Anti-corrosion sheet for rail, rail covering structure and manufacturing method of rail covering structure

A fiber-reinforced prepreg with curable resin addresses the complexity and durability issues of existing rail corrosion prevention methods by providing a durable and easily applied sheet with high insulation resistance and barrier properties, effectively preventing rail corrosion.

JP2024164802APending Publication Date: 2024-11-27SEKISUI CHEMICAL CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024030338
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-15
Filing Date
2024-02-29
Publication Date
2024-11-27

AI Technical Summary

Technical Problem

Existing rail corrosion prevention methods, such as those using polyvinyl chloride covers, are complex to apply and lack durability, necessitating a more straightforward and durable solution.

Method used

A fiber-reinforced prepreg with a curable resin is used to create a rail corrosion prevention sheet that meets specific electrical resistance, barrier, and durability criteria, including a resistance value of 5×10^6 Ω, AC and DC breakdown voltages of 20 kV and 15 kV, and low water and chloride ion permeability, with a glass fiber reinforcing member and photocurable resin.

Benefits of technology

The solution provides a simple and durable rail corrosion prevention sheet that effectively blocks electrical contact, preventing corrosion by ensuring high insulation resistance and barrier properties, while maintaining flexibility and ease of application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024164802000001_ABST
    Figure 2024164802000001_ABST
Patent Text Reader

Abstract

To provide an anti-corrosion sheet for rails that is easy to build and excellent at durability, for solving the problem of the conventional technologies in which it is troublesome to prepare a rail protection cover according to the shapes of various rails and in addition durability is required for rail anti-corrosion members.SOLUTION: A sheet is made of fiber-reinforced prepreg, and when resin of the fiber-reinforced prepreg is cured, the resistance value measured in the direct current insulation resistance test of JIS E 1203:2007 is 5×106 Ω or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a sheet for preventing rail corrosion, a rail covering structure, and a method for manufacturing a rail covering structure. [Background technology]

[0002] Electricity, which powers trains, flows through the rails. This makes the rails susceptible to corrosion (so-called electrolytic corrosion). Even slight corrosion of the rails can cause the rails to break. In response to this problem, members for preventing rail corrosion have been proposed with the aim of preventing rail corrosion. For example, Patent Document 1 proposes a rail protection cover that is a polyvinyl chloride molded body that covers approximately the lower half of the rail (see Patent Document 1). According to the invention described in Patent Document 1, rail corrosion is prevented by blocking electrical contact between the rail and the ground. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2010-203096 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, in the invention of Patent Document 1, it is cumbersome to prepare rail protection covers according to various rail shapes. In addition, durability is required for members for preventing rail corrosion. The present invention has been made in consideration of the above circumstances, and has an object to provide a sheet for preventing rail corrosion that is easy to apply and has excellent durability. [Means for solving the problem]

[0005] The present invention has the following aspects. <1> A fiber-reinforced prepreg having a reinforcing member and a curable resin, When the curable resin is cured, the resistance measured by the DC insulation resistance test of JIS E 1203:2007 is 5×10 6 A sheet for preventing rail corrosion with a resistance of Ω or more. <2> The voltage measured by the AC breakdown voltage test of JIS C 2110-1:2016 in the cured state of the curable resin is 20 kV or more. <1> The rail corrosion prevention sheet according to claim 1. <3> In a cured state, the voltage measured by the DC breakdown voltage test of JIS C 2110-2:2016 is 15 kV or more. <1> or <2> The rail corrosion prevention sheet according to claim 1. <4> In a cured state of the curable resin, the water permeation amount measured by the water permeation test of the corrosion protection coating layer in Appendix F of JIS A 7502-2:2015 is 0.15 g or less; <1> ~ <3> 2. A rail corrosion prevention sheet according to claim 1 . <5> When the curable resin is cured, the chloride ion blocking ability measured by the quality standard for surface protection work "medium corrosion protection type C" is 1.0 x 10 -3 mg / cm 2 - days or less, <1> ~ <4> 2. A rail corrosion prevention sheet according to claim 1 . <6> When the curable resin is cured, the oxygen barrier property measured by the quality standard for surface protection work "medium corrosion protection type C" is 1.00 mol / m 2 - Age or younger, <1> ~ <5> 2. A rail corrosion prevention sheet according to claim 1 . <7> The reinforcing member includes glass fiber. <1> ~ <6> 2. A rail corrosion prevention sheet according to claim 1 . <8> The curable resin includes a photocurable resin. <1> ~ <7> 2. A rail corrosion prevention sheet according to claim 1 .

[0006] <9> A rail and a coating layer covering at least a bottom surface of the rail, The coating layer is <1> ~ <8> 2. A rail covering structure comprising a cured product of the rail corrosion prevention sheet according to any one of claims 1 to 11.

[0007] <10> applying an adhesive to at least a bottom surface of the rail; On the surface to which the adhesive is applied, <1> ~ <8> A step of attaching the rail corrosion prevention sheet according to any one of the above items; A step of irradiating the rail corrosion prevention sheet with energy rays to harden the hardening resin of the fiber reinforced prepreg to form a coating layer; A method for manufacturing a rail covering structure comprising the steps of: <11> The adhesive has a resistance of 5×10 when measured by a direct current insulation resistance test according to JIS E 1203:2007 for a cured product of the adhesive. 6 Ω or more, <10> A method for manufacturing a covering structure for a rail according to claim 1. Effect of the Invention

[0008] The rail corrosion prevention sheet of the present invention is easy to apply and has excellent durability. [Brief description of the drawings]

[0009] [Figure 1] 1 is a cross-sectional view showing a rail covering structure according to one embodiment of the present invention; [Diagram 2] FIG. 2 is a perspective view showing a flammability test of a coating layer of a rail coating structure according to one embodiment of the present invention. [Diagram 3] 1 is a perspective view showing a method for manufacturing a rail covering structure according to one embodiment of the present invention; [Figure 4] 4A to 4C are cross-sectional views showing a method for manufacturing a rail covering structure according to one embodiment of the present invention. [Diagram 5] 4A to 4C are cross-sectional views showing a method for manufacturing a rail covering structure according to one embodiment of the present invention. [Figure 6]FIG. 2 is a schematic diagram illustrating a measurement method for a fatigue test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present invention will now be described with reference to the drawings. (Rail corrosion prevention sheet) The rail corrosion prevention sheet has a fiber-reinforced prepreg. The fiber-reinforced prepreg is an uncured resin sheet including a reinforcing member and a curable resin. In the fiber-reinforced prepreg, the reinforcing member is impregnated with the curable resin. The sheet for preventing rail corrosion may be made of only fiber-reinforced prepreg, or may have a layer (optional layer) other than the fiber-reinforced prepreg. The optional layers include a primer layer, an adhesive layer, a paint layer, and the like. The sheet for preventing rail corrosion is attached to the construction surface of the rail (the area where the coating layer is to be provided) and then the curable resin of the fiber-reinforced prepreg is cured to form the coating layer (the cured product of the sheet for preventing rail corrosion).

[0011] Examples of the reinforcing member include inorganic fibers such as glass fibers, organic fibers such as vinylon fibers, and metal fibers such as carbon fibers and steel fibers. Among these, glass fibers are preferred as the reinforcing member from the viewpoint of improving insulation properties.

[0012] The form of the fiber is not particularly limited, and examples thereof include a form in which fibers such as tow, cloth, chopped fiber, and continuous fiber are aligned in one direction; a form in which continuous fibers are woven in the warp and weft directions; a form in which the direction of the tow is aligned in one direction and held by auxiliary weft threads; a form in which a plurality of fiber sheets in which the direction of the fibers is aligned in one direction are overlapped and stitched together with auxiliary threads so that the directions of the fibers are different; and a form in which the fibers are nonwoven. Among these, nonwoven fabrics are preferred from the viewpoint of isotropic arrangement of the fibers. Among them, a chopped strand mat of glass fiber is suitable as the reinforcing member, since the use of the chopped strand mat as the reinforcing member can improve the insulation property and the flexibility.

[0013] The content of the reinforcing member is preferably 10 to 35 mass%, more preferably 15 to 30 mass%, and even more preferably 18 to 23 mass%, based on the total mass of the fiber-reinforced prepreg. When the content of the reinforcing member is equal to or more than the above lower limit, the strength and durability of the sheet for preventing rail corrosion can be further increased. When the content of the reinforcing member is equal to or less than the above upper limit, the flexibility of the sheet for preventing rail corrosion can be further increased.

[0014] Examples of the curable resin include photocurable resins, thermosetting resins, etc. Among them, from the viewpoint of facilitating application, photocurable resins are preferred as the curable resin. Examples of the photocurable resin include photocurable vinyl ester resin, photocurable unsaturated polyester resin, photocurable epoxy resin, etc. Among these, photocurable vinyl ester resin is preferred from the viewpoint of corrosion resistance.

[0015] The content of the curable resin is preferably 65 to 90 mass%, more preferably 70 to 85 mass%, and even more preferably 77 to 82 mass%, based on the total mass of the fiber-reinforced prepreg. When the content of the curable resin is equal to or more than the lower limit, the flexibility of the sheet for preventing rail corrosion can be further increased. When the content of the curable resin is equal to or less than the upper limit, the content of the reinforcing member can be increased, and the strength and durability of the sheet for preventing rail corrosion can be further increased.

[0016] The weight of the rail corrosion prevention sheet is 1500g / m 2 More than 3500g / m 2 Less than 2000 g / m is preferable. 2 More than 3000g / m 2 The following is more preferable. When the basis weight is equal to or more than the above lower limit, the corrosion resistance can be further improved. When the basis weight is equal to or less than the above upper limit, the flexibility of the sheet for preventing rail corrosion is increased, and the sheet can more easily conform to the application surface.

[0017] The thickness of the sheet for preventing rail corrosion is preferably 3.0 mm or less, more preferably 2.0 mm or less. When the thickness is equal to or less than the upper limit value, the flexibility of the sheet for preventing rail corrosion is increased, and the sheet can more easily conform to the application surface. The thickness of the sheet for preventing rail corrosion is preferably 1.0 mm or more, and more preferably 1.5 mm or more. When the thickness of the sheet for preventing rail corrosion is equal to or more than the above lower limit, the corrosion resistance can be further improved.

[0018] (Rail covering structure) FIG. 1 is a cross-sectional view showing a rail covering structure according to one embodiment of the present invention. In addition, the drawings used in the following explanation may show characteristic parts in an enlarged manner for the sake of convenience in order to make the features easier to understand, and the dimensional ratios of each component may differ from the actual ones.

[0019] As shown in FIG. 1, a rail covering structure 30 includes a rail 10 and a covering layer 20 covering a portion of the rail 10 . The rail 10 has a head portion 11, a web portion 12, and a bottom portion 13. The rail 10 has the bottom portion 13, the web portion 12, and the head portion 11, which are successively arranged vertically from below to above. The cross section of the bottom portion 13 is substantially triangular. The bottom portion 13 has a bottom surface 13a that contacts the installation surface such as the surface of the sleeper, and one bottom upper surface 13b and the other bottom upper surface 13c that are continuous with the bottom surface 13a and rise from one end 13d and the other end 13e of the bottom portion 13. The abdomen 12 has a generally rectangular cross-sectional shape. The abdomen 12 has both side surfaces (one abdomen side surface 12a and the other abdomen side surface 12b) that are continuous with one bottom upper surface 13b and the other bottom upper surface 13c of the bottom 13. The head 11 has a substantially rectangular cross-sectional shape.

[0020] In this embodiment, the coating layer 20 covers the bottom surface 13a, the ends 13d and 13e, the bottom upper surfaces 13b and 13c, and a part of the abdominal side surfaces 12a and 12b. That is, the coating layer 20 covers the bottom 13 and a part of the abdominal portion 12. In the present invention, the coating layer 20 only needs to cover the bottom surface 13a and not the head portion 11, and may not cover a part or all of the abdominal side surfaces 12a and 12b, or a part or all of the bottom upper surfaces 13b and 13c. However, from the viewpoint of further enhancing the corrosion prevention effect, it is preferable that the coating layer 20 covers a part or all of the bottom 13 and the abdominal portion. The covering layer 20 may cover not only the rail 10 but also any portion where corrosion due to electricity (galvanic corrosion) is expected to occur.

[0021] In this embodiment, the covering layer 20 has no space between it and the rail 10. In the present invention, the covering layer 20 may have a space between a part of it and the rail 10. However, in order to more effectively prevent the intrusion of water or air between the rail 10 and the covering layer 20, it is preferable that the covering layer 20 has no space between it and the rail 10.

[0022] An adhesive layer may be provided between the covering layer 20 and the rail 10. By providing the adhesive layer, the covering layer 20 can be more firmly adhered to the rail 10. The adhesive layer is a layer of a cured adhesive. Furthermore, a primer layer may be provided between the adhesive layer and the rail 10. By providing the primer layer, the adhesive layer and the rail 10 can be bonded more firmly. There may be no adhesive layer, and only a primer layer may be provided between the rail 10 and the covering layer 20. By providing a primer layer, stronger adhesion can be achieved compared to the case where only the covering layer 20 is provided.

[0023] The covering layer 20 is a cured product of the sheet for preventing rail corrosion. The covering layer 20 is formed by curing the curable resin of the sheet for preventing rail corrosion. The sheet for preventing rail corrosion adheres to the rail 10 and hardens, blocking contact with air and water and preventing corrosion of the rail 10. At the same time, the hardened sheet for preventing rail corrosion is integrated with the rail 10, reinforcing the strength of the rail 10.

[0024] The covering layer 20 may be made of one continuous sheet for preventing rail corrosion, or may be made of a combination of two or more sheets for preventing rail corrosion. In order to simplify the process of attaching the covering layer 20 to the rail 10, it is preferable that the covering layer 20 be made of one continuous sheet for preventing rail corrosion.

[0025] The cured product of the sheet for preventing rail corrosion (i.e., the curable resin in a cured state) preferably has flame retardancy according to a flammability test for railway vehicles, and more preferably is non-flammable. During maintenance and inspection, the rail head is ground using a grinding vehicle, which generates sparks. For this reason, the coating layer 20 of the rail coating structure described below must be attached to the iron (rail) and must be flame-retardant or higher (not burn when the source of fire is far away).

[0026] The flammability test for railway vehicles will now be explained. Flammability tests for railway vehicles are conducted in accordance with the methods described in "Guide to Flammability Tests of Materials for Railway Vehicles - Flammability Tests - JRMA (Japan Railway Rolling Stock and Machinery Association)." The combustion test (non-metallic materials for railway vehicles) method is as shown in Figure 2, in which a B5 test material (182 mm x 257 mm) 110 is held at a 45° incline and placed on a stand 130 made of a material with low thermal conductivity such as cork so that the center of the bottom of the fuel container 120 is 25.4 mm (1 inch) vertically below the center of the underside (burning surface) of the test material 110, 0.5 mL of pure ethyl alcohol is poured into the fuel container 120 and ignited, and the pure ethyl alcohol is left to burn out. The combustion judgment is made separately during and after the combustion of the pure ethyl alcohol. During the combustion of the pure ethyl alcohol, the ignition, flame, smoke generation, flame state, etc. of the test material 110 are observed. After the combustion of the pure ethyl alcohol, the residual flame, residual dust, carbonization, and deformation state are investigated. When the test material 110 is a hygroscopic material, the pre-test treatment of the test material 110 is as follows: cut to a specified size, place it in a well-ventilated room away from direct sunlight, at least 1 m away from the floor, and leave it for at least 5 days. The conditions in the test room are temperature: 15℃~30℃, humidity: 60%~75%, and no air movement.

[0027] The resistance value (DC insulation resistance value) measured in the DC insulation resistance test (under the following measurement conditions) of the coating layer 20 (cured product of the sheet for preventing rail corrosion) according to JIS E 1203:2007 is 5×10 6 Ω or more, 5×10 8 Ω or more is preferable, 5×10 10 Ω or more is more preferable. If the DC insulation resistance value is equal to or greater than the lower limit, the passage of electricity from the rail 10 to the ground can be prevented, and corrosion of the rail 10 due to the current can be prevented. The upper limit of the DC insulation resistance value is not particularly limited. The DC insulation resistance value is adjusted by a combination of the types of the curable resin and reinforcing member of the sheet for preventing rail corrosion, the thickness of the coating layer 20, and the like.

[0028] <Measurement conditions> Applied voltage: 500V DC x 1 min. Conditioning: 20℃ x 48 hours. Test equipment: High Resistance Meter 4339B (Agilent Technologies). Test specimen: Width 20 mm x length 40 mm x thickness 1.5 mm.

[0029] The voltage (AC breakdown voltage) measured in the covering layer 20 by the AC breakdown voltage test of JIS C 2110-1:2016 (measurement conditions below) is preferably 20 kV or more, more preferably 30 kV or more, and even more preferably 40 kV or more. When the AC breakdown voltage is equal to or more than the lower limit, it is possible to prevent current flow from the rail 10 to the ground and prevent corrosion of the rail 10 due to current. The upper limit of the AC breakdown voltage is not particularly limited. The AC insulation resistance value is adjusted by a combination of the types of curable resin and reinforcing member of the sheet for preventing rail corrosion, the thickness of the covering layer 20, and the like.

[0030] <Measurement conditions> Test atmosphere: in oil. Temperature: 23℃. Test equipment: AC / DC insulation breakdown tester, YST-243AT-100 type. Boost speed: 3kV / sec.

[0031] The voltage (DC breakdown voltage) measured in the covering layer 20 by the DC breakdown voltage test of JIS C 2110-2:2016 (measurement conditions below) is preferably 15 kV or more, more preferably 30 kV or more, and even more preferably 40 kV or more. If the DC breakdown voltage is equal to or more than the lower limit, the passage of electricity from the rail 10 to the ground can be prevented, and corrosion of the rail 10 due to current can be better prevented. The upper limit of the DC breakdown voltage is not particularly limited. The DC breakdown voltage is adjusted by a combination of the types of the curable resin and reinforcing member of the sheet for preventing rail corrosion, the thickness of the covering layer 20, and the like.

[0032] <Measurement conditions> Test atmosphere: in oil. Temperature: 23℃. Test equipment: AC / DC insulation breakdown tester, YST-243AT-100 type. Boost speed: 5kV / sec.

[0033] The coating layer 20 has a water permeability of preferably 0.15 g or less, more preferably 0.10 g or less, and even more preferably 0.05 g or less, as measured by the water permeability test for anticorrosive coating layers in Appendix F of JIS A 7502-2:2015. If the water permeability is equal to or greater than the lower limit, the contact of moisture with the surface of the rail 10 can be prevented, and corrosion of the rail 10 can be better prevented. The lower limit of the water permeability is not particularly limited. This water permeability is adjusted by a combination of the types of curable resin and reinforcing member of the sheet for preventing rail corrosion, the thickness of the coating layer 20, and the like.

[0034] To determine the water permeability of the coating layer 20 as specified in Appendix F of JIS A 7502-2, a test specimen is prepared according to the method described in "a) In the case of the applied lining method" in "F3.2 Preparation of test specimen" of Appendix F. Specifically, the test specimen was a flexible plate (a regular octagon inscribed in a circle with a thickness of 6 mm and a diameter of 150 mm) specified in JIS A 5430, on which the coating layer 20 was laminated.

[0035] Using this test specimen, a water permeability test is performed at a water pressure of 0.29 MPa for 1 hour in accordance with "7.6 (water permeability test)" of JIS A 1404. The mass difference (p2-p1) between the mass p1 of the flexible plate before the water permeability test and the mass p2 of the flexible plate after the water permeability test is wiped off is defined as the water permeability of the coating layer 20.

[0036] The coating layer 20 has a chloride ion blocking ability of 1.0×10 as measured by the quality standard for surface protection work, "medium corrosion protection type C." -3 mg / cm 2 ·days or less is preferable, 0.9×10 -3 mg / cm 2 Days or less is preferable, and 0.8×10 -3 mg / cm 2 When the chloride ion blocking property is equal to or less than the above upper limit, the contact of salt with the surface of the rail 10 can be prevented, and corrosion of the rail 10 can be prevented more effectively. The lower limit of the chloride ion blocking property is not particularly limited, but is substantially 0.7×10 -3 mg / cm 2The chloride ion blocking property is adjusted by combining the types of curable resin and reinforcing member of the sheet for preventing rail corrosion, the thickness of the coating layer 20, and the like. The "Quality standard for surface protection work, Medium corrosion protection type C" is the quality standard for surface protection work, "Medium corrosion protection type C" in Part 2 Concrete structures, Volume 2 Surface protection guidelines for concrete structures, Hanshin Expressway Co., Ltd., "Guidelines for repairing road structures," (July 2018).

[0037] The coating layer 20 has an oxygen barrier property of 1.00 mol / m as measured by the quality standard for surface protection work, "medium corrosion protection type C." 2 · years or less is preferable, 0.10 mol / m 2 Less than 0.05 mol / m is preferable. 2 It is even more preferable that the oxygen barrier property is equal to or less than one year. When the oxygen barrier property is equal to or less than the above upper limit, contact of oxygen with the surface of the rail 10 can be prevented, and corrosion of the rail 10 can be prevented more effectively. The lower limit of the oxygen barrier property is not particularly limited. The oxygen barrier property is adjusted by a combination of the types of the curable resin and reinforcing member of the sheet for preventing rail corrosion, the thickness of the coating layer 20, etc.

[0038] In the covering layer 20, the amount of wear measured under the following measurement conditions using an apparatus described in JIS A 1452:2015 is preferably smaller than the amount of wear of a mortar plate. Such an amount of wear can further increase the durability of the covering layer 20. This amount of wear is adjusted by combining the types of curable resin and reinforcing member of the sheet for preventing rail corrosion, the thickness of the covering layer 20, and the like.

[0039] <Measurement conditions> -Specimen size: 50mm x 50mm. Number of samples: n=3 each. Abrasive material: Silicon carbide abrasive 2C as specified in JIS R 6111, 4.1.2, Table 6. Fall height: 65cm Total fall weight: 10kg.

[0040] The main wear amount of the coating layer 20 is preferably 30% by mass or less of the wear amount of the mortar plate, more preferably 20% by mass or less, and further preferably 10% by mass or less. The smaller the amount of wear of the coating layer 20, the more the deterioration of the coating layer 20 caused by wear between the coating layer 20 and flying pebbles and sand is suppressed.

[0041] In the coating layer 20, the amount of wear in the JIS K 7204 wear test is preferably 0.5% by mass or less, more preferably 0.3% by mass or less, and even more preferably 0.1% by mass or less. When the amount of wear is equal to or less than the upper limit, durability can be further improved. The lower limit of the amount of wear is not particularly limited. This amount of wear is adjusted by a combination of the types of curable resin and reinforcing member of the sheet for preventing rail corrosion, the thickness of the coating layer 20, and the like.

[0042] It is preferable that the coating layer 20 has no abnormalities on the impact surface measured under the following conditions in accordance with the bending and impact test methods for building boards of JIS A 1408:2017.

[0043] <Measurement conditions> - Method of specimen placement: S1: Full support on sand. Weight classification: spherical weight: W2-1000. Weight fall height: 50cm.

[0044] The coating layer 20 is preferably transparent. If the coating layer 20 is transparent, the remaining air can be visually confirmed during the deaeration operation, and the corrosion state of the surface of the rail 10 can be easily visually confirmed. In addition, if there is an adhesive layer between the coating layer 20 and the rail 10, it is preferable that the coating layer 20 and the adhesive layer are transparent. Here, being transparent means that visible light passes through to such an extent that the surface of the rail 10 can be seen, for example, 20% or more of visible light passes through.

[0045] (Method of manufacturing rail covering structure) The method for producing a rail covering structure of this embodiment is a method for providing a covering layer 20 on a rail using the rail corrosion prevention sheet of the present invention.

[0046] The manufacturing method for the rail covering structure of this embodiment preferably includes the steps of applying a primer to the construction surface of the rail (hereinafter referred to as "step A1"), applying an adhesive to the construction surface via the primer (hereinafter referred to as "step B1"), attaching a rail corrosion prevention sheet to the adhesive-coated surface of the construction surface (hereinafter referred to as "step C1"), and curing the curable resin of the rail corrosion prevention sheet to form a coating layer (hereinafter referred to as "step D1").

[0047] In the manufacturing method of the rail covering structure of the present embodiment, it is preferable to carry out surface preparation (surface treatment) on the surface of the rail 10, particularly the surface to be worked on, to remove rust prior to step A1.

[0048] Methods for preparing the base include, for example, scraping with a grinder or sandpaper.

[0049] "Process A1" In step A1, a primer is applied to the construction surface of the rail 10. In detail, the primer is applied to both side surfaces (one side surface 12a and the other side surface 12b) of the abdominal portion 12 of the rail 10, one boundary 12c and the other boundary 12d between the abdominal portion 12 and the bottom portion 13, the bottom surface 13a of the bottom portion 13 of the rail 10, one bottom upper surface 13b and the other bottom upper surface 13c of the bottom portion 13 of the rail 10, and one end 13d and the other end 13e of the bottom portion 13 of the rail 10. The construction surface may include at least the bottom surface 13a.

[0050] The method for applying the primer to the surface to be applied is not particularly limited, but for example, a brush application method, a roller application method, a spray application method, etc. can be used.

[0051] The amount of primer applied is 0.05 kg / m per unit area of ​​the application surface. 2 More than 0.25kg / m2 Less than 0.1 kg / m is preferable. 2 More than 0.2kg / m 2 The following is more preferable. If the amount of primer applied is equal to or greater than the above lower limit, the adhesion between the rail 10 and the adhesive can be improved. If the amount of primer applied is equal to or less than the above upper limit, the primer can be applied more uniformly to the object.

[0052] Examples of the primer include an epoxy resin-based primer, a urethane resin-based primer, a polyester resin-based primer, a polypropylene resin-based primer, etc. Among these, the urethane resin-based primer is preferred from the viewpoint of workability. The primer may be of the wet curing type or the room temperature curing type, but from the viewpoint of workability on site, the wet curing type is preferable. After applying the primer, leave it to cure until it is no longer tacky.

[0053] "Process B1" In step B1, adhesive is applied to the construction surface via the primer applied in step A1. In this embodiment, adhesive is applied via the primer to both side surfaces (one side surface 12a and the other side surface 12b) of the inner portion 12 of the rail 10, the bottom surface 13a of the bottom portion 13 of the rail 10, and one bottom upper surface 13b and the other bottom upper surface 13c of the bottom portion 13 of the rail 10.

[0054] The method for applying the adhesive to the application surface is not particularly limited, but for example, a brush application method, a spray application method, etc. can be used.

[0055] The amount of adhesive applied is 0.5 kg / m per unit area of ​​the application surface. 2 More than 2.0kg / m 2 Less than 0.7kg / m is preferable. 2 More than 1.2kg / m 2 The following is more preferable. If the amount of adhesive applied is equal to or more than the above lower limit, the surface of the rail 10 and the covering layer 20 can be more firmly bonded. If the amount of adhesive applied is equal to or less than the above upper limit, workability is improved.

[0056] In step B1, an adhesive layer may be formed by applying an adhesive and curing the applied adhesive, or step C1 may be performed immediately after applying the adhesive.

[0057] The adhesive is preferably a two-liquid adhesive. Examples of two-liquid adhesives include epoxy resin adhesives, vinyl ester resin adhesives, and unsaturated polyester resin putty containing glass fiber. Among these, vinyl ester resin adhesives are preferred from the viewpoint of corrosion resistance.

[0058] The adhesive has a resistance (DC insulation resistance) of 5 x 10 or less when measured by the DC insulation resistance test of JIS E 1203:2007 (measurement conditions below) for the cured adhesive. 6 Ω or more is preferable, 5×10 8 Ω or more is preferable, 5×10 10 Ω or more is more preferable. When the ends of two prepreg sheets are butted together to form a joint of the covering layer 20, a part of the adhesive layer (cured adhesive) may leak at this joint. If the DC insulation resistance value of the cured adhesive is equal to or greater than the above lower limit, even if the adhesive layer is exposed, it is possible to prevent current from passing from the rail 10 to the ground, and to more effectively prevent corrosion of the rail 10 due to electric current. There is no particular limit to the upper limit of the DC insulation resistance value of the cured adhesive. The DC insulation resistance value is adjusted depending on the type of adhesive. <Measurement conditions> ·Applied voltage: 500V DC x 1min. Conditioning: 20℃ x 48 hours. Test equipment: High Resistance Meter 4339B (Agilent Technologies). The adhesive was cured to create a 5mm thick plate, which was then cut to create a test specimen measuring 20mm wide x 40mm long x 5mm thick. Two φ5mm holes were drilled in the centre of the test specimen before measurements were taken.

[0059] "Process C1" In step C1, first, a rail corrosion prevention sheet is attached to one of the abdominal side surfaces 12a of the rail 10 to which the adhesive is applied. Next, the rail corrosion prevention sheet is folded at the boundary 12c between the abdominal portion 12 and the bottom portion 13, and attached to one of the bottom upper surfaces 13b of the bottom portion 13 of the rail 10. Next, the rail corrosion prevention sheet is folded at one end 13d of the bottom portion 13 of the rail 10, and attached to the bottom surface 13a of the bottom portion 13 of the rail 10. Next, the rail corrosion prevention sheet is folded at the other end 13e of the bottom portion 13 of the rail 10, and attached to the other bottom upper surface 13c of the bottom portion 13 of the rail 10. Next, the rail corrosion prevention sheet is folded at the boundary 12d between the abdominal portion 12 and the bottom portion 13, and attached to the other abdominal side surface 12b of the rail 10.

[0060] In step C1, a plurality of rail corrosion prevention sheets may be used, and the plurality of rail corrosion prevention sheets may be overlapped with each other in the longitudinal direction of the rail 10. Alternatively, the longitudinal end faces of the plurality of rail corrosion prevention sheets may be butted against each other so that the plurality of rail corrosion prevention sheets do not overlap with each other. When the adhesive layer has low insulation and insulation needs to be ensured by the covering layer 20, overlapping is preferable in terms of ensuring insulation. By overlapping the rail corrosion prevention sheets with each other, the covering layer 20 formed is less likely to peel off, so that the barrier between the external environment and the rail 10 can be maintained. It is preferable to butt the rail corrosion prevention sheets together in order to prevent steps from occurring due to overlapping of the sheets. However, the most preferable method is to apply a single sheet of rail corrosion prevention sheet over the entire length of the rail.

[0061] For example, as shown in Figures 3 and 4, a case will be described in which a first rail corrosion prevention sheet 21 and a second rail corrosion prevention sheet 22 are used as rail corrosion prevention sheets. For example, a case will be described in which the first rail corrosion prevention sheet 21 and the second rail corrosion prevention sheet 22 are attached to one bottom upper surface 13b of the bottom 13 of the rail 10, the other end 13e of the bottom 13, and the bottom surface 13a of the bottom 13. A primer 40 is applied to one bottom upper surface 13b of the bottom 13 of the rail 10, the other end 13e of the bottom 13, and the bottom surface 13a of the bottom 13. Next, adhesive 50 is applied via primer 40 to one bottom upper surface 13b of bottom 13 of rail 10, the other end 13e of bottom 13, and bottom surface 13a of bottom 13. Next, the first rail corrosion prevention sheet 21 is attached to one bottom upper surface 13b of the bottom portion 13 of the rail 10, the other end 13e of the bottom portion 13, and the bottom surface 13a of the bottom portion 13 via an adhesive 50. Next, the second rail corrosion prevention sheet 22 is attached to one bottom upper surface 13b of the bottom 13 of the rail 10, the other end 13e of the bottom 13, and the bottom surface 13a of the bottom 13 via an adhesive 50. At this time, one end 22a of the second rail corrosion prevention sheet 22 in the longitudinal direction of the rail 10 is overlapped on one end 21a of the first rail corrosion prevention sheet 21 in the longitudinal direction of the rail 10. In this case, the one end 21a of the first rail corrosion prevention sheet 21 and the one end 22a of the second rail corrosion prevention sheet 22 are preferably bonded to each other via a primer and adhesive applied to the one end 21a of the first rail corrosion prevention sheet 21. In this manner, after the rail corrosion prevention sheets 21, 22 are attached to the rail 10, it is possible to maintain the insulation between both side surfaces (one side surface 12a and the other side surface 12b) of the abdominal portion 12 of the rail 10, one boundary 12c and the other boundary 12d between the abdominal portion 12 and the bottom portion 13, the bottom surface 13a of the bottom portion 13 of the rail 10, one bottom upper surface 13b and the other bottom upper surface 13c of the bottom portion 13 of the rail 10, and one end 13d and the other end 13e of the bottom portion 13 of the rail 10 and the external environment. The overlapping length (W shown in FIG. 4) between one end 21a of first rail corrosion prevention sheet 21 and one end 22a of second rail corrosion prevention sheet 22 may be 0 mm or more, or 10 mm or more.

[0062] 5, the end face 21b of the first rail corrosion prevention sheet 21 and the end face 22b of the second rail corrosion prevention sheet 22 may be butted against each other, and the first rail corrosion prevention sheet 21 and the second rail corrosion prevention sheet 22 may be attached to the rail 10 with an adhesive 50. In this manner, the rail corrosion prevention sheets do not overlap each other near the boundary 23 between the first rail corrosion prevention sheet 21 and the second rail corrosion prevention sheet 22, making it possible to make the thickness of the coating layer uniform. When the end face 21b of the first rail corrosion prevention sheet 21 and the end face 22b of the second rail corrosion prevention sheet 22 are butted together to attach the rail corrosion prevention sheets to the rail 10, it is preferable that the adhesive used in step B1 has a DC insulation resistance value in the preferred range described above in a hardened state (i.e., in the state of the adhesive layer).

[0063] "Process D1" In step D1, the curable resin of the sheet for preventing rail corrosion is cured by energy ray irradiation to form the covering layer 20. The type of energy ray is appropriately determined depending on the type of curable resin, and examples thereof include ultraviolet rays, electromagnetic waves, heat, and the like. In step D1, the amount of energy radiation to be irradiated is not particularly limited, and is adjusted as appropriate depending on the type and amount of the curable resin in the sheet for preventing rail corrosion.

[0064] Through the above steps, the bottom 13 of the rail 10 is covered with the covering layer 20, and both side surfaces of the web portion 12 of the rail 10 that is continuous with the bottom 13 of the rail 10 are covered with the covering layer 20, thereby forming a rail covering structure.

[0065] According to the rail covering structure of this embodiment, the bottom of the rail and both side surfaces of the rail body are covered with a covering layer. The covering layer has a specific range of resistance measured in a DC insulation resistance test, and therefore can block leakage current from contact points between the rail fixing jig (e.g., rail connector) and the rail, the bottom of the rail, etc., and prevent electrolytic corrosion of the rail.

[0066] According to the method for manufacturing a rail covering structure of this embodiment, the sheet for preventing rail corrosion is unlikely to float after being attached to the rail, and a structure for preventing rail corrosion can be easily manufactured. Therefore, it is possible to prevent electrical corrosion of the rail caused by leakage current from contact points between the rail fixing jig and the rail, the bottom of the rail, etc.

[0067] (Other embodiments) It should be noted that the present invention is not limited to the above-described embodiment. The manufacturing method for the rail covering structure of this embodiment includes a step of applying a primer to the construction surface of the rail (hereinafter referred to as "step A1"), a step of applying an adhesive to the rail corrosion prevention sheet (hereinafter referred to as "step B2"), a step of attaching the adhesive-coated surface of the rail corrosion prevention sheet to the construction surface via the primer (hereinafter referred to as "step C2"), and a step of hardening the rail corrosion prevention sheet by irradiating it with energy rays (hereinafter referred to as "step D1"). That is, the manufacturing method of the rail covering structure of this embodiment differs from the manufacturing method of the above-described embodiment in that step B2 is used instead of step B1, and step C2 is used instead of step C1.

[0068] In the method for preventing corrosion of a rail according to the present embodiment, it is also preferable to carry out surface preparation (surface treatment) on the surface of the rail 10 to remove rust prior to step A2.

[0069] "Process A1" In step A1, a primer is applied to the surface of the rail 10 to be installed.

[0070] "Process B2" In step B2, an adhesive is applied to the sheet for preventing rail corrosion. The method for applying the adhesive to the sheet for preventing rail corrosion is not particularly limited, but for example, a brush coating method, a spray coating method, a dipping method, etc. can be used. The adhesive is the same as that used in the above-mentioned step B1.

[0071] The amount of adhesive to be applied is 0.5 kg / m per unit area of ​​the surface of the rail corrosion prevention sheet. 2 More than 2.0kg / m 2 Less than 0.7kg / m is preferable. 2 More than 1.2kg / m 2 The following is more preferable. When the amount of adhesive applied is equal to or more than the above-mentioned lower limit, the rail 10 and the rail corrosion prevention sheet can be more firmly bonded. When the amount of adhesive applied is equal to or less than the above-mentioned upper limit, workability is improved. The rail corrosion prevention sheet may be a single continuous sheet, or may be a combination of two or more sheets. In order to simplify the process of attaching the sheet to the rail 10, the rail corrosion prevention sheet is preferably a single continuous sheet.

[0072] "Process C2" In step C2, the adhesive-coated surface of the rail corrosion prevention sheet is attached to the bottom 13 and web portion 12 of the rail 10 via a primer, similar to step C1 described above.

[0073] "Process D1" In step D1, the curable resin of the sheet for preventing rail corrosion is cured by irradiation with energy rays.

[0074] Through the above steps, the covering layer 20 is provided on a portion of the rail 10, forming a rail covering structure.

[0075] According to the method for manufacturing a rail covering structure of this embodiment, the application time can be reduced by utilizing the time it takes for the primer to harden to apply adhesive to the application surface of the rail corrosion prevention sheet.

[0076] In the above embodiment, the step A1 of applying a primer to the rail is included before the step B1 or B2, but the present invention is not limited to this. Depending on the type of adhesive used in the step B1 or B2, the step A1 may not be included. In the above-described embodiment, there is a step B1 of applying an adhesive to the application surface via a primer or a step B2 of applying an adhesive to the rail corrosion prevention sheet, but the present invention is not limited thereto. For example, if the rail corrosion prevention sheet has adhesiveness, it can be applied without using an adhesive, so the rail corrosion prevention sheet may be directly attached to the rail 10. Alternatively, the rail corrosion prevention sheet may be attached via a primer.

[0077] Although the embodiment of the present invention has been described in detail above with reference to the drawings, the embodiment is merely an example of the present invention. Therefore, the present invention is not limited to the configuration of the embodiment, and it goes without saying that even if there are design changes within the scope of the present invention, they are included in the present invention. In addition, for example, when multiple configurations are included in each embodiment, it goes without saying that possible combinations of these configurations are included even if not specifically stated. In addition, when multiple examples or modified examples are disclosed as the present invention, it goes without saying that possible combinations of configurations across these are included even if not specifically stated. In addition, it goes without saying that the configurations depicted in the drawings are included even if not specifically stated. Furthermore, when the term "etc." is used, it is used to mean that equivalents are included. EXAMPLES

[0078] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0079] (Materials used) <Rail corrosion prevention sheet> Sheet 1: Reinforcement material = glass chopped strand mat, hardening resin = vinyl ester, basis weight: 2580g / m 2 Dimensions: Thickness 1.5 mm, length 400 mm, width 400 mm, DC insulation resistance value after curing = 4.6 x 10 14Ω, AC breakdown voltage after curing = 20 kV, DC breakdown voltage after curing = 15 kV, water permeability after curing = 0.15 g, chloride ion blocking property after curing = 0.7 × 10 -3 mg / cm 2 -day, oxygen barrier after curing = 0.01 mol / m 2 ·year. Sheet 2: Reinforcement material = glass chopped strand mat, hardening resin = polyester, basis weight: 2580g / m 2 Dimensions: Thickness 1.5 mm, length 400 mm, width 400 mm, DC insulation resistance value after curing = 4.6 x 10 14 Ω, AC breakdown voltage after curing = 20 kV, DC breakdown voltage after curing = 15 kV, water permeability after curing = 0.15 g, chloride ion blocking property after curing = 0.7 × 10 -3 mg / cm 2 -day, oxygen barrier after curing = 0.01 mol / m 2 ·year.

[0080] <Primer> - Urethane primer: Thinkbond Primer U-100 (product name), manufactured by Sekisui Chemical Co., Ltd. <Adhesive> Base material: Vinyl ester adhesive, Pasting Primer V200 (product name), manufactured by Sekisui Chemical Co., Ltd. Hardener: Mepox D (product name), manufactured by Sekisui Chemical Co., Ltd. The DC insulation resistance of the cured adhesive, which was a mixture of the base agent and the curing agent, was measured using the method described above. It was 1.3 × 10 16 It was Omega.

[0081] (Evaluation method) <Fatigue test> As shown in Fig. 6, a sleeper 220, a track pad 210, and a rail covering structure 30 were placed in this order on an H-beam 230. The rail covering structure 30 was fixed to the sleeper 220 with a rail fastening jig 200. Then, a load test was performed 10 million times on the center of the rail with a load of 5 to 100 kN in the vertical downward direction. After that, the appearance of the rail covering structure (bottom surface: surface in contact with the track pad 210, fastening jig part: surface in contact with the rail fastening jig 200 and its vicinity) was observed and evaluated according to the following criteria.

[0082] ≪Judgment criteria≫ ◎: No visible change in appearance. ○: Whitening was confirmed by visual inspection. ×: Lifting, peeling, or cracking was visually confirmed.

[0083] <Corrosion prevention effect> The test was conducted based on the salt spray test method of JIS Z 2371. The base material used was a 70mm square piece of SS400, and the surface was treated by attaching 3M's CNS Bevel Black for power tools #120 to a scraping device to polish the surface. Next, a primer was applied to the polished surface by a brush coating method. Next, the adhesive was applied by a brush coating method, and immediately thereafter, the prepreg sheet in Table 2 was attached while squeezing the adhesive out. Any excess adhesive from the prepreg sheet was lightly wiped off, and five test pieces were prepared. The test pieces were arranged in a salt spray device (CYP-90a: manufactured by Suga Test Instruments), and a salt solution (sodium chloride, concentration 5±0.5%, specific gravity: 1.029-1.036, pH: 6.5-7.2) prepared based on the neutral salt spray test method described in JIS Z 2371 4.2.1 was placed in the salt solution supply tank, after which salt spray was performed (spray: 35±1°C, spray rate: 1.5±0.5mL / hr). The state of surface corrosion was visually confirmed 1,000 hours after the salt water spray, with the state before the salt water spray being regarded as 0 hours. The state of the rail surface was evaluated according to the following criteria.

[0084] ≪Judgment criteria≫ ○: No corrosion was observed between the coating layer and the rail. △: Some corrosion was observed between the coating layer and the rail. ×: Corrosion was observed between the coating layer and the rail, and peeling of the coating layer was observed.

[0085] (Examples 1 to 2) Both sides of the rail web, the bottom surface of the rail base, and the top surface of the rail base were prepared with sandpaper to remove rust from these surfaces. Next, the rust particles on the surface of the rail were wiped off with a cloth soaked in acetone. Next, a urethane primer was applied to the bottom and the web of the rail and allowed to cure until no tack (stickiness) remained. Next, an adhesive mixture of a base agent and a hardener was applied to the bottom and the abdomen of the rail via a urethane primer. Next, a rail corrosion prevention sheet as shown in Table 1 was attached to the adhesive-coated surface of the bottom and the abdomen of the rail to obtain a rail covering structure of each example. When attaching the rail corrosion prevention sheet, the sheet was pressed against the rail to push out the adhesive between the rail and the sheet for preventing rail corrosion together with any air bubbles, thereby preventing any air bubbles from remaining between the rail and the sheet for preventing rail corrosion. Immediately after (0 min) the sheet for preventing rail corrosion was attached to the rail, and 5 min after the sheet for preventing rail corrosion was attached to the rail, it was visually confirmed that there was no lifting or peeling. After the rail corrosion prevention sheet was attached to the rail, natural light was irradiated (for 20 minutes) in an environment of 23°C to harden the prepreg and harden the adhesive, thereby obtaining the rail covering structure of each example. The rail coating structures obtained in each example were subjected to a fatigue test and an evaluation of the corrosion prevention effect, and the results are shown in the table.

[0086] Comparative Example 1 Instead of sheet 1, paint (epoxy paint) was applied to the rail, and the coating (weight = 110 g / m 2A rail coating structure was obtained in which the coating layer was 100%. The obtained rail coating structure was subjected to a fatigue test and evaluated for corrosion prevention effect, and the results are shown in the table.

[0087] Comparative Example 2 A rail covering structure was prepared by attaching tape 1 (masking tape, acrylic tape containing polyethylene cloth) to the rail instead of sheet 1. The obtained rail covering structure was subjected to a fatigue test and evaluated for corrosion prevention effect, and the results are shown in the table.

[0088] [Table 1]

[0089] As shown in Table 1, in Examples 1 and 2 in which the present invention was applied, the fatigue test results were: bottom surface = "A", fastening portion = "O", and corrosion prevention effect = "O". Comparative Example 1 in which the coating film was used as the covering layer and Comparative Example 2 in which Seal 1 was used as the covering layer were rated "X" in the fatigue test (fastening jig portion) and in the corrosion prevention effect. From these results, it was confirmed that application of the present invention can prevent corrosion and increase durability. [Explanation of symbols]

[0090] 10 Rail 13a Bottom 20 Covering layer 21, 22 Rail corrosion prevention sheet 30 Rail Covering Structure

Claims

1. A fiber-reinforced prepreg having a reinforcing member and a curable resin, In a cured state, the curable resin has a resistance of 5×10 6 A sheet for preventing rail corrosion with a resistance of Ω or more.

2. The rail corrosion prevention sheet according to claim 1, wherein the voltage measured by an AC breakdown voltage test of JIS C 2110-1:2016 in a cured state of the curable resin is 20 kV or more.

3. The rail corrosion prevention sheet according to claim 1, wherein the voltage measured by a DC breakdown voltage test of JIS C 2110-2:2016 in a cured state of the curable resin is 15 kV or more.

4. The rail corrosion prevention sheet according to claim 1, wherein the curable resin has a water permeability of 0.15 g or less as measured by a water permeability test for a corrosion-resistant coating layer in accordance with Annex F of JIS A 7502-2:2015 in a cured state.

5. In the cured state of the curable resin, the chloride ion blocking property measured according to the quality standard for surface protection work "medium corrosion protection type C" is 1.0 x 10 -3 mg / cm 2 The sheet for preventing rail corrosion according to claim 1, wherein the corrosion resistance is 50-150 days or less.

6. In the cured state, the curable resin has an oxygen barrier property of 1.00 mol / m as measured by the quality standard for surface protection work, "medium corrosion protection type C." 2 The sheet for preventing rail corrosion according to claim 1, wherein the sheet has a wear resistance of 1 year or less.

7. The rail corrosion prevention sheet according to claim 1 , wherein the reinforcing member includes glass fiber.

8. The rail corrosion prevention sheet according to claim 1 , wherein the curable resin includes a photocurable resin.

9. A rail and a coating layer covering at least a bottom surface of the rail, A rail covering structure, wherein the covering layer is a cured product of the rail corrosion prevention sheet according to any one of claims 1 to 8.

10. applying an adhesive to at least a bottom surface of the rail; A step of attaching the rail corrosion prevention sheet according to any one of claims 1 to 8 to the surface on which the adhesive is applied; A step of irradiating the rail corrosion prevention sheet with energy rays to harden the hardening resin of the fiber reinforced prepreg to form a coating layer; A method for manufacturing a rail covering structure comprising the steps of:

11. The adhesive has a resistance of 5×10 or less when the cured product of the adhesive is measured by a direct current insulation resistance test according to JIS E 1203:2007. 6 The method for manufacturing a rail covering structure according to claim 10, wherein the resistance of the rail covering structure is Ω or more.

Citation Information

Patent Citations

  • Rail protecting cover

    JP2010203096A