Reflection suppression sheet and manufacturing method therefor, as well as reflection suppressing paint and additive
The anti-reflection sheet with polyurethane resin foam particles addresses the need for improved reflection suppression in optical devices by utilizing a base layer and resin layer with porous resin particles, achieving enhanced reflection suppression in the visible light region.
Patent Information
- Application Number
- JP2023079895
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-15
- Publication Date
- 2024-11-27
AI Technical Summary
Existing anti-reflection sheets and paints do not achieve high enough reflection suppression, particularly in optical devices like cameras and head-up displays, necessitating improved materials and methods.
An anti-reflection sheet comprising a base layer and a resin layer with porous resin particles made of polyurethane resin foam containing carbon black, manufactured through a wet film forming method, grinding, and application of an anti-reflection paint containing these particles.
The anti-reflection sheet achieves superior reflection suppression, especially in the visible light region, by utilizing the unique structure of polyurethane resin foam particles with protrusions and internal pores, enhancing image quality in optical devices.
Smart Images

Figure 2024164431000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an anti-reflection sheet and a manufacturing method thereof, as well as an anti-reflection paint and an additive, and more particularly to an anti-reflection sheet composed of a base layer and a resin layer having a binder resin and porous resin particles and a manufacturing method thereof, an anti-reflection paint containing a binder resin and porous resin particles, and an additive containing porous resin particles. [Background technology]
[0002] Today, in optical devices such as cameras and video cameras, stray light caused by diffuse reflection and scattering in the optical path of the lens barrel, etc., affects image quality, etc., so measures to prevent stray light are taken by attaching anti-reflection sheets or applying anti-reflection paint to the optical path of the lens barrel, aperture, etc. Such anti-reflection sheets and anti-reflection paints are also used in, for example, automobile meters and so-called head-up displays (HUDs). As the resin layer constituting the above-mentioned antireflection sheet and the antireflection coating material used in producing the antireflection sheet, those containing a binder resin and resin particles are known (Patent Documents 1 and 2). In Patent Document 1, porous spherical PMMA fine particles are used as the resin particles, and at least some of the PMMA fine particles protrude from the surface of the resin layer to cover almost the entire surface. In Patent Document 2, irregular fibers having multiple protrusions are used as the resin particles, and tips of the multiple protrusions of the irregular fibers protrude from the surface of the resin layer. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 5655387 [Patent Document 2] JP 2020-8843 A Summary of the Invention [Problem to be solved by the invention]
[0004] Thus, although various anti-reflection sheets, anti-reflection paints, and additives used therein are known, there is still a demand for anti-reflection sheets with a high anti-reflection effect. In view of these problems, the present invention provides an anti-reflection sheet having a high anti-reflection effect and a method for producing the same, as well as an anti-reflection paint and additives suitable for the same. [Means for solving the problem]
[0005] That is, the antireflection sheet according to the invention of claim 1 is a reflection-suppressing sheet comprising a base layer and a resin layer having a binder resin and porous resin particles, The porous resin particles are characterized in that they are made of polyurethane resin foam slices containing carbon black. The method for producing an antireflection sheet according to the invention of claim 3 is a method for producing an antireflection sheet including a base layer and a resin layer having a binder resin and porous resin particles, comprising: A step of obtaining a polyurethane resin sheet containing carbon black by a wet film forming method; grinding the polyurethane resin sheet to obtain polyurethane resin foam slices as porous resin particles; A step of mixing the porous resin particles with a binder resin to obtain an anti-reflection coating material; and applying the antireflection coating material to a substrate to form the resin layer, thereby obtaining an antireflection sheet. The anti-reflection coating material according to the invention of claim 6 is an anti-reflection coating material containing a binder resin and porous resin particles, The porous resin particles are characterized in that they are made of polyurethane resin foam slices containing carbon black. The additive according to the invention of claim 7 is an additive containing porous resin particles, The porous resin particles are particles made of polyurethane resin foam slices having a plurality of protrusions and a maximum Feret diameter A of 10 to 100 μm, The porous resin particles have openings on the surface having a minimum Feret diameter B2 of 1 to 50 μm, and the ratio of the maximum Feret diameter B1 to the minimum Feret diameter B2 of the openings is 1.5 to 5.0, and the openings have a communicating structure that communicates with other holes that are not open on the surface, The porous resin particles are characterized in that they contain 1 to 35 parts by mass of carbon black relative to 100 parts by mass of the porous resin particles. Effect of the Invention
[0006] According to the above-mentioned invention, it is possible to provide an antireflection sheet and an antireflection paint having a high antireflection effect, as well as additives suitable for these. [Brief description of the drawings]
[0007] [Figure 1] 1 is a schematic cross-sectional view of an anti-reflection sheet according to an embodiment of the present invention; [Diagram 2] Enlarged photo of porous resin particles [Diagram 3] Diagram of the sampling device [Figure 4] Enlarged photo of polyurethane resin sheet [Diagram 5] Graph showing experimental results on anti-reflection effect DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Referring now to the illustrated embodiment, FIG. 1 shows a schematic cross-sectional view of a reflection-suppressing sheet 1 according to the present invention. The reflection-suppressing sheet 1 is composed of a base layer 2 and a resin layer 3, and the resin layer 3 is composed of a binder resin 4 and porous resin particles 5. When manufacturing the reflection-suppressing sheet 1, as described below, a reflection-suppressing paint according to the present invention containing a binder resin 4 and porous resin particles 5 is used, and when preparing the reflection-suppressing paint, an additive according to the present invention containing the porous resin particles 5 is used.
[0009] For example, polymer films, foam materials (sponges), and fiber substrates such as woven fabrics, nonwoven fabrics, and knitted fabrics can be used for the substrate layer 2. Among these, foam materials and fiber substrates are preferred because the resulting antireflection sheet 1 can be attached to curved surfaces and uneven surfaces, and among fiber substrates, nonwoven fabrics are preferred. The fiber substrates may be impregnated with resin. When a nonwoven fabric is used as the base layer 2, the thickness is preferably from 10 to 5000 μm, more preferably from 50 to 2500 μm, and even more preferably from 100 to 2000 μm. When a nonwoven fabric is used as the base layer 2, the basis weight is 5 to 2000 g / m 2 is preferable, and 10 to 1500 g / m 2 More preferably, 50 to 1300 g / m 2 is even more preferred. By using a nonwoven fabric for the base layer 2, the fibers used in the nonwoven fabric and the resin layer are entangled at the interface between the resin layer 3 and the base layer 2, thereby preventing peeling.
[0010] The resin layer 3 is composed of a black binder resin 4 and fine porous resin particles 5 containing carbon black. As shown in FIG. 1, the porous resin particles 5 are scattered on the surface of the resin layer 3, and each porous resin particle 5 includes aggregates in which the binder resin has permeated the inside of the particle. Commercially available black paints containing acrylic resins, urethane resins, epoxy resins, alkyd resins, polyester resins, etc., containing black pigments such as carbon black, as main components, can be used as the binder resin 4. These black paints can be used alone or in combination of two or more kinds.
[0011] FIG. 2 is a photograph of the porous resin particle 5 enlarged 500 times, and as described in detail below, it is a slice of polyurethane resin foam having a maximum Feret's diameter A of approximately 10 to 100 μm, with multiple protrusions 5a formed on the outer surface of each porous resin particle 5 and numerous small openings having an approximately elliptical shape formed on the surface. The porous resin particles 5 in the present invention are relatively soft fine particles made of polyurethane resin foam, unlike the fine particles made of PMMA or polyester described in Patent Documents 1 and 2, and are soft and spongy, so that the binder resin can easily penetrate into the porous resin particles, and some of the binder resin is in an agglomerated state on the surface.
[0012] Next, a method for producing the additive containing the porous resin particles 5 will be described. FIG. 3 shows an additive manufacturing apparatus 11 for manufacturing the above-mentioned additive, which includes a supply roller 12 for supplying a polyurethane resin sheet S, a buff roller 13 for grinding the surface of the sheet S, a recovery box 14 for recovering the porous resin particles 5 produced by grinding, and a recovery roller 15 for recovering the sheet S after grinding. A polyurethane resin sheet S for collecting the porous resin particles 5 is wound around the supply roller 12, and while the sheet S is being fed from the supply roller 12, the sheet S is taken up by the recovery roller 15, thereby moving the sheet S at a predetermined speed. In addition, a holding roller 16 is provided between the supply roller 12 and the recovery roller 15 at a position opposite the buff roller 13, and the sheet S is ground by the buff roller 13 as it passes between the buff roller 13 and the holding roller 16. Sandpaper of the required coarseness is attached to the outer periphery of the buff roller 13, and the buff roller 13 is pressed against the sheet S while rotating to grind the surface of the sheet S. The particles generated during this process become the porous resin particles 5 and are collected in the collection box 14.
[0013] The polyurethane resin sheet S used to collect the porous resin particles 5 is a polyurethane resin foam, and is manufactured using a conventionally known wet membrane-forming method, through a preparation process of preparing a polyurethane resin solution, a coagulation / regeneration process of continuously applying the polyurethane resin solution to a membrane-forming substrate and coagulating and regenerating the polyurethane resin into a sheet shape in an aqueous coagulation liquid, and a washing / drying process of washing and drying the coagulated / regenerated polyurethane resin.
[0014] In the preparation step, a polyurethane resin, a water-miscible organic solvent capable of dissolving the polyurethane resin, required additives, and carbon black are mixed together to dissolve the polyurethane resin. The polyurethane resin can be selected from polyester-based, polyether-based, polycarbonate-based, and other resins. Commercially available resins such as "Crisbon" (trade name) manufactured by DIC Corporation, "Sanpren" (trade name) manufactured by Sanyo Chemical Industries, Ltd., and "Rezamin" (trade name) manufactured by Dainichiseika Color & Chemicals Mfg. Co., Ltd. may be used, or a resin having the desired properties may be produced by oneself. The organic solvent may be an aprotic organic solvent. More specifically, N,N-dimethylformamide (hereinafter abbreviated as DMF), N,N-dimethylacetamide (DMAc), dimethylsulfoxide (DMSO), etc. may be mentioned, but in this example, DMF is used. Here, the polyurethane resin is dissolved in DMF to a concentration of 20 to 40 mass %. As the additives, a hydrophilic additive that promotes pore formation in order to control the size and amount (number) of pores formed in the resin, a hydrophobic additive that stabilizes the regeneration of the polyurethane resin, etc. can be used.
[0015] The polyurethane resin constituting the sheet S preferably has a 100% modulus of 1 to 40 MPa, and more preferably has a 100% modulus of 2 to 25 MPa. When the 100% modulus is within the above range, the polyurethane resin stretches when the surface of the sheet S is ground, easily deforming the openings into an approximately elliptical shape, making it possible to enlarge the voids in the porous resin particles 5, and the stretched and broken parts are more likely to remain as protrusions 5a. The modulus is an index of the hardness of a resin, and is the value obtained by dividing the load applied when an unfoamed resin sheet is stretched 100% (stretched to twice its original length) by the cross-sectional area (hereinafter, sometimes referred to as the 100% modulus). The higher this value, the harder the resin is.
[0016] In addition, the matrix component of the polyurethane resin that constitutes the sheet S has a breaking strength (kg / mm 2 ) × breaking elongation (%) is preferably from 25 to 1,500, more preferably from 35 to 1,000, and even more preferably from 50 to 800. Here, the breaking elongation is preferably 50 to 300%. The breaking elongation indicates the degree of elongation when the resin is stretched until it breaks, and the larger the value, the easier it is to elongate and deform. The breaking strength is 0.5 to 5.0 kg / mm 2 The breaking strength indicates the stress when the resin is stretched until it breaks, and the larger the value, the tougher the resin is and the greater its rigidity. And the breaking strength (kg / mm 2 When the value of (x) × (elongation at break (%)) is in the range of 25 to 1500, the resin that has been stretched and deformed can be plastically deformed to form the protrusions 5a that remain stretched without returning to their original shape, thereby improving the reflection suppressing effect. Breaking strength (kg / mm 2 If the value of breaking strength (kg / mm ) × breaking elongation (%) is less than 25, the resin is easily torn and difficult to elongate, making it difficult to form the protrusions 5a. 2 If the value of (length x length at break (%)) x breaking elongation (%) exceeds 1500, the stretched resin will return to its original shape, making it difficult to form the protrusions 5a.
[0017] The breaking elongation is measured by punching out sheet S into an approximately dumbbell shape, clamping the measurement sample between the upper and lower air chucks of the measuring machine, and starting the measurement at a tensile speed of 100 mm / min and an initial gripping distance of 50 mm. The value at which the measured value reaches its peak (break) is taken as the strength (maximum load). The test was carried out twice, and the breaking strength (kgf / mm 2 The breaking strength was calculated from the average value of the calculated values. The breaking elongation of the polyurethane resin sheet is the elongation at the time of break in the above tensile measurement, and the breaking strength and elongation during tension were measured using a universal testing machine (Tensilon universal testing machine RTC-1210A, manufactured by A&D Co., Ltd.) according to a method conforming to Japanese Industrial Standards (JIS K6550).
[0018] The carbon black functions as a black pigment for suppressing light reflection and is also used as a non-elastic filler, and the amount of carbon black contained per 100 parts by mass of the polyurethane resin solution is preferably 1 to 35 parts by mass, more preferably 3 to 30 parts by mass, and even more preferably 5 to 25 parts by mass. When the carbon black is within the above range, the resulting porous resin particles effectively suppress reflection, and the carbon black imparts appropriate brittleness to the polyurethane resin sheet, making it easy to form elongated protrusions 5a and small openings having a roughly elliptical shape extending in a certain direction.
[0019] In the coagulation and regeneration step, the polyurethane resin solution obtained in the preparation step is applied in a substantially uniform manner in the form of a sheet onto a belt-shaped film-forming substrate at room temperature using a coating device such as a knife coater. At this time, the coating thickness (coating amount) of the polyurethane resin solution is adjusted by adjusting the gap (clearance) between the knife coater or the like and the film-forming substrate. In this embodiment, the coating thickness is adjusted so that the thickness of the polyurethane resin sheet after drying (film thickness) is in the range of 200 to 3000 μm.
[0020] Next, the polyurethane resin solution applied to the film-forming substrate is continuously guided into a coagulation liquid (aqueous coagulation liquid) whose main component is water, which is a poor solvent for polyurethane resin. To the coagulation liquid, an organic solvent such as DMF or a polar solvent other than DMF may be added in order to adjust the regeneration speed of the polyurethane resin, but in this example, water is used. In the coagulating liquid, a film is first formed at the interface between the polyurethane resin solution and the coagulating liquid, and countless micropores that constitute a skin layer are formed in the polyurethane resin immediately adjacent to the film. The polyurethane resin is then regenerated with an open-cell structure by the cooperative phenomenon of the diffusion of DMF in the polyurethane resin solution into the coagulating liquid and the infiltration of water into the polyurethane resin.
[0021] Here, we will explain the foaming that accompanies the regeneration of polyurethane resin. After a coating is formed in the coagulation liquid, the cohesive force of the polyurethane resin increases, so regeneration progresses rapidly in the polyurethane resin immediately adjacent to the coating, and a skin layer is formed. Therefore, after the skin layer is formed, the polyurethane resin in the polyurethane resin solution before solidification moves to the skin layer side and aggregates. As a result, the amount of polyurethane resin on the film-forming substrate side decreases, and bubbles are formed that are larger on the film-forming substrate side than on the skin layer side. By removing the solvent from the polyurethane resin solution, that is, by replacing DMF with water, large bubbles are formed, and the micropores in the skin layer and the large bubbles communicate with the small bubbles in a network-like manner. FIG. 4 shows a photograph of the surface of sheet S enlarged 500 times, which shows that numerous small openings with diameters of 1 to 50 μm are formed in the resin walls between the larger openings, and these large and small openings form a communicating structure that allows air to flow between them and other holes that are not open on the surface.
[0022] In the washing and drying step, the polyurethane resin sheet S regenerated in the coagulation regeneration step is washed in a washing liquid such as water to remove DMF remaining in the polyurethane resin, and then dried. In this embodiment, a cylinder dryer equipped with a cylinder having an internal heat source is used to dry the polyurethane resin. The polyurethane resin is dried by passing along the circumferential surface of the cylinder. The polyurethane resin sheet S thus obtained is then wound into a roll and used as the supply roller 12 of the additive manufacturing apparatus 11.
[0023] Next, a step of obtaining the porous resin particles 5 from the polyurethane resin sheet S supplied from the supply roller 12 is carried out using the additive manufacturing apparatus 11, thereby producing the additive. The feed speed of the sheet S by the supply roller 12 in the additive manufacturing apparatus 11 is set in the range of 0.5 to 15 m / min, and the buff roller 13 is fitted with sandpaper preferably having a grit size of 100 to 350, more preferably having a grit size of 150 to 250, and the buff roller 13 is pressed against the sheet S while rotating at a rotation speed of 1000 to 3000 rpm. In this embodiment, sandpaper is used for the buff roller 13, but any type of buff roller that can perform uniform processing (grinding and removing), such as a diamond buff roller, can be used. When the buff roller 13 rotates and comes into contact with the surface of the polyurethane resin sheet S, part of the polyurethane resin on the surface of the polyurethane resin sheet S is pulled and stretched due to friction with the buff roller 13, and the stretched part becomes thinner and then breaks, becoming porous resin particles 5 and being collected in the collection box 14. In this case, the multiple protrusions 5a formed on the porous resin particles 5 can be obtained by adjusting the buff size, the feed speed of the supply roller 12 and the sheet, the rotation speed of the buff roller, etc., depending on the modulus of the polyurethane resin used in the polyurethane resin sheet S.
[0024] In this manner, the porous resin particles 5 obtained by stretching and breaking the polyurethane sheet S supplied from the supply roller 12 are particles having a plurality of protrusions 5a and a maximum Feret's diameter A of 10 to 100 μm. In addition, small openings of 1 to 50 μm having a roughly elliptical shape extending in a certain direction are formed on the surface of the porous resin particles 5, and these large and small openings form a communicating structure that allows ventilation between them and other holes that are not open on the surface. Furthermore, in the porous resin particles 5 of this embodiment, the small openings include openings having a minimum Feret diameter B2 of 1 to 50 μm and a ratio of the maximum Feret diameter B1 to the minimum Feret diameter B2 of 1.5 to 5.0. The minimum Feret diameter B2 is preferably 1 to 30 μm, and more preferably 1 to 20 μm. The maximum Feret diameter A of the porous resin particles 5, and the maximum Feret diameter B1 and minimum Feret diameter B2 of the small pores present on the surface of the porous resin particles 5 can be determined from a scanning electron microscope (SEM) photograph. Specifically, the Feret's diameter can be obtained by using, for example, image analysis software ImageJ (registered trademark) for the image file of the porous resin particle 5 observed by SEM. The maximum Feret diameter A of the porous resin particle 5 is the diameter at which the distance between the parallel lines is the largest when the porous resin particle 5 is sandwiched between parallel lines. The maximum Feret diameters of 30 randomly selected porous resin particles 5 were measured, and the average value of these was designated as the maximum Feret diameter A. The maximum Feret diameter B1 of the openings is the diameter at which the distance between the parallel lines is the largest when the openings are sandwiched between parallel lines, and the minimum Feret diameter B2 is the diameter at which the distance between the parallel lines is the smallest when the openings are sandwiched between parallel lines. The maximum Feret diameter and the minimum Feret diameter were measured for 30 random openings formed in the porous resin particles 5, and their average values were taken as the maximum Feret diameter B1 and the minimum Feret diameter B2. The average value of the maximum Feret diameter / minimum Feret diameter value for the above-mentioned 30 random openings was taken as the ratio of the maximum Feret diameter B1 to the minimum Feret diameter B2.
[0025] Furthermore, in the porous resin particles 5, the portions broken off from the polyurethane resin are stretched and plastically deformed to form a plurality of sharp, geometrical protrusions 5a. Some of the protrusions 5a have the generally elliptical openings that extend in one direction when stretched.
[0026] The porous resin particles 5 thus obtained are used as an additive, and the above-mentioned anti-reflection coating material can be obtained by putting the above-mentioned binder resin 4 and the additive consisting of the above-mentioned porous resin particles 5 into a mixer and stirring them. In this embodiment, the porous resin particles 5 are preferably contained in a range of 0.1 to 30 parts by mass, more preferably in a range of 0.5 to 20 parts by mass, and even more preferably in a range of 1 to 10 parts by mass, per 100 parts by mass of the black paint (binder resin 4) used. By making the amount 30 parts by mass or less, it is possible to prevent the porous resin particles 5 from falling off from the formed resin layer 3. In addition, it is possible to prevent an excessive increase in the viscosity of the antireflection coating material, and therefore it is possible to prevent unevenness during application. By making the amount 0.1 parts by mass or more, it is possible to obtain a good antireflection effect.
[0027] When the reflection-suppressing sheet 1 is produced using the reflection-suppressing paint, the reflection-suppressing paint is applied to the surface of the base layer 2. At that time, the reflection-suppressing paint may be sprayed with a spray gun or applied with a brush or coater. Also, various printing techniques can be used, such as flexographic printing, which is a type of letterpress printing, gravure printing, which is a type of intaglio printing, and screen printing, which is a type of stencil printing. Thereafter, the base layer 2 coated with the antireflection paint is dried at a predetermined temperature for a predetermined period of time, thereby obtaining the antireflection sheet 1. The anti-reflection coating material of this embodiment can also be applied directly to the surface of an object.
[0028] The following experiments were conducted on the anti-reflection sheets 1 of Examples 1 and 2 of the present invention, which were created based on the above examples, and on a conventionally known comparative anti-reflection sheet that did not contain the additive made of the porous resin particles 5. Here, the maximum Feret diameter A, maximum Feret diameter B1, and minimum Feret diameter B2 of the porous resin particles 5 used in the reflection-suppressing sheet 1 are measured as follows. The Feret's diameter is measured by observing the porous resin particles 5 under an electron microscope (manufactured by JEOL Ltd., JMS-5500LV) and randomly selecting 30 points of the porous resin particles 5 as measurement samples. The extracted image is then analyzed using the image processing software ImageJ, the image is binarized, and the maximum Feret's diameter A of the porous resin particles 5, the maximum Feret's diameter B1 of the small openings present on the surface of the porous resin particles 5, and the minimum Feret's diameter B2 are measured. The maximum Ferret diameter A, maximum Ferret diameter B1, and minimum Ferret diameter B2 are calculated as the average values of the maximum and minimum Ferret diameters of any 30 points. The ratio of the maximum Ferret diameter B1 to the minimum Ferret diameter B2 is calculated as the average value of the maximum Ferret diameter / minimum Ferret diameter value of any 30 points.
[0029] Example 1 The resin layer 3 of the antireflection sheet 1 according to Example 1 is a mixture of 2 parts by mass of an additive made of porous resin particles 5 produced according to the above-mentioned manufacturing method, per 100 parts by mass of the binder resin 4. A commercially available black paint was used as the binder resin 4. The binder resin solution to which the porous resin particles 5 as the additive were added was mixed in a mixer to prepare an anti-reflection coating material. 2 The antireflection sheet 1 was obtained by applying the above-mentioned coating material to the surface of the nonwoven fabric serving as the base layer 2 using a screen printing technique.
[0030] Example 2 The antireflection sheet 1 of Example 2 was obtained in the same manner as in Example 1, except that 5 parts by mass of porous resin particles 5 were mixed with the antireflection sheet 1 of Example 1.
[0031] Comparative Example In the comparative example, unlike the above-mentioned Examples 1 and 2, the above-mentioned additive was not mixed, and the antireflection sheet 1 having the resin layer 3 that did not contain the porous resin particles 5 was used. The same substrate layer 2 as in Examples 1 and 2 was used, and an antireflection coating material made of the same binder resin 4 as in Examples 1 and 2 was used to obtain an antireflection sheet 1 in a similar manner.
[0032] FIG. 5 shows a graph of the measurement results for evaluating the anti-reflection function for the above-mentioned Examples 1 and 2 and the comparative example, with the vertical axis of the graph showing the reflectance (%) of the anti-reflection sheet 1 and the horizontal axis showing the wavelength (nm) of the reflected light. In the experiment, the total reflectance of the anti-reflection sheet 1 was measured, and the reflectance was measured using a spectrophotometer (Shimadzu Corporation, SolidSpec-3700DUV) and light with a wavelength of 250 to 2500 nm.
[0033] The experimental results showed that the anti-reflection sheets 1 of Examples 1 and 2 showed better reflectance than the anti-reflection sheet of the comparative example as the wavelength of light became longer, and particularly good anti-reflection effects were obtained in the infrared region with long wavelengths. Although the mechanism of action has not been made clear, it is presumed that the absorption and scattering of light incident on the reflection-suppressing sheet 1 is influenced by the characteristic structures obtained by ductile fracture of the polyurethane resin sheet, such as the protrusions 5a formed on the porous resin particles 5 that constitute the additive of the present invention, and the small openings formed on the surface, as well as the convex shapes of the porous resin particles formed when the sheet is made into an reflection-suppressing sheet and scattered at least on the surface of the resin layer. Furthermore, the above experimental results confirmed that the antireflection sheet 1 of Example 2 had a higher antireflection effect mainly in the visible light region than the antireflection sheet 1 of Example 1. [Explanation of symbols]
[0034] 1 Anti-reflection sheet 2 Base layer 3 resin layer 4 binder resin 5 Porous resin particle 5a Protrusion
Claims
1. An antireflection sheet comprising a base layer and a resin layer having a binder resin and porous resin particles, The reflection-suppressing sheet is characterized in that the porous resin particles are made of pieces of polyurethane resin foam containing carbon black.
2. The porous resin particles are scattered at least on the surface of the resin layer, 2. The antireflection sheet according to claim 1, further comprising porous resin particles each having the binder resin permeated therein and aggregated therein.
3. A method for producing an antireflection sheet including a base layer and a resin layer having a binder resin and porous resin particles, comprising: A step of obtaining a polyurethane resin sheet containing carbon black by a wet film forming method; grinding the polyurethane resin sheet to obtain polyurethane resin foam slices as porous resin particles; A step of mixing the porous resin particles with a binder resin to obtain an anti-reflection coating material; and applying the anti-reflection coating material to a substrate to obtain an anti-reflection sheet having the resin layer formed thereon.
4. 4. The method for producing an antireflection sheet according to claim 3, wherein in the step of obtaining the polyurethane resin sheet, 1 to 35 parts by mass of carbon black is mixed with 100 parts by mass of the porous resin particles.
5. In the step of obtaining the porous resin particles, The surface has an opening with a minimum Feret diameter B2 of 1 to 50 μm, and the minimum Feret diameter B 2 Maximum Feret diameter B 1 a ratio of 1.5 to 5.0, and the above-mentioned openings have a communicating structure that allows ventilation with other openings that are not open on the surface.
6. An anti-reflection coating material containing a binder resin and porous resin particles, The anti-reflection coating material is characterized in that the porous resin particles are made of pieces of polyurethane resin foam containing carbon black.
7. An additive comprising porous resin particles, The porous resin particles are particles made of polyurethane resin foam slices having a plurality of protrusions and a maximum Feret diameter A of 10 to 100 μm, The porous resin particles have a minimum Feret diameter B 2 has an opening of 1 to 50 μm, and the minimum Feret diameter B of the opening 2 Maximum Feret diameter B 1 the ratio of the openings is 1.5 to 5.0, and the openings have a communicating structure that communicates with other holes that are not open on the surface, The porous resin particles contain 1 to 35 parts by mass of carbon black per 100 parts by mass of the porous resin particles.
8. The matrix resin constituting the porous resin particles is a polyurethane resin, and has a 100% modulus of 1 to 40 MPa and a breaking strength (kg / mm 2 8. The additive according to claim 7, characterized in that the ratio of the elastic modulus (Ag) to the elongation at break (%) is 25 to 1,500.
Citation Information
Patent Citations
Diphenyl ether derivative* and herbicide containing diphenyl ether derivative
JP1981055387A
Anti-reflective coating material, optical member with Anti-reflective film, optical device, and image capturing device