, per 100 parts by mass of rubber.

[0086] The amount of the antioxidant mixed in the rubber composition is, for example, 30 parts by mass or less, preferably 10 parts by mass or less, and more preferably 5 parts by mass or less, per 100 parts by mass of rubber.

[0087] The rubber composition may further contain carbon black. Examples of carbon black include, but are not limited to, carbon blacks of various classes such as SRF, FEF, HAF, ISAF, and SAF.

[0088] The amount of carbon black contained is preferably 0.5 to 100 parts by mass, more preferably 1 to 90 parts by mass, and particularly preferably 2 to 80 parts by mass, based on 100 parts by mass of rubber.

[0089] Vulcanization conditions in B process In step B, the rubber composition obtained in step A is appropriately added with the above-mentioned compounding materials, and vulcanized to obtain a rubber vulcanizate. That is, a rubber composition for crosslinking is obtained. In step B, the above-mentioned compounding materials (e.g., vulcanizing agent, etc.) are added to the rubber composition obtained in step A, and kneading is preferably performed at 100°C or higher. The rubber vulcanizate is obtained by heating preferably at 120 to 230°C for 1 minute to 3 hours. A mold may also be used during vulcanization.

[0090] Use of rubber composition The rubber vulcanizate obtained in step B can be used for various purposes as a rubber product. The shape of the rubber vulcanizate is not particularly limited, and it can be used as a tire, a tube, a belt, a hose, an industrial product, etc.

[0091] As described above, the rubber vulcanizate has a small hysteresis loss, and therefore, when used as a tire, for example, it can reduce energy loss during tire running and rolling resistance, and therefore can be suitably used in rubber parts that are used dynamically, such as tires (especially tread portions).

[0092] EXAMPLES

[0093] The present invention will be described in more detail in the following examples, but is not limited thereto.

[0094] (Synthesis Example 1) Preparation of a silane coupling agent represented by formula (X) ((EtO) 3 Si-(CH 2 ) 3 -SC(=O)-C 17 H 35 (Production) To a solution of 98.66 g of 3-mercaptopropyltriethoxysilane in 1300 ml of petroleum ether (boiling range 50-70°C) was added 48.15 g of triethylamine at 5°C, followed by dropwise addition of 125.35 g of stearic acid chloride using a heatable dropping funnel. After heating at reflux for 90 min, the cooled suspension was filtered, the filter cake was rewashed twice with petroleum ether, the resulting filtrates were combined and the solvent was removed. 1 The silane coupling agent represented by formula (X) was identified by H-NMR analysis and 186.71 g (organosilicon compound 1) was obtained. The physical properties are shown below. 1 H NMR (400 MHz, CDCl 3 )δ3.8(q, J=6.8Hz, 6H), 2.9(t, J=7.2Hz, 2H), 2.5(t, J=8.0Hz, 2H), 1.7-1.6(m, 4 H), 1.4-1.2(m, 28H), 1.2(t, J=6.8Hz, 9H), 0.9(t, J=6.8Hz, 3H), 0.8-0.6(m, 2H)

[0095] [Production of Rubber Vulcanizate] Examples 1-2, Comparative Examples 1-2 The kneading test was carried out using a Labo Plastomill 10C100 (manufactured by Toyo Seiki Co., Ltd.) equipped with a 250cc Banbury mixer-type attachment BR-250. The temperature of the device was 100°C with oil circulation heating, and the rotor rotation speed of the mixer was constant at 80 rpm. The compounding test was carried out on a 100g rubber basis. The procedure was to masticate the rubber component for 30 seconds, then add the chemicals shown in the compounding (I) in Table 1, and knead for 30 seconds. Next, the chemicals shown in the compounding (II) in Table 1 were added and kneaded for 3 minutes, after which a rubber composition was obtained (step A). ​​The amount of the organosilicon compound in the examples and comparative examples was adjusted so that the amount of silicon in the organosilicon compound in the examples and comparative examples was the same. The amount of sulfur added in the examples and comparative examples was adjusted so that the amount of sulfur in the system was the same. The discharged rubber composition was cooled on a 6-inch roll at room temperature, and then the crosslinking agent components shown in the compounding (III) in Table 1 were added and kneaded for 6 minutes to obtain a rubber vulcanizate (uncrosslinked sheet) with a thickness of about 2 mm (step B). The next day, the remaining compound was subjected to heat press crosslinking at 160°C for 20 minutes to obtain a test sample (crosslinked sheet). In Examples 1 and 2, the basic compound was added in step A, and in Comparative Examples 1 and 2, the basic compound was added in step B.

[0096] <Dynamic viscoelasticity test> A test piece with a width of 4 mm, length of 25 mm, and thickness of 2 mm was punched out from the test sample (crosslinked sheet), and tan δ was measured using Rheogel-4000 manufactured by UBM Co., Ltd. under the conditions of a chuck distance of 20 mm, an initial strain of 0.05%, and 10 Hz. The measurement temperature range was -40 to 80°C.

[0097] The compounding agents used in the examples and comparative examples are shown below. *1 JSR Corporation SL552 *2 Nipsil AQ (BET specific surface area 215m) manufactured by Tosoh Silica Corporation 2 / g) *3 Sunthene 415 manufactured by Nippon Oil Corporation *4 Sakura Stearic Acid, manufactured by NOF Corporation *5 Nocrac 6C manufactured by Ouchi Shinko Chemical Industry Co., Ltd. *6 Momentive Performance Materials, product name "NXT" *7 Zinc oxide type 2 manufactured by Sakai Chemical Industry Co., Ltd. *8 1,3-diphenylguanidine manufactured by Ouchi Shinko Chemical Industry Co., Ltd. *9 Noccela CZ manufactured by Ouchi Shinko Chemical Industry Co., Ltd. *10 Colloidal sulfur manufactured by Hosoi Chemical Industry Co., Ltd. *11 3-Aminopropyltriethoxysilane manufactured by Tokyo Chemical Industry Co., Ltd.

[0098] [Table 1]

[0099] The test samples (crosslinked sheets) obtained in Examples 1 and 2 and Comparative Examples 1 and 2 were subjected to the above-mentioned dynamic viscoelasticity test. The results are shown in Table 2.

[0100] [Table 2]

[0101] As shown in Table 2, in Examples 1 and 2 using the manufacturing method of the present invention (in step A, basic compound (D) is added and kneaded), compared with Comparative Examples 1 and 2 using a general manufacturing method (in step B, basic compound (D) is added and kneaded), tan δ at 0°C is large, suggesting excellent grip properties, and tan δ at 60°C is small, suggesting excellent fuel economy. Usually, as the tan δ value at 60°C decreases, the tan δ value at 0°C also tends to decrease, but Example 1 using the organosilicon compound of the present invention is preferable in that it is excellent in both grip properties and fuel economy.

[0102] (Synthesis Example 2) Production of a silane coupling agent represented by formula (Y-2) In a 1000mL three-neck flask equipped with a thermometer and a magnetic stirrer, 10.8g (82.3mmol) of 6-aminohexanoic acid (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.), 50g of ultrapure water, 150g of THF (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.), and 12.5g (123.4mmol) of triethylamine (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) were added. The flask was cooled to 5°C while stirring with a magnetic stirrer, and then 13.4g (82.3mmol) of n-octanoyl chloride (manufactured by Tokyo Chemical Industry Co., Ltd.) was added. The temperature was then raised to room temperature and stirred overnight. After the reaction was completed, the mixture was concentrated under reduced pressure to remove THF, and the pH was adjusted to 1 with hydrochloric acid. The resulting white solid was filtered, and the filter residue was washed with ultrapure water. The resulting filter residue was dissolved in ethanol, and ultrapure water was added thereto to cause recrystallization. The obtained solid was filtered, and the filter residue was washed with ultrapure water and dried to obtain 20.0 g (yield 97%) of N-octanoyl-6-aminohexanoic acid.

[0103] 20.0 g (77.7 mmol) of N-octanoyl-6-aminohexanoic acid obtained above, 500 g of dichloromethane (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), 18.5 g (77.7 mmol) of 3-mercaptopropyltriethoxysilane (manufactured by Tokyo Chemical Industry Co., Ltd.), and 0.95 g (7.8 mmol) of N,N-dimethyl-4-aminopyridine (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were added to a 500 mL three-neck flask equipped with a thermometer and a magnetic stirrer. The flask was cooled to 5°C while stirring with a magnetic stirrer, and then 17.6 g (85.5 mmol) of N,N'-dicyclohexylcarbodiimide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added. The mixture was then heated to room temperature and stirred for 3 hours. After the reaction was completed, the reaction solution was filtered and the filtrate was concentrated under reduced pressure, and then purified by silica gel chromatography (n-hexane / ethyl acetate = 8 / 2) to obtain 26.6 g (72% yield) of organosilicon compound 2 (formula [4]) as a colorless, transparent liquid. The physical properties are shown below. 1 H NMR (400 MHz, CDCl 3)δ 5.4(br, 1H), 3.8(q, J=6.8Hz, 6H), 3.2(q, J=6.8Hz, 2H), 2.9(t, J=7.6Hz, 2H), 2.5(t, J=7.6Hz, 2H), 2.1(t, J=7.6 Hz, 2H), 1.7-1.6(m, 6H), 1.6-1.4(m, 2H), 1.4-1.3(m, 10H), 1.2(t, J=6.8Hz, 9H), 0.9-0.8(m, 3H), 0.7-0.6(m, 2H)

[0104] [ka]

[0105] (Synthesis Example 3) Production of a silane coupling agent represented by formula (Y-1) In a 200 mL three-neck flask equipped with a thermometer and a magnetic stirrer, 12.0 g (53.8 mmol) of N-carbobenzoxy-L-alanine (manufactured by Tokyo Chemical Industry Co., Ltd.), 120 g of dichloromethane (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), 12.8 g (53.8 mmol) of 3-mercaptopropyltriethoxysilane (manufactured by Tokyo Chemical Industry Co., Ltd.), and 0.66 g (5.4 mmol) of N,N-dimethyl-4-aminopyridine (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were added. The flask was cooled to 5°C while stirring with a magnetic stirrer, and then 12.2 g (59.1 mmol) of N,N'-dicyclohexylcarbodiimide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added. The mixture was then heated to room temperature and stirred for 3 hours. After the reaction was completed, the reaction solution was filtered and the filtrate was concentrated under reduced pressure, and then purified by silica gel chromatography (n-hexane / ethyl acetate = 9 / 1) to obtain 19.5 g (82% yield) of organosilicon compound 3 (formula [5]) as a colorless, transparent liquid. The physical properties are shown below. 1 H NMR (500 MHz, CDCl 3 )δ 7.4-7.3(m, 5H), 5.3-5.2(m, 1H), 5.2-5.1(m, 2H), 4.5-4.4(m, 1H), 3.8(q, J=7.0Hz, 6H), 2.9 (t, J=7.5Hz, 2H), 1.8-1.6(m, 2H), 1.4(d, J=7.5Hz, 3H), 1.2(t, J=7.0Hz, 9H), 0.8-0.7(m, 2H)

[0106] [ka]

[0107] A rubber vulcanizate was produced in the same manner as in Example 1 according to the formulation shown in Table 3, and a test sample (crosslinked sheet) was obtained. The test sample was subjected to the dynamic viscoelasticity test described above, and the results are shown in Table 4.

[0108] [Table 3]

[0109] [Table 4]

[0110] As shown in Table 4, in Examples 3 and 4 (in step A, basic compound (D) was added and kneaded) using the manufacturing method of the present invention, the tan δ at 0°C was large, suggesting excellent grip properties, and the tan δ at 60°C was small, suggesting excellent fuel efficiency.

Claims

1. a step (step A) of kneading rubber (A), an inorganic filler (B), a silane coupling agent (C), and a basic compound (D) to obtain a rubber composition; The method for producing a rubber vulcanizate includes a step (step B) of adding a vulcanizing agent to the rubber composition obtained in the step A, and vulcanizing the rubber composition to obtain a rubber vulcanizate, The silane coupling agent (C) is at least one selected from the group consisting of (protected) mercapto-based organosilicon compounds, organosilicon compounds having a skeleton of an amino acid or a derivative thereof, and condensates thereof, and compounds represented by formula (X). (R) 1 O) 3 Si-R 2 -S-C(=O)-C 17 H 35 …(X) [In formula (X), R 1 are each independently H or (C 1 ~C 8 ) alkyl, R 2 is a straight chain (C 1 ~C 8 ) double bonded hydrocarbon or branched chain (C 1 ~C 8 ) double bonded hydrocarbons, saturated (C 1 ~C 8 ) double bond hydrocarbon or unsaturated (C 1 ~C 8 ) means a double bonded hydrocarbon, and the alkyl group C 17 H 35 is branched or linear.

2. In the formula (X), R 1 is ethyl, R 2 CH 2 CH 2 CH 2 and the alkyl group C 17 H 35 The method for producing a rubber vulcanizate according to claim 1 , wherein is a linear silane coupling agent.

3. The method for producing a rubber vulcanizate according to claim 1, wherein the organosilicon compound having a skeleton of an amino acid or a derivative thereof is an organosilicon compound represented by formula [Y-1] and / or an organosilicon compound represented by formula [Y-2], or a condensate thereof. (R 3 O) 3 Si-R 4 -S-C(=O)-C(-R 5 )-NH-R 6 …[Y-1] [In formula [Y-1], R 3 are each independently H or (C 1 ~C 8 ) alkyl, R 4 is a straight chain (C 1 ~C 8 ) double bonded hydrocarbon or branched chain (C 1 ~C 8 ) double bonded hydrocarbons, saturated (C 1 ~C 8 ) double bond hydrocarbon or unsaturated (C 1 ~C 8 ) double bonded hydrocarbon, R 5 is hydrogen or an organic group; R 6 is hydrogen or a protecting group for an amino group; or (R 7 O) 3 Si-R 8 -S-C(=O)-R 9 -NH-R 10 …[Y-2] [In formula [Y-2], R 7 are each independently H or (C 1 ~C 8 ) alkyl, R 8 is a straight chain (C 1 ~C 8 ) double bonded hydrocarbon or branched chain (C 1 ~C 8 ) double bonded hydrocarbons, saturated (C 1 ~C 8 ) double bond hydrocarbon or unsaturated (C 1 ~C 8 ) double bonded hydrocarbon, R 9 is a divalent hydrocarbon group having 1 to 20 carbon atoms which may contain a substituted or unsubstituted aromatic ring, R 10 is hydrogen or a protecting group for an amino group.

4. 2. The method for producing a rubber vulcanizate according to claim 1, wherein the (protected) mercapto-based organosilicon compound is a compound represented by the general formula [Z]. R 11 n (R 12 ) 3-n -Si-R 13 -S-C-R 14 …[Z] (In formula [Z], R 11 are each independently a hydrocarbon group, R 12 each independently represents an alkoxy group, R 13 is a divalent hydrocarbon group, R 14 is a monovalent hydrocarbon having 1 to 18 carbon atoms. n is an integer of 0, 1, or 2.

5. The method for producing a rubber vulcanizate according to any one of claims 1 to 4, wherein the rubber (A) is one or more selected from natural rubber (NR), polyisoprene rubber (IR), styrene butadiene copolymer rubber (SBR), polybutadiene rubber (BR), acrylonitrile butadiene copolymer rubber (NBR), chloroprene rubber (CR), ethylene propylene copolymer rubber (EPDM), and butyl rubber (IIR).

Citation Information

Patent Citations

  • Production of sulfur-containing organosilicon compound and production of its synthetic intermediate

    JP2000103794A

Cited By

  • Rubber composition and tire

    JP2023097015A

  • Rubber composition and tires

    JP7834475B2