Negative electrode for power storage device, and power storage device
The negative electrode structure with tailored polymers (A and B) addresses adhesion issues in silicon-based active materials, enhancing durability and capacity by suppressing expansion and reducing resistance in power storage devices.
Patent Information
- Application Number
- JP2023079845
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-15
- Publication Date
- 2024-11-27
AI Technical Summary
Conventional negative electrodes for power storage devices face issues with insufficient adhesion of new active materials like silicon, which undergo significant volume changes during lithium ion storage, leading to electrode deterioration and poor durability.
A negative electrode structure comprising a first layer with a polymer (A) containing specific repeating units and a second layer with a polymer (B) with different compositions, enhancing adhesion and binding forces between the current collector and active materials, thereby suppressing electrode expansion and reducing resistance.
The improved adhesion and binding forces effectively suppress electrode expansion, enhance capacity, and improve cycle characteristics by maintaining structural integrity and reducing internal resistance.
Smart Images

Figure 2024164397000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a negative electrode for an electricity storage device, and to an electricity storage device including the negative electrode. [Background technology]
[0002] With the technological development and increasing demand for mobile devices, the demand for secondary batteries as an energy source is rapidly increasing. Among these secondary batteries, lithium-ion secondary batteries, which have high energy density and voltage, have been commercialized.
[0003] Currently, in order to overcome various problems associated with lithium ion secondary batteries, technology is being considered in which the electrodes used in lithium ion secondary batteries are multi-layered, with each layer having different physical properties (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2021-5461 A Summary of the Invention [Problem to be solved by the invention]
[0005] Conventional negative electrodes for electricity storage devices have a large capacity for absorbing lithium ions, and the adhesion is not sufficient for practical use of new active materials such as silicon materials, which have a large volume change associated with the absorption and release of lithium ions. Such negative electrodes for electricity storage devices have an issue in that the durability required for practical use is not sufficiently obtained because the electrode deteriorates due to the negative electrode active material falling off after repeated charging and discharging.
[0006] Some aspects of the present invention provide a negative electrode for an electricity storage device that can effectively suppress electrode expansion and reduce the internal resistance of the electrode by improving the adhesive strength between the negative electrode current collector and the negative electrode mixture layer and the binding strength between active materials. Also, some aspects of the present invention provide an electricity storage device that includes such an electricity storage device negative electrode and thereby has improved capacity and cycle characteristics. [Means for solving the problem]
[0007] The present invention has been made to solve at least a part of the above-mentioned problems, and can be realized in any of the following aspects.
[0008] One aspect of the negative electrode for an electricity storage device according to the present invention is a negative electrode current collector; and a negative electrode mixture layer formed on the negative electrode current collector, the negative electrode mixture layer includes a first layer formed on the negative electrode current collector and a second layer formed on the first layer, the first layer includes a first negative electrode active material and a polymer (A), the polymer (A) contains 0.1% by mass or more and less than 5% by mass of a repeating unit (a1) derived from an unsaturated carboxylic acid, when the total amount of the repeating units contained in the polymer (A) is 100% by mass; the second layer includes a second negative electrode active material and a polymer (B), When the total amount of repeating units contained in the polymer (B) is taken as 100% by mass, the polymer (B) contains 5% by mass or more and 20% by mass or less of repeating units (a1) derived from an unsaturated carboxylic acid.
[0009] In one embodiment of the negative electrode for an electricity storage device, the polymer (A) contains 20% by mass or more and less than 40% by mass of repeating units (a3) derived from an aromatic vinyl compound, when the total amount of repeating units contained in the polymer (A) is 100% by mass; When the total amount of repeating units contained in the polymer (B) is taken as 100% by mass, the polymer (B) may contain 1% by mass or more and less than 20% by mass of repeating units (a3) derived from an aromatic vinyl compound.
[0010] In any one of the embodiments of the negative electrode for an electricity storage device, the polymer (A) contains 15% by mass or more and 60% by mass or less of repeating units (a2) derived from a conjugated diene compound, when the total amount of repeating units contained in the polymer (A) is 100% by mass; When the total amount of repeating units contained in the polymer (B) is taken as 100 mass%, the polymer (B) may contain 15 mass% or more and 60 mass% or less of repeating units (a2) derived from a conjugated diene compound.
[0011] In any one of the embodiments of the negative electrode for an electricity storage device, the polymer (A) contains a repeating unit (a4) derived from an unsaturated carboxylate ester in an amount of 1 mass% or more and 20 mass% or less, when the total amount of repeating units contained in the polymer (A) is 100 mass%, When the total amount of repeating units contained in the polymer (B) is taken as 100% by mass, the polymer (B) may contain 1% by mass or more and 20% by mass or less of repeating units (a4) derived from an unsaturated carboxylate ester.
[0012] In any one of the embodiments of the negative electrode for an electricity storage device, the polymer (A) contains 5% by mass or more and 40% by mass or less of a repeating unit (a5) derived from an α,β-unsaturated nitrile compound, when the total amount of the repeating units contained in the polymer (A) is 100% by mass; When the total amount of repeating units contained in the polymer (B) is 100% by mass, the polymer (B) may contain 5% by mass or more and 40% by mass or less of repeating units (a5) derived from an α,β-unsaturated nitrile compound.
[0013] In any one of the embodiments of the negative electrode for an electricity storage device, the polymer (A) and the polymer (B) are each in the form of particles, The number average particle size of the particles of the polymer (A) is 50 nm or more and less than 150 nm, The number average particle size of the particles of the polymer (B) may be 150 nm or more and 300 nm or less.
[0014] One aspect of the electricity storage device according to the present invention is The negative electrode for an electricity storage device according to any one of the above aspects is provided. Effect of the Invention
[0015] The negative electrode for an electricity storage device according to the present invention improves the adhesive strength between the negative electrode current collector and the negative electrode mixture layer and the binding strength between the active materials, thereby effectively suppressing electrode expansion and reducing the internal resistance of the electrode, thereby improving the capacity and cycle characteristics of the electricity storage device. [Brief description of the drawings]
[0016] [Figure 1] 1 is a cross-sectional view that illustrates a schematic structure of a negative electrode for an electricity storage device according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Preferred embodiments of the present invention will be described in detail below. Note that the present invention is not limited to the embodiments described below, and should be understood to include various modified examples that are implemented within the scope of the present invention.
[0018] In this specification, "-(meth)acrylic acid" refers to -acrylic acid or -methacrylic acid, and "-(meth)acrylate" refers to -acrylate or -methacrylate.
[0019] In this specification, a numerical range described as "X to Y" is interpreted as including the numerical value X as the lower limit and including the numerical value Y as the upper limit.
[0020] 1. Negative electrodes for energy storage devices FIG. 1 is a cross-sectional view that shows a schematic structure of an electricity storage device negative electrode 100 according to one embodiment of the present invention. As shown in FIG. 1, the electricity storage device negative electrode 100 according to this embodiment includes a negative electrode current collector 10 and a negative electrode mixture layer 20 formed on the negative electrode current collector 10. The negative electrode mixture layer 20 includes a first layer 20a formed on the negative electrode current collector 10 and a second layer 20b formed on the first layer 20a. The first layer 20a includes a first negative electrode active material and a polymer (A), and when the total of the repeating units included in the polymer (A) is taken as 100% by mass, the polymer (A) contains 0.1% by mass or more and less than 5% by mass of a repeating unit (a1) derived from an unsaturated carboxylic acid. The second layer 20b contains a second negative electrode active material and a polymer (B). When the total amount of repeating units contained in the polymer (B) is taken as 100 mass%, the polymer (B) contains 5 mass% or more and 20 mass% or less of repeating units (a1) derived from an unsaturated carboxylic acid.
[0021] 1 is merely an example for explaining one embodiment of the present invention, and the present invention is not limited thereto. The negative electrode for an electricity storage device according to this embodiment will be described in detail below.
[0022] 1.1.Negative electrode current collector The negative electrode current collector 10 may be selected from the group consisting of copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer substrate coated with a conductive metal, and combinations thereof. Among these, copper foil and copper foam are preferred.
[0023] The thickness of the negative electrode current collector 10 is preferably 1 μm to 50 μm, more preferably 5 μm to 30 μm, and particularly preferably 8 μm to 20 μm.
[0024] 1.2.Negative electrode composite layer Negative electrode mixture layer 20 includes a first layer 20a formed on negative electrode current collector 10, and a second layer 20b formed on first layer 20a.
[0025] The negative electrode 100 for an electricity storage device according to this embodiment can be manufactured by a method including a step of forming a first layer 20a containing a first negative electrode active material and a polymer (A) on a negative electrode current collector 10 (step 1), and a step of forming a second layer 20b containing a second negative electrode active material and a polymer (B) on the first layer 20a (step 2).
[0026] Step 1 is a step of forming a first layer 20a on a negative electrode current collector 10. The first layer 20a is formed on the negative electrode current collector 10 by dissolving or depositing a first negative electrode active material and a polymer (A) in a liquid medium. The slurry for the negative electrode of the first electricity storage device produced by dispersing the slurry is coated and dried, or the slurry for the negative electrode of the first electricity storage device is coated on another support and then peeled off from the support to obtain a film of the slurry for the negative electrode of the first electricity storage device, which is then laminated onto the negative electrode collector 10.
[0027] The step of coating the negative electrode current collector 10 with the slurry for the negative electrode of the first electricity storage device can be carried out by a conventional method, specifically, by a method such as bar coating, casting, or spraying.
[0028] In addition, the process of drying after coating the slurry for the negative electrode of the first electricity storage device is a process for removing the liquid medium contained in the slurry, and may be performed by a conventional drying method such as hot air drying, natural drying, or heating.
[0029] Next, step 2 is a step of forming a second layer 20b containing a second negative electrode active material and a polymer (B) on the first layer 20a formed in step 1. The second layer 20b is formed by coating a slurry for a negative electrode of a second electricity storage device, which is produced by dissolving or dispersing the second negative electrode active material and the polymer (B) in a liquid medium, on the first layer 20a and drying it, or by coating the slurry for a negative electrode of a second electricity storage device on another support, and then peeling it off from the support to obtain a film, which is then laminated on the first layer 20a.
[0030] The negative electrode mixture layer 20 having the above-mentioned configuration may have a thickness ratio of the first layer 20a to the total thickness of the first layer 20a and the second layer 20b of 0.5 or less. When the thickness ratio of the first layer 20a is 0.5 or less, migration of the polymer (A) in the first layer 20a can be suppressed, and a decrease in adhesion between the negative electrode current collector 10 and the first negative electrode active material can be prevented. Considering the reduction in the migration of the polymer (A) and the remarkable effect of improving the adhesion between the negative electrode current collector 10 and the first negative electrode active material, the thickness ratio of the first layer 20a to the total thickness of the first layer 20a and the second layer 20b is preferably 0.1 to 0.5, more preferably 0.1 to 0.4.
[0031] In addition, under the condition that the above-mentioned range of thickness ratio is satisfied, the average thickness of the first layer 20a may be 10 μm to 1000 μm. When the first layer 20a has a thickness within the above range, migration of the polymer (A) of the first layer 20a can be reduced, and the adhesion between the negative electrode current collector 10 and the first negative electrode active material and the performance of the electricity storage device can be improved using a small amount of binder. Considering the reduction in the migration of the polymer (A) and the remarkable effect of improving the adhesion between the negative electrode current collector 10 and the first negative electrode active material due to the reduction, the average thickness of the first layer 20a is preferably 20 μm to 500 μm.
[0032] In the negative electrode composite layer 20 of the negative electrode for the electric storage device according to this embodiment, the first layer 20a contains a polymer (A) having a relatively low acid content, and the second layer 20b contains a polymer (B) having a relatively high acid content. Of these, the second layer 20b tends to be more susceptible to structural deterioration due to expansion and contraction of the active material than the first layer 20a. The slurry for the second electric storage device negative electrode used in forming the second layer 20b contains the polymer (A) having a relatively high acid content, and therefore has excellent polymer mechanical properties in the electrolyte, and can alleviate the stress generated during expansion and contraction. As a result, structural deterioration of the negative electrode for the electric storage device can be suppressed. On the other hand, the slurry for the first electric storage device negative electrode used in forming the first layer 20a contains the polymer (A) having a relatively low acid content, and therefore is more compatible with the electrolyte, and the first layer 20a in which lithium ions are more likely to diffuse can be formed. In this way, it is believed that the first layer 20a contains a polymer (A) having a relatively low acid content, and the second layer 20b contains a polymer (B) having a relatively high acid content, thereby providing excellent adhesion between the negative electrode current collector 10 and the negative electrode mixture layer 20, effectively suppressing electrode expansion, and improving the cycle characteristics of the electricity storage device. In particular, the use of the polymer (A) contained in the first layer 20a provides excellent adhesion between the negative electrode active material, the conductive assistant, and the negative It is believed that this can play a role in helping the bonding between electrode active materials, thereby reducing the internal resistance of the negative electrode for an electricity storage device.
[0033] The content of the polymer (B) in the second layer 20b is preferably 1% by mass to 20% by mass with respect to the total mass of the second layer 20b. When the polymer (B) is contained in the second layer 20b in an amount within the above range, the adhesion between the negative electrode active materials in the second layer 20b is excellent, and therefore the electrical conductivity and energy density in the second layer 20b can be improved. Considering the improvement in adhesion due to the inclusion of the polymer (B) in the second layer 20b and the remarkable effect of improving the electrical conductivity and energy density in the negative electrode, the content of the polymer (B) is preferably 1% by mass to 10% by mass, and more preferably 1% by mass to 7% by mass with respect to the total mass of the second layer 20b.
[0034] The second layer 20b having the above-mentioned configuration may have an average thickness with a thickness ratio to the average thickness of the first layer 20a exceeding 1. Considering the remarkable improvement effect by optimizing the binder properties required depending on the thickness in the negative electrode, the thickness ratio of the first layer 20a to the second layer 20b is preferably 1-3:5-9.
[0035] Furthermore, under the condition that the above-mentioned range of the thickness ratio is satisfied, the average thickness of the second layer 20b is preferably 10 μm to 1000 μm, more preferably 20 μm to 500 μm, and particularly preferably 30 μm to 300 μm.
[0036] In the negative electrode for an electricity storage device according to this embodiment, the ratio of the thickness of the first layer 20a to the total thickness of the first layer 20a and the second layer 20b is 0.1 to 0.5, and the ratio of the thickness of the first layer 20a to the thickness of the second layer 20b may be 1-3:5-9.
[0037] In the negative electrode for an electricity storage device according to this embodiment as described above, the total loading amount of the first negative electrode active material and the second negative electrode active material contained in the first layer 20a and the second layer 20b is preferably 50 mg / 25 cm 2 ~1000mg / 25cm 2 and more preferably 50 mg / 25 cm 2 ~500mg / 25cm 2 It is.
[0038] The negative electrode for an electricity storage device according to this embodiment may contain a polymer (A) and a polymer (B) together with the particulate first and second negative electrode active materials, thereby forming micropores in each active material layer. Specifically, the negative electrode for an electricity storage device according to this embodiment may have a porosity of preferably 10 volume % to 50 volume %, more preferably 20 volume % to 40 volume %, relative to the total volume of the first layer 20a and the second layer 20b.
[0039] In the present invention, the porosity can be measured by BET (Brunauer-Emmett-Teller) measurement method or mercury porosimetry (Hg porosimetry).
[0040] The above-mentioned first and second electricity storage device negative electrode slurries will be described in detail below.
[0041] 1.2.1. Slurry for negative electrode of first electricity storage device The first electricity storage device negative electrode slurry contains a polymer (A) and a first negative electrode active material.
[0042] 1.2.1.1. Polymer (A) The polymer (A) functions as a binder for exhibiting the ability to bond the first negative electrode active materials together, the ability to adhere to the negative electrode current collector and the first layer, and the ability to adhere to the second layer and the first layer. The polymer (A) contained in the slurry for the first electricity storage device negative electrode may be in a latex state dispersed in a liquid medium, or may be in a state dissolved in a liquid medium. When the polymer (A) is in the form of a latex dispersed in a liquid medium, the stability of the slurry for the negative electrode of the first electricity storage device is improved, and the applicability of the slurry to the negative electrode current collector 10 is improved, which is preferable.
[0043] The content of the polymer component in the slurry for the negative electrode of the first power storage device is preferably 1 to 8 parts by mass, more preferably 1 to 7 parts by mass, and particularly preferably 1.5 to 6 parts by mass, relative to 100 parts by mass of the first negative electrode active material. When the content of the polymer component is within the above range, the dispersibility of the first negative electrode active material in the slurry is good, and the coating property of the slurry is also excellent. Here, the polymer component includes the polymer (A), a polymer other than the polymer (A) that is added as necessary, and a thickener, etc. Below, the repeating unit constituting the polymer (A), the physical properties of the polymer (A), and the production method will be described in that order.
[0044] <Repeating units constituting polymer (A)> The polymer (A) contains 0.1% by mass or more and less than 5% by mass of repeating units (a1) (hereinafter, simply referred to as "repeating units (a1)") derived from an unsaturated carboxylic acid, when the total of the repeating units contained in the polymer (A) is taken as 100% by mass. The content of the repeating units (a1) is preferably 0.2% by mass or more, more preferably 0.3% by mass or more. The content of the repeating units (a1) is preferably 4% by mass or less, more preferably 3% by mass or less. When the polymer (A) contains the repeating units (a1) within the above range, a first layer that is easily compatible with the electrolyte and in which lithium ions are easily diffused can be formed. In addition, the viscosity of the slurry can be reduced, so that the smoothness (leveling property) of the first layer surface is improved during coating and drying, and the thickness of the negative electrode mixture layer can be made uniform. In addition, since the polymer compositions of the polymer (A) and the polymer (B) are similar, the adhesion between the first layer and the second layer can be improved.
[0045] The unsaturated carboxylic acid is not particularly limited, but may be one or more selected from monocarboxylic acids and dicarboxylic acids (including anhydrides) such as acrylic acid, methacrylic acid, crotonic acid, maleic acid, fumaric acid, itaconic acid, etc. The unsaturated carboxylic acid may be one or more selected from acrylic acid, methacrylic acid, itaconic acid, etc.
[0046] In addition to the repeating unit (a1), the polymer (A) may contain a repeating unit derived from another monomer copolymerizable therewith. Examples of such repeating units include a repeating unit (a2) derived from a conjugated diene compound (hereinafter also simply referred to as "repeating unit (a2)"), a repeating unit (a3) derived from an aromatic vinyl compound (hereinafter also simply referred to as "repeating unit (a3)"), a repeating unit (a4) derived from an unsaturated carboxylic acid ester (hereinafter also simply referred to as "repeating unit (a4)"), a repeating unit (a5) derived from an α,β-unsaturated nitrile compound (hereinafter also simply referred to as "repeating unit (a5)"), a repeating unit (a6) derived from (meth)acrylamide (hereinafter also simply referred to as "repeating unit (a6)"), and a repeating unit (a7) derived from a compound having a sulfonic acid group (hereinafter also simply referred to as "repeating unit (a7)").
[0047] The content of the repeating unit (a2) derived from a conjugated diene compound is preferably 15% by mass or more and 60% by mass or less, when the total of the repeating units contained in the polymer (A) is taken as 100% by mass. The content of the repeating unit (a2) is more preferably 17% by mass or more, and particularly preferably 20% by mass or more. The content of the repeating unit (a2) is more preferably 57% by mass or less, and particularly preferably 55% by mass or less. When the polymer (A) contains the repeating unit (a2) within the above range, the dispersibility of the first negative electrode active material becomes good, and a homogeneous first layer can be prepared, so that the structural defects of the electrode plate are eliminated and good repeated charge / discharge characteristics may be exhibited. In addition, the surface of the first negative electrode active material is coated with the repeating unit (a2). Since the polymer (A) can be given elasticity and the adhesiveness can be improved by the elasticity of the polymer (A), the polymer (A) may exhibit good charge-discharge durability characteristics.
[0048] The repeating unit (a2) derived from a conjugated diene compound is preferably not hydrogenated by an oil phase hydrogenation method or an aqueous phase hydrogenation method. When the polymer (A) contains the repeating unit (a2) derived from a non-hydrogenated conjugated diene compound, the polymer (A) can be imparted with elasticity, and the elasticity of the polymer (A) can further improve the adhesion in some cases.
[0049] The conjugated diene compound is not particularly limited, but examples thereof include 1,3-butadiene, 2-methyl-1,3-butadiene, 2,3-dimethyl-1,3-butadiene, 2-chloro-1,3-butadiene, etc., and one or more selected from these can be used. Among these, 1,3-butadiene is particularly preferred.
[0050] The content of the repeating unit (a3) derived from an aromatic vinyl compound is preferably 20% by mass or more and less than 40% by mass, when the total of the repeating units contained in the polymer (A) is taken as 100% by mass. The content of the repeating unit (a3) is more preferably 21% by mass or more, and particularly preferably 22% by mass or more. The content of the repeating unit (a3) is more preferably 35% by mass or less, and particularly preferably 30% by mass or less. When the polymer (A) contains the repeating unit (a3) within the above range, the polymer (A) dispersed in the electrode is prevented from fusing with each other, and the permeability of the electrolyte is improved, so that the repeated charge / discharge characteristics may be improved. Furthermore, the polymer (A) may exhibit good adhesion to graphite or the like that may be used as the first negative electrode active material.
[0051] The aromatic vinyl compound is not particularly limited, but examples thereof include styrene, α-methylstyrene, p-methylstyrene, vinyltoluene, chlorostyrene, divinylbenzene, and the like, and one or more selected from these can be used.
[0052] When the total of the repeating units contained in the polymer (A) is taken as 100% by mass, the total amount of the repeating units (a1), (a2) and (a3) is preferably 50% by mass or more, more preferably 55% by mass or more. When the total amount of the repeating units (a1), (a2) and (a3) is within the above range, the dispersibility of the first negative electrode active material is good, and fusion between the polymers (A) dispersed in the electrode can be suppressed, improving adhesion and electrolyte permeability, and thus the electrode may exhibit good repeated charge / discharge characteristics and good charge / discharge durability characteristics.
[0053] The content of the repeating unit (a4) derived from the unsaturated carboxylate ester is preferably 1% by mass or more and 20% by mass or less, when the total of the repeating units contained in the polymer (A) is taken as 100% by mass. The content of the repeating unit (a4) is more preferably 2% by mass or more, and particularly preferably 3% by mass or more. The content of the repeating unit (a4) is more preferably 18% by mass or less, and particularly preferably 15% by mass or less. When the polymer (A) contains the repeating unit (a4) within the above range, the affinity between the polymer (A) and the electrolyte is improved, and an increase in internal resistance due to the binder becoming an electric resistance component in the electricity storage device is suppressed, and a decrease in adhesion due to excessive absorption of the electrolyte may be prevented.
[0054] Among the unsaturated carboxylic acid esters, (meth)acrylic acid esters can be preferably used. Specific examples of (meth)acrylic acid esters include, for example, methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, and isobutyl (meth)acrylate. , n-amyl (meth)acrylate, isoamyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, ethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate Examples of the acrylates include methacrylate, allyl (meth)acrylate, 2-hydroxymethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 5-hydroxypentyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, glycerin mono(meth)acrylate, and glycerin di(meth)acrylate, and one or more selected from these can be used. Among these, one or more selected from methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, cyclohexyl (meth)acrylate, ethylene glycol di(meth)acrylate, and 2-hydroxyethyl (meth)acrylate are preferred, and methyl (meth)acrylate is particularly preferred.
[0055] The content of the repeating unit (a5) derived from an α,β-unsaturated nitrile compound is preferably 5% by mass or more and 40% by mass or less, when the total of the repeating units contained in the polymer (A) is taken as 100% by mass. The content of the repeating unit (a5) is more preferably 7% by mass or more, and particularly preferably 10% by mass or more. The content of the repeating unit (a5) is more preferably 35% by mass or less, and particularly preferably 30% by mass or less. By containing the repeating unit (a5) in the polymer (A) within the above range, it is possible to reduce the dissolution of the polymer (A) in the electrolyte solution, and the decrease in adhesion due to the electrolyte solution may be suppressed. In addition, the increase in internal resistance due to the polymer component dissolved in the electricity storage device becoming an electric resistance component may be suppressed.
[0056] The α,β-unsaturated nitrile compound is not particularly limited, and examples thereof include acrylonitrile, methacrylonitrile, α-chloroacrylonitrile, α-ethylacrylonitrile, vinylidene cyanide, etc., and one or more selected from these can be used. Among these, one or more selected from the group consisting of acrylonitrile and methacrylonitrile are preferred, and acrylonitrile is particularly preferred.
[0057] The content of the repeating unit (a6) derived from (meth)acrylamide is preferably 0 to 10% by mass when the total of the repeating units contained in the polymer (A) is taken as 100% by mass. The content of the repeating unit (a6) is more preferably 1% by mass or more, particularly preferably 2% by mass or more. The content of the repeating unit (a6) is preferably 8% by mass or less, more preferably 5% by mass or less. When the polymer (A) contains the repeating unit (a6) within the above range, the dispersibility of the first negative electrode active material in the slurry may be improved. In addition, the flexibility of the obtained first layer may become appropriate, and the adhesion between the negative electrode current collector and the first layer may be improved. Furthermore, the bonding ability between the first negative electrode active materials containing a carbon material such as graphite or a silicon material may be increased, so that a first layer having better flexibility and adhesion to the negative electrode current collector may be obtained.
[0058] Examples of (meth)acrylamides include, but are not limited to, acrylamide, methacrylamide, N-isopropylacrylamide, N,N-dimethylacrylamide, N,N-dimethylmethacrylamide, N,N-diethylacrylamide, N,N-diethylmethacrylamide, N,N-dimethylaminopropylacrylamide, N,N-dimethylaminopropylmethacrylamide, N-methylol acrylamide, N-methylol methacrylamide, diacetone acrylamide, maleic acid amide, and tert-butyl acrylamide. One or more selected from these may be used.
[0059] The content of the repeating unit (a7) derived from a compound having a sulfonic acid group is preferably 0 to 10 mass% when the total of the repeating units contained in the polymer (A) is taken as 100 mass%. The content of the repeating unit (a7) is more preferably 0.5 mass% or more, and particularly preferably 1 mass% or more. The content of the repeating unit (a7) is more preferably 8 mass% or less, and particularly preferably 5 mass% or less.
[0060] The compound having a sulfonic acid group is not particularly limited, but includes compounds such as vinyl sulfonic acid, styrene sulfonic acid, allyl sulfonic acid, sulfoethyl (meth)acrylate, sulfopropyl (meth)acrylate, sulfobutyl (meth)acrylate, 2-acrylamido-2-methylpropanesulfonic acid, 2-hydroxy-3-acrylamidopropanesulfonic acid, 3-allyloxy-2-hydroxypropanesulfonic acid, and alkali salts thereof, and one or more selected from these can be used.
[0061] <Physical properties of polymer (A)> (number average particle size) When the polymer (A) is in the form of latex (particles) dispersed in a liquid medium, the number average particle size of the particles is preferably 50 nm or more and less than 150 nm, more preferably 50 nm or more and 145 nm or less, and particularly preferably 50 nm or more and 140 nm or less. When the number average particle size of the particles of the polymer (A) is within the above range, the stress generated during the expansion and contraction of the first layer can be alleviated. As a result, the adhesion of the negative electrode mixture layer is improved, and good charge and discharge durability characteristics may be exhibited.
[0062] The number average particle size of the polymer (A) particles is the average particle size obtained from images of 50 particles observed with a transmission electron microscope (TEM). An example of a transmission electron microscope is the "H-7650" manufactured by Hitachi High-Tech Corporation.
[0063] <Method for producing polymer (A)> The method for producing the polymer (A) is not particularly limited, but for example, it can be an emulsion polymerization method carried out in the presence of a known emulsifier (surfactant), chain transfer agent, polymerization initiator, etc. As the emulsifier (surfactant), chain transfer agent, and polymerization initiator, compounds described in Japanese Patent No. 5999399 and the like can be used.
[0064] 1.2.1.2. First negative electrode active material The first negative electrode active material may be a compound capable of reversibly inserting and extracting lithium. Specific examples include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium, such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloys, Sn alloys, and Al alloys; and SiOx(0 <x<2)、SnO 2 Examples of the metallic compounds include metal oxides that can be doped and dedoped with lithium, such as vanadium oxide and lithium vanadium oxide; and composites containing the metallic compounds and carbonaceous materials, such as Si-C composites or Sn-C composites. Any one or a mixture of two or more of these can be used.
[0065] Among the above-listed first negative electrode active materials, those containing a metallic compound and / or a carbonaceous material are preferred, and a mixture of a silicon material and a carbonaceous material is more preferred. Silicon materials have a larger lithium absorption capacity per unit weight than other active materials, and therefore can increase the storage capacity of the resulting power storage device, thereby increasing the output and energy density of the power storage device. On the other hand, carbonaceous materials are less susceptible to the effects of the charge and discharge that accompany them. Since the volume change is smaller than that of a silicon material, by using a mixture of a silicon material and a carbonaceous material as the negative electrode active material, the effect of the volume change of the silicon material can be mitigated, and the adhesion between the negative electrode current collector and the negative electrode composite layer can be further improved.
[0066] When silicon (Si) is used as the negative electrode active material, while it has a high capacity, it can undergo a large volume change when absorbing lithium. This causes silicon materials to pulverize due to repeated expansion and contraction, which can cause peeling from the current collector and separation of the negative electrode active materials from each other, and can easily disrupt the conductive network inside the negative electrode mixture layer. This property causes the charge / discharge durability of the energy storage device to deteriorate extremely in a short period of time.
[0067] According to the negative electrode for an electricity storage device according to this embodiment, even when a silicon material is used, the above-mentioned problems do not occur, and good electrical properties can be exhibited. The reason for this is believed to be that the polymer (A) can firmly bind the silicon material, and at the same time, even if the silicon material expands in volume by absorbing lithium, the polymer (A) can expand and contract to maintain the state in which the silicon material is firmly bound.
[0068] The content of the silicon material in 100% by mass of the first negative electrode active material is preferably 1% by mass or more, more preferably 2 to 50% by mass, even more preferably 3 to 45% by mass, and particularly preferably 10 to 40% by mass. When the content of the silicon material in 100% by mass of the first negative electrode active material is within the above range, an electricity storage device having an excellent balance between improved output and energy density of the electricity storage device and charge / discharge durability characteristics can be obtained.
[0069] The first negative electrode active material is preferably in the form of particles The average particle size of the first negative electrode active material is preferably 0.1 to 100 μm, and more preferably 1 to 20 μm.
[0070] Other ingredients In addition to the above-mentioned components, other components may be added to the slurry for the first electricity storage device negative electrode as necessary, such as a polymer other than the polymer (A), a thickener, a liquid medium, a conductive assistant, a pH adjuster, a corrosion inhibitor, cellulose fiber, etc.
[0071] <Polymers other than polymer (A)> The slurry for the negative electrode of the first power storage device may contain a polymer other than the polymer (A). Such a polymer is not particularly limited, but may be an acrylic polymer containing an unsaturated carboxylic acid ester or a derivative thereof as a structural unit, or a fluorine-based polymer such as PVDF (polyvinylidene fluoride). These polymers may be used alone or in combination of two or more. By containing these polymers, flexibility and adhesion may be further improved.
[0072] <Thickener> The slurry for the first electricity storage device negative electrode may contain a thickener. By containing a thickener, the coatability of the slurry and the charge / discharge characteristics of the resulting electricity storage device can be further improved in some cases.
[0073] Specific examples of the thickener include cellulose compounds such as carboxymethyl cellulose, methyl cellulose, and hydroxypropyl cellulose; poly(meth)acrylic acid; ammonium salts or alkali metal salts of the cellulose compounds or the poly(meth)acrylic acid; polyvinyl alcohol (co)polymers such as polyvinyl alcohol, modified polyvinyl alcohol, and ethylene-vinyl alcohol copolymers; (meth)acrylic acid, maleic acid, and fumaric acid. Examples of the water-soluble polymer include a saponified copolymer of an unsaturated carboxylic acid such as acrylic acid and a vinyl ester. Among these, alkali metal salts of carboxymethylcellulose and alkali metal salts of poly(meth)acrylic acid are preferred.
[0074] Commercially available products of these thickeners include, for example, alkali metal salts of carboxymethylcellulose such as CMC1120, CMC1150, CMC2200, CMC2280, and CMC2450 (all manufactured by Daicel Corporation).
[0075] When the slurry for the negative electrode of the first electricity storage device contains a thickener, the content of the thickener is preferably 5 parts by mass or less, and more preferably 0.1 to 3 parts by mass, per 100 parts by mass of the total solid content of the slurry for the negative electrode of the first electricity storage device.
[0076] <Liquid medium> The slurry for the negative electrode of the first power storage device contains a liquid medium. The liquid medium is preferably an aqueous medium containing water, and more preferably water. The aqueous medium can contain a non-aqueous medium other than water. Examples of the non-aqueous medium include amide compounds, hydrocarbons, alcohols, ketones, esters, amine compounds, lactones, sulfoxides, and sulfone compounds, and one or more selected from these can be used. By using an aqueous medium as the liquid medium, the slurry for the negative electrode of the first power storage device has a lower adverse effect on the environment and is safer for workers who handle it.
[0077] The content ratio of the non-aqueous medium contained in the aqueous medium is preferably 10% by mass or less, more preferably 5% by mass or less, and particularly preferably substantially not contained, in 100% by mass of the aqueous medium. Here, "substantially not contained" means to the extent that the non-aqueous medium is not intentionally added as the liquid medium, and it may include the non-aqueous medium unavoidably mixed in when preparing the slurry for the negative electrode of the first power storage device.
[0078] The content ratio of the liquid medium in the slurry for the negative electrode of the first power storage device is preferably such that the solid content concentration in the slurry (which refers to the ratio of the total mass of components other than the liquid medium in the slurry to the total mass of the slurry. The same applies hereinafter) is 30 to 70% by mass, and more preferably 40 to 60% by mass.
[0079] <Conductive aid> The slurry for the negative electrode of the first power storage device may further contain a conductive aid for the purpose of imparting conductivity and buffering the volume change of the first negative electrode active material due to the ingress and egress of lithium ions.
[0080] Specific examples of the conductive aid include carbons such as activated carbon, acetylene black, ketjen black, furnace black, graphite, carbon fiber, fullerene, and carbon nanotube. Among these, acetylene black, ketjen black, or carbon nanotube can be preferably used. The content ratio of the conductive aid is preferably 20 parts by mass or less, more preferably 1 to 15 parts by mass, and particularly preferably 2 to 10 parts by mass with respect to 100 parts by mass of the first negative electrode active material.
[0081] <pH adjuster> The slurry for the negative electrode of the first power storage device may further contain a pH adjuster for the purpose of suppressing the corrosion of the negative electrode current collector according to the type of the first negative electrode active material.
[0082] Examples of the pH adjuster include hydrochloric acid, phosphoric acid, sulfuric acid, acetic acid, formic acid, ammonium phosphate, Examples include ammonium sulfate, ammonium acetate, ammonium formate, ammonium chloride, sodium hydroxide, potassium hydroxide, etc. Among these, sulfuric acid, ammonium sulfate, sodium hydroxide, and potassium hydroxide are preferred.
[0083] <Corrosion inhibitor> The slurry for the negative electrode of the first electricity storage device may further contain a corrosion inhibitor for the purpose of suppressing corrosion of the negative electrode current collector depending on the type of the first negative electrode active material.
[0084] Examples of the corrosion inhibitor include ammonium metavanadate, sodium metavanadate, potassium metavanadate, ammonium metatungstate, sodium metatungstate, potassium metatungstate, ammonium paratungstate, sodium paratungstate, potassium paratungstate, ammonium molybdate, sodium molybdate, potassium molybdate, and the like. Among these, ammonium paratungstate, ammonium metavanadate, sodium metavanadate, potassium metavanadate, and ammonium molybdate are preferred.
[0085] <Cellulose fiber> The slurry for the negative electrode of the first power storage device may further contain cellulose fibers. Known cellulose fibers can be used. By containing the cellulose fibers, the adhesion of the first negative electrode active material to the negative electrode current collector may be improved. It is considered that the fibrous cellulose fibers bond adjacent first negative electrode active materials to each other in a fibrous form by linear adhesion or linear contact, thereby preventing the first negative electrode active material from falling off and improving the adhesion to the negative electrode current collector.
[0086] 1.2.1.4. Method for preparing slurry for negative electrode of first electricity storage device The slurry for the negative electrode of the first power storage device may be produced by any method as long as it contains the polymer (A) and the first negative electrode active material. From the viewpoint of producing a slurry having better dispersibility and stability more efficiently and inexpensively, it is preferable to produce the slurry by adding the first negative electrode active material and optional additive components used as necessary to the dispersion of the polymer (A) produced by the above <Production method of the polymer (A)> and mixing them. Specific examples of the production method include the method described in Japanese Patent No. 5999399.
[0087] 1.2.2. Slurry for negative electrode of second electricity storage device The slurry for the second electricity storage device negative electrode contains a polymer (B) and a second negative electrode active material.
[0088] 1.2.2.1. Polymer (B) The polymer (B) functions as a binder for expressing the ability to bond the second negative electrode active materials together and the ability to adhere to the first layer and the second layer. The polymer (B) contained in the slurry for the second electric storage device negative electrode may be in a latex form dispersed in a liquid medium, or may be dissolved in a liquid medium, but is preferably in a latex form dispersed in a liquid medium. When the polymer (B) is in a latex form dispersed in a liquid medium, the stability of the slurry for the second electric storage device negative electrode becomes good, and the coating property of the slurry to the first layer becomes good, which is preferable.
[0089] The content of the polymer component in the slurry for the negative electrode of the second power storage device is preferably 1 to 8 parts by mass, more preferably 1 to 7 parts by mass, and particularly preferably 1.5 to 6 parts by mass, relative to 100 parts by mass of the second negative electrode active material. When the content of the polymer component is within the above range, the dispersibility of the second negative electrode active material in the slurry is good, and the coating properties of the slurry are also excellent. Here, the polymer component includes polymer (B) and polymer (B) other than the polymer (B) that is added as necessary. The polymer (B) includes a polymer and a thickener, etc. The repeating units constituting the polymer (B), the physical properties of the polymer (B), and the production method thereof will be described below in that order.
[0090] <Repeating units constituting polymer (B)> The polymer (B) contains 5% by mass or more and 20% by mass or less of repeating units (a1) derived from an unsaturated carboxylic acid, when the total of the repeating units contained in the polymer (B) is taken as 100% by mass. The content of the repeating units (a1) is preferably 6% by mass or more, more preferably 7% by mass or more. The content of the repeating units (a1) is preferably 19% by mass or less, more preferably 18% by mass or less. By containing the repeating units (a1) within the above range, the polymer (A) has excellent mechanical properties in the electrolyte, and can relieve stress generated during expansion and contraction, thereby suppressing deterioration of the electrode structure, such as changes in electrode thickness. As the unsaturated carboxylic acid, one or more compounds selected from those listed in the description of the polymer (A) can be used.
[0091] In addition to the repeating unit (a1), the polymer (B) may contain a repeating unit derived from another monomer copolymerizable therewith. Examples of such repeating units include a repeating unit (a2) derived from a conjugated diene compound, a repeating unit (a3) derived from an aromatic vinyl compound, a repeating unit (a4) derived from an unsaturated carboxylic acid ester, a repeating unit (a5) derived from an α,β-unsaturated nitrile compound, a repeating unit (a6) derived from (meth)acrylamide, and a repeating unit (a7) derived from a compound having a sulfonic acid group.
[0092] The content of the repeating unit (a2) derived from the conjugated diene compound is preferably 15% by mass or more and 60% by mass or less, when the total of the repeating units contained in the polymer (B) is taken as 100% by mass. The content of the repeating unit (a2) is more preferably 17% by mass or more, and particularly preferably 20% by mass or more. The content of the repeating unit (a2) is more preferably 57% by mass or less, and particularly preferably 55% by mass or less. When the polymer (B) contains the repeating unit (a2) within the above range, the dispersibility of the second negative electrode active material is improved, and a homogeneous negative electrode mixture layer can be prepared, so that the structural defects of the electrode plate are eliminated and good repeated charge / discharge characteristics may be exhibited. In addition, the polymer (B) covering the surface of the second negative electrode active material can be given elasticity, and the polymer (B) can be stretched to improve adhesion, so that good charge / discharge durability characteristics may be exhibited. As the conjugated diene compound, one or more compounds selected from those listed in the description of the polymer (A) can be used.
[0093] The repeating unit (a2) derived from a conjugated diene compound is preferably not hydrogenated by an oil phase hydrogenation method or an aqueous phase hydrogenation method. When the polymer (B) contains the repeating unit (a2) derived from a non-hydrogenated conjugated diene compound, the polymer (B) can be imparted with elasticity, and the elasticity of the polymer (B) can further improve the adhesion in some cases.
[0094] The content of the repeating unit (a3) derived from an aromatic vinyl compound is preferably 1% by mass or more and less than 20% by mass, when the total of the repeating units contained in the polymer (B) is taken as 100% by mass. The content of the repeating unit (a3) is more preferably 2% by mass or more, and particularly preferably 3% by mass or more. The content of the repeating unit (a3) is more preferably 19% by mass or less, and particularly preferably 18% by mass or less. When the polymer (B) contains the repeating unit (a3) within the above range, the polymer (B) dispersed in the electrode is prevented from fusing with each other, and the permeability of the electrolyte is improved, so that the repeated charge / discharge characteristics may be improved. Furthermore, the polymer may exhibit good adhesion to graphite or the like used as the second negative electrode active material. As the aromatic vinyl compound, the following may be mentioned in the description of the polymer (A). One or more compounds selected from the compounds listed may be used.
[0095] When the total of the repeating units contained in the polymer (A) is taken as 100% by mass, the total amount of the repeating units (a1), (a2) and (a3) is preferably 50% by mass or more, more preferably 60% by mass or more, and particularly preferably 70% by mass or more. When the total amount of the repeating units (a1), (a2) and (a3) is within the above range, the dispersibility of the second negative electrode active material is good, and the fusion of the polymers (B) dispersed in the electrode can be suppressed, and the adhesion and the permeability of the electrolyte are improved, so that good repeated charge / discharge characteristics and good charge / discharge durability characteristics may be exhibited.
[0096] The content of the repeating unit (a4) derived from the unsaturated carboxylate ester is preferably 1% by mass or more and 20% by mass or less, when the total of the repeating units contained in the polymer (B) is taken as 100% by mass. The content of the repeating unit (a4) is more preferably 2% by mass or more, and particularly preferably 3% by mass or more. The content of the repeating unit (a4) is more preferably 18% by mass or less, and particularly preferably 15% by mass or less. When the polymer (B) contains the repeating unit (a4) within the above range, the affinity between the polymer (B) and the electrolyte is improved, and the increase in internal resistance due to the binder becoming an electric resistance component in the electricity storage device is suppressed, and the decrease in adhesion due to excessive absorption of the electrolyte may be prevented. As the unsaturated carboxylate, one or more compounds selected from those listed in the description of the polymer (A) can be used.
[0097] The content of the repeating unit (a5) derived from an α,β-unsaturated nitrile compound is preferably 5% by mass or more and 40% by mass or less, when the total of the repeating units contained in the polymer (B) is taken as 100% by mass. The content of the repeating unit (a5) is more preferably 7% by mass or more, and particularly preferably 10% by mass or more. The content of the repeating unit (a5) is more preferably 35% by mass or less, and particularly preferably 30% by mass or less. By containing the repeating unit (a5) in the polymer (B) within the above range, it is possible to reduce the dissolution of the polymer (B) in the electrolyte solution, and the decrease in adhesion due to the electrolyte solution may be suppressed. In addition, the increase in internal resistance due to the polymer component dissolved in the electricity storage device becoming an electric resistance component may be suppressed. As the α,β-unsaturated nitrile compound, one or more compounds selected from the compounds listed in the description of the polymer (A) can be used.
[0098] The content of the repeating unit (a6) derived from (meth)acrylamide is preferably 0 to 10% by mass, when the total of the repeating units contained in the polymer (B) is taken as 100% by mass. The content of the repeating unit (a6) is more preferably 1% by mass or more, and particularly preferably 2% by mass or more. The content of the repeating unit (a6) is preferably 8% by mass or less, and more preferably 5% by mass or less. When the polymer (B) contains the repeating unit (a6) within the above range, the dispersibility of the second negative electrode active material in the slurry may be improved. In addition, the flexibility of the obtained second layer may become appropriate, and the adhesion between the first layer and the second layer may be improved. Furthermore, since the bonding ability between the second negative electrode active materials containing a carbon material such as graphite or a silicon material can be increased, the second layer may have better flexibility and adhesion to the first layer. As the (meth)acrylamide, one or more compounds selected from the compounds listed in the description of the polymer (A) may be used.
[0099] The content of the repeating unit (a7) derived from a compound having a sulfonic acid group is preferably 0 to 10% by mass when the total of the repeating units contained in the polymer (B) is taken as 100% by mass. The content of the repeating unit (a7) is more preferably 0.5% by mass or more, and particularly preferably 1% by mass or more. It is more preferably 8 mass % or less, and particularly preferably 5 mass % or less. As the compound having a sulfonic acid group, one or more compounds selected from the compounds listed in the description of the polymer (A) can be used.
[0100] <Physical properties of polymer (B)> (number average particle size) When the polymer (B) is in the form of latex (particles) dispersed in a liquid medium, the number average particle diameter of the particles is preferably 150 nm or more and 300 nm or less, more preferably 150 nm or more and 290 nm or less, and particularly preferably 150 nm or more and 280 nm or less. When the number average particle diameter of the particles of the polymer (B) is within the above range, the stress generated during expansion and contraction can be effectively alleviated, and deterioration of the electrode structure such as a change in electrode thickness can be suppressed in some cases. In addition, the contact area with the liquid medium can be reduced, and the particles of the polymer (B) are easily adsorbed on the surface of the second negative electrode active material, so that the particles of the polymer (B) can move in accordance with the movement of the second negative electrode active material. As a result, migration can be suppressed, and deterioration of electrical characteristics can be reduced in some cases. The number average particle diameter of the particles of the polymer (B) can be measured by the same method as that for measuring the number average particle diameter of the particles of the polymer (A).
[0101] <Method for producing polymer (B)> The method for producing the polymer (B) is not particularly limited, but for example, it can be an emulsion polymerization method carried out in the presence of a known emulsifier (surfactant), chain transfer agent, polymerization initiator, etc. As the emulsifier (surfactant), chain transfer agent, and polymerization initiator, compounds described in Japanese Patent No. 5999399 and the like can be used.
[0102] 1.2.2.2.Second negative electrode active material The second negative electrode active material may be one or more selected from the compounds listed in the description of the first negative electrode active material. The second negative electrode active material may be the same as or different from the first negative electrode active material, but is preferably the same as the first negative electrode active material.
[0103] Other ingredients In addition to the above-mentioned components, other components may be added to the slurry for the negative electrode of the second electricity storage device as necessary. Examples of such components include polymers other than the polymer (B), thickeners, liquid media, conductive assistants, pH adjusters, corrosion inhibitors, cellulose fibers, etc. As for these components, one or more selected from the compounds listed in the description of the slurry for the negative electrode of the first electricity storage device can be used, and the amounts used can be the same.
[0104] 2. Energy storage devices The electric storage device according to one embodiment of the present invention includes the above-mentioned negative electrode for the electric storage device. The electric storage device according to this embodiment further includes a positive electrode for the electric storage device and a separator in addition to the negative electrode for the electric storage device, contains an electrolyte solution, and can be manufactured according to a conventional method. A specific method for manufacturing the electric storage device according to this embodiment includes, for example, stacking the negative electrode for the electric storage device and the positive electrode for the electric storage device via a separator, rolling or folding the stack according to the battery shape, and storing the stack in a battery container, and injecting an electrolyte solution into the battery container and sealing the container. The shape of the battery can be any appropriate shape, such as a coin type, a cylindrical type, a square type, or a laminate type.
[0105] The above-mentioned electric storage device can be applied to lithium ion secondary batteries, electric double layer capacitors, lithium ion capacitors, etc., which require discharging at a high current density. Among these, lithium ion secondary batteries are particularly preferred. In the electric storage device according to this embodiment, As the members other than the negative electrode for a lithium ion secondary battery, a known member for an electric double layer capacitor, or a lithium ion capacitor can be used.
[0106] 3. Working Example The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the examples and comparative examples, "parts" and "%" are by mass unless otherwise specified.
[0107] 3.1 Example 1 3.1.1. Polymer synthesis and property evaluation (1) Synthesis of polymer (A1) A particle dispersion of polymer (A1) was obtained by one-stage polymerization as shown below. A monomer mixture consisting of 400 parts by mass of water, 50 parts by mass of 1,3-butadiene, 24.9 parts by mass of styrene, 0.1 parts by mass of acrylic acid, 10 parts by mass of methyl methacrylate, and 15 parts by mass of acrylonitrile, 0.1 parts by mass of tert-dodecyl mercaptan as a chain transfer agent, 2 parts by mass of sodium alkyl diphenyl ether disulfonate as an emulsifier, and 0.2 parts by mass of potassium persulfate as a polymerization initiator was charged into a reactor, and polymerization was carried out at 70°C for 24 hours while stirring, and the reaction was terminated at a polymerization conversion rate of 98%. Unreacted monomers were removed from the particle dispersion of polymer (A1) thus obtained, and after concentration, a 10% aqueous sodium hydroxide solution and water were added to obtain a particle dispersion of polymer (A1) with a solid content concentration of 20% by mass and a pH of 8.0.
[0108] (2) Synthesis of polymer (B1) A particle dispersion of polymer (B1) was obtained by one-stage polymerization as shown below. A monomer mixture consisting of 400 parts by mass of water, 5 parts by mass of acrylic acid, 50 parts by mass of 1,3-butadiene, 15 parts by mass of styrene, 5 parts by mass of methyl methacrylate, and 25 parts by mass of acrylonitrile, 0.1 parts by mass of tert-dodecyl mercaptan as a chain transfer agent, 2 parts by mass of sodium alkyl diphenyl ether disulfonate as an emulsifier, and 0.2 parts by mass of potassium persulfate as a polymerization initiator was charged into a reactor, and polymerization was carried out at 70°C for 24 hours while stirring, and the reaction was terminated at a polymerization conversion rate of 98%. Unreacted monomers were removed from the particle dispersion of polymer (B1) thus obtained, and after concentration, a 10% aqueous sodium hydroxide solution and water were added to obtain a particle dispersion of polymer (B1) with a solid content concentration of 20% by mass and a pH of 8.0.
[0109] (3) Measurement of number average particle size A drop of latex obtained by diluting the polymer particle dispersion liquid obtained above to 0.1 wt% was dropped onto a collodion support film with a pipette, and a drop of 1 wt% phosphotungstic acid solution was further dropped onto the collodion support film with a pipette, and the sample was air-dried for 12 hours to prepare a sample. The sample thus prepared was observed at a magnification of 10K (magnification) using a transmission electron microscope (TEM, Hitachi High-Tech Corporation, model number "H-7650"), and image analysis was performed using the HITACHI EMIP program to calculate the average particle size of 50 randomly selected polymer particles, and the average value was taken as the number average particle size. The results are shown in Table 1 below.
[0110] 3.1.2. Preparation of slurry for negative electrodes of energy storage devices (1) Synthesis of silicon material (negative electrode active material) A mixture of crushed silicon dioxide powder (average particle size 10 μm) and carbon powder (average particle size 35 μm) was heat-treated for 10 hours under nitrogen gas flow (0.5 NL / min) in an electric furnace adjusted to a temperature range of 1100°C to 1600°C, to obtain silicon oxide powder (average particle size 8 μm) represented by the composition formula SiOx (x = 0.5 to 1.1). 300 g of this silicon oxide powder was charged into a batch-type heating furnace, and while maintaining a reduced pressure of 100 Pa absolute pressure using a vacuum pump, the temperature was increased from room temperature (25°C) to 1100°C at a heating rate of 300°C / h. Next, while maintaining the pressure in the heating furnace at 2000 Pa, methane gas was introduced at a flow rate of 0.5 NL / min. While the powder was being introduced, a heat treatment (graphite coating treatment) was carried out at 1100°C for 5 hours. After the graphite coating treatment was completed, the powder was cooled to room temperature at a temperature drop rate of 50°C / h to obtain about 330 g of graphite-coated silicon oxide powder. This graphite-coated silicon oxide was a conductive powder (negative electrode active material) in which the surface of silicon oxide was coated with graphite, and had an average particle size of 10.5 µm. The proportion of the graphite coating was 2 mass% when the entirety of the obtained graphite-coated silicon oxide was taken as 100 mass%.
[0111] (2) Preparation of slurry for the negative electrode of the first power storage device A two-shaft planetary mixer (manufactured by Primix Corporation, product name "TK Hivismix 2P-03") was charged with 1 part by mass (solid content equivalent, added as an aqueous solution with a concentration of 2% by mass) of a thickener (product name "CMC2200", manufactured by Daicel Corporation), 2 parts by mass of a polymer (A1) (solid content equivalent, added as a particle dispersion of the polymer (A1) obtained above), 80 parts by mass (solid content equivalent) of artificial graphite (manufactured by Resonac Corporation, product name "MAG") which is a highly crystalline graphite as a negative electrode active material, 20 parts by mass (solid content equivalent) of the graphite-coated silicon oxide powder obtained above, and 1 part by mass of carbon (manufactured by Denka Company, Ltd., acetylene black) as a conductive assistant, and the mixture was stirred at 60 rpm for 1 hour to obtain a paste. Water was added to the obtained paste to adjust the solid concentration to 48% by mass, and then the mixture was stirred at 200 rpm for 2 minutes, at 1800 rpm for 5 minutes, and then further stirred under reduced pressure (approximately 2.5 × 10 4 The mixture was stirred and mixed at 1,800 rpm for 1.5 minutes at 1000 Pa to prepare a first electricity storage device negative electrode slurry (C / Si=80 / 20) containing 19.6 mass % Si in the negative electrode active material.
[0112] (3) Preparation of slurry for the negative electrode of the second power storage device A slurry for the negative electrode of a second electricity storage device was prepared in the same manner as for the slurry for the negative electrode of the first electricity storage device, except that the polymer (A1) was changed to the polymer (B1).
[0113] 3.1.3. Manufacturing of negative electrodes for energy storage devices The slurry for the negative electrode of the first electricity storage device obtained above was uniformly applied by a doctor blade method onto the surface of a negative electrode current collector made of copper foil with a thickness of 20 μm so that the film thickness after drying would be 50 μm, and the coating was dried at 60° C. for 10 minutes and then at 120° C. for 10 minutes. After that, the layer density was 1.5 g / cm 3 The mixture was pressed with a roll press machine so as to obtain a first layer.
[0114] The slurry for the negative electrode of the second electricity storage device obtained above was uniformly applied onto the first layer obtained above by a doctor blade method so that the film thickness after drying would be 50 μm, and the coating was dried at 60° C. for 10 minutes and then at 120° C. for 10 minutes. After that, the density of the layer was 1.5 g / cm 3 By pressing the mixture with a roll press machine so as to obtain a negative electrode for an electricity storage device having a negative electrode mixture layer consisting of a first layer and a second layer.
[0115] 3.1.4. Manufacturing and evaluation of energy storage devices (1) Manufacturing the counter electrode (positive electrode) A two-shaft planetary mixer (manufactured by Primix Corporation, product name "TK Hivismix 2P-03") was mixed with 4 parts by mass (solid content equivalent) of an electrochemical device electrode binder (manufactured by Kureha Corporation, product name "KF Polymer #1120"), 3 parts by mass of a conductive additive (manufactured by Denka Co., Ltd., product name "Denka Black 50% Pressed Product"), and LiCoO with an average particle diameter of 5 μm as a positive electrode active material. 2 100 parts by mass (solid content equivalent) of 1,2-dichloropropanediol (manufactured by Hayashi Chemical Industries, Ltd.) and 36 parts by mass of N-methylpyrrolidone (NMP) were added and stirred at 60 rpm for 2 hours. NMP was added to the obtained paste to adjust the solid content concentration to 65% by mass, and then agitated at 200 rpm for 2 minutes, at 1800 rpm for 5 minutes, and further under reduced pressure (approximately 2.5×10 4 The mixture was stirred and mixed at 1,800 rpm for 1.5 minutes at 1000 Pa to prepare a slurry for the positive electrode of an electricity storage device. The slurry for the positive electrode of an electricity storage device was uniformly applied to the surface of a positive electrode current collector made of aluminum foil by a doctor blade method so that the thickness of the film after the solvent removal would be 80 μm, and the solvent was removed by heating at 120° C. for 20 minutes. Thereafter, the density of the positive electrode active material layer was 3.0 g / cm 3 A counter electrode (positive electrode) was obtained by pressing the mixture using a roll press machine so that the resultant mixture was as follows:
[0116] (2) Assembly of lithium-ion battery cells In a glove box substituted with Ar gas so that the dew point is -80°C or less, the negative electrode for the electricity storage device manufactured above was punched out to a diameter of 16.16 mm and placed on a two-electrode coin cell (manufactured by Hosen Co., Ltd., product name "HS Flat Cell"). Next, a separator made of a polypropylene porous film punched out to a diameter of 24 mm (manufactured by Celgard Co., Ltd., product name "Celgard #2400") was placed on the cell, and 500 μL of electrolyte was poured in so as to prevent air from entering. The counter electrode (positive electrode) manufactured above was punched out to a diameter of 15.95 mm and placed on the cell, and the exterior body of the two-electrode coin cell was sealed with screws to assemble a lithium-ion battery cell (electricity storage device). The electrolyte used here was LiPF 6 This is a solution in which the above is dissolved at a concentration of 1 mol / L.
[0117] (3) Evaluation of electrode expansion The lithium-ion battery cell manufactured above was charged at a constant current (1.0 C) in a thermostatic chamber adjusted to 45° C., and when the voltage reached 4.2 V, charging was continued at a constant voltage (4.2 V). The charging was completed (cut off) when the current value reached 0.05 C. Thereafter, discharging was started at a constant current (1.0 C), and the discharging was completed (cut off) when the voltage reached 3.0 V, and the discharge capacity of the first cycle was calculated. The lithium-ion battery cell after 300 charge / discharge cycles was disassembled, and the negative electrode for the power storage device was washed and dried with dimethyl carbonate, and the inhibition rate of electrode expansion was calculated using the following formula (1) and evaluated according to the following criteria. The evaluation results are shown in Table 1 below. Electrode expansion inhibition rate (%) = (1 - ((negative electrode film thickness at the 300th cycle) - (negative electrode film thickness at the 1st cycle)) ÷ negative electrode film thickness at the 1st cycle) × 100 (1) (Evaluation Criteria) 5 points: Electrode expansion suppression rate is 95% or more. 4 points: Electrode expansion suppression rate is 90% or more but less than 95%. 3 points: Electrode expansion suppression rate is 85% or more but less than 90%. 2 points: Electrode expansion suppression rate is between 80% and 85%. 1 point: Electrode expansion suppression rate is 75% or more but less than 80%. 0 points: Electrode expansion suppression rate is less than 75%.
[0118] (4) Evaluation of resistance increase rate The non-aqueous secondary battery manufactured above was charged at a constant current (1.0C) in a thermostatic chamber adjusted to 25°C, and when the voltage reached 4.2V, charging was continued at a constant voltage (4.2V), and charging was completed (cut-off) when the current value reached 0.05C. Discharge was then started at a constant current (0.05C), and charging was completed (cut-off) when the voltage reached 3.0V, and the discharge capacity at the 0th cycle was calculated. Furthermore, charging was started at a constant current (1.0C), and charging was continued at a constant voltage (4.2V) when the voltage reached 4.2V, and charging was completed (cut-off) when the current value reached 0.01C. Discharge was then started at a constant current (1.0C), and discharging was completed (cut-off) when the voltage reached 3.0V, and the discharge capacity at the 1st cycle was calculated. In this manner, charging and discharging were repeated 300 times. After repeating the charge and discharge 300 times, the charge and discharge were performed in the same manner as in the 0th cycle, and the discharge capacity in the 301st cycle was evaluated. The resistance increase rate was calculated by the following formula (2) and evaluated according to the following criteria. Resistance increase rate (%) = ((discharge capacity at 301st cycle - discharge capacity at 300th cycle)) / (discharge capacity at 0th cycle - discharge capacity at 1st cycle) × 100 (2) (Evaluation standard) 5 points: Resistance increase rate is between 100% and 110%. 4 points: Resistance increase rate is between 110% and 120%. 3 points: Resistance increase rate is between 120% and 130%. 2 points: Resistance increase rate is between 130% and 140%. 1 point: Resistance increase rate is between 140% and 150%. 0 points: Resistance increase is 150% or more.
[0119] In the measurement conditions, "1C" refers to the current value at which a cell with a certain capacity is discharged at a constant current and the discharge is completed in 1 hour. For example, "0.1C" refers to the current value at which the discharge is completed in 10 hours, and "10C" refers to the current value at which the discharge is completed in 0.1 hour.
[0120] (5) Evaluation of cycle characteristics The lithium-ion battery cell manufactured above was charged at a constant current (1.0C) in a thermostatic chamber adjusted to 25°C, and when the voltage reached 4.2V, charging was continued at a constant voltage (4.2V). The charging was completed (cut-off) when the current value reached 0.05C. Thereafter, discharging was started at a constant current (1.0C), and the discharging was completed (cut-off) when the voltage reached 3.0V, and the discharge capacity of the first cycle was calculated. In this manner, charging and discharging were repeated 300 times. The capacity retention rate was calculated using the following formula (3) and evaluated according to the following criteria. The evaluation results are shown in Table 1 below. Capacity retention rate (%) = ((discharge capacity at 300th cycle) / (discharge capacity at 1st cycle)) × 100 (3) (Evaluation Criteria) 5 points: Capacity retention is 95% or more. 4 points: Capacity retention is between 90% and 95%. 3 points: Capacity retention is between 85% and 90%. 2 points: Capacity retention is between 80% and 85%. 1 point: Capacity retention is between 75% and 80%. 0 points: Less than 75% capacity retention.
[0121] 3.2. Examples 2 to 18 and Comparative Examples 1 to 6 Polymer particle dispersions with a solid content concentration of 20 mass % and pH 8.0 were obtained in the same manner as in the above section "3.1.1. Polymer synthesis and property evaluation", except that the type and amount of each monomer was as shown in the following Tables 1 to 3. Otherwise, a slurry for an electricity storage device negative electrode was prepared in the same manner as in Example 1, and an electricity storage device negative electrode and an electricity storage device were fabricated and evaluated in the same manner as in Example 1.
[0122] 3.3.Evaluation Results The following Tables 1 to 3 show the polymer compositions, the measurement results of each physical property, and the evaluation results used in Examples 1 to 18 and Comparative Examples 1 to 6. The values showing the polymer compositions shown in Tables 1 to 3 show parts by mass.
[0123] [Table 1]
[0124] [Table 2]
[0125] [Table 3]
[0126] The monomers in Tables 1 to 3 above respectively represent the following compounds. <Unsaturated carboxylic acid> ·AA: Acrylic acid ·MAA: Methacrylic acid ·TA: Itaconic acid <Conjugated diene compounds> BD: 1,3-butadiene <Aromatic vinyl compounds> ST: Styrene <Unsaturated carboxylic acid ester> MMA: Methyl methacrylate <α,β-unsaturated nitrile compounds> ·AN: Acrylonitrile
[0127] The evaluation results in Tables 1 to 3 show that, according to Examples 1 to 18, the first layer contains a polymer (A) having a relatively low acid content, and the second layer contains a polymer (B) having a relatively high acid content, so that the adhesion between the negative electrode current collector and the negative electrode mixture layer is improved and electrode expansion can be effectively suppressed. It can also be seen that the binding strength between the negative electrode active materials is improved, and therefore the cycle characteristics of the electricity storage device are improved.
[0128] The present invention is not limited to the above-described embodiments, and various modifications are possible. The present invention includes configurations that are substantially the same as those described in the embodiments (for example, configurations with the same functions, methods, and results, or configurations with the same purpose and effect). The present invention also includes configurations in which non-essential parts of the configurations described in the above-described embodiments are replaced with other configurations. Furthermore, the present invention also includes configurations that have the same effects as the configurations described in the above-described embodiments, or that can achieve the same purpose. Furthermore, the present invention also includes configurations in which publicly known technology is added to the configurations described in the above-described embodiments. [Explanation of symbols]
[0129] 10... negative electrode current collector, 20... negative electrode mixture layer, 20a... first layer, 20b... second layer, 100... negative electrode for power storage device
Claims
1. a negative electrode current collector; and a negative electrode mixture layer formed on the negative electrode current collector, the negative electrode mixture layer includes a first layer formed on the negative electrode current collector and a second layer formed on the first layer, The first layer includes a first negative electrode active material and a polymer (A), the polymer (A) contains a repeating unit (a1) derived from an unsaturated carboxylic acid in an amount of 0.1% by mass or more and less than 5% by mass, when the total amount of repeating units contained in the polymer (A) is 100% by mass; The second layer includes a second negative electrode active material and a polymer (B), a negative electrode for an electricity storage device, wherein the polymer (B) contains 5% by mass or more and 20% by mass or less of a repeating unit (a1) derived from an unsaturated carboxylic acid, when the total amount of repeating units contained in the polymer (B) is taken as 100% by mass.
2. the polymer (A) contains 20% by mass or more and less than 40% by mass of a repeating unit (a3) derived from an aromatic vinyl compound, when the total amount of the repeating units contained in the polymer (A) is 100% by mass; 2. The electric storage device negative electrode according to claim 1, wherein the polymer (B) contains 1 mass% or more and less than 20 mass% of a repeating unit (a3) derived from an aromatic vinyl compound, when the total of the repeating units contained in the polymer (B) is 100 mass%.
3. the polymer (A) contains 15% by mass or more and 60% by mass or less of a repeating unit (a2) derived from a conjugated diene compound, when the total amount of the repeating units contained in the polymer (A) is 100% by mass; 3. The electric storage device negative electrode according to claim 1, wherein the polymer (B) contains 15 mass% or more and 60 mass% or less of repeating units (a2) derived from a conjugated diene compound, when the total of the repeating units contained in the polymer (B) is 100 mass%.
4. the polymer (A) contains a repeating unit (a4) derived from an unsaturated carboxylate ester in an amount of 1 mass% or more and 20 mass% or less, when the total amount of repeating units contained in the polymer (A) is 100 mass%, 3. The electric storage device negative electrode according to claim 1 or 2, wherein the polymer (B) contains 1 mass % or more and 20 mass % or less of a repeating unit (a4) derived from an unsaturated carboxylic acid ester, when the total amount of the repeating units contained in the polymer (B) is 100 mass %.
5. the polymer (A) contains 5% by mass or more and 40% by mass or less of a repeating unit (a5) derived from an α,β-unsaturated nitrile compound, when the total amount of the repeating units contained in the polymer (A) is 100% by mass, 3. The electricity storage device negative electrode according to claim 1 or 2, wherein the polymer (B) contains 5 mass% or more and 40 mass% or less of a repeating unit (a5) derived from an α,β-unsaturated nitrile compound, when the total amount of the repeating units contained in the polymer (B) is 100 mass%.
6. The polymer (A) and the polymer (B) are each in the form of particles, The number average particle size of the particles of the polymer (A) is 50 nm or more and less than 150 nm, 3. The negative electrode for an electricity storage device according to claim 1 or 2, wherein the particles of the polymer (B) have a number average particle size of 150 nm or more and 300 nm or less.
7. An electricity storage device comprising the electricity storage device negative electrode according to claim 1 or 2.
Citation Information
Patent Citations
Non-aqueous electrolyte secondary battery
JP2021005461A