Sealing sheet and display having resin composition layer
The sealing sheet with a resin composition layer addresses embeddability and light resistance issues in micro LED displays, ensuring high clarity and longevity by using a (meth)acrylic resin and specific embeddability improvers, enhancing adhesion and resistance.
Patent Information
- Application Number
- JP2023079778
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-15
- Publication Date
- 2024-11-27
- Estimated Expiration
- 2043-05-15
Smart Images

Figure 2024164361000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to an encapsulating sheet, and more particularly, to an encapsulating sheet including a resin composition layer for encapsulating a plurality of light-emitting elements used in various products including, for example, electronic devices and displays, and a display equipped with the resin composition layer. [Background technology]
[0002] In recent years, displays have been actively developed using various light-emitting elements in order to achieve higher performance. Specifically, various display specifications are being researched, such as backlit displays using liquid crystal or quantum dots, displays using self-emitting elements such as mini / micro LEDs and organic EL, plasma displays, and electrophoretic displays, and a wide range of uses are being considered, from large display applications such as signage and televisions to small-sized devices such as tablets, personal computers, smartphones, and wearable devices. In particular, the development of displays using LEDs is progressing day by day, and Patent Document 1 describes a thermosetting resin composition that encapsulates LED elements. Micro LED displays are attracting the most attention as a next-generation display technology. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2023-12051 A Summary of the Invention [Problem to be solved by the invention]
[0004] Patent Document 1 describes a sheet-shaped resin composition for encapsulating optical semiconductor elements, which has excellent heat resistance. However, in LED elements, which have been getting smaller in recent years, the spacing between the LED elements is becoming narrower, and it is difficult for the sheet-shaped resin composition described in Patent Document 1 to fill the space (embedding) by following the micro-sized LED elements. If there is space between the LED elements and the encapsulating resin composition, light is refracted, and the clarity of the display is deteriorated. Furthermore, when displays are used outdoors, they require high light resistance, but existing encapsulating sheets tend to yellow over time when exposed to sunlight, causing the images shown on the display to turn yellow. In order to create a display that is clear and has little yellowing over time, an encapsulating sheet that has excellent embedding properties and light resistance is required.
[0005] The present disclosure has been made in consideration of the above problems, and has an object to provide a display having an encapsulating sheet and a resin composition layer that are excellent in embeddability and light resistance, even when applied to a display using not only LED elements but also a plurality of various light-emitting elements such as organic EL as a light source. Another objective is to provide an encapsulating sheet that has excellent adhesion to a substrate and excellent zipping properties from the viewpoint of simplifying the manufacturing process of micro LED displays. [Means for solving the problem]
[0006] As a result of intensive studies, the present inventors have found that the above problems can be solved by the encapsulating sheet described below, and have completed the present inventions [1] to [7] below. [1]: An encapsulating sheet for encapsulating light-emitting elements used in a display having a plurality of light-emitting elements as a light source, the encapsulating sheet comprising a resin composition layer containing a resin (A) and an embeddability improver (B), the resin (A) having a glass transition temperature (Tg) of −30 to 40° C. and a weight average molecular weight (Mw) of 10,000 to 1,000,000, the embeddability improver (B) containing a phosphorus-containing compound (B1) and a phenolic hydroxyl group-containing compound (B2), and the resin composition layer having a thickness Ta of 1 to 100 μm. [2]: The resin (A) is a (meth)acrylic resin (a), The (meth)acrylic resin (a) is a copolymer having a structural unit derived from an acrylic acid alkyl ester (a1) having a linear, branched or cyclic saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms, and a structural unit derived from a methacrylic acid alkyl ester (a2) having a linear, branched or cyclic saturated aliphatic hydrocarbon group having 1 to 8 carbon atoms. The encapsulating sheet according to [1]. [3]: The encapsulating sheet according to [2], wherein the (meth)acrylic resin (a) further contains a structural unit derived from (meth)acrylic acid (a3). [4]: The encapsulating sheet according to [1], wherein the resin (A) is contained in an amount of 76 to 99.9 mass% based on the total mass of the resin composition layer. [5]: The encapsulating sheet according to [1], wherein the content of the embeddability improver (B) is 0.1 to 15 mass % based on the total mass of the resin composition layer. [6]: The encapsulating sheet according to [1], wherein a mass ratio B1:B2 of the phosphorus-containing compound (B1) to the phenolic hydroxyl group-containing compound (B2) in the embeddability improver (B) is 0.1:1 to 10:1. [7]: The encapsulating sheet according to any one of [1] to [6], wherein the resin composition layer has a loss tangent (Tan δ40) at 40° C. obtained by dynamic viscoelasticity measurement at a frequency of 10 Hz in a tensile mode of 0.8 to 2.0. [8]: A display having an encapsulating layer comprising the resin composition layer of the encapsulating sheet according to [7]. Effect of the Invention
[0007] According to the present disclosure, it is possible to provide an encapsulating sheet that has excellent embedding properties and light resistance even when applied to a display that uses a plurality of light-emitting elements as a light source. In addition to the above, the present disclosure also makes it possible to provide an encapsulating sheet that has excellent embeddability, light resistance, adhesion to a substrate, and zipping properties even when applied to a display that uses a micro LED element as a light source. [Brief description of the drawings]
[0008] [Figure 1] FIG. 2 is a schematic cross-sectional view showing an example of a laminate configuration of an encapsulating sheet. [Diagram 2] 1A to 1C are schematic cross-sectional views showing a process of sealing a plurality of light-emitting elements on a substrate having the light-emitting elements. [Diagram 3] FIG. 1 is a cross-sectional view showing an example of a test substrate simulating a micro LED substrate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The present disclosure will be described in detail below. Note that the embodiment described below is an example of the present disclosure. The present disclosure is not limited to the following embodiment, and includes modified examples that are implemented within the scope of the present disclosure. In this specification, a numerical range specified by using "~" includes the numerical values before and after "~" as the lower and upper limit ranges. (Meth)acrylic acid refers to acrylic acid and methacrylic acid. In addition, unless otherwise noted, each of the various components appearing in this specification may be used independently, either alone or in combination of two or more.
[0010] In the present disclosure, the resin (A) has a weight average molecular weight (Mw) of 10,000 or more and 1,000,000 or less, the glass transition temperature (Tg) of the resin (A) is -30°C to 40°C, the embeddability improver (B) contains a phosphorus-containing compound (B1) and a phenolic hydroxyl group-containing compound (B2), and the thickness Ta of the resin composition layer is 1 to 100 μm, thereby improving light resistance and embeddability. Furthermore, adhesion and zipping properties can also be improved. The present inventors' speculations regarding the above effects are described in the following items.
[0011] [Form of encapsulating sheet] The encapsulating sheet of the present disclosure includes at least a resin composition layer. The encapsulating sheet may have a structure in which a resin composition layer 2 and a release liner 4 are laminated as shown in Fig. 1(a), or a structure in which the resin composition layer 2 is laminated with a substrate 3 as shown in Fig. 1(b). The number of laminated structures with the substrate or the release liner is not particularly limited.
[0012] The release liner may be a polyester film such as polyethylene terephthalate, polybutylene terephthalate, or polyethylene naphthalate, or a plastic film or sheet such as a polyolefin film such as polypropylene or polyethylene, to which a release agent such as silicone resin is applied to provide a release layer. There is no particular limitation on the thickness of the release liner, but it is about 10 to 200 μm.
[0013] The substrate is not particularly limited, and examples thereof include various optical films such as plastic films, anti-reflection (AR) films, polarizing plates, and retardation plates. Examples of the plastic films include polyvinyl chloride films, polyethylene films, polyethylene terephthalate (PET) films, polyurethane films, nylon films, polyolefin films, triacetyl cellulose films, and cycloolefin films. The thickness of the substrate is not particularly limited, and is preferably 10 to 2000 μm. The encapsulating sheet of the present disclosure preferably has a three-layer structure of substrate / resin composition layer / release liner.
[0014] The encapsulating sheet of the present disclosure most preferably has a three-layer structure of a first release liner 4a / a resin composition layer 2 / a second release liner 4b, as shown in FIG. 1(c). The first release liner and the second release liner can be arbitrarily selected, and the same release liner may be used. From the perspective of handling, it is preferable that the first release liner is a light release liner and the second release liner is a heavy release liner. The thickness Tl of the light release liner is preferably in the range of 10 to 150 μm, and the thickness Th of the heavy release liner is preferably in the range of 25 to 200 μm, and it is preferable to satisfy the relationship of Tl < Th. Further, when the sealing sheet is in a roll form, it is preferable to provide the light release liner on the outer side of the roll. The release force of the first release liner and the second release liner can be adjusted by the release treatment of the adhesion surface with the resin composition layer of each release liner. For example, it can be adjusted by the type of release agent, the coating amount of the release agent, and the surface roughness of the release layer. When it is desired to reduce the value of the release force, treatments such as roughening the surface roughness and increasing the coating amount of the release agent are effective. When it is desired to increase the value of the release force, the opposite adjustment may be made. When taking the three-layer structure shown in Fig. 1(c), a manufacturing method in which the resin composition layer 2 is formed on the second release liner 4b and then the first release liner 4a is bonded is preferable.
[0015] After manufacturing the sealing sheet or while manufacturing the sealing sheet, a sealing sheet roll can be obtained by winding the sealing sheet around a core in a roll shape. The winding length can be designed according to the application. From the perspective of improving productivity, it is preferably 50 m or more, and more preferably 100 m or more. The winding length is preferably 10,000 m or less from the perspective of manufacturing yield.
[0016] The sealing sheet of the present disclosure is preferably used for sealing light-emitting elements used in a display having a plurality of light-emitting elements as light sources. Displays having a plurality of light-emitting elements as light sources include, for example, displays that require high quality, such as organic EL display panels and micro LED display panels. The resin composition layer constituting the encapsulating sheet is preferably laminated by directly adhering it to the adherend. The adherend to be adhered is not particularly limited, but is preferably acrylic, urethane, polycarbonate, epoxy, polyimide, glass, paper, cloth, aluminum, ceramic, or polyethylene terephthalate. Furthermore, the adherend is more preferably one having a substrate electrode portion made of metal, or one having a plurality of light-emitting element portions such as a backlight module, LED, or organic EL. In addition, one having a plurality of light-emitting element portions may further have a light-shielding layer between the light-emitting element portions.
[0017] Since the resin composition layer constituting the encapsulating sheet has high conformability to uneven surfaces, it is suitable to use the resin composition layer by filling the gaps between the light-emitting elements while conforming to a plurality of light-emitting elements. By filling the gaps between the light-emitting elements with the resin composition layer, a sealing layer made of the resin composition layer is formed. The sealing layer has a function of fixing the adjacent light-emitting elements and preventing them from falling off or becoming biased. In particular, since the resin composition layer of the encapsulating sheet of the present disclosure can conform to micro-sized light-emitting elements, micro LEDs are more suitable as light-emitting elements, and it is more preferable to use the resin composition layer as a sealing layer for a micro LED display panel. A micro LED is a tiny LED chip that is 50μm or less than 100μm in size. By mounting multiple micro LEDs (chips) on a substrate with wiring and circuits, a display is formed that uses multiple light-emitting elements as light sources. Micro LEDs are made up of GaAs, GaP, AlGaInP, InGaN or other LED elements, sealing resin that seals them, a package substrate, electrodes, etc., and have an operating temperature of 25 to 60°C. An example of a process for forming a sealing layer will be described below with reference to FIG.
[0018] Step (a): Step of placing the encapsulating sheet As shown in FIG. 2(a), the resin composition layer of the encapsulating sheet is placed on a substrate having a plurality of light-emitting elements so as to directly cover the light-emitting elements. When the encapsulating sheet has a first release liner and a second release liner, the first release liner is peeled off to expose the resin composition layer, and then the encapsulating sheet is placed as described above. The second release liner may be peeled off immediately after placement, or may be peeled off after the pressing step described below. In this specification, the term "plurality of light-emitting elements" is not particularly limited as long as it is two or more light-emitting elements. In display applications, the number of light-emitting elements used is determined by the display size and the number of pixels. The color of the light emitted by the light emitting element is not particularly limited, and an organic EL light emitting element or an LED light emitting element can be used. Examples of the color of the light emitted include red, green, and blue. The size of the light-emitting element is 100 μm or less in thickness and 40,000 μm in plan view area. 2 The thickness is preferably 50 μm or less, and the area in plan view is preferably 10,000 μm or less. 2 More preferably, the thickness is 20 μm or less and the area in plan view is 2500 μm or less. 2 The following are even more preferred: The distance between the light emitting elements mounted on the substrate is, for example, 10 to 5000 μm. When a set of red, green, and blue light emitting elements is mounted on the substrate as one pixel, the distance between the pixels is, for example, 10 to 2000 μm, preferably 20 to 1800 μm, and more preferably 500 to 1500 μm. The distance between the light emitting elements in one pixel is, for example, 10 to 200 μm, preferably 10 to 100 μm, and more preferably 20 to 60 μm.
[0019] Process (b): Pressing process As shown in Fig. 2(b), the resin composition layer is fluidized by pressing and filled around and between a plurality of light emitting elements. The resin composition layer filled around and between a plurality of light emitting elements becomes a sealing layer. The pressing method is not particularly limited, but heat pressing and vacuum pressing are preferred. From the viewpoint of the filling property of the resin composition layer, the temperature during pressing is preferably 20 to 200°C, more preferably 30 to 150°C, further preferably 40 to 130°C, and most preferably 60 to 110°C. In order to improve the adhesion to the light emitting element or the adherend, heat aging may be further performed after pressing. The heating temperature is preferably 40 to 250°C, more preferably 80 to 220°C, and even more preferably 100 to 190°C. The heating time is preferably 30 to 300 minutes, more preferably 60 to 240 minutes, and even more preferably 90 to 180 minutes. By setting the heating temperature and heating time as described above, the residual stress in the resin composition layer can be removed and the adhesion surface can be smoothed. Heat aging may be performed after the step (c) described later.
[0020] Step (c): Etching step In step (c), etching is performed to remove or thin the sealing layer on the light-emitting element. By removing the sealing layer, the brightness of the light-emitting element is increased and visibility during light emission is ensured. The thickness of the sealing layer after etching is preferably about the same as the thickness of the light-emitting element as shown in FIG. 2(c-1) or less than the thickness of the light-emitting element as shown in FIG. 2(c-2). Note that the sealing layer does not have to be completely removed from the light-emitting element, as long as it is substantially removed, and some thin film may remain. Also, if visibility can be ensured, step (c) may be omitted. The etching method is not particularly limited, but preferred examples include wet etching methods such as chemical polishing using chemicals, physical polishing using an abrasive, laser etching, plasma etching using argon plasma or oxygen plasma, and dry etching methods such as ion beam etching. From the viewpoint of reducing surface irregularities, it is preferable to use wet etching and dry etching in combination. Alternatively, physical etching such as plasma processing may be used. For example, the etching conditions may be dry etching using a mixed gas of CF4 / O2 / N2 in an anisotropic plasma device at an output of 1500-3000 W for 180-600 seconds. In this case, the gas supply rate of CF4 may be, for example, 50-100 sccm, the gas supply rate of O2 may be, for example, 500-1000 sccm, and the gas supply rate of N2 may be, for example, 50-100 sccm.
[0021] As described above, through steps (a) to (c), the sealing layer can be formed from the resin composition layer. Next, the components of the encapsulating sheet of the present disclosure will be described in detail while citing preferred examples.
[0022] [Resin composition layer] The resin composition layer contains a resin (A) and an embeddability improver (B), and preferably further contains a crosslinking agent, and may contain other components. In the present disclosure, the resin (A) is a substance that has a function of bonding and fixing objects together as a binder, specifically, a function of bonding and fixing a substrate having a light-emitting element or a plurality of light-emitting elements.
[0023] The loss tangent (tan δ40) at 40°C obtained by dynamic viscoelasticity measurement of the resin composition layer of the present disclosure is preferably 0.8 to 2.2, more preferably 1.0 to 2.0, and even more preferably 1.5 to 1.9. By setting tan δ40 in the above range, the diffusibility of the pressure applied to the resin composition layer in the pressing process is improved, and the embedding property, adhesion to the adherend, and zipping property are improved. If tan δ40 is lower than 0.8, the diffusibility of the resin composition layer is too high in the pressing process, so that the resin composition layer is likely to flow, and the end of the sealing layer after the pressing process becomes thin. If tan δ40 is higher than 2.2, the diffusibility of the resin composition layer is too low in the pressing process, so that the fluidity of the resin composition layer is deteriorated, and an air space is formed between the adherend and the sealing layer. The above-mentioned loss tangent (tan δ) is the ratio of loss modulus / storage modulus obtained by dynamic viscoelasticity measurement in a tensile mode at a frequency of 10 Hz and at -50 to 150°C. Tan δ40 can be adjusted by the type and composition of resin (A). When resin (A) contains (meth)acrylic resin (a), tan δ40 can be increased by increasing the content of methacrylic acid alkyl ester (a2), and when it is desired to lower tan δ40, the opposite can be done.
[0024] In addition, the peak top temperature (tan δ peak temperature) of the loss tangent (tan δ) obtained by dynamic viscoelasticity measurement of the resin composition layer of the present disclosure refers to the temperature at which the tan δ peak is maximum, and when there are two or more peaks, refers to the lowest peak temperature. The tan δ peak temperature is preferably between 0 and 60°C, more preferably between 15 and 55°C, and even more preferably between 35 and 45°C. When the tan δ peak temperature is in the above range, the network structure of the molecular chain of the resin composition layer and the embeddability improver (B) can be stabilized through the heat aging process, and the residual stress of the resin can be sufficiently removed, thereby improving the adhesion to the adherend. The tan δ peak temperature of the present disclosure can be adjusted by the type and composition of the resin (A), the type and amount of the crosslinking agent, the type and amount of the embeddability improver (B), and the amount of other components. When the resin (A) contains a (meth)acrylic resin (a), the tan δ peak temperature can be increased by increasing the content of a monomer having a high homopolymer glass transition temperature (Tg), and the opposite can be used to lower the tan δ peak temperature. The glass transition temperature (Tg) of the homopolymer in the present disclosure can be the value described in POLYMER HANDBOOK, 1999, FOURTH EDITION. Specifically, examples of monomers having a homopolymer glass transition temperature (Tg) of 0° C. or higher include methyl acrylate, cyclohexyl acrylate, methyl methacrylate, and butyl methacrylate, and examples of monomers having a homopolymer glass transition temperature (Tg) of 0° C. or lower include butyl acrylate, hexyl acrylate, 2-ethylhexyl acrylate, lauryl acrylate, and 2-ethylhexyl methacrylate.
[0025] In addition, the peak top strength (tan δ peak strength) of the loss tangent (tan δ) in the range of -50 to 80°C obtained by dynamic viscoelasticity measurement of the resin composition layer of the present disclosure is the value of the loss tangent (tan δ) when the peak of tan δ is maximum, and when there are two or more peaks, it refers to the top strength of the peak on the lowest temperature side. The tan δ peak strength is preferably 0.8 to 2.2, more preferably 1.0 to 2.0, and even more preferably 1.5 to 1.9. By setting the tan δ peak strength within the above range, the absorption of pressure applied to the resin composition layer in the pressing step is improved, and the resin composition layer follows the light emitting element while forming a uniform sealing layer, improving embeddability. The tan δ peak intensity of the present disclosure can be adjusted by the type and composition of the resin (A). When the resin (A) contains a (meth)acrylic resin (a), the tan δ peak intensity can be lowered by increasing the content of the acrylic acid alkyl ester (a1), and when it is desired to increase the tan δ peak intensity, the opposite can be done.
[0026] The dynamic viscoelasticity and loss tangent (tan δ) in the present disclosure were measured by the methods described in the Examples below. When the resin composition layer contains a crosslinking agent, the crosslinking reaction caused by heating is in an incomplete state at the time of measurement.
[0027] From the viewpoint of embeddability and zipping property, the thickness Ta of the resin composition layer is 1 to 100 μm, preferably 3 to 50 μm, and more preferably 5 to 35 μm. By making the thickness Ta of the resin composition layer 1 μm or more, the stress when peeling off the release liner is efficiently dispersed, and sufficient zipping property is exhibited. In addition, the pressure in the pressing process is diffused within the resin composition layer, and sufficient embeddability is exhibited. When the thickness Ta of the resin composition layer is 100 μm or less, the pressure loss caused by the resin composition layer absorbing the pressure applied in the pressing process is small, and the resin composition layer flows sufficiently, so that excellent embeddability is exhibited. In addition, the stress applied to the resin composition layer when peeling off the release liner is less likely to be biased, so that excellent zipping property is exhibited. If the thickness Ta of the resin composition layer is smaller than 1 μm, the pressure is not fully dispersed in the resin composition layer when the resin composition layer flows during the pressing process, and bias is likely to occur, resulting in poor embedding properties. In addition, the stress applied to the resin composition layer when the release liner is peeled off is not fully dispersed, resulting in poor zipping properties. If the thickness Ta of the resin composition layer is larger than 100 μm, the end of the resin composition layer is likely to flow when the resin composition layer flows during the pressing process, the thickness of the resin composition layer becomes non-uniform, and a difference in the applied pressure occurs, resulting in poor embedding properties. In addition, cohesive failure is likely to occur in the resin composition layer, resulting in poor zipping properties. The resin composition layer may be in the form of a single layer or a laminate of two or more layers. The thickness Ta in the present disclosure was measured by the method described in the Examples below.
[0028] [Method of forming resin composition layer] The method for forming the resin composition layer is not particularly limited, but a suitable example is a method for forming a resin composition layer by coating a resin composition in which an arbitrary solvent is added to the components constituting the resin composition layer. The solvent is added for the purpose of adjusting the viscosity level to a level suitable for coating. For coating, known coating machines and techniques such as a comma coater, a die coater, a roll coater, a lip coater, a reverse coater, a gravure coater, a bar coater, a curtain coater, dip coating, spin coating, silk screen, casting, etc. The solvent contained in the resin composition can be removed by a drying process after coating. In a preferred embodiment, the resin composition can be applied to a support such as a release liner or a substrate, and then the applied film is heated and dried using a hot air oven, an infrared heater, etc., to form a resin composition layer on one side of the support. Furthermore, in order to increase the crosslink density of the resin composition layer, it is preferable to perform an aging treatment such as leaving it to stand under specific temperature conditions, or to irradiate it with UV or the like.
[0029] [Resin composition] The resin composition can be obtained by mixing the solvent, the resin (A), and the embeddability improver (B) while stirring. The optional solvent is used for the purpose of adjusting the viscosity and other processing suitability when mixing the resin (A) and the embeddability improver (B), so that any solvent that is compatible with the resin (A), such as an ester type, an ether ester type, an ether type, an alcohol type, or an aromatic type, can be appropriately used. Specifically, acetone, 2-butanone, ethyl acetate, cyclohexanone, toluene, xylene, isopropyl alcohol, and N-methyl-2-pyrrolidone are preferred examples. For stirring, a known stirring device can be used, and a disperser, mixer, shaker, homogenizer, etc. are preferred.
[0030] To obtain the resin composition, a two or more-stage manufacturing process may be used in which, first, a mixture is prepared by mixing the embeddability improver (B) with the resin (A) and an optional solvent, and, second, the resin (A), a crosslinking agent, and other components are added as necessary.
[0031] Resin (A) The resin (A) may be any of a thermosetting resin, a photocurable resin, and a thermoplastic resin, and may be used alone or in combination of two or more. From the viewpoint of embeddability, it is preferable to include at least one thermosetting resin. The thermosetting resin is a resin having a plurality of functional groups that can be utilized in a crosslinking reaction by heating, and may have a functional group capable of self-crosslinking. The resin may also include a thermosetting monomer, but in this embodiment, from the viewpoint of coating film strength, it is preferable to use a thermosetting resin having a weight average molecular weight (Mw) of 10,000 or more.
[0032] Suitable examples of the thermosetting resin include (meth)acrylic resin (a), maleic acid resin, polybutadiene resin, polyester resin, condensation type polyester resin, addition type polyester resin, melamine resin, urethane resin such as polyurethane resin and polyurethane urea resin, epoxy resin, polycarbonate resin, oxetane resin, phenoxy resin, polyimide resin, polyamideimide resin, alkyd resin, amino resin, polylactic acid resin, oxazoline resin, benzoxazine resin, silicon resin, fluororesin, etc. From the viewpoint of embedding property, it is preferable to contain at least one of (meth)acrylic resin (a), epoxy resin, urethane resin, polycarbonate resin, and polyamide resin. Furthermore, from the viewpoint of adhesion to the adherend and zipping property, it is more preferable to contain (meth)acrylic resin (a). In addition, from the viewpoint of light resistance, it is most preferable to contain (meth)acrylic resin (a) which has high transparency and is not easily oxidized and deteriorated.
[0033] The functional group of the thermosetting resin may be appropriately selected depending on the combination with the crosslinking agent described later, and examples thereof include hydroxyl group, carboxyl group, amino group, epoxy group, oxetanyl group, oxazoline group, oxazine group, aziridine group, thiol group, isocyanate group, blocked isocyanate group, and silanol group. From the viewpoint of compatibility with the embeddability improving agent (B), carboxyl group, hydroxyl group, and epoxy group are preferred. When the thermosetting resin has a carboxyl group, the acid value of the thermosetting resin is preferably 1 to 50 mgKOH / g, more preferably 3 to 30 mgKOH / g, and even more preferably 5 to 20 mgKOH / g. By making the acid value of the thermosetting resin 1mgKOH / g or more, the crosslinking density with the crosslinking agent is optimized while maintaining good intermolecular forces with the adherend, improving light resistance, adhesion, and zipping properties.By making the acid value of the thermosetting resin 50mgKOH / g or less, the intermolecular forces with the adherend can be maintained good and the amount of carboxyl groups remaining after the crosslinking reaction, which promotes yellowing of the resin, can be appropriately adjusted, improving light resistance, adhesion, and zipping properties. The acid value in this disclosure was measured by the method described in the Examples below.
[0034] In the present disclosure, the urethane resin is a general term for a compound containing two or more urethane bonds in one molecule. The urethane resin can be obtained by reacting a polyisocyanate with a polyol. The polyisocyanate may have two or more isocyanate groups in one molecule, and from the viewpoint of compatibility with the embeddability improver (B), diisocyanate or triisocyanate is preferred, and diisocyanate is more preferred. The diisocyanate may be appropriately selected from known aliphatic diisocyanates such as hexamethylene diisocyanate and known aromatic diisocyanates such as benzene-1,3-diisocyanate. In addition, an isocyanate-terminated prepolymer obtained by reacting a polyol with an excess of polyisocyanate may be used as an intermediate of the urethane resin. The polyol may have two or more hydroxyl groups in one molecule, and from the viewpoint of compatibility with the embeddability improver (B), a diol or triol is preferred, and a diol is more preferred. The diol may be appropriately selected from known aliphatic diols such as ethylene glycol and known aromatic diols such as benzene diol. Prepolymers such as polyether polyols, polyester polyols, and polycarbonate polyols may also be used.
[0035] The urethane resin may be a polyurethane urea resin further having a urea bond, which can be synthesized, for example, by reacting a urethane resin having an isocyanate group at its terminal with a polyamine. The polyamine may have two or more amino groups in one molecule, and is preferably a diamine or triamine, more preferably a diamine, from the viewpoint of compatibility with the embeddability improver (B). The diamine may be appropriately selected from known aliphatic diamines such as ethylenediamine and known aromatic diamines such as phenylenediamine.
[0036] The photocurable resin may be any resin having one or more unsaturated bonds in one molecule that undergo a crosslinking reaction when exposed to light. Suitable examples of the photocurable resin include acrylic resin, maleic acid resin, polybutadiene resin, polyester resin, polyurethane resin, epoxy resin, oxetane resin, phenoxy resin, polyimide resin, polyamide resin, alkyd resin, amino resin, polylactic acid resin, oxazoline resin, benzoxazine resin, silicone resin, and fluororesin. The photocurable resin may also have a functional group that can be utilized in a crosslinking reaction upon heating.
[0037] When the resin composition layer contains a photocurable resin, it is preferable that the resin composition layer also contains an initiator. Examples of the initiator include a triazine-based photopolymerization initiator, a borate-based photopolymerization initiator, a carbazole-based photopolymerization initiator, an acetophenone-based photopolymerization initiator, and an oxime ester-based photopolymerization initiator. Among these, acetophenone-based photopolymerization initiators and oxime ester-based photopolymerization initiators are preferred since they cause less yellowing during the heat aging process. From the viewpoint of preventing yellowing, the content of the initiator is preferably 0.5 to 10 mass %, and more preferably 0.5 to 5 mass %, based on the total amount (100 mass %) of the resin composition layer.
[0038] Examples of thermoplastic resins include butyral resins, styrene-maleic acid copolymers, chlorinated polyethylene, chlorinated polypropylene, polyvinyl chloride, vinyl chloride-vinyl acetate copolymers, polyvinyl acetate, polyester resins, vinyl resins, alkyd resins, polystyrene resins, polyamide resins, rubber resins, cyclized rubber resins, celluloses, polyethylenes (HDPE, LDPE), polybutadiene, and polyimide resins.
[0039] The weight average molecular weight (Mw) of the resin (A) is 10,000 to 1,000,000. From the viewpoint of light resistance and adhesion, it is more preferably 25,000 to 300,000, and even more preferably 50,000 to 150,000. By making the weight average molecular weight (Mw) 10,000 or more, the length of the molecular chain is suitable, so that the entanglement of the molecular chain in the heat aging process is extremely easily loosened, and by optimizing it, the conformability to the adherend can be made suitable, so that the adhesion can be improved. By making it 1,000,000 or less, the compatibility with the embeddability improver (B) is good, the influence of yellowing due to oxidative deterioration caused by irradiation of light can be prevented, and light resistance can be improved. The ratio (Mw / Mn) of the number average molecular weight (Mn) to the weight average molecular weight (Mw), which indicates the degree of dispersion of the resin (A), is preferably 1 to 5, more preferably 2 to 4.5, and even more preferably 2.5 to 4. By setting Mw / Mn within the above range, the flow rate when the resin is heated is made uniform within the resin, making it easier to control the fluidity of the resin and improving embeddability. In addition, the rate at which the resin wets the adherend is also made uniform, improving adhesion. The weight average molecular weight (Mw) and number average molecular weight (Mn) are values calculated in terms of polystyrene measured by gel permeation chromatography (GPC). The weight average molecular weight (Mw) and number average molecular weight (Mn) in this disclosure were measured by the method described in the Examples below.
[0040] The glass transition temperature (Tg) of the resin (A) is -30°C to 40°C. From the viewpoints of light resistance, embeddability, and adhesion, -20°C to 30°C is more preferable, -10°C to 25°C is even more preferable, 0°C to 20°C is even more preferable, and 5°C to 15°C is most preferable. By setting the glass transition temperature (Tg) to -30°C or higher, the fluidity and wettability of the resin (A) in the pressing step can be made suitable, and the embeddability and adhesion can be improved. Furthermore, in the heat aging step, a network structure of the resin (A) and the embeddability improver (B) is easily formed, improving light resistance. By setting the glass transition temperature (Tg) to 40° C. or less, when pressure is applied to the resin composition layer in the pressing process, the molecular motion of the resin (A) contained in the resin composition layer becomes active, and the entanglement of molecular chains becomes easy to loosen. When the entanglement of molecular chains is loosened, it becomes possible for the resin to deform so as to conform to an uneven adherend such as a substrate or a light emitting element, and the space between the light emitting element and the resin composition layer can be reduced, leading to improved embeddability. In addition, the compatibility with the embeddability improver (B) is improved, preventing the influence of yellowing due to oxidative deterioration caused by light and improving light resistance. Furthermore, the entanglement of the molecular chains of the resin composition layer and the coordination of the embeddability improver (B) are optimized during heat aging, and residual stress is removed, so that the sealing layer becomes smooth and the adhesion to the adherend is improved. If the glass transition temperature (Tg) is lower than -30°C, the fluidity of the resin (A) in the pressing process becomes too high, the thickness of the sealing layer is not uniform, the resin at the end of the sealing layer flows and becomes thin, the function of fixing the light-emitting element is not exhibited, the adhesion is deteriorated, and the embeddability becomes poor. Also, in the heat aging process, it becomes difficult to form a network structure between the resin (A) and the embeddability improver (B), and the light resistance is deteriorated. If the glass transition temperature (Tg) is higher than 40° C., the fluidity of the resin (A) is low, making it difficult for the resin (A) to conform to the irregularities of the light-emitting element, resulting in poor embeddability. In addition, the wettability to the adherend is low, resulting in poor adhesion, and the compatibility between the embeddability improver (B) and the resin (A) becomes unstable, resulting in poor light resistance.
[0041] In the present application, the glass transition temperature (Tg) of the resin (A) refers to the glass transition temperature (Tg) before heat curing and before photocuring when the resin (A) contains a thermosetting resin or a photocurable resin. The glass transition temperature (Tg) of the resin (A) in the present disclosure is measured by the method described in the examples below.
[0042] The content of the resin (A) is preferably 76 to 99.9 mass% based on the total amount (100 mass%) of the resin composition layer, more preferably 81 to 99 mass%, and even more preferably 86 to 95 mass%. When two or more types of resin (A) are contained, the content of each of the resins (A) is preferably 10 mass% or more, and the total content is preferably in the above-mentioned range. By setting the content of resin (A) within the above range, light resistance, embeddability, adhesion, and zipping properties are good. If the content of resin (A) is lower than 76 mass%, the network structure of resin (A) and embeddability improver (B) is difficult to optimize, resulting in poor light resistance. In addition, embeddability improver (B) becomes difficult to move during the pressing process, resulting in poor embeddability, and the intermolecular force derived from resin (A) becomes weak, resulting in poor adhesion and zipping properties.
[0043] [(Meth)acrylic resin (a)] In the present disclosure, the (meth)acrylic resin (a) is preferably an acrylic copolymer obtained by copolymerizing a (meth)acrylic acid ester monomer. A suitable example of the (meth)acrylic acid ester monomer is a (meth)acrylic acid alkyl ester monomer. When forming a crosslinked structure, a (meth)acrylic copolymer obtained by copolymerizing a functional group-containing monomer and a (meth)acrylic acid ester monomer is preferred.
[0044] The (meth)acrylic acid alkyl ester monomer is a compound in which an alkyl group or a cycloalkyl group is introduced by esterifying (meth)acrylic acid, and the alkyl group or the cycloalkyl group may be any of a linear, branched, or cyclic saturated aliphatic hydrocarbon group. The saturated aliphatic hydrocarbon group is preferably a saturated aliphatic hydrocarbon group having 1 to 20 carbon atoms, and more preferably a saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms. Specific examples include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, and (meth)acrylic acid. Decyl, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, nonadecyl (meth)acrylate, eicosyl (meth)acrylate, lauryl (meth)acrylate, cyclohexyl (meth)acrylate, 4-n-butylcyclohexyl (meth)acrylate, isobornyl (meth)acrylate, etc. Among these, in view of compatibility with the embeddability improver (B), it is particularly preferable to use methyl (meth)acrylate, n-butyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and lauryl (meth)acrylate.
[0045] The structural unit derived from a (meth)acrylic acid alkyl ester monomer is preferably 1 to 100 mass%, more preferably 20 to 99.9 mass%, and further preferably 80 to 99.7 mass%, relative to 100 mass% of the (meth)acrylic resin (a).
[0046] The (meth)acrylic resin (a) preferably contains a functional group-containing monomer. Examples of the functional group-containing monomer include a carboxy group-containing monomer, a hydroxyl group-containing monomer, an epoxy group-containing monomer, and an amino group-containing monomer. By including a functional group-containing monomer, the cohesive strength of the resin (A) is improved, and a tough resin composition layer can be obtained.
[0047] Examples of the carboxyl group-containing monomer include (meth)acrylic acid, β-carboxyethyl (meth)acrylate, p-carboxybenzyl (meth)acrylate, carboxypentyl (meth)acrylate, itaconic acid, maleic acid, fumaric acid, crotonic acid, citraconic acid, and isocrotonic acid. Among these, (meth)acrylic acid is particularly preferred from the viewpoint of adhesion.
[0048] Examples of the hydroxyl group-containing monomer include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)methyl (meth)acrylate. Among these, from the viewpoint of adhesion, 4-hydroxybutyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate are more preferred.
[0049] Examples of epoxy group-containing monomers include glycidyl (meth)acrylate, methyl glycidyl (meth)acrylate, 3,4-epoxycyclohexylmethyl (meth)acrylate, and 6-methyl-3,4-epoxycyclohexylmethyl (meth)acrylate.
[0050] Examples of the amino group-containing monomer include monoalkylamino (meth)acrylates such as monomethylaminoethyl (meth)acrylate, monoethylaminoethyl (meth)acrylate, monomethylaminopropyl (meth)acrylate, and monoethylaminopropyl (meth)acrylate.
[0051] The total amount of structural units derived from functional group-containing monomers is preferably 0.1 to 20% by mass relative to 100% by mass of the (meth)acrylic resin (a). By setting the amount within this range, the cohesive strength can be adjusted by reaction with the crosslinking agent. The amount of the structural unit derived from the carboxyl group-containing monomer is preferably 0.1 to 10% by mass relative to 100% by mass of the (meth)acrylic resin (a). When the amount is within the above range, the adhesion to the adherend can be improved. Furthermore, the content of the structural unit derived from the hydroxyl group-containing monomer is preferably 0.1 to 10 mass % relative to 100 mass % of the (meth)acrylic resin (a). By being in this range, the adhesion to the adherend can be adjusted.
[0052] The (meth)acrylic resin (a) may contain structural units derived from other monomers copolymerizable with (meth)acrylic acid alkyl esters and functional group-containing monomers. Examples of such monomers include monomers having an alkyleneoxy group and other vinyl monomers. Examples of such monomers include methoxyethyl acrylate, methoxydiethylene glycol acrylate, vinyl acetate, vinyl crotonate, styrene, acrylonitrile, and acrylamide. The structural units derived from the other monomers are preferably 0.1 to 20% by mass in 100% by mass of the (meth)acrylic copolymer.
[0053] A more preferred example of the (meth)acrylic resin (a) is a (meth)acrylic copolymer having one or more structural units derived from an acrylic acid alkyl ester (a1) having a linear, branched or cyclic saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms, and one or more structural units derived from a methacrylic acid alkyl ester (a2) having a linear, branched or cyclic saturated aliphatic hydrocarbon group having 1 to 8 carbon atoms. By containing one or more structural units derived from an alkyl acrylate (a1) having a linear, branched or cyclic saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms, interaction with the adherend interface is easily exhibited in a short contact time, and the gap between the light-emitting element and the resin composition layer during embedding can be reduced, contributing to improved embeddability.
[0054] The (meth)acrylic resin (a) contains one or more structural units derived from a methacrylic acid alkyl ester (a2) having a linear, branched or cyclic saturated aliphatic hydrocarbon group having 1 to 8 carbon atoms, and therefore the (meth)acrylic resin (a) easily wets and spreads over the adherend interface over a long contact time, thereby reducing the gap between the light-emitting element and the resin composition layer during embedding, and contributing to improved embeddability.
[0055] From the viewpoint of optimizing the interaction with the adherend interface in a short contact time and improving embeddability and adhesion, the acrylic acid alkyl ester (a1) having a linear, branched or cyclic saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms is preferably an acrylic acid alkyl ester having a linear, branched or cyclic saturated aliphatic hydrocarbon group having 1 to 8 carbon atoms, and more preferably an acrylic acid alkyl ester having a linear, branched or cyclic saturated aliphatic hydrocarbon group having 1 to 4 carbon atoms. Moreover, the saturated aliphatic hydrocarbon group of the acrylic acid alkyl ester (a1) having a linear, branched or cyclic saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms is more preferably a linear or branched chain. From the viewpoint of improving embeddability and adhesion, the total mass of structural units derived from the acrylic acid alkyl ester (a1) having a linear, branched or cyclic saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms is preferably 1 to 95 mass%, more preferably 5 to 70 mass%, and even more preferably 7 to 60 mass%, based on 100 mass% of the (meth)acrylic resin (a).
[0056] From the viewpoint of optimizing the wetting and spreading on the adherend interface over a long contact time and improving embeddability and adhesion, the methacrylic acid alkyl ester (a2) having a linear, branched or cyclic saturated aliphatic hydrocarbon group having 1 to 8 carbon atoms is preferably a methacrylic acid alkyl ester having a linear, branched or cyclic saturated aliphatic hydrocarbon group having 1 to 4 carbon atoms. Moreover, the saturated aliphatic hydrocarbon group of the methacrylic acid alkyl ester (a2) having a linear, branched or cyclic saturated aliphatic hydrocarbon group having 1 to 8 carbon atoms is more preferably a linear or branched chain. From the viewpoint of improving embeddability and adhesion, the total mass of structural units derived from the methacrylic acid alkyl ester (a2) having a linear, branched or cyclic saturated aliphatic hydrocarbon group having 1 to 8 carbon atoms is preferably 1 to 95 mass%, more preferably 30 to 90 mass%, and even more preferably 35 to 85 mass%, relative to 100 mass% of the (a) (meth)acrylic resin.
[0057] In the (meth)acrylic resin (a), the ratio of the total mass of structural units derived from the acrylic acid alkyl ester (a1) having a linear, branched or cyclic saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms to the total mass of structural units derived from the methacrylic acid alkyl ester (a2) having a linear, branched or cyclic saturated aliphatic hydrocarbon group having 1 to 8 carbon atoms is preferably 1:0.4 to 1:20, more preferably 1:0.6 to 1:15, even more preferably 1:1 to 1:13, and most preferably 1:5 to 1:9. By setting the content within the above range, it is possible to improve light resistance, optimize the intermolecular interactions within the (meth)acrylic resin (a), and develop the fluidity of the resin that provides good embedding properties. In addition, it is possible to optimize the wettability of the (meth)acrylic resin (a) to the adherend, thereby improving adhesion.
[0058] A more preferred example of the (meth)acrylic resin (a) is a (meth)acrylic copolymer which contains, in addition to structural units derived from an acrylic acid alkyl ester (a1) having a linear, branched or cyclic saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms and structural units derived from a methacrylic acid alkyl ester (a2) having a linear, branched or cyclic saturated aliphatic hydrocarbon group having 1 to 8 carbon atoms, one or more structural units derived from (meth)acrylic acid (a3). The total mass of the structural units derived from the (meth)acrylic acid (a3) is preferably 0.1 to 15 mass%, more preferably 0.3 to 10 mass%, and even more preferably 0.5 to 5 mass%, relative to 100 mass% of the (meth)acrylic resin (a). By setting it within the above range, the adhesion due to the intermolecular interaction with the adherend can be improved. From the viewpoint of improving the adhesion to the adherend, the (meth)acrylic acid (a3) is more preferably methacrylic acid.
[0059] A more preferred example of the functional group-containing monomer constituting the (meth)acrylic resin (a) is one in which the (meth)acrylic acid (a3) and the hydroxyl group-containing monomer are not simultaneously contained, which allows the cohesive strength of the (meth)acrylic resin (a) to be adjusted and the adhesion to be increased.
[0060] The (meth)acrylic resin (a) is obtained by polymerizing an acrylic monomer mixture. During polymerization, a polymerization initiator can be used as necessary. The content of the polymerization initiator is, for example, 0.01 to 10% by mass relative to 100% by mass of the monomer mixture. The polymerization method is not limited. For example, polymerization can be performed by solution polymerization, bulk polymerization, emulsion polymerization, or suspension polymerization, and solution polymerization is most preferable because of ease of polymerization control. Examples of the solvent used in solution polymerization include acetone, methyl acetate, ethyl acetate, toluene, xylene, anisole, methyl ethyl ketone, and cyclohexanone. The polymerization temperature can be, for example, 60 to 120°C, and the polymerization time can be about 2 to 12 hours.
[0061] The polymerization initiator is preferably a radical polymerization initiator. As the radical polymerization initiator, peroxides and azo compounds are suitable. Examples of the azo compound include 2,2'-azobisbutyronitrile such as 2,2'-azobisisobutyronitrile (abbreviation: AIBN) and 2,2'-azobis(2-methylbutyronitrile); 2,2'-azobisvaleronitrile such as 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile) and 2,2'-azobis(2,4-dimethylvaleronitrile); 2,2'-azobispropionitrile such as 2,2'-azobis(2-hydroxymethylpropionitrile); and 1,1'-azobis-1-alkanenitrile such as 1,1'-azobis(cyclohexane-1-carbonitrile). Examples of the peroxide include dialkyl peroxides such as di-t-butyl peroxide, dicumyl peroxide, t-butylcumyl peroxide, α,α'-bis(t-butylperoxy-m-isopropyl)benzene, and 2,5-di(t-butylperoxy)hexyne-3; peroxy esters such as t-butyl peroxybenzoate, t-butyl peroxyacetate, and 2,5-dimethyl-2,5-di(benzoylperoxy)hexane; ketone peroxides such as cyclohexanone peroxide, 3,3,5-trimethylcyclohexanone peroxide, and methylcyclohexanone peroxide; 2,2-bis(4,4-di-t-butylperoxycyclohexyl)propane, Examples of the peroxyketals include 1,1-bis(t-butylperoxy)3,3,5-trimethylcyclohexane, 1,1-bis(t-butylperoxy)cyclohexane, and n-butyl-4,4-bis(t-butylperoxy)valerate; hydroperoxides such as cumene hydroperoxide, diisopropylbenzene hydroperoxide, and 2,5-dimethylcyclohexane-2,5-dihydroperoxide; diacyl peroxides such as benzoyl peroxide, decanoyl peroxide, lauroyl peroxide, and 2,4-dichlorobenzoyl peroxide; and peroxydicarbonates such as bis(t-butylcyclohexyl)peroxydicarbonate.
[0062] [Embeddability improver (B)] In the present embodiment, the embeddability improver (B) is a compound having a function of improving the fluidity of the resin (A) and improving the embeddability between a plurality of light emitting elements, and contains a phosphorus-containing compound (B1) and a phenolic hydroxyl group-containing compound (B2). The embeddability is improved by containing both the phosphorus-containing compound (B1) and the phenolic hydroxyl group-containing compound (B2) in the resin composition layer. In addition, there is an effect of improving light resistance, adhesion, and zipping resistance. The present inventors assume the following mechanism. First, in the pressing process, the embeddability improver (B) moves freely enough to penetrate between the molecular chains of the resin (A), thereby cutting off the intermolecular interactions of the resin (A) and helping the resin (A) to be uniformly loosened, thereby improving the fluidity, and the resin composition layer is deformed to follow the light emitting element. Thereafter, the phosphorus atom site of the phosphorus-containing compound (B1) is weakly coordinated to the phenolic hydroxyl group site of the phenolic hydroxyl group-containing compound (B2) while penetrating into the molecular chain of the resin (A) having the weight average molecular weight (Mw) specified in the present disclosure, forming a uniform network structure, suppressing further deformation of the resin composition layer, leading to improved embeddability. In addition, the intermolecular interactions of the resin (A) are suitably adjusted, resulting in good adhesion. Furthermore, the phosphorus-containing compound (B1) and the phenolic hydroxyl group-containing compound (B2) have a radical trapping function, and the resin (A) and the embeddability improver (B) form a uniform network structure, thereby efficiently expressing the radical trapping function and improving light resistance. In addition, the intermolecular interaction between the adherend and the resin (A) is appropriately adjusted, improving adhesion, and the stress applied when peeling off the release liner is uniformly distributed, improving zipping properties.
[0063] The mass ratio B1:B2 of the phosphorus-containing compound (B1) and the phenolic hydroxyl group-containing compound (B2) in the embeddability improver (B) is preferably 0.1:1 to 10:1, more preferably 0.5:1 to 5:1, and even more preferably 1:1 to 3:1. By setting it in the above range, the molecular chain of the resin (A) and the embeddability improver (B) form a uniform network structure, improving the embeddability. In addition, the embeddability improver (B) can fully exert its radical trapping function, resulting in excellent light resistance. Furthermore, the coordination of the phosphorus-containing compound (B1) and the phenolic hydroxyl group-containing compound (B2) becomes favorable, and the aggregation properties of the resin (A) are not inhibited, resulting in good zipping properties.
[0064] From the viewpoint of embeddability and adhesion, the content of the embeddability improver (B) is preferably 0.1 to 15 mass %, more preferably 0.3 to 10 mass %, and even more preferably 0.5 to 5 mass % in the total amount (100 mass %) of the resin composition layer. By setting it in the above range, embeddability, adhesion, light resistance, and zipping resistance are improved.
[0065] [Phosphorus-containing compounds (B1)] The phosphorus-containing compound (B1) used in the present disclosure is not particularly limited as long as it contains phosphorus in the molecule, but is preferably one having a molecular weight of less than 10,000, more preferably 30 to 5,000, and even more preferably 30 to 2,000. The phosphorus-containing compound (B1) may be used alone or in combination of two or more. From the viewpoint of compatibility and embeddability, it is preferable to use one or more solid compounds at room temperature and one or more liquid compounds in combination. Known phosphorus-containing compounds include tris(2-ethylhexyl)phosphite, tridecyl phosphite, trilauryl phosphite, tris(tridecyl)phosphite, tristearyl phosphite, phenyl isooctyl phosphite, phenyl isodecyl phosphite, phenyl di(tridecyl)phosphite, diphenyl isooctyl phosphite, diphenyl isodecyl phosphite, diphenyl tridecyl phosphite, triphenyl phosphite, tricresyl phosphite, tris(no (nylphenyl) phosphite, 4,4'-isopropylidenediphenol alkyl phosphite, trisnonylphenyl phosphite, trisdinonylphenyl phosphite, tris(2,4-di-t-butylphenyl) phosphite, tris(biphenyl) phosphite, bis(decyl)pentaerythritol diphosphite (synonym: 3,9-bis(decyloxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane), bis(tridecyl)pentaerythritol diphosphite phyto (synonym: 3,9-bis(tridecyloxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane), distearyl pentaerythritol diphosphite (synonym: 3,9-bis(octadecyloxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane), di(nonylphenyl)pentaerythritol diphosphite (synonym: 3,9-bis(nonylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5 .5]undecane), di(2,4-di-t-butylphenyl)pentaerythritol diphosphite (synonym: 3,9-bis(2,4-di-tert-butyl-4-methylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane), di(2,6-di-t-butylphenyl)pentaerythritol diphosphite (synonym: 3,9-bis(2,6-di-tert-butyl-4-methylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane), phenyl bisphenol A pentaerythritol diphosphite, tetratridecyl 4,4'-butylidene bis(3-methyl-6-t-butylphenol) diphosphite, hexatridecyl 1,1,3-tris(2-methyl-4-hydroxy-5-t-butylphenyl)butane triphosphite, 3,5-di-t-butyl-4-hydroxybenzyl phosphite diethyl ester, sodium bis(4-t-butylphenyl) phosphite, sodium-2,2-methylene-bis(4,6-di-t-butylphenyl)-phosphite, 1,3-bis(diphenoxyphosphonyloxy)-benzene, ethyl bis(2,4-ditert-butyl-6-methylphenyl) phosphite, etc. can be suitably used. In addition, oligomer type compounds having a phosphite structure and a molecular weight of less than 10,000 can also be used. In particular, compounds having a triphenyl phosphite skeleton, compounds having a trialkyl phosphite skeleton, compounds having a diphenyl monoalkyl phosphite skeleton, compounds having a monophenyl dialkyl phosphite skeleton, and compounds having a 2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane skeleton are preferred from the viewpoints of light resistance and embedding properties. The phenyl skeleton may contain a substituent such as t-butyl. More specifically, tris(2,4-di-t-butylphenyl)phosphite, tris(2-ethylhexyl)phosphite, bis(decyl)pentaerythritol diphosphite, bis(tridecyl)pentaerythritol diphosphite, distearyl pentaerythritol diphosphite, di(nonylphenyl)pentaerythritol diphosphite, di(2,4-di-t-butylphenyl)pentaerythritol diphosphite, di(2,6-di-t-butylphenyl)pentaerythritol diphosphite, and phenyl bisphenol A pentaerythritol diphosphite are more preferred, and distearyl pentaerythritol diphosphite and di(2,6-di-t-butylphenyl)pentaerythritol diphosphite are even more preferred.
[0066] Specific examples of the phosphorus-containing compound (B1) include "ADEKA STAB PEP-8, PEP-36, C, TPP, HP-10, 135A, 1500, 2112, 2112RG, 3010, 1178, 4C, 24G, 2" manufactured by ADEKA Corporation, "IRGAFOS (registered trademark) 168, 168FF, 38, 126, P-EPQ, 12" manufactured by BASF Japan Ltd., "SUMILIZER (registered trademark) GP" manufactured by Sumitomo Chemical Co., Ltd., and "JP-360, JP-351, JP-3CP, JP-308E, JPE-308E, JP-310, JP-312" manufactured by Johoku Chemical Industry Co., Ltd. L, JP-333E, JPM-308, JPM-311, JPM-313, JPP-100, JA-805, JPH-1200, JPP-88, JPE-10, JPE-13R, JP-318E, JPP-2000PT, JP-650, JPH-3800, JC-356, "Everaox (registered trademark) 168, 201, 202, 203, 204" manufactured by Nagamitsu Chemical Co., Ltd., "Hostanox (registered trademark) P-EPQ (registered trademark)" manufactured by Clariant, and "Ultranox (registered trademark) 626" manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.
[0067] The content of the phosphorus-containing compound (B1) relative to the total amount (100 mass%) of the resin composition layer is preferably 0.05 to 10 mass%, more preferably 0.2 to 7 mass%, and further preferably 0.4 to 6 mass%.
[0068] [Phenol-containing hydroxyl group compound (B2)] The phenolic hydroxyl group-containing compound (B2) used in the present disclosure is a compound that contains a phenolic hydroxyl group in the molecule and does not contain phosphorus. The molecular weight is preferably less than 10,000, more preferably 94 to 5,000, and even more preferably 94 to 3,000. The phenolic hydroxyl group-containing compound (B2) may be used alone or in combination of two or more kinds. Known phenolic hydroxyl group-containing compounds (B2) include 2,6-di-t-butylphenol, 2,6-di-t-butyl-4-methylphenol, 2,6-di-t-butyl-4-ethylphenol, 2,6-di-t-butyl-4-s-butylphenol, 2,6-di-t-butyl-4-hydroxymethylphenol, pentaerythritol tetrakis[3-[3,5-di(tert-butyl)-4-hydroxyphenyl]propionate], thiodiethylene bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl]propionate], and thiodiethylene bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl]propionate]. bis(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)-propionate, N,N′-(hexane-1,6-diyl)bis(3,5-di-tert-butyl-4-hydroxybenzenepropanamide), 3-(4-hydroxy-3,5-diisopropylphenyl)octylpropionate, 2,4-dimethyl-6-(1-methylpentadecyl)phenol, 2,4,6-tris(4-hydroxy-3,5-di-tert-butylbenzyl)mesitylene, bis[[3 ,5-Di(tert-butyl)-4-hydroxybenzyl]ethylphosphonate]calcium, 2,4-bis(octylthiomethyl)-6-methylphenol, bis(3-tert-butyl-4-hydroxy-5-methylbenzenepropanoic acid)ethylene bis(oxyethylene), 1,6-hexanediol bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], tris[(3,5-di-tert-butyl-4-hydroxyphenyl)methyl]-1,3,5-triazinane-2,4 ,6-trione, 6-(4-hydroxy-3,5-di-tert-butylanilino)-2,4-bis(octylthio)-1,3,5-triazine, 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 4,4',4''-(1-methylpropanyl-3-ylidene)tris(6-tert-butyl-m-cresol), 6,6'-di-tert-butyl-4,4'-butylidene di-m-cresol, octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 3,9-bis{2-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1-dimethylethyl}-2,4,8,10-tetraoxaspiro[5.5]undecane, 1,3,5-tris(3,5-di-tert-butyl-4-hydroxyphenylmethyl)-2,4,6-trimethylbenzene, etc. can be used. In particular, from the viewpoint of light resistance and embedding properties, phenolic hydroxyl group-containing compounds having a hindered type skeleton in which two tert-butyl groups are bonded to the ortho positions of a phenolic hydroxyl group, or a semihindered type skeleton in which one tert-butyl group is bonded to one of the ortho positions of a phenolic hydroxyl group and one methyl group is bonded to the other, are preferred. Pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 3,9-bis{2-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1-dimethylethyl}-2,4,8,10-tetraoxaspiro[5.5]undecane, and 1,3,5-tris(3,5-di-tert-butyl-4-hydroxyphenylmethyl)-2,4,6-trimethylbenzene are even more preferred.
[0069] Specific examples of the phenolic hydroxyl group-containing compound (B2) include "ADEKA STAB AO-20, AO-30, AO-40, AO-50, AO-50F, AO-50T, AO-60, AO-60G, AO-80, and AO-330" manufactured by ADEKA Corporation, "KEMINOX Examples of suitable fluororesin products include "9425, 179" manufactured by Sumitomo Chemical Co., Ltd., "SUMILIZER (registered trademark) GA-80, GM, GS, GA-80, MDP-S, WX-R, WX-RC, BBM-S" manufactured by Sumitomo Chemical Co., Ltd., "IRGANOX (registered trademark) 1010, 1010FF, 1035, 1035FF, 1076, 1076FD, 1098, 1135, 1141, 1330, 1425WL, 1520L, 245, 245FF, 259, 3114, 565" manufactured by BASF Japan Ltd., "Yoshinox BB, 425" manufactured by Mitsubishi Chemical Corporation, and "Hostanox (registered trademark) O3, O310" manufactured by Clariant.
[0070] The content of the phenolic hydroxyl group-containing compound (B2) relative to the total amount (100 mass%) of the resin composition layer is preferably 0.04 to 5 mass%, more preferably 0.1 to 3.5 mass%, and even more preferably 0.2 to 3 mass%.
[0071] [Crosslinking agent] The resin composition layer of the present disclosure may contain a crosslinking agent. In particular, when the resin (A) contains a thermosetting resin, it is preferable to use a crosslinking agent to promote the formation of a crosslinked structure. The crosslinking agent may be used alone or in combination of two or more. The crosslinking agent undergoes a crosslinking reaction with the reactive functional groups of the resin (A) during the heat pressing or heat aging in the pressing process, thereby strengthening the adhesion to the adherend such as the light emitting element, etc. In addition, the crosslinking agent can increase the cohesive force of the resin composition layer, resulting in good zipping properties. The crosslinking agent has a plurality of functional groups capable of reacting with the functional groups of the resin (A). Examples of the crosslinking agent include known compounds such as silane coupling agents, epoxy compounds, acid anhydride group-containing compounds, imidazole compounds, isocyanate compounds, aziridine compounds, and amine compounds. From the viewpoint of adjusting the loss tangent (tan δ) of the resin composition layer, silane coupling agents, epoxy compounds, aziridine compounds, imidazole compounds, and isocyanate compounds are preferred, and epoxy compounds are more preferred.
[0072] The epoxy compound is a compound having two or more epoxy groups in one molecule. As for the properties of the epoxy compound, by using a liquid, the tan δ peak temperature of the resin composition layer can be lowered, and the light emitting element and the resin composition layer can be closely attached to each other. On the other hand, by using a solid, the tan δ peak temperature of the resin composition layer can be increased, and the stickiness of the resin composition layer can be controlled, thereby adjusting the zipping property. As the epoxy compound, for example, a glycidyl ether type epoxy compound, a glycidyl amine type epoxy compound, a glycidyl ester type epoxy compound, a cyclic aliphatic (alicyclic) epoxy compound, etc. are preferable. Moreover, from the viewpoint of light resistance, it is more preferable that the epoxy compound is a high-purity hydrogenated epoxy resin.
[0073] Examples of the glycidyl ether type epoxy compound include cresol novolac type epoxy compounds, tris(glycidyloxyphenyl)methane, and tetrakis(glycidyloxyphenyl)ethane. Examples of the glycidylamine type epoxy compound include tetraglycidyldiaminodiphenylmethane and tetraglycidylmetaxylylenediamine.
[0074] Examples of the glycidyl ester type epoxy compound include diglycidyl phthalate, diglycidyl hexahydrophthalate, and diglycidyl tetrahydrophthalate.
[0075] Examples of cyclic aliphatic (alicyclic) epoxy compounds include epoxycyclohexylmethyl-epoxycyclohexanecarboxylate, bis(epoxycyclohexyl)adipate, and the like.
[0076] Examples of the aziridine compound include trimethylolpropane-tri-β-aziridinylpropionate, tetramethylolmethane-tri-β-aziridinylpropionate, N,N'-diphenylmethane-4,4'-bis(1-aziridinecarboxamide), N,N'-hexamethylene-1,6-bis(1-aziridinecarboxamide), tris-2,4,6-(1-aziridinyl)-1,3,5-triazine, and 4,4'-bis(ethyleneiminocarbonylamino)diphenylmethane.
[0077] The imidazole compounds are 2-methylimidazole, 2-phenyl-4-methylimidazole, 2,4-dimethylimidazole, 2-phenylimidazole, imidazole, 2-undecylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1')]- Examples of imidazole compounds include ethyl-s-triazine, 2,4-diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, and 2-phenyl-4-methyl-5-hydroxymethylimidazole. Further examples include compounds with improved storage stability, such as a type insoluble in a solvent obtained by reacting an imidazole compound with an epoxy resin, or a type in which an imidazole compound is encapsulated in a microcapsule.
[0078] The isocyanate compound is an isocyanate having two or more isocyanate groups. The isocyanate compound is preferably, for example, an isocyanate monomer such as an aromatic polyisocyanate, an aliphatic polyisocyanate, an araliphatic polyisocyanate, or an alicyclic polyisocyanate, as well as a biuret, a nurate, or an adduct thereof.
[0079] Examples of aromatic polyisocyanates include 1,3-phenylene diisocyanate, 4,4'-diphenyl diisocyanate, 1,4-phenylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 4,4'-toluidine diisocyanate, 2,4,6-triisocyanate toluene, 1,3,5-triisocyanate benzene, dianisidine diisocyanate, 4,4'-diphenyl ether diisocyanate, and 4,4',4"-triphenylmethane triisocyanate.
[0080] Examples of aliphatic polyisocyanates include trimethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate (also known as HDI), pentamethylene diisocyanate, 1,2-propylene diisocyanate, 2,3-butylene diisocyanate, 1,3-butylene diisocyanate, dodecamethylene diisocyanate, and 2,4,4-trimethylhexamethylene diisocyanate.
[0081] Examples of the aromatic aliphatic polyisocyanate include ω,ω'-diisocyanate-1,3-dimethylbenzene, ω,ω'-diisocyanate-1,4-dimethylbenzene, ω,ω'-diisocyanate-1,4-diethylbenzene, 1,4-tetramethylxylylene diisocyanate, and 1,3-tetramethylxylylene diisocyanate.
[0082] Examples of alicyclic polyisocyanates include 3-isocyanatemethyl-3,5,5-trimethylcyclohexyl isocyanate (also known as IPDI, isophorone diisocyanate), 1,3-cyclopentane diisocyanate, 1,3-cyclohexane diisocyanate, 1,4-cyclohexane diisocyanate, methyl-2,4-cyclohexane diisocyanate, methyl-2,6-cyclohexane diisocyanate, 4,4'-methylenebis(cyclohexyl isocyanate), and 1,4-bis(isocyanatemethyl)cyclohexane.
[0083] The biuret form is a self-condensation product having a biuret bond formed by self-condensation of an isocyanate monomer, for example, a biuret form of hexamethylene diisocyanate.
[0084] The nurate form is a trimer of an isocyanate monomer, such as a trimer of hexamethylene diisocyanate, a trimer of isophorone diisocyanate, or a trimer of tolylene diisocyanate.
[0085] The adduct is a bifunctional or higher isocyanate compound obtained by reacting an isocyanate monomer with a bifunctional or higher low-molecular active hydrogen-containing compound. Examples of the adduct include a compound obtained by reacting trimethylolpropane with hexamethylene diisocyanate, a compound obtained by reacting trimethylolpropane with tolylene diisocyanate, a compound obtained by reacting trimethylolpropane with xylylene diisocyanate, a compound obtained by reacting trimethylolpropane with isophorone diisocyanate, and a compound obtained by reacting 1,6-hexanediol with hexamethylene diisocyanate.
[0086] The isocyanate compound is preferably a trifunctional isocyanate compound from the viewpoint of forming a sufficient crosslinked structure. The isocyanate compound is more preferably an adduct which is a reaction product between an isocyanate monomer and a trifunctional low molecular weight active hydrogen-containing compound, and a nurate. The isocyanate compound is preferably a trimethylolpropane adduct of hexamethylene diisocyanate, a nurate of hexamethylene diisocyanate, a trimethylolpropane adduct of tolylene diisocyanate, a nurate of tolylene diisocyanate, a trimethylolpropane adduct of isophorone diisocyanate, or a nurate of isophorone diisocyanate, and more preferably a trimethylolpropane adduct of hexamethylene diisocyanate, a trimethylolpropane adduct of tolylene diisocyanate, or a trimethylolpropane adduct of isophorone diisocyanate.
[0087] In the present disclosure, from the viewpoint of coating film resistance against scratches, it is preferable to contain two or more kinds of crosslinking agents. From the viewpoint of adjusting the loss tangent (tan δ) of the resin composition layer, specifically, a suitable example includes two or more kinds selected from a silane coupling agent, an epoxy compound, an aziridine compound, and an isocyanate compound, and more preferably, an example in which an epoxy compound is used in combination with one or more of a silane coupling agent, an epoxy compound, an aziridine compound, and an isocyanate compound is used in combination.
[0088] The content of the crosslinking agent (total content when two or more kinds are used in combination) is preferably 0.01 to 30 mass% based on the total amount (100 mass%) of the resin composition layer, more preferably 0.05 to 20 mass%, and even more preferably 0.1 to 10 mass%. By setting the content within the above range, the compatibility, embeddability, and zipping property of the embeddability improver (B) can be suitably adjusted.
[0089] [Other ingredients] The resin composition layer of the present disclosure may contain other components within the scope of the present disclosure, such as inorganic fillers, colorants, dispersants, surface conditioning additives, curing accelerators, curing retarders, softeners, antistatic agents, lubricants, antiblocking agents, and adhesion improvers. From the viewpoint of controlling the film properties such as diffusivity, reflectivity, light-shielding property, and viscoelasticity of the resin composition layer, it is preferable to contain an inorganic filler, a dispersant, a surface conditioning additive, a curing accelerator, a curing retarder, and an adhesion improver.
[0090] Examples of inorganic fillers include inorganic compounds that do not contain phosphorus, such as silica, alumina, magnesium hydroxide, barium sulfate, calcium carbonate, titanium oxide, zinc oxide, antimony trioxide, magnesium oxide, talc, kaolinite, mica, basic magnesium carbonate, sericite, montmorolinite, kaolinite, bentonite, boron nitride, aluminum nitride, and titanium nitride. Among these, from the viewpoint of the coating film resistance to scratches, titanium oxide, titanium nitride, silica, talc, mica, kaolinite, and montmorillonite are preferred, and titanium oxide, titanium nitride, and silica are more preferred. In the present disclosure, from the viewpoint of coating film resistance, two or more kinds of inorganic fillers may be contained. Specifically, a preferred example is a combination of silica and one or more selected from titanium oxide, titanium nitride, silica, talc, mica, kaolinite, and montmorillonite.
[0091] From the viewpoint of embeddability, the content of the inorganic filler (total content when two or more types are included) is preferably 0.01 to 10 mass% and more preferably 0.1 to 5 mass% based on the total amount (100 mass%) of the resin composition layer. By including the inorganic filler in the above range, the effect of increasing the fluidity of the resin composition layer in the pressing step is easily achieved, and the embeddability is improved.
[0092] The average primary particle size (hereinafter, particle size) of the inorganic filler is preferably 1 to 100 nm. By making the particle size 1 nm or more, it is easy to maintain the viscosity of the resin composition at a level suitable for coating. In addition, by making the particle size 100 nm or less, the coating film resistance is improved. The particle size of the inorganic filler can be determined from the average value of about 20 primary particles that can be observed in an image magnified about 50,000 to 1,000,000 times by a transmission electron microscope (TEM).
[0093] The inorganic filler can also be dispersed in the resin (A) by mechanical crushing. It is preferable to use a dispersant for the dispersion treatment. In the present disclosure, the dispersant has a function of imparting a repulsive force between particles so that the particles divided through the above-mentioned dispersion treatment do not aggregate again. As the dispersant, a conventionally known compound can be used, for example, a cationic, anionic, or nonionic surfactant or polymer dispersant having a weight average molecular weight (Mw) of 1,000 to 9,999, or a pigment derivative dispersant that does not contain a phenolic hydroxyl group or phosphorus.
[0094] Examples of the surface conditioning additive include compounds that do not contain phenolic hydroxyl groups and phosphorus, among surfactants such as silicone, silicone acrylic, acrylic, fluorine, and acetylene glycol, which have a weight average molecular weight (Mw) of 1,000 to 9,999. Among these, it is particularly preferable to contain a silicone or silicone acrylic surfactant from the viewpoint of adhesion to the adherend. The silicon-based surface conditioning additive is preferably, for example, a modified polysiloxane compound in which an organic group is introduced into a part of the methyl group of polydimethylsiloxane. Examples of modification include polyether modification, methylstyrene modification, alcohol modification, alkyl modification, aralkyl modification, fatty acid ester modification, epoxy modification, amine modification, amino modification, and mercapto modification, but are not particularly limited thereto. These modification methods can be used in combination. Among them, polyether modified polysiloxane compounds and aralkyl modified polysiloxane compounds are preferred in terms of compatibility and the like. As the silicone acrylic surface conditioning additive, for example, a siloxane-modified acrylic resin, which is a graft copolymer of an acrylic resin and a siloxane compound, is preferred from the viewpoint of compatibility and the like. From the viewpoint of coating suitability, the content of the surface conditioning additive is preferably 0.01 to 10 mass %, and more preferably 0.1 to 5 mass %, based on the total amount (100 mass %) of the resin composition layer.
[0095] The resin composition layer of the present disclosure preferably contains a curing accelerator in order to adjust the crosslinking rate and the physical properties of the resin composition layer. The curing accelerator is not particularly limited and can be appropriately selected. Specific examples of the curing accelerator include, for example, an amine-based curing accelerator, a guanidine-based curing accelerator, and a metal-based curing accelerator. These may be used alone or in combination of two or more. From the viewpoint of coating suitability, the content of the curing accelerator is preferably 0.01 to 10 mass %, and more preferably 0.1 to 5 mass %, based on the total amount (100 mass %) of the resin composition layer.
[0096] The adhesion improver may be an oligomer having a weight average molecular weight (Mw) of 1,000 to 9,999 that does not contain a phenolic hydroxyl group or phosphorus. Examples of the adhesive improver include acrylic resins, urethane acrylic resins, rosin resins, terpene resins, alicyclic petroleum resins, and aromatic petroleum resins. The weight average molecular weight (Mw) of the adhesion improver is more preferably from 2,000 to 8,000, and further preferably from 3,000 to 5,000. From the viewpoints of adhesion to an adherend and zipping properties, the content of the adhesion improver is preferably 0.1 to 20 mass %, and more preferably 1 to 15 mass %, based on the total amount (100 mass %) of the resin composition layer. EXAMPLES
[0097] The present disclosure will be specifically described below with reference to examples and comparative examples, but the present disclosure is not particularly limited to the examples. In the following description, "parts" and "%" represent "parts by mass" and "% by mass", respectively, unless otherwise specified.
[0098] The values obtained in this example were obtained by the following method. [Glass transition temperature (Tg) of resin (A)] The coating solution of resin (A) was applied onto the release layer of a 75 μm-thick second release liner (Mitsui Chemicals Tohcello, SP-PET-O3) so that the thickness after drying was 25 μm. After drying for 3 minutes in a hot air oven at 100 ° C, the release layer side of a 50 μm-thick first release liner (Mitsui Chemicals Tohcello, SP-PET-O1) was attached to the resin (A) side. The first and second release liners were then peeled off, and the Tg of the resulting resin (A) was measured using a differential scanning calorimeter (TA Instruments, "Discovery DSC 2500"). Approximately 2 mg of the sample was placed in an aluminum pan, weighed, and set in the differential scanning calorimeter. The same type of aluminum pan without the sample was used as a reference, and the sample was held at 100 ° C for 5 minutes, and then quenched to -50 ° C using liquid nitrogen. Thereafter, the temperature was increased at a rate of 5° C. / min, and the glass transition temperature (Tg) of the resin (A) was determined from the obtained DSC chart.
[0099] [Weight average molecular weight (Mw) and number average molecular weight (Mn)] The weight average molecular weight (Mw) and number average molecular weight (Mn) were measured using a GPC "LC-GPC system" manufactured by Shimadzu Corporation, and the weight average molecular weight (Mw) and number average molecular weight (Mn) were calculated by conversion using polystyrene with a known molecular weight as a standard substance. Device name: Shimadzu Corporation, LC-GPC system "Prominence" Column: Four GMHXL columns manufactured by Tosoh Corporation and one HXL-H column manufactured by Tosoh Corporation were connected together. Mobile phase solvent: Tetrahydrofuran Flow rate: 1.0mL / min Column temperature: 40℃
[0100] [Solid content] The mass of the aluminum cup (W0) was measured using a precision balance. Next, about 1 g of sample was placed in the aluminum cup, and the mass of the sample in the aluminum cup (W1) was measured using a precision balance. The sample in the aluminum cup was heated in an oven at 150°C for 120 minutes, then removed from the oven and returned to room temperature. The residual mass (W2) of the sample in the aluminum cup after heating was measured using a precision balance. The solid content was then calculated using the formula (W2-W0) / (W1-W0)×100(%).
[0101] [Acid value] The "acid value" herein refers to the acid value per 1 g of solid content of resin (A), and was determined by potentiometric titration in accordance with JIS K 0070.
[0102] Resin (A) [Production Example of (Meth)acrylic Resin (a) (R-1)] A reaction vessel (hereinafter simply referred to as "reaction vessel") equipped with a stirrer, a thermometer, a reflux condenser, a dropping device, and a nitrogen inlet tube was charged with 80 parts of ethyl acetate, 35 parts of methyl acrylate, 34.4 parts of 2-ethylhexyl acrylate, 30 parts of 2-ethylhexyl methacrylate, 0.3 parts of acrylic acid, 0.3 parts of hydroxybutyl acrylate, and 0.1 parts of 2,2'-azobisisobutyronitrile as an initiator, and the atmosphere in the reaction vessel was replaced with nitrogen gas. Then, the mixture was heated to 65°C while stirring under a nitrogen atmosphere to start the reaction. The reaction solution was then reacted at 65°C for 4 hours. After the reaction was completed, the mixture was cooled and diluted with ethyl acetate to obtain a solution of acrylic resin (R-1) with a weight average molecular weight (Mw): 20,000, a dispersity (Mw / Mn): 2, a glass transition temperature (Tg): -32°C, an acid value: 2mgKOH / g, and a solid content: 25%.
[0103] [Production Examples of (Meth)acrylic Resins (a) (R-2 to R-12)] (Meth)acrylic resins (a) (R-2 to R-12) were produced in the same manner as for the production of (meth)acrylic resin (a) (R-1), except that the compositions and blending amounts (parts by mass) were changed to those shown in Table 1. Note that blanks indicate that no blend was used, and the solid content was 25% in all cases.
[0104] [Table 1]
[0105] The abbreviations in the table are as follows. [Acrylic acid alkyl ester (a1)] MA: Methyl acrylate (saturated aliphatic hydrocarbon group with 1 carbon atom) BA: n-Butyl acrylate (saturated aliphatic hydrocarbon group with 4 carbon atoms) HA: Hexyl acrylate (saturated aliphatic hydrocarbon group with 6 carbon atoms) CHA: Cyclohexyl acrylate (saturated aliphatic hydrocarbon group with 6 carbon atoms) 2EHA: 2-ethylhexyl acrylate (saturated aliphatic hydrocarbon group with 8 carbon atoms) LA: Lauryl acrylate (saturated aliphatic hydrocarbon group with 12 carbon atoms) [Methacrylic acid alkyl ester (a2)] MMA: Methyl methacrylate (saturated aliphatic hydrocarbon group with 1 carbon atom) nBMA: n-butyl methacrylate (saturated aliphatic hydrocarbon group with 4 carbon atoms) 2EHMA: 2-ethylhexyl methacrylate (saturated aliphatic hydrocarbon group with 8 carbon atoms) [(Meth)acrylic acid (a3)] AA: Acrylic acid MAA: Methacrylic acid [others] 4HBA: Hydroxybutyl acrylate
[0106] [Production example of urethane resin (R-13)] A glass flask equipped with a stirrer, a thermometer, a reflux condenser, a nitrogen inlet tube, and a pressure reducing device was charged with 166 parts of terephthalic acid, 146 parts of adipic acid, 212 parts of 3-methyl-1,5-pentanediol, and 25 parts of ethylene glycol, and stirred while passing nitrogen gas through it. The temperature was gradually raised under normal pressure, and the mixture was reacted at 200 to 230°C for about 8 hours to obtain a liquid with an acid value of 43 mgKOH / g. Then, 0.01 parts of tetra-n-butoxytitanium was charged, and after nitrogen replacement, the mixture was stirred at 180°C for 30 minutes under a sealed condition. Then, the mixture was reacted at 230°C and 5 mmHg for 2 hours to obtain a polyester diol with an acid value of 1.1 mgKOH / g, a hydroxyl value of 114.2 mgKOH / g, a weight average molecular weight (Mw): 982, and a hue of 10 (APHA method, the same below). Next, 734 parts of the polyester diol, 23.9 parts of dimethylolpropionic acid, 219 parts of toluene diisocyanate, and 242 parts of toluene were charged into a reaction vessel equipped with a stirrer, a thermometer, a reflux condenser, a dropping device, and a nitrogen inlet tube, and reacted for 8 hours at 50° C. under a nitrogen atmosphere. 1200 parts of toluene were added to this to obtain a solution of a urethane prepolymer having an isocyanate group at its terminal. Next, the obtained prepolymer solution was heated to 70°C, and while maintaining the temperature, a solution containing 20.0 parts of 1,3-diaminopropane, 3.1 parts of benzylamine, 600 parts of 2-propanol, and 961 parts of toluene was added dropwise over 1 hour. After the dropwise addition, the mixture was allowed to react at 70°C for another 6 hours to obtain a solution of urethane resin (R-13) with a weight average molecular weight (Mw): 150,000, a dispersity (Mw / Mn): 4.5, a glass transition temperature (Tg): 18°C, an acid value: 10 mgKOH / g, and a solid content: 25%.
[0107] [Example 1] [Production Example of Resin Composition] As the resin (A), the above-mentioned (meth)acrylic resin (a) (R-2) solution: 374 parts (resin (A) 93.5 parts, solvent 280.5 parts), as the embeddability improver (B), 1 part of ADK STAB PEP-36, which is a phosphorus-containing compound (B1), 0.5 parts of AO-80, which is a phenolic hydroxyl group-containing compound (B2), 5 parts of epoxy-based crosslinking agent jER (registered trademark) YX8034 (manufactured by Mitsubishi Chemical Corporation), which is a crosslinking agent as other components, and 55 parts of 2-butanone as a solvent were sequentially added while stirring with a disperser, and stirred until sufficiently uniform. Next, filtration was performed with a membrane filter with a pore size of 10 μm to remove coarse foreign matter that would cause coating unevenness, and a resin composition with a non-volatile content of 23% was obtained. The amounts of the embeddability improver (B) and other components were calculated as solid contents.
[0108] [Production example of encapsulating sheet] The resin composition was applied onto the release layer of a 75 μm-thick second release liner (Mitsui Chemicals Tohcello, SP-PET-O3) so that the thickness after drying was 25 μm, and dried for 3 minutes in a hot air oven at 100° C. to form a resin composition layer. Next, the release layer side of a 50 μm-thick first release liner (Mitsui Chemicals Tohcello, SP-PET-O1) was attached to the exposed resin composition layer, and aged at 0° C. for 7 days to obtain an encapsulating sheet of Example 1 in which the first release liner / resin composition layer / second release liner were laminated in this order.
[0109] [Thickness of encapsulating sheet (Tt), thickness of resin composition layer (Ta), thickness of first release liner (Tl), thickness of second release liner (Th)] Ten equally spaced points were determined from one end to the other end of the encapsulating sheet cut to a size of 10 cm x 10 cm, and the thicknesses of the ten points were measured, and the average value was taken as the thickness Tt of the encapsulating sheet. Next, the first release liner was peeled off from the encapsulating sheet, and the thicknesses of the peeled first release liner at the ten points corresponding to the same positions as described above were measured. The average value was taken as Tl. Thereafter, the second release liner was further peeled off from the resin composition layer, and the thicknesses of the peeled second release liner at the ten points corresponding to the same positions as described above were measured. The average value was taken as Th. The thickness Ta of the resin composition layer was calculated by the following (Formula 1). The thickness was measured using an MH-15M (manufactured by Nikon Corporation). Ta = Tt - Tl - Th (Equation 1)
[0110] [Loss tangent (tan δ) of resin composition layer] In the above-mentioned manufacturing example of the encapsulating sheet, a separately prepared encapsulating sheet was cut to a size of 0.5 cm x 2 cm so that the thickness after drying would be 50 μm, and the first release liner and the second release liner were peeled off. The dynamic viscoelasticity of the obtained resin composition layer was measured using a dynamic viscoelasticity measuring device DVA-200 / L2 (manufactured by IT Measurement and Control Co., Ltd.) at a frequency of 10 Hz, a measurement temperature range of -50 to 150 ° C., a heating rate of 5 ° C. / min, and a tensile mode, and the loss tangent (tan δ) was plotted. From the obtained graph, the loss tangent (tan δ40) at 40 ° C., the peak top temperature of the loss tangent (tan δ) (tan δ peak temperature), and the peak top intensity of the loss tangent (tan δ) (tan δ peak intensity) were read.
[0111] [Evaluation method and criteria] [Light resistance] The sealing sheet was cut to 2 cm x 5 cm, and a glass plate (blue plate glass, manufactured by Kawamura Kuzo Shoten Co., Ltd.) having a thickness of 1.1 mm was attached to the surface from which the first release liner was peeled off, and pressure-bonded by heat pressing (100 ° C, 5 MPa, 5 minutes). Furthermore, the second release liner of the sealing sheet was peeled off, and the test piece consisting of the glass plate and the resin composition layer was left at rest for 120 minutes under a condition of 180 ° C, thereby adhering the glass plate and the resin composition layer to each other. Next, the spectral transmittance of the resin composition layer on the glass plate at 380 nm was measured using a UV-visible spectrophotometer V-570 manufactured by JASCO Corporation, and the obtained value was taken as the initial transmittance. The resin composition layer on the glass plate was placed in a xenon weather meter XL75 manufactured by Suga Test Instruments Co., Ltd., and exposed for 300 hours under the conditions of a black panel temperature of 50°C and an irradiation dose of 100,000 Lux. After exposure, the spectral transmittance at 380 nm was measured in the same manner as the initial transmittance, and the obtained value was taken as the transmittance after exposure. The change in transmittance was calculated using the formula "|Initial transmittance-Transmittance after exposure|=Change in transmittance". The evaluation criteria were as follows, with A to C being considered as good. A: The change in transmittance is less than 0.2 B: The change in transmittance is 0.2 or more and less than 0.4 C: The change in transmittance is 0.4 or more and less than 0.6 D: The change in transmittance is 0.6 or more.
[0112] [Embeddability] A glass substrate (size 1cm x 1cm, width of recess 20μm, height of protrusion 20μm, width of protrusion 20μm) with an uneven surface was prepared to mimic the uneven surface of the micro LED substrate. A schematic cross-sectional view of the test substrate is shown in Figure 3. The sealing sheet was cut into a size of 2 cm x 2 cm, the first release liner or the second release liner was peeled off to expose the resin composition layer, and the sheet was placed on the uneven portion of the glass substrate. Thereafter, the release liner on the opposite side was peeled off to remove the resin composition layer remaining on the side of the glass substrate, and a 50 μm thick TPX (Opulant X-44B, manufactured by Mitsui Chemicals Tocello Co., Ltd.) and a 2.0 mm thick PVC film (Celeb T, manufactured by Okamoto Co., Ltd.) were laminated in order as a cushioning material on the exposed surface, and cardboard was laminated to prevent sticking. Next, the test piece was pressed against the substrate surface from above at 5 MPa and 100°C for 20 minutes, and the unevenness of the glass substrate was filled with the resin composition layer to form an encapsulating layer. After pressing, the cushioning material and the cardboard were peeled off. The resin composition layer protruding from the glass substrate of the obtained test piece was roughly removed using a cutter, and the resin composition layer remaining on the side of the glass substrate was removed by sanding, exposing the side of the glass substrate, allowing the uneven portion to be observed. The embeddability was evaluated by observing 20 randomly selected recesses of the glass substrate with an electron microscope. When the maximum gap between the resin composition layer and the glass substrate in the recesses of the glass substrate was 5 μm or less, the groove was deemed to be embedded. The evaluation criteria were as follows, with A to C being considered as good. A: 18 or more recessed grooves B: 17 or less recessed grooves, 15 or more recessed grooves C: 14 or less recessed grooves, 12 or more recessed grooves D: 11 or fewer recesses
[0113] [Adhesion] The encapsulating sheet was cut to 2 cm x 8 cm, and a glass plate (blue plate glass, manufactured by Kawamura Kuzo Shoten Co., Ltd.) having a thickness of 1.1 mm and a size of 2.5 cm x 10 cm was attached to the surface from which the first release liner was peeled off, and pressure-bonded by heat pressing (100°C, 5 MPa, 5 minutes). Furthermore, the second release liner of the encapsulating sheet was peeled off, and the test piece consisting of the glass plate and the resin composition layer was left to stand for 120 minutes under a condition of 180°C, thereby bonding the glass plate and the resin composition layer to each other, and a test piece consisting of the glass plate and the resin composition layer was prepared. According to JIS K 5600-5-6 (cross-cut method), a lattice pattern (25 squares) of 1 mm squares was created on the resin composition layer using a cross-cut guide and a cutter knife, and Nichiban Co., Ltd.'s adhesive tape "CT1835" was attached to the lattice-cut portion and firmly adhered to the resin composition layer. Within 5 minutes of adhesion, the tape was pulled off at an angle close to 60° in 0.5 to 1.0 seconds. The state of the peeled resin composition layer was observed to evaluate adhesion. The evaluation criteria were as follows, with A to C being considered as good. A: 0 pieces completely peeled off, only the edge of the cut had no partial peeling B: 0 pieces completely peeled off, partial peeling only at the edge of the cut C: 1 to 2 peeled squares D: 3 or more peeled squares
[0114] [Zipping] The sealing sheet was cut to 2 cm x 8 cm, and a glass plate (blue plate glass, manufactured by Kawamura Kuzo Shoten Co., Ltd.) with a thickness of 1.1 mm and a size of 2.5 cm x 10 cm was attached to the surface from which the first release liner was peeled off, and pressure-bonded by heat pressing (100°C, 5 MPa, 5 minutes). Three of these test pieces were prepared, and each was subjected to heat aging treatment under the following three levels of conditions. Condition (1) 60 minutes at 220°C, condition (2) 120 minutes at 180°C, and condition (3) 240 minutes at 120°C. After heat aging, the test pieces were left to stand for more than 1 hour under conditions of 23°C and 50% relative humidity. Next, the second release liner was peeled off from the resin composition layer at a peel angle of 90° and a peel speed of 300 mm / min. The resin composition layer of the obtained test piece was observed to see whether or not zipping occurred. The evaluation criteria were as follows, with A to C being considered as good. A: No zipping was observed under any heat aging conditions. B: Zipping was observed under any one of the heat aging conditions. C: Zipping was observed under any of the two heat aging conditions. D: Zipping was observed under all heat aging conditions.
[0115] All of the above evaluations were made on a four-point scale, with A being the most outstanding evaluation, B being the next best evaluation, C being good evaluation, and D being evaluation of failure to achieve target performance. Note that all performance evaluations A to C correspond to the present disclosure.
[0116] [Examples 2 to 41], [Comparative Examples 1 to 7] The encapsulating sheets were produced and evaluated in the same manner as in Example 1, except that the contents and thicknesses Ta were changed to those shown in Tables 2 to 5. Any other components were added at the same time. In Tables 2 to 5, the amounts of the resin (A), embeddability improver (B), and other components are calculated as solid contents, and blank spaces indicate that the components are not blended.
[0117] The abbreviations in the table are as follows. B1-1: Phosphorus-containing compound (ADEKA STAB PEP-36, manufactured by ADEKA Corporation, containing 2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane skeleton, molecular weight 633) B1-2: Phosphorus-containing compound (ADEKA STAB HP-10, manufactured by ADEKA Corporation, containing a diphenyl monoalkyl phosphite skeleton, molecular weight 583) B1-3: Phosphorus-containing compound (ADEKA STAB 3010, manufactured by ADEKA Corporation, containing trialkyl phosphite skeleton, molecular weight 503) B2-1: Phenolic hydroxyl group-containing compound (ADEKA STAB AO-80, manufactured by ADEKA Corporation, semi-hindered type, molecular weight 741) B2-2: Phenolic hydroxyl group-containing compound (Adeka STAB AO-330, manufactured by ADEKA Corporation, hindered type, molecular weight 775) B2-3: Phenolic hydroxyl group-containing compound (IRGANOX (registered trademark) 1010, manufactured by BASF Japan, hindered type, molecular weight 1,178) C-1: Epoxy compound (jER (registered trademark) YX8034, manufactured by Mitsubishi Chemical Corporation) C-2: Isocyanate compound (Cosmonate (registered trademark) T100, manufactured by Mitsui Fine Chemicals, Inc.) C-3: Aziridine compound (ChemiTite (registered trademark) PZ-33, manufactured by Nippon Shokubai Co., Ltd.) C-4: Silane coupling agent (KBE-403, Shin-Etsu Silicone Co., Ltd.) F-1: Silica (AEROSIL® R972, manufactured by Evonik Degussa)
[0118] [Table 2]
[0119] [Table 3]
[0120] [Table 4]
[0121] [Table 5]
[0122] In the present disclosure, in the case of an encapsulating sheet in which the glass transition temperature (Tg) of the resin (A) is outside the range of -30 to 40°C, it is found that there is a problem with embeddability as shown in Comparative Examples 1 and 2. In addition, in the case of an encapsulating sheet in which the thickness Ta of the resin composition layer is outside the range of 1 to 100 µm, it is found that there is a problem with embeddability and zipping property as shown in Comparative Examples 3 and 4. Furthermore, in the case where the embeddability improver (B) does not contain both the phosphorus-containing compound (B1) and the phenolic hydroxyl group-containing compound (B2), it is found that there are problems with light resistance, embeddability and adhesion as shown in Comparative Examples 5 to 7. As shown in Table 5, the encapsulating sheets of Comparative Examples 1 to 7 could not achieve a balanced and satisfactory high level of light resistance and embeddability, and also could not achieve a satisfactory high level of adhesion and zipping resistance. In contrast, according to Examples 1 to 41, the encapsulating sheet of the present disclosure exhibits excellent light resistance and is also excellent in embedding property as shown in Tables 2 to 5. Furthermore, since the encapsulating sheet of the present disclosure is also excellent in adhesion and zipping property, it was found that the encapsulating sheet of the present disclosure can be suitably used for sealing a plurality of light emitting elements. [Explanation of symbols]
[0123] 1: Encapsulating sheet 2: Resin composition layer 3: Base material 4: Release liner 4a: First release liner 4b: Second release liner 5: Light emitting element 6: Substrate 7: Glass substrate
Claims
1. An encapsulating sheet for encapsulating light-emitting elements used in a display using a plurality of light-emitting elements as a light source, The encapsulating sheet includes a resin composition layer containing a resin (A) and an embeddability improver (B), The resin (A) has a glass transition temperature (Tg) of −30 to 40° C. and a weight average molecular weight (Mw) of 10,000 to 1,000,000; The embeddability improver (B) contains a phosphorus-containing compound (B1) and a phenolic hydroxyl group-containing compound (B2), The encapsulating sheet, wherein the resin composition layer has a thickness Ta of 1 to 100 μm.
2. The resin (A) is a (meth)acrylic resin (a), The (meth)acrylic resin (a) comprises a structural unit derived from an alkyl acrylate ester (a1) having a linear, branched or cyclic saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms, The encapsulating sheet according to claim 1, which is a copolymer having a structural unit derived from a methacrylic acid alkyl ester (a2) having a linear, branched or cyclic saturated aliphatic hydrocarbon group having 1 to 8 carbon atoms.
3. The encapsulating sheet according to claim 2 , wherein the (meth)acrylic resin (a) further contains a structural unit derived from (meth)acrylic acid (a3).
4. The encapsulating sheet according to claim 1, wherein the resin (A) is contained in an amount of 76 to 99.9% by mass based on the total mass of the resin composition layer.
5. The encapsulating sheet according to claim 1, wherein the content of the embeddability improver (B) is 0.1 to 15 mass% based on the total mass of the resin composition layer.
6. The encapsulating sheet according to claim 1, wherein the mass ratio B1:B2 of the phosphorus-containing compound (B1) to the phenolic hydroxyl group-containing compound (B2) in the embeddability improver (B) is 0.1:1 to 10:
1.
7. The encapsulating sheet according to any one of claims 1 to 6, wherein the resin composition layer has a loss tangent (tan δ40) at 40 ° C. obtained by dynamic viscoelasticity measurement in a tensile mode at a frequency of 10 Hz of 0.8 to 2.
0.
8. A display having an encapsulating layer comprising the resin composition layer of the encapsulating sheet according to claim 7.
Citation Information
Patent Citations
Resin composition for solar cell back face protective sheet
JP2014241383A
Curable resin composition, dry film, cured product, and electronic component
JP2022022562A
Photosensitive coloring composition, cured film using the same, color filter, optical filter, image display device, solid-state imaging device, and infrared sensor
JP7221348B1
Resin composition
WO2011111847A1
Flux-compatible epoxy-phenolic adhesive compositions for low gap underfill applications
WO2022211838A1
Cited By
Sheets for forming sealing layers, and composite sheets
JP7928606B1