Seal material

A thermoplastic elastomer-based sealing material with hollow glass powder ensures uniform distribution and low specific gravity, addressing uneven dispersion issues and enhancing surface smoothness and installation ease.

JP2024164368APending Publication Date: 2024-11-27KINUGAWA RUBBER IND CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023079787
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-15
Publication Date
2024-11-27

Smart Images

  • Figure 2024164368000005
    Figure 2024164368000005
  • Figure 2024164368000006
    Figure 2024164368000006
  • Figure 2024164368000007
    Figure 2024164368000007
Patent Text Reader

Abstract

To provide a technique capable of lowering specific gravity of a seal material by suppressing variation in the specific gravity and also contributing to surface smoothness.SOLUTION: In a seal material, an elastic material obtained by blending and kneading at least a thermoplastic elastomer and hollow glass powder is used, and the elastic material is injection-molded so as to form the seal material. In the elastic material, 5-50 pts.wt. of the glass powder is blended with 100 pts.wt. of the thermoplastic elastomer. The glass powder has a true density of 0.20-0.60 g / cm3 and a mean particle size of 20-60 μm. The specific gravity of the seal material is 0.40-1.20. The glass powder made of, for example, soda-lime-borate glass, and having compressive strength of 60-200 MPa, is applied.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a sealing material, and relates to a technique applicable, for example, between a body panel and a window glass of an automobile. [Background technology]

[0002] For example, elastic bodies such as sealing materials attached to the body of an automobile (e.g., sealing materials between the body panel and the window glass) are required to be made lighter (lower specific gravity) as automobiles become more electrified and to contribute to recent global environmental measures (e.g., improving automobile fuel efficiency, etc.).

[0003] One example of a method for reducing the weight of a sealing material is to use an elastic material containing a foaming material such as a chemical foaming agent or a thermally expandable balloon, and then mold the elastic material at a predetermined temperature to foam the foaming material (for example, to micro-foam the solid part, etc.), thereby forming foam cells inside the sealing material and reducing its specific gravity.

[0004] However, the foamable material mixed into the elastic material as described above is easily affected by the molding conditions (molding temperature, molding pressure) of the sealing material, and therefore may not foam as desired.

[0005] For example, when foam cells are formed near the surface of the sealing material, the surface of the sealing material becomes uneven, and the surface smoothness is reduced. Furthermore, when the foamable material foams non-uniformly, the specific gravity of the sealing material (for example, the specific gravity of each part of the sealing material) is likely to vary. In such a case, it is possible that the yield of the product, particularly in a product that requires a smooth surface, will decrease.

[0006] Therefore, in Patent Document 1, an attempt is considered to reduce the specific gravity of a sealing material without forming the foam cells described above by extruding an elastic material that contains hollow glass powder (hereinafter simply referred to as hollow glass powder) instead of a foamable material. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2006-56491 A Summary of the Invention [Problem to be solved by the invention]

[0008] In the case of a sealing material obtained by simply extruding an elastic material containing hollow glass powder, as in Patent Document 1, for example, the hollow glass powder may be unevenly dispersed inside the sealing material, resulting in large variations in the specific gravity of the sealing material.

[0009] The present invention has been made in consideration of the technical problems described above, and aims to provide a technology that can suppress the variation in specific gravity in a sealing material, thereby reducing the specific gravity, and also contribute to surface smoothness. [Means for solving the problem]

[0010] The sealing material according to the present invention can contribute to solving the above problems. One embodiment of the sealing material is a sealing material obtained by injection molding an elastic material obtained by blending and kneading at least a thermoplastic elastomer and hollow glass powder, the elastic material being blended in a ratio of 5 to 50 parts by weight of the glass powder to 100 parts by weight of the thermoplastic elastomer, and the glass powder has a true density of 0.20 to 0.60 g / cm. 3 The sealing material has an average particle size of 20 to 60 μm, and a specific gravity of 0.40 to 1.20.

[0011] In the above-mentioned embodiment, the glass powder may be made of soda-lime-borate glass and may have a compressive strength of 60 MPa to 200 MPa (preferably 80 MPa to 200 MPa). Also, the thermoplastic elastomer may be mainly composed of polyvinyl chloride resin.

[0012] The thermoplastic elastomer may be blended with 40 to 130 parts by weight of a plasticizer and 20 to 60 parts by weight of calcium carbonate per 100 parts by weight of polyvinyl chloride resin, and the Shore A hardness of the sealing material may be 60 to 80.

[0013] The polyvinyl chloride resin may be characterized in that it has a complex viscosity at a temperature of 150° C. of 1.0 to 2.0 kPa·s.

[0014] The sealing material may be a quarter glass seal that can be attached between a body panel and a window glass of an automobile. Effect of the Invention

[0015] According to the present invention, it is possible to suppress the variation in specific gravity in the sealing material, thereby making it possible to reduce the specific gravity, and it is also possible to contribute to surface smoothness. [Brief description of the drawings]

[0016] [Figure 1] FIG. 2 is an external view for explaining product sample S. [Diagram 2] FIG. 2 is a schematic explanatory diagram showing a method for observing friction characteristics in Verification Example 1. [Diagram 3] A photograph showing the cross section of product sample SM3 photographed by SEM (cross-sectional photograph of product sample SM3 enlarged 400 times). [Figure 4] Complex viscosity characteristics versus temperature change. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] The sealing material according to the embodiment of the present invention is completely different from a configuration obtained by simply extruding an elastic material containing hollow glass powder (hereinafter, simply referred to as a conventional configuration).

[0018] That is, the sealing material of this embodiment uses an elastic material obtained by blending and kneading at least a thermoplastic elastomer and a hollow glass powder, and is injection molded from the elastic material. The elastic material has a true density of 0.20 to 0.60 g / cm3 per 100 parts by weight of the thermoplastic elastomer. 3 The hollow glass powder having an average particle size of 20 to 60 μm is blended in an amount of 5 to 50 parts by weight.

[0019] According to the sealing material of this embodiment, the hollow glass powder mixed with the elastic material can reduce the specific gravity (for example, the specific gravity can be set to 0.40 to 1.20) without forming foam cells inside the sealing material, and the desired surface smoothness can be easily obtained. In addition, the hollow glass powder is distributed so as to be uniformly dispersed inside the sealing material, and it is possible to suppress the variation in the specific gravity of the sealing material. This may contribute significantly to the product yield.

[0020] The sealing material of this embodiment may be formed by injection molding an elastic material in which a predetermined hollow glass powder is appropriately mixed with a thermoplastic elastomer as described above, and various design modifications are possible.

[0021] In other words, it is possible to appropriately apply common technical knowledge in various fields (e.g., the injection molding field, the sealing material field, the thermoplastic elastomer field, the hollow glass powder field, etc.) and, as necessary, to appropriately refer to prior art documents, etc., and to modify the design, as shown in the following example.

[0022] Example <Examples of elastic materials that can be used as sealing materials> The elastic material to be used in the sealing material must contain at least a thermoplastic elastomer as the base material of the elastic material and a thermoplastic elastomer having a true density of 0.20 to 0.60 g / cm. 3The thermoplastic elastomer can be injection molded by mixing and kneading the above-mentioned hollow glass powder appropriately, and the hollow glass powder can be mixed in a ratio of 5 to 50 parts by weight per 100 parts by weight of the thermoplastic elastomer.

[0023] The thermoplastic elastomer can be appropriately applied as long as it is used, for example, as a sealing material for automobiles. Examples of the thermoplastic elastomer include those mainly composed of rubber material, resin, etc., and specific examples of the thermoplastic elastomer include those mainly composed of polyvinyl chloride resin, TPV, etc.

[0024] Examples of polyvinyl chloride resins include TH-800 manufactured by Taiyo Vinyl, S1008 manufactured by Kaneka, and TK-800 manufactured by Shin-Etsu Chemical Co., Ltd., and it is preferable to use one suitable for injection molding.

[0025] The hollow glass powder has a strength sufficient to prevent it from being broken during kneading after being mixed with a thermoplastic elastomer (hereinafter simply referred to as kneading) or during injection molding, and can be appropriately dispersed and distributed in the sealing material after the injection molding, and various embodiments can be applied. Examples of such hollow glass powder include those formed into hollow powder using soda-lime borosilicate glass and having a pressure resistance strength (when the non-destructive survival rate of the hollow powder is 90% or more) in the range of 60 MPa to 200 MPa.

[0026] If the pressure resistance of the hollow glass powder is too low, less than 60 MPa, the hollow glass powder is difficult to withstand the stress (for example, shear force during kneading) that may act during kneading or injection molding, and is easily broken. If a large amount of the broken hollow glass powder exists inside the sealing material, the specific gravity of the target sealing material cannot be reduced as desired. In addition, the broken hollow glass powder may be distributed unevenly inside the sealing material, and in that case, the specific gravity of the sealing material may vary greatly. For this reason, the hollow glass powder is preferably applied with a pressure resistance of 60 MPa or more, and more preferably with a pressure resistance of 80 MPa or more.

[0027] On the other hand, the upper limit of the pressure resistance of the hollow glass powder is not particularly limited, but as long as it is within a range not exceeding 200 MPa, it is possible to sufficiently suppress the pressure resistance so that the hollow glass powder is not destroyed during kneading or injection molding and so that the hollow glass powder is not unevenly dispersed inside the sealing material.

[0028] Moreover, the hollow glass powder may be applied after previously subjecting the outer peripheral surface of the hollow glass powder to a surface treatment so as to enhance adhesion to a thermoplastic elastomer when the hollow glass powder is blended with an elastic material.

[0029] In addition to the thermoplastic elastomer and hollow glass powder, the elastic material may contain various additives taking into consideration, for example, the mixability of the elastic material and the dispersibility of the hollow glass powder. One example of such an additive is the addition of a plasticizer or a filler.

[0030] The types and amounts of additives such as plasticizers and fillers can be appropriately set so that the Shore A hardness of the desired sealing material is within the range of about 60 to 80, which enables the sealing material to fully exhibit the various functions required of the sealing material (e.g., sealing ability, installation ability).

[0031] Specific examples of plasticizers include diisononyl phthalate (DINP; for example, Vinycizer 90 manufactured by Kao Corporation, Sansocizer DINP manufactured by New Japan Chemical Co., Ltd., DINP manufactured by J-Plus Corporation, etc.), di-2-ethylhexyl phthalate (DOP; for example, Vinycizer 80 manufactured by Kao Corporation, Sansocizer DOP manufactured by New Japan Chemical Co., Ltd., DOP manufactured by J-Plus Corporation, etc.), di-n-decyl phthalate (DDP; for example, Vinycizer 105 manufactured by Kao Corporation, etc.), diisodecyl phthalate (DIDP; for example, Sansocizer DIDP manufactured by New Japan Chemical Co., Ltd.), etc., which may be blended in an amount of 40 to 130 parts by weight per 100 parts by weight of the thermoplastic elastomer. As for fillers, calcium carbonate (for example, calcium carbonate suitable for polyvinyl chloride includes NITOREX #23PS and NCC·P #2300 manufactured by Nitto Funka Co., Ltd., and Success 200R manufactured by Omi Chemical Industry Co., Ltd.) can be used in an amount of 20 to 60 parts by weight per 100 parts by weight of thermoplastic elastomer.

[0032] According to the elastic material containing a plasticizer as described above, the kneadability is improved, so that the hollow glass powder contained in the elastic material is more likely to be distributed uniformly within the sealing material after injection molding, making it possible to further suppress variations in the specific gravity of the sealing material.

[0033] In addition to blending a plasticizer as described above, another method is to set the viscosity of the thermoplastic elastomer itself to be low (for example, to set the complex viscosity at a temperature of 150°C to 1.0 to 2.0 kPa s as in Verification Example 4 described later).

[0034] <An example of injection molding> In the case of injection molding of an elastic material, a mold having a cavity of a shape corresponding to the target sealing material is used, and the sealing material is formed by injecting the elastic material into the cavity. For example, the steps of clamping the mold, injecting the elastic material, opening the mold, and removing the molded product are carried out in that order.

[0035] As a specific example, the elastic material injection process may include a filling process in which the elastic material is injected into the cavity of a mold at a predetermined pressure (primary pressure) to fill the cavity, a pressure holding process in which the state in which the elastic material is filled in the cavity is maintained at a predetermined pressure (secondary pressure), and a cooling process in which the elastic material in the cavity is cooled and solidified.

[0036] The conditions of each step of injection molding are not particularly limited, and can be set to the same conditions as those of a sealing material (solid molding) that does not use hollow glass powder. However, depending on the shape of the cavity (i.e., the shape of the intended sealing material), etc., the specific gravity balance of the sealing material after injection molding may be easily uneven, or unintended patterns (jetting, flow marks, etc.) may be easily formed. If there is such a possibility, in addition to appropriately setting the conditions of each step (for example, setting the injection speed, temperature, etc. of the elastic material, or the temperature of the mold, etc.), the viscosity of the elastic material itself may be reduced (for example, by blending a plasticizer or setting the viscosity of the thermoplastic elastomer itself to be low) to increase the kneadability of the elastic material and the dispersibility of the hollow glass powder.

[0037] <Example of sealing material> The shape and other aspects of the sealant are not particularly limited, and may be any shape that can be attached to any position of an automobile and can perform the desired functions at the attachment location. An example is a shape that can be attached to the body panel, door panel, sash, etc. of an automobile, and a specific example is a quarter glass seal that can be attached between the body panel (quarter panel) and the window glass (quarter glass).

[0038] When a sealing material and another resin product (such as a molding for a glass run) are attached adjacent to each other, it is preferable to make the glossiness of both the products equal so that they have a unified appearance. As a specific example, since many moldings for glass runs in general automobiles are products with low glossiness (for example, products with a gloss value of about 5), it is preferable to similarly keep the glossiness of a sealing material that is attached adjacent to the molding low.

[0039] <Verification example 1> First, 5 to 40 parts by weight of hollow glass powder was mixed with 100 parts by weight of polyvinyl chloride resin, and kneaded using an open roll (roll surface temperature 160°C, kneading time 5 minutes) to obtain various elastic materials M1 to M4 shown in Table 1. Note that S1008 manufactured by Kaneka Corporation was used as the polyvinyl chloride resin (also used in verification examples 2 to 4 described later), and iM16K manufactured by 3M Corporation (true density 0.46 g / cm3) was used as the hollow glass powder. 3 , compressive strength 110 MPa, average particle size 20 μm) were applied. In addition, as a reference example, an elastic material P1 that does not contain hollow glass powder was also obtained.

[0040] Then, each of the elastic materials P1, M1 to M4 is injection molded using a mold having a cavity of a desired shape to produce a product sample S of a quarter glass seal for a commercially available car having an approximately rectangular shape as shown in FIG. P1 ,S M1 ~S M4 (Hereinafter, these will be referred to simply as product sample S. P2 ,S P3 ,S M5 ~S M10A sample of the elastic material was prepared (also referred to as product sample S) and its specific gravity characteristics, friction characteristics, and attachment properties were measured by the methods described below, with the results shown in Table 1. In the injection molding, the filling process (primary temperature 185°C, primary injection pressure 60 MPa), pressure holding process (primary pressure 30 MPa), and cooling process (cooling time 17 seconds) were appropriately performed in the elastic material injection process. Of the four corners a to d of product sample S shown in Figure 1, corner a was formed at the position closest to the gate side of the mold.

[0041] <Specific gravity characteristics> The specific gravity of each product sample S was measured by the underwater displacement method based on JIS K 7112 Method A.

[0042] <Friction characteristics> (See Fig. 2 of JP2016-000485) First, each product sample S was punched into a rectangular plate shape (a rectangular plate shape of 5 mm × 100 mm) to prepare each test piece 20 shown in FIG. 2. Next, dirt on one end face of the test piece 20 (the face on which the weight member 22 described later is placed) was wiped off with alcohol, and then the test piece 20 was placed on a support table (test table) 21 of a friction coefficient measuring instrument (HEIDON-14D manufactured by Shinto Scientific) as shown in FIG. 2 (placed so that the base is located at the bottom and the covering is located at the top in the figure). Then, the weight member 22, which constitutes an R50 spherical glass and to which a load of 0.98 N is applied, was placed on one end face of the test piece 20 (placed with the R50 spherical side), and the weight member 22 was slid (sliding while contacting one end face of the test piece 20) in the horizontal direction (the longitudinal direction of the test piece 20; the direction of the arrow in the figure) at a speed of 1000 mm / min to measure the static friction coefficient (μs) and the dynamic friction coefficient (μd). The stylus used in the friction coefficient measurement device had a stylus tip radius of 2 μm.

[0043] <Installability> Each product sample S was manually installed in a specified installation position of an actual quarter glass seal for commercially available vehicles, and the installation ability was evaluated. In the installation ability section of Table 1, the symbol "〇" indicates that the product sample S could be installed, and the symbol "◎" indicates that the product sample S could be installed more easily than in the case of the symbol "〇". [Table 1] According to the results shown in Table 1, product sample S M1 ~S M4 In this case, product sample S P1 Compared to sample S, as the amount of hollow glass powder added increased, the specific gravity and friction became lower and the installation ease improved. M1 ~S M4 It was found that one of the reasons why friction decreased as the amount of hollow glass powder added increased is that the hollow glass powder exposed on the surface of product sample S contributed to the decrease in friction.

[0044] <Verification example 2> First, various hollow glass powders were appropriately mixed with 100 parts by weight of polyvinyl chloride resin and kneaded using an open roll (roll surface temperature 160°C, kneading time 5 minutes) to obtain various elastic materials P2, M5 to M7 shown in Table 2. The hollow glass powder was K20 (true density 0.20 g / cm) manufactured by 3M. 3 , compression strength 3.4MPa, average grain size 60μm), S32HS (true density 0.32g / cm 3 , compressive strength 41MPa, average grain size 25μm), iM16K and Y12000 (true density 0.60g / cm3) manufactured by Seishin Enterprise Co., Ltd. 3 , compressive strength 82 MPa, average grain size 48 μm) were applied.

[0045] The specific gravity of each of the elastic materials P2, M5 to M7 itself and the product sample S obtained by press molding each of the elastic materials P2, M5 to M7 are P2 ,S M5 ~S M7 The specific gravity of each of the elastic materials P2, M5 to M7 was obtained by injection molding in the same manner as in Verification Example 1.P2 ,S M5 ~S M7 The specific gravity of and were observed by the same underwater displacement method as in Verification Example 1, and the observation results shown in Table 2 were obtained. In the press molding, a press molding die having a cavity similar to that in the case of injection molding was used, and press molding was appropriately performed by a general press molding method (the cavity of the die was filled with an elastic material, and press molding was performed at a pressure of 20 MPa and a pressurization time of 2 minutes and 30 seconds). [Table 2] According to the results shown in Table 2, product sample S M5 ~S M7 The specific gravity of each product sample S P2 The reason for this is that the specific gravity of product sample S is lower than that of the product sample S. P2 In the case of sample S, it is considered that the hollow glass powder was broken during kneading or molding of the elastic material P2 because the pressure resistance of the hollow glass powder mixed in the elastic material P2 was too low. M5 ~S M7 It was found that the hollow glass powder mixed in the elastic materials M5 to M7 was prevented from being destroyed during kneading and molding.

[0046] <Verification example 3> Product sample S shown in Table 1 P1 ,S M3 The specific gravity variation, dimensional stability, glossiness, and color difference were observed using the methods described below, and the results are shown in Table 3. M3 When the cross section was photographed using an SEM, the results shown in Figure 3 were obtained.

[0047] <Variation in specific gravity> Using the same underwater replacement method as in Verification Example 1, each product sample S P1 ,S M3 The specific gravity of each of the four corners a to d was measured. P1 ,S M3 The weight of each was also measured.

[0048] <Dimensional stability (shape stability against temperature changes)> Each product sample S P1 ,S M3 The deformation amount was measured when the specimen was placed in an atmosphere where the temperature changed within the range of -40°C to 90°C, and each linear expansion coefficient α (1 / °C) was derived based on the following formula (1). In the following formula (1), L0 is the reference dimension of product sample S at a temperature of 23°C, L1 is the dimension of product sample S at a temperature of -40°C, L2 is the dimension of product sample S at a temperature of 90°C, and Δt is the temperature difference (-40°C to 90°C).

[0049] α=((L0-L1)+(L2-L0)) / (Δt×L0)...(1).

[0050] <Glossiness> Each product sample S was measured using a Konica Minolta gloss meter (GM-60S). P1 ,S M3 The surfaces were observed and the gloss values ​​of each were calculated.

[0051] <Color difference> Each product sample S was measured using a spectrophotometer (CM-2600d) manufactured by Konica Minolta. P1 ,S M3 The surface of the product sample S is observed. P1 Based on the standard, the product sample S M3 The hue differences ΔE and ΔL were derived. [Table 3] According to the results shown in Table 3, product sample S M3 In the case of the product sample S, the specific gravity of each of the corners a to d is approximately the same, and the variation in the specific gravity is sufficiently suppressed. P1 In addition, it was found that the product sample S M3 is product sample S P1 In comparison, the product sample S itself was lighter in weight and had better dimensional stability.

[0052] In addition, product sample S M3 is product sample SP1 The glossiness is lower than that of the molding of a typical glass run for an automobile (e.g., gloss value of about 5), and the hue differences ΔE and ΔL are sufficiently small. The reason for this is that, as shown in Figure 3, the product sample S M3 The surface of the o It was found that the surface of the hollow glass powder (shown by a dotted line in FIG. 1) had a sufficiently good surface smoothness, although it had very slight microscopic irregularities due to the hollow glass powder, and the particle size of the hollow glass powder was sufficiently small, so that the gloss of the surface was sufficiently suppressed.

[0053] <Verification example 4> First, 50 parts by weight of hollow glass powder (iM16K) was mixed with 100 parts by weight of polyvinyl chloride resin, and further, 100 to 125 parts by weight of diisononyl phthalate and 25 to 50 parts by weight of calcium carbonate were mixed, and the mixture was appropriately kneaded in the same manner as in Verification Example 1 to obtain various elastic materials M8 to M10 shown in Table 4. Note that Kao Corporation's Vinylsizer 90 was used for diisononyl phthalate, and Nitorex #23PS, manufactured by Nitto Powder Chemical Co., Ltd., was used for calcium carbonate. As a reference example, elastic material P3 without hollow glass powder was also obtained.

[0054] The complex viscosity of each of the elastic materials P3, M8 to M10 was measured by the method described below, and the results shown in Table 4 and Figure 4 were obtained. In addition, each of the elastic materials P3, M8 to M10 was injection molded in the same manner as in Verification Example 1 to obtain product samples S P3 ,S M8 ~S M10 The appearance of each corner a side was observed, and the results are shown in Table 4.

[0055] <Complex viscosity> Using the viscoelasticity measuring device (RPA2000 manufactured by Alpha Technologies, USA), the complex viscosity η of each elastic material P3, M8 to M10 at temperatures of 150°C to 190°C, speed of 50 rad / s, and strain of 13.95 was measured. * (kPa·s), respectively.

[0056] <Appearance> The corner a of the product sample S was visually inspected for the presence or absence of unintended patterns (jetting, flow marks, etc.). [Table 4] According to the results shown in Table 4 and Figure 4, the complex viscosity η * It was found that the elastic material M10 was suppressed and the kneading property was improved. In particular, in the elastic material M10, the product sample S obtained by injection molding the elastic material M10 was M10 Since the appearance of the glass was good, it was found that the dispersibility of the hollow glass powder was also high.

[0057] Therefore, for the elastic material M10, the complex viscosity η at a temperature of 150°C is * The design was modified appropriately so that the value was within the range of 1.0 to 2.0 kPa·s, and the product sample S M10 When the results were observed, it was confirmed that a good appearance was obtained similar to the results shown in Table 4, and the dispersibility of the hollow glass powder was sufficiently high.

[0058] Although the present invention has been described in detail above only with respect to the specific examples, it will be apparent to those skilled in the art that various modifications are possible within the scope of the technical concept of the present invention, and it is natural that such modifications fall within the scope of the claims.

[0059] For example, the polyvinyl chloride resin, hollow glass powder, plasticizer, filler, etc., which are applied to the elastic material, are not limited to the products shown in Verification Examples 1 to 4, and various products can be applied. In other words, even if products other than those shown in Verification Examples 1 to 4 are applied (for example, the products explained in the item <<Examples>> are appropriately applied), it is sufficient to at least fall within the scope of the claims, and it is possible to achieve the same effects as those of Verification Examples 1 to 4. [Explanation of symbols]

[0060] S: Product sample (sealing material) S0…Surface a~d…corner

Claims

1. A sealing material made by injection molding an elastic material obtained by blending and kneading at least a thermoplastic elastomer and hollow glass powder, The elastic material is a blend of 5 to 50 parts by weight of the glass powder with respect to 100 parts by weight of the thermoplastic elastomer, The glass powder has a true density of 0.20 to 0.60 g / cm 3 and the average particle size is 20 to 60 μm; The specific gravity of the sealing material is 0.40 to 1.

20.

2. 2. The sealing material according to claim 1, wherein the glass powder is made of soda-lime-borate glass and has a pressure resistance of 60 MPa to 200 MPa.

3. 3. The sealing material according to claim 1, wherein the thermoplastic elastomer is mainly composed of polyvinyl chloride resin.

4. The thermoplastic elastomer is blended with 40 to 130 parts by weight of a plasticizer and 20 to 60 parts by weight of calcium carbonate per 100 parts by weight of polyvinyl chloride resin, 3. The sealing material according to claim 1, wherein the sealing material has a Shore A hardness of 60 to 80.

5. 5. The sealing material according to claim 4, wherein the polyvinyl chloride resin has a complex viscosity at a temperature of 150° C. of 1.0 to 2.0 kPa·s.

6. 3. The sealing material according to claim 1, which is a quarter glass seal that can be installed between a body panel and a window glass of an automobile.

Citation Information

Patent Citations

  • Low-specific-gravity high-performance sealing agent for vehicle

    JP1999092747A

  • Thermoplastic elastomer composition

    JP2003183449A

  • Sealant

    JP2006056491A

  • Resin composition and heat insulating member formed of the same

    JP2013124295A

  • Sealing composition and method of producing the same

    JP2015196817A