Method for decomposing thermosetting cured resin, method for producing phenolic compound, method for producing epoxy resin, and method for producing composite material

By mixing cured thermosetting resins with organic solvents and then alkali compounds, the decomposition process is accelerated, improving efficiency and yield of phenol compounds and inorganic substances, facilitating the production of epoxy resins and composite materials.

JP2024165140APending Publication Date: 2024-11-28MITSUBISHI CHEM CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023081042
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-16
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Conventional methods for decomposing cured thermosetting resins, such as epoxy resin, are inefficient and time-consuming, leading to prolonged decomposition times and reduced yield of valuable phenol compounds.

Method used

A method involving the sequential mixing of a thermosetting resin with an organic solvent followed by an alkali compound, which allows for the efficient decomposition of cured thermosetting resins into phenol compounds and inorganic substances, utilizing alkali metal compounds like sodium hydroxide for faster decomposition.

Benefits of technology

This method significantly reduces decomposition time and enhances the yield of phenol compounds, enabling the co-production of phenol compounds and inorganic substances like carbon fibers, with the potential to produce epoxy resins and composite materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024165140000001
    Figure 2024165140000001
  • Figure 2024165140000002
    Figure 2024165140000002
Patent Text Reader

Abstract

To provide a method for efficiently decomposing a thermosetting cured resin.SOLUTION: A method for decomposing a thermosetting cured resin includes: a first mixing step for mixing a thermosetting cured resin with an organic solvent to prepare a liquid mixture; a second mixing step following the first mixing step for mixing the liquid mixture with an alkali compound; and a decomposition step following the second mixing step for decomposing the thermosetting cured resin.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for decomposing a cured thermosetting resin, a method for producing a phenolic compound, a method for producing an epoxy resin, and a method for producing a composite material. [Background technology]

[0002] Thermosetting resins are used in various applications because they can be highly reinforced by blending fillers, additives, etc. Among them, epoxy resins are important materials used in various applications such as adhesives, insulating materials, paints, casting materials, and composite materials because they exhibit excellent adhesive properties, electrical properties, and heat resistance.

[0003] On the other hand, a cured thermosetting resin obtained by curing a thermosetting resin does not melt and is difficult to dissolve in a general-purpose solvent. This is because the cured thermosetting resin has a complex structure that is crosslinked three-dimensionally. Therefore, when chemically recycling a cured thermosetting resin, it is necessary to decompose and dissolve the cured thermosetting resin with a treatment liquid containing an alkaline compound or the like. For example, a method for decomposing and dissolving a cured thermosetting resin is known, as described in Patent Document 1. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2019-99734 A Summary of the Invention [Problem to be solved by the invention]

[0005] In a conventionally known method for decomposing a cured thermosetting resin, an organic solvent and an alkaline compound are first mixed to prepare a treatment liquid, and then the cured epoxy resin is decomposed and dissolved. However, such a decomposition method requires time for decomposition, and there is room for improvement in terms of efficiency. In addition, since the decomposition requires time, the generated phenol compounds are also decomposed, and therefore, this method is not an efficient method for producing phenol compounds.

[0006] Specifically, according to Patent Document 1, the decomposition time is as long as 10 hours, and therefore there is a problem with the decomposition conditions from the viewpoint of efficient recovery of phenol compounds.

[0007] The present invention has been made in view of the above circumstances. That is, an object of the present invention is to provide a method for decomposing a cured thermosetting resin material, which is an efficient decomposition method. [Means for solving the problem]

[0008] As a result of intensive research to solve the above problems, the present inventors have found that the thermosetting resin cured product can be efficiently decomposed by mixing the thermosetting resin cured product with an organic solvent and then supplying an alkaline compound. They have also found that the above method can be used to produce a phenolic compound. They have also found that the phenolic compound and the inorganic substance can be co-produced by using a thermosetting resin cured product containing an inorganic substance. They have also found a method for producing an epoxy resin from the obtained phenolic compound, and a method for producing a composite material from the epoxy resin and the inorganic substance recovered from the thermosetting resin cured product. That is, the present invention includes the following inventions.

[0009] [1] A method for decomposing a cured thermosetting resin, comprising the steps of: a first mixing step of mixing a cured thermosetting resin with an organic solvent to obtain a mixed liquid; a second mixing step of mixing the mixed solution with an alkaline compound after the first mixing step; and a decomposition step of decomposing the cured thermosetting resin material after the second mixing step. The decomposition method of the cured thermosetting resin, comprising the steps of: [2] The method for decomposing a cured thermosetting resin material according to [1], wherein the alkali compound is an alkali metal compound. [3] The method for decomposing a cured thermosetting resin material according to [2], wherein the alkali metal compound is at least one selected from the group consisting of alkali metal hydroxides, alkali metal phosphates, alkali metal carbonates, and metal alkoxides. [4] The method for decomposing a cured thermosetting resin according to any one of [1] to [3], wherein the cured thermosetting resin is a cured epoxy resin. [5] A method for producing a phenol compound from a cured thermosetting resin, comprising the steps of: The thermosetting resin cured product contains an inorganic substance, A step of decomposing the cured thermosetting resin by the method for decomposing the cured thermosetting resin according to [1], and The method for producing a phenol compound includes, after the decomposition step, an inorganic matter recovery step of recovering the inorganic matter. [6] The method for producing a phenol compound according to [5], wherein the inorganic material is one or more selected from the group consisting of carbon fiber and glass fiber. [7] The method for producing a phenol compound according to [5] or [6], wherein the epoxy resin cured product is a phenol-type epoxy resin cured product. [8] The method for producing a phenol compound according to any one of [5] to [7], wherein the phenol compound is a bisphenol. [9] A method for producing an epoxy resin, comprising a reaction step of reacting a phenol compound obtained by the method for producing a phenol compound according to any one of [5] to [8] with epihalohydrin.

[10] A method for producing a composite material, comprising a step of curing an epoxy resin composition containing an epoxy resin obtained by the method for producing an epoxy resin according to [9] and the inorganic substance obtained by the method for producing a phenol compound according to any one of [5] to [8]. Effect of the Invention

[0010] According to the present invention, it is possible to provide an efficient method for decomposing a cured thermosetting resin material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The following is a detailed description of the embodiments of the present invention, but the present invention is not limited to the following description, and can be modified as desired without departing from the scope of the present invention. In addition, in this specification, when a numerical value or physical property value is enclosed before and after "~", the values ​​before and after the "~" are included.

[0012] 1. Method for decomposing cured thermosetting resin A first embodiment of the present invention is a method for decomposing a cured thermosetting resin material, the method including: a first mixing step of mixing a cured thermosetting resin material with an organic solvent to obtain a mixed liquid; a second mixing step of mixing the mixed liquid with an alkali compound after the first mixing step; and a decomposition step of decomposing the cured thermosetting resin material after the second mixing step.

[0013] 1-1. First mixing process The first mixing step is a step of mixing a cured thermosetting resin with an organic solvent to obtain a mixed liquid. The method of mixing the cured thermosetting resin with an organic solvent is not particularly limited, and examples thereof include a method of immersing the cured thermosetting resin in an organic solvent.

[0014] In the first mixing step, there is no need to perform heating, and the mixed liquid can be prepared by mixing the cured thermosetting resin and the organic solvent at room temperature of about 5° C. or higher and 35° C. or lower.

[0015] 1-2. Second mixing process The second mixing step is a step of mixing the mixed liquid with an alkaline compound after the first mixing step. In a conventionally known method for decomposing a cured thermosetting resin material, an organic solvent and an alkaline compound are first mixed to prepare a treatment liquid, and then the cured epoxy resin material is decomposed and dissolved. However, the present inventors have found that, by setting the timing of supplying the alkaline compound after mixing the cured thermosetting resin material with the organic solvent as in the present embodiment, the cured thermosetting resin material can be sufficiently decomposed in a shorter time than in the conventional method. The reason for this is unclear, but the present inventors speculate as follows. First, it is speculated that when a cured thermosetting resin is mixed with an organic solvent, the cured thermosetting resin swells and softens due to the organic solvent, making it easier to decompose, and thus improving the decomposition efficiency. On the other hand, it is speculated that when a treatment liquid is first prepared by mixing an organic solvent with an alkaline compound, and then the cured thermosetting resin is mixed, the presence of the alkaline compound inhibits the swelling and softening of the cured thermosetting resin, and thus the decomposition efficiency does not improve.

[0016] In the second mixing step, the alkaline compound may be mixed with the mixed liquid in a solid state or in a solution state. When mixing the alkaline compound with the mixed liquid, the mixed liquid may or may not be heated. When the mixed liquid is heated, the temperature of the mixed liquid is preferably 80° C. or higher, more preferably 100° C. or higher, and even more preferably 120° C. or higher, from the viewpoint of the temperature decrease due to the latent heat of volatile components (e.g., water and alcohol) generated when the alkaline compound is supplied. On the other hand, this temperature is preferably 300° C. or lower, more preferably 260° C. or lower, and even more preferably 220° C. or lower, from the viewpoint of the boiling point of the organic solvent.

[0017] 1-3. Decomposition process The decomposition step is a step of decomposing the cured thermosetting resin contained in the mixed liquid after the second mixing step. The method of decomposing the cured thermosetting resin is not particularly limited, and a known decomposition method or a decomposition method similar to a known decomposition method can be appropriately adopted. Specifically, a method of heating the mixed liquid after the second mixing step (hereinafter also referred to as a treatment liquid) to decompose the cured thermosetting resin is suitable.

[0018] The reaction vessel is not particularly limited as long as it is capable of contacting the treatment liquid with the cured thermosetting resin material. As long as the vessel can be used as a decomposition tank, it may be box-shaped, cylindrical, mesh-like cage-shaped, or made of a porous material. The ratio of the volume of the thermosetting resin placed in the container to the volume of the container (filling rate) is From the viewpoint of dissolution efficiency, it is preferably within the range of 5% or more and 25% or less.

[0019] From the viewpoint of improving the decomposition efficiency of the cured thermosetting resin material, the temperature of the treatment liquid in the decomposition step is preferably 100° C. or higher, more preferably 130° C. or higher, and even more preferably 150° C. or higher. On the other hand, from the viewpoint of suppressing the denaturation of the treatment liquid and the decomposition products, this temperature is preferably 300° C. or lower, more preferably 250° C. or lower, and even more preferably 200° C. or lower.

[0020] The contact time between the treatment liquid and the cured thermosetting resin may be a time sufficient for the cured thermosetting resin to be sufficiently decomposed and dissolved, and varies depending on the type of thermosetting resin, the type and concentration of the decomposer and organic solvent, and the treatment temperature, but is preferably 0.5 hours or more and 8 hours or less.

[0021] The alkali compound is preferably an alkali metal compound. Examples of the alkali metal compound include metal compounds such as metal hydrides, metal hydroxides, metal borohydrides, metal carbonates, and metal alkoxides. Of these, the alkali compound is preferably one or more selected from the group consisting of alkali metal hydroxides, alkali metal phosphates, alkali metal carbonates, and metal alkoxides, and is more preferably a metal alkoxide. In addition, examples of the metal in the alkali compound include alkali metals such as lithium, sodium, and potassium, and is preferably at least one of sodium and potassium, and is more preferably sodium. Therefore, the alkali compound is preferably one or more selected from the group consisting of sodium compounds and potassium compounds, and is more preferably one or more selected from the group consisting of sodium hydroxide, potassium hydroxide, sodium alkoxide, and potassium alkoxide, and is even more preferably sodium alkoxide.

[0022] Among the above compounds, the alkali compound is preferably a metal alkoxide. A metal alkoxide is a compound in which the hydrogen atom of a hydroxyl group of an alcohol is substituted with a metal, and can be obtained by adding a metal to an alcohol.

[0023] The alcohol used to obtain the metal alkoxide is not particularly limited, and examples thereof include methanol, ethanol, 1-butanol, 2-butanol, 2-methyl-1-propanol, 2-methyl-2-propanol, 1-pentanol, 2-pentanol, 3-pentanol, 2-methyl-1-butanol, 2-methyl-2-butanol, 3-methyl-1-butanol, 3-methyl-2-butanol, 2,2-dimethyl-1-propanol, 1-hexanol, 2-Hexanol, 3-Hexanol, 2-Methyl-1-pentanol, 4-Methyl-2-pentanol, 2-Ethyl-1-butanol, 1-Heptanol, 2-Heptanol, 3-Heptanol, 2-Ethylhexanol, Dodecanol, Cyclohexanol, 1-Methylcyclohexanol, 2-Methylcyclohexanol, 3-Methylcyclohexanol, 4-Methylcyclohexanol, Benzyl alcohol, Phenoxyethanol, 1-(2-Hydroxyethyl) Examples of suitable alcohols include (2-methoxyethyl)-2-pyrrolidone, diacetone alcohol, ethylene glycol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monobutyl ether, diethylene glycol, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monopropyl ether, diethylene glycol monobutyl ether, triethylene glycol, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, tetraethylene glycol, polyethylene glycol (molecular weight 200 to 400), 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, 1,5-pentanediol, glycerin, and dipropylene glycol. These alcohols may be used alone. Two or more of them may be used in any combination and in any ratio.

[0024] The metal alkoxide may be in a solid state or a solution state. From the viewpoint of the decomposition efficiency of the thermosetting resin cured material B, the metal alkoxide is preferably at least one selected from the group consisting of sodium methoxide, sodium ethoxide, sodium propoxide, sodium isopropoxide, sodium benzyl alkoxide (sodium benzyl oxide), potassium methoxide, potassium ethoxide, potassium propoxide, isopropoxide, and potassium benzyl alkoxide (potassium benzyl oxide).

[0025] The alkaline compounds may be used alone or as a mixture of two or more kinds in any combination and in any ratio.

[0026] 1-4. Thermosetting resin cured product The thermosetting resin cured product according to the present embodiment is obtained by curing a thermosetting resin in the presence or absence of a curing accelerator, without using a curing agent or using a curing agent, and preferably by curing a thermosetting resin using a curing agent. In addition, the thermosetting resin cured product preferably has a structure derived from a phenol compound in its structure (e.g., a structural unit, a terminal structure, a crosslinked structure, etc.).

[0027] The thermosetting resin is not particularly limited, but preferably includes, for example, a copolymer of a phenolic compound and another monomer, a homopolymer of an epoxidized product of a phenolic compound, and a copolymer of an epoxidized product of a phenolic compound and another monomer. Such thermosetting resins include, for example, epoxy resins and phenolic resins. Among them, the thermosetting resin cured product is preferably an epoxy resin cured product, and is particularly preferably a phenol-type epoxy resin cured product.

[0028] The phenol compound is not particularly limited, and may be, for example, a monohydric phenol compound, a dihydric phenol compound, a bisphenol compound, or the like.

[0029] Examples of monovalent phenolic compounds include phenol, o-cresol, m-cresol, p-cresol, p-ethylphenol, p-isopropylphenol, p-tert-butylphenol, p-cumylphenol, p-cyclohexylphenol, p-octylphenol, p-nonylphenol, 2,4-xylenol, p-methoxyphenol, p-hexyloxyphenol, p-decyloxyphenol, o-chlorophenol, m-chlorophenol, p-chlorophenol, p-bromophenol, pentabromophenol, and penta Examples of such phenols include chlorophenol, o-nitrophenol, m-nitrophenol, p-nitrophenol, 2,4,6-trinitrophenol, o-phenolsulfonic acid, m-phenolsulfonic acid, p-phenolsulfonic acid, p-phenylphenol, p-isopropenylphenol, 2,4-di(1'-methyl-1'-phenylethyl)phenol, β-naphthol, α-naphthol, p-(2',4',4'-trimethylchromanyl)phenol, and 2-(4'-methoxyphenyl)-2-(4''-hydroxyphenyl)propane.

[0030] Examples of the divalent phenol compound include hydroquinone, resorcinol, and 2-methylresorcinol.

[0031] Examples of bisphenol compounds include 2,2'-biphenol, 4,4'-biphenol, 1,5-naphthalenediol, 2,7-naphthalenediol, bis(4-hydroxyphenyl)methane (i.e., bisphenol F), bis{(4-hydroxy-3,5-dimethyl)phenyl}methane, 1,1-bis(4-hydroxyphenyl)ethane (s Bisphenol E), 1,1-bis(4-hydroxyphenyl)-1-phenylethane (i.e., bisphenol AP), 2,2-bis(4-hydroxyphenyl)hexafluoropropane (i.e., bisphenol AF), 2,2-bis(4-hydroxyphenyl)propane (i.e., bisphenol A), 2,2-bis{(4-hydroxy-3-methyl)phenyl}propane, 2,2-bis{(4-hydroxy-3,5-dimethyl)phenyl}propane, 2,2-bis{(3,5-dibromo-4-hydroxy)phenyl}propane, 2,2-bis{(3-isopropyl-4-hydroxy)phenyl}propane, 2,2-bis{(4-hydroxy-3-phenyl)phenyl}propane, 2-(4-hydroxyphenyl)-2-(3-carboxy-4-hydroxyphenyl)propane, 2-(2-hydroxyphenyl)-2-(4-hydroxyphenyl)propane, 1-(4-hydroxyphenyl)-1,3,3-trimethyl-5-hydroxyindan, 2-(4-hydroxyphenyl)-[3-{2-(4-hydroxyphenyl)propan-2-yl}-4-hydroxyphenyl bisphenol B), 1,1-bis(4-hydroxyphenyl)-1,1-diphenylmethane (i.e., bisphenol BP), 4,4′-isopropylidenebis(2-methylphenol) (i.e., bisphenol C), 2,2-bis(4-hydroxy-3-isopropylphenyl)propane (i.e., bisphenol G), 2,2-bis(4-hydroxyphenyl)-3-methylbutane, 2,2-bis(4-hydroxyphenyl)-3,3-dimethylbutane , 2,4-bis(4-hydroxyphenyl)-2-methylbutane, 2,2-bis(4-hydroxyphenyl)pentane, 2,2-bis(4-hydroxyphenyl)-4-methylpentane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)-4-isopropylcyclohexane, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, 9,9-bis(4-hydroxyphenyl)fluorene, 9,9-bis{(4-hydroxy-3-methyl)phenyl}fluorene, α,Examples of the hydroxydiphenyl ether include α'-bis(4-hydroxyphenyl)-o-diisopropylbenzene, α,α'-bis(4-hydroxyphenyl)-m-diisopropylbenzene, α,α'-bis(4-hydroxyphenyl)-p-diisopropylbenzene, 1,3-bis(4-hydroxyphenyl)-5,7-dimethyladamantane, 4,4'-dihydroxydiphenyl sulfone (i.e., bisphenol S), 4,4'-dihydroxydiphenyl sulfoxide, 4,4'-dihydroxydiphenyl sulfide, 4,4'-dihydroxydiphenyl ketone, 4,4'-dihydroxydiphenyl ether, and 4,4'-dihydroxydiphenyl ester.

[0032] Of these, the phenol compound is preferably a bisphenol compound, more preferably selected from 2,2-bis(4-hydroxyphenyl)propane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, 2,2-bis(4-hydroxyphenyl)hexafluoropropane, 2,2-bis(4-hydroxyphenyl)butane, 1,1-bis(4-hydroxyphenyl)-1,1-diphenylmethane, 4,4'-isopropylidenebis(2-methyl-phenol), 1,1-bis(4-hydroxyphenyl)ethane, bis(4-hydroxyphenyl)methane, 2,2-bis(4-hydroxy-3-isopropylphenyl), and 4,4'-dihydroxydiphenylsulfone, and even more preferably 2,2-bis(4-hydroxyphenyl)propane.

[0033] The epoxy resin is not particularly limited, and examples thereof include diglycidyl ethers of the above bisphenol compounds; bisphenol type epoxy resins such as bisphenol A type epoxy resins, bisphenol F type epoxy resins, and bisphenol S type epoxy resins; novolac epoxy resins such as phenol novolac type epoxy resins, cresol novolac type epoxy resins, and bisphenol A novolac type epoxy resins; biphenyl type epoxy resins; glycidyl ester type epoxy resins; glycidyl amine type epoxy resins; linear aliphatic epoxy resins; alicyclic epoxy resins; heterocyclic epoxy resins; and alkyl substituted, halogenated and hydrogenated products thereof.

[0034] In the technical field of the present invention, "epoxy resin" includes polymers containing repeating units and epoxy compounds with a monomolecular structure (i.e., non-polymer compounds), both of which are sometimes expressed and sold as "epoxy resins". A mixture of two or more epoxy resins may also be simply called "epoxy resin". In this specification, "epoxy resin" refers to any of polymers containing repeating units, epoxy compounds with a monomolecular structure, and mixtures thereof.

[0035] The cured thermosetting resin may be a cured product of one type of thermosetting resin, or a cured product of a mixture of two or more types of thermosetting resins in any combination and ratio.

[0036] In this specification, a curing agent means a substance that contributes to the crosslinking reaction and / or chain extension reaction of a thermosetting resin. Even substances that are usually called "curing accelerators" are considered to be curing agents as long as they contribute to the crosslinking reaction and / or chain extension reaction of a thermosetting resin.

[0037] Examples of the curing agent for the thermosetting resin include phenol-based curing agents, polyisocyanate-based curing agents, amine-based curing agents, acid anhydride-based curing agents, imidazole-based curing agents, amide-based curing agents, mercaptan-based curing agents, cationic polymerization initiators, organic phosphine-based curing agents, phosphonium salt-based curing agents, and tetraphenyl boronate-based curing agents. Of these, the curing agent is preferably an acid anhydride-based curing agent. When the thermosetting resin is an epoxy resin, the curing agent is particularly preferably an acid anhydride-based curing agent, and therefore, the thermosetting resin curing agent is particularly preferably an epoxy resin cured by an acid anhydride-based curing agent.

[0038] Examples of phenol-based curing agents include bisphenols such as bisphenol A, bisphenol F, bisphenol S, bisphenol B, bisphenol AD, bisphenol Z, and tetrabromobisphenol A; biphenols such as 4,4'-biphenol and 3,3',5,5'-tetramethyl-4,4'-biphenol; benzenediols such as catechol, resorcin, and hydroquinone; and polyfunctional phenols such as naphthalenediols. The hydrogen atoms bonded to the aromatic rings of these compounds may be substituted with non-interfering substituents, such as halogeno groups, alkyl groups, aryl groups, ether groups, ester groups, sulfur, phosphorus, and organic substituents containing heteroelements such as silicon. In this specification, "benzenediols" refers to compounds having one benzene ring and two hydroxyl groups directly bonded to this benzene ring.

[0039] The phenol-based curing agent may be novolak resins and resol resins which are polycondensates of the above-mentioned polyfunctional phenols and aldehydes, and novolak resins and resol resins which are polycondensates of monofunctional phenols such as phenol, cresol, and alkylphenol and aldehydes.

[0040] Examples of polyisocyanate-based curing agents include tolylene diisocyanate, methylcyclohexane diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate, xylylene diisocyanate, hydrogenated xylylene diisocyanate, dimer acid diisocyanate, trimethylhexamethylene diisocyanate, and lysine triisocyanate.

[0041] The polyisocyanate-based curing agent is a compound having the above polyisocyanate compound and an amino group and a hydroxyl group. , polyisocyanate compounds obtained by reacting a carboxyl group with a compound having at least two active hydrogen atoms such as water; and trimers to pentamers of the above-mentioned polyisocyanate compounds.

[0042] Examples of the amine-based curing agent include aliphatic primary amines, aliphatic secondary amines, aliphatic tertiary amines, aromatic primary amines, aromatic secondary amines, aromatic tertiary amines, cyclic amines, guanidines, and urea derivatives. More specific examples of the amine-based curing agent include triethylenetetramine, diaminodiphenylmethane, diaminodiphenylether, metaxylenediamine, dicyandiamide (DICY), 1,8-diazabicyclo(5,4,0)-7-undecene, 1,5-diazabicyclo(4,3,0)-5-nonene, dimethylurea, and guanylurea.

[0043] Examples of acid anhydride curing agents include condensates of maleic anhydride and unsaturated compounds, phthalic anhydride, 4-methylhexahydrophthalic anhydride, hexahydrophthalic anhydride, and trimellitic anhydride.

[0044] Examples of imidazole-based curing agents include 1-isobutyl-2-methylimidazole, 2-methylimidazole, 1-benzyl-2-methylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, and benzimidazole. Although imidazole-based curing agents also function as curing accelerators, they are classified as curing agents in this embodiment.

[0045] Examples of the amide-based curing agent include polyamide resins.

[0046] Examples of the mercaptan curing agent include polysulfide type mercaptan compounds, thioester type mercaptan compounds, and thioether type mercaptan compounds.

[0047] The cationic polymerization initiator generates cations by heat or irradiation with active energy rays, and examples of the initiator include aromatic onium salts. Specifically, SbF 6- , B.F. 4 -, AsF 6- , P.F. 6- , C.F.3 SO 3 2 - and B(C 6 F 5 ) 4- and an aromatic cation component containing an atom selected from iodine, sulfur, nitrogen, and phosphorus. The aromatic onium salt is preferably one or more salts selected from the group consisting of diaryliodonium salts and triarylsulfonium salts.

[0048] Examples of the organic phosphine curing agent include tributylphosphine, methyldiphenylphosphine, triphenylphosphine, diphenylphosphine, and phenylphosphine.

[0049] Examples of phosphonium salt curing agents include tetraphenylphosphonium tetraphenylborate, tetraphenylphosphonium ethyltriphenylborate, and tetrabutylphosphonium tetrabutylborate.

[0050] Examples of the tetraphenylborate-based curing agent include 2-ethyl-4-methylimidazole·tetraphenylborate, and N-methylmorpholine·tetraphenylborate.

[0051] The curing agent may be used alone or as a mixture of two or more kinds in any combination and in any ratio.

[0052] The thermosetting resin cured product may be a product obtained by curing a thermosetting resin using a curing accelerator. The curing accelerator is not particularly limited, and known curing accelerators for epoxy resins, such as urea compounds such as 3-(3,4-dichlorophenyl)-1,1-dimethylurea (DCMU), alkali metal compounds, imidazole compounds, tertiary amine compounds, quaternary ammonium salts, and organic phosphorus compounds, can be used. The curing accelerator may be used alone or as a mixture of two or more kinds in any combination and in any ratio.

[0053] The cured thermosetting resin may be mixed with other components to form a composite material, as long as the effects of the present invention are not impaired. Examples of the other components include inorganic substances and thermoplastic resins. The other components may be used alone or as a mixture of two or more kinds in any combination and ratio.

[0054] The inorganic substance is not particularly limited, but examples thereof include carbon, glass, metal, and metal compounds such as fused silica, crystalline silica, alumina, calcium carbonate, calcium sulfate, talc, and boron nitride. The inorganic substance may be in the form of fiber, particle, foil, etc., and is preferably fiber. Among these, the inorganic substance is preferably one or more types selected from the group consisting of carbon fiber and glass fiber, and more preferably carbon fiber.

[0055] The fibers may be in the form of a nonwoven fabric or a woven fabric. If in the form of a woven fabric, it may be a cross material made by weaving fiber bundles, or a UD (Uni-Directional) material in which fiber bundles are arranged in one direction.

[0056] Examples of the thermoplastic resin include polyethylene and polypropylene.

[0057] 1-5. Organic Solvents The organic solvent is not particularly limited, and examples thereof include alcohol-based solvents, ether-based solvents, aromatic solvents, etc. Among these, the organic solvent is preferably an alcohol-based solvent because it has excellent solubility for decomposition products of the cured thermosetting resin. The organic solvent may be used alone or as a mixture of two or more kinds in any combination and in any ratio.

[0058] Examples of alcohol-based solvents include 1-butanol, 2-butanol, 2-methyl-1-propanol, 2-methyl-2-propanol, 1-pentanol, 2-pentanol, 3-pentanol, 2-methyl-1-butanol, 2-methyl-2-butanol, 3-methyl-1-butanol, 3-methyl-2-butanol, 2,2-dimethyl-1-propanol, 1-hexanol, 2-hexanol, 3-hexanol, 2-methyl-1- Examples of the alcohol include pentanol, 4-methyl-2-pentanol, 2-ethyl-1-butanol, 1-heptanol, 2-heptanol, 3-heptanol, 2-ethylhexanol, dodecanol, cyclohexanol, 1-methylcyclohexanol, 2-methylcyclohexanol, 3-methylcyclohexanol, 4-methylcyclohexanol, benzyl alcohol, and phenoxyethanol, and benzyl alcohol is preferred.

[0059] Examples of ether solvents include diethyl ether, dipropyl ether, dibutyl ether, butyl methyl ether, butyl ethyl ether, diisoamyl ether, hexyl methyl ether, octyl methyl ether, cyclopentyl methyl ether, and dicyclopentyl ether.

[0060] Examples of aromatic solvents include benzene, toluene, xylene, alkylbenzenes such as trimethylbenzene and ethylbenzene, and alkylnaphthalenes such as methylnaphthalene, ethylnaphthalene, and dimethylnaphthalene.

[0061] Since the decomposition of the cured thermosetting resin is preferably carried out under normal heating conditions, the boiling point of the organic solvent under atmospheric pressure is preferably 100°C or higher, more preferably 120°C or higher, and even more preferably 150°C or higher. From this viewpoint, benzyl alcohol (boiling point: 205° C.) is a preferred organic solvent.

[0062] The treatment liquid may further contain other components as necessary, such as a surfactant and a low-viscosity solvent.

[0063] From the viewpoint of improving the decomposition efficiency of the cured thermosetting resin material, the concentration of the alkaline compound in the treatment liquid is preferably 0.001 mol / L or more and 100 mol / L or less, more preferably 0.005 mol / L or more and 50 mol / L or less, and even more preferably 0.01 mol / L or more and 20 mol / L or less. By setting the concentration of the alkaline compound to the above lower limit or more, the cured thermosetting resin material can be efficiently decomposed. By setting the concentration of the alkaline compound to the above upper limit or less, the cured thermosetting resin material can be decomposed without increasing the viscosity of the treatment liquid.

[0064] 2. Method for producing phenolic compounds The second embodiment of the present invention is a method for producing a phenolic compound from a cured thermosetting resin, the cured thermosetting resin containing an inorganic substance, the method including a step of decomposing the cured thermosetting resin using the method for decomposing a cured thermosetting resin according to the first embodiment, and an inorganic substance recovery step of recovering the inorganic substance after the decomposition step. The phenolic compound produced by the production method according to this embodiment is a compound derived from a monomer, a curing agent, an end-capping agent, etc. of a thermosetting resin. The phenolic compound produced by the production method according to this embodiment is preferably a bisphenol. Examples of the inorganic substance include the inorganic substances explained in the above section "1-4. Cured thermosetting resin".

[0065] 2-1. Inorganic matter recovery process The manufacturing method of this embodiment includes an inorganic substance recovery process in which the phenol compound or its salt and the inorganic substance are separated after the decomposition process of the first embodiment and the inorganic substance is recovered, thereby making it possible to obtain each of the phenol compound of the second embodiment and the inorganic substance of this embodiment.

[0066] The method for recovering the inorganic substances is not particularly limited, and can be carried out by a known separation method such as filtration, sedimentation separation, stretching separation, etc. The recovered inorganic substances can be recycled.

[0067] 3. Epoxy resin manufacturing method The third embodiment of the present invention is a method for producing an epoxy resin, which includes a reaction step of reacting the phenol compound obtained by the production method according to the second embodiment of the present invention with epihalohydrin. Since the production method according to this embodiment uses, as a raw material, a phenol compound obtained by decomposing a cured thermosetting resin, hereinafter, the epoxy resin produced by the production method according to this embodiment may be referred to as a "recycled epoxy resin."

[0068] In the reaction step, the recycled epoxy resin is produced by a known one-step method for producing recycled epoxy resin or a method similar thereto. This is a method for obtaining a recycled epoxy resin by reacting a raw hydroxy compound with epihalohydrin. In this embodiment, the raw hydroxy compound contains a phenol compound obtained by the production method according to the second embodiment of the present invention, and may contain a polyhydric hydroxy compound (hereinafter, sometimes referred to as a "polyhydric hydroxy compound") as necessary.

[0069] The term "polyhydric hydroxy compound" is a general term for dihydric or higher phenol compounds and dihydric or higher alcohol compounds, and may be the same compound as the phenol compound obtained by the production method according to the first embodiment of the present invention. In the one-stage method for producing recycled epoxy resin, the "hydroxy compound raw material" is the total hydroxy compound including the phenol compound obtained by the production method according to the second embodiment of the present invention and the polyhydric hydroxy compound used as needed.

[0070] Examples of polyhydric hydroxy compounds include various polyhydric phenols such as bisphenol A, tetramethyl bisphenol A, bisphenol F, tetramethyl bisphenol F, bisphenol S, bisphenol C, bisphenol AD, bisphenol AF, hydroquinone, resorcin, methyl resorcin, biphenol, tetramethyl biphenol, dihydroxynaphthalene, dihydroxydiphenyl ether, thiodiphenols, phenol novolac resins, cresol novolac resins, phenol aralkyl resins, biphenyl aralkyl resins, naphthol aralkyl resins, terpene phenol resins, dicyclopentadiene phenol resins, bisphenol A novolac resins, naphthol novolac resins, brominated bisphenol A, and brominated phenol novolac resins; various phenols and benzaldehyde, hydroxybenzaldehyde, etc. polyhydric phenol resins obtained by a condensation reaction of xylene resin with phenols; various phenol resins such as co-condensation resins of heavy oils or pitches with phenols and formaldehydes; chain aliphatic diols such as ethylene glycol, trimethylene glycol, propylene glycol, 1,3-butanediol, 1,4-butanediol, 1,3-pentanediol, 1,4-pentanediol, 1,5-pentanediol, and 1,6-hexanediol; cyclic aliphatic diols such as cyclohexanediol and cyclodecanediol; and polyalkylene ether glycols such as polyethylene ether glycol, polyoxytrimethylene ether glycol, and polypropylene ether glycol.

[0071] In the reaction step, a phenol compound and a polyhydric hydroxy compound are dissolved in epihalohydrin to form a homogeneous solution, and the reaction is allowed to proceed.

[0072] Examples of epihalohydrin include epichlorohydrin, β-methylepichlorohydrin, epibromohydrin, etc. Among these, epihalohydrin is particularly preferably epichlorohydrin from the viewpoints of reactivity, availability of raw materials, and versatility of the resulting epoxy resin. The epihalohydrin may be used alone or in any combination of two or more kinds in any ratio.

[0073] The amount of epihalohydrin used is usually 1.0 equivalent or more and 14.0 equivalent or less, and preferably 2.0 equivalent or more and 10.0 equivalent or less, per equivalent of the total hydroxyl group of the hydroxy compound raw material (total hydroxy compounds). By setting the amount of epihalohydrin to the above lower limit or more, it is easy to control the polymerizing reaction, and the obtained recycled epoxy resin can have an appropriate epoxy equivalent. In addition, by setting the amount of epihalohydrin to the above upper limit or less, production efficiency tends to be improved.

[0074] Next, while stirring the solution, an alkali metal hydroxide is added in an amount of preferably 0.1 to 3.0 equivalents, more preferably 0.8 to 2.0 equivalents per equivalent of the total hydroxyl groups of the hydroxy compound raw material, in the form of a solid or aqueous solution, to react. By setting the amount of alkali metal hydroxide to the above lower limit or more, the unreacted hydroxyl groups and the generated epoxy resin are less likely to react, and therefore the polymerizing reaction can be easily controlled. In addition, by setting the amount of alkali metal hydroxide to the above upper limit or less, the generation of impurities due to side reactions can be suppressed. Examples of alkali metal hydroxides include sodium hydroxide and potassium hydroxide.

[0075] The reaction can be carried out under normal pressure or under reduced pressure. The reaction temperature is preferably 20° C. or higher and 200° C. or lower, more preferably 40° C. or higher and 150° C. or lower. By setting the reaction temperature to the above lower limit or higher, the reaction can be easily progressed and controlled. In addition, by setting the reaction temperature to the above upper limit or lower, side reactions can be suppressed and the amount of by-products can be reduced.

[0076] The reaction is carried out while dehydrating the reaction liquid by azeotroping while maintaining a predetermined temperature as necessary, cooling the volatilized steam, separating the condensate obtained, and returning the oil content without moisture to the reaction system. In order to suppress a rapid reaction, the alkali metal hydroxide is added intermittently or continuously in small amounts over a period of preferably 0.1 to 24 hours, more preferably 0.5 to 10 hours. By setting the addition time of the alkali metal hydroxide to the above lower limit or more, the reaction can be prevented from proceeding rapidly, making it easier to control the reaction temperature. In addition, by setting the addition time of the alkali metal hydroxide to the above upper limit or less, the amount of by-products can be reduced.

[0077] The reaction may be carried out in the presence of a catalyst, such as quaternary ammonium salts, such as tetramethylammonium chloride and tetraethylammonium bromide; tertiary amines, such as benzyldimethylamine and 2,4,6-tris(dimethylaminomethyl)phenol; imidazoles, such as 2-ethyl-4-methylimidazole and 2-phenylimidazole; phosphonium salts, such as ethyltriphenylphosphonium iodide; and phosphines, such as triphenylphosphine.

[0078] The reaction may be carried out in an inert organic solvent, such as alcohols, such as ethanol and isopropanol; ketones, such as acetone, methyl ethyl ketone, and methyl isobutyl ketone; ethers, such as dioxane and ethylene glycol dimethyl ether; glycol ethers, such as methoxypropanol; and aprotic polar solvents, such as dimethylsulfoxide and dimethylformamide.

[0079] After the reaction is completed, a typical post-treatment in the field of organic synthesis may be carried out, such as removing insoluble by-product salts by filtration or washing with water, followed by distilling off unreacted epihalohydrin by heating and / or distillation under reduced pressure.

[0080] 4. Manufacturing method of composite materials A fourth embodiment of the present invention is a method for producing a composite material, comprising a curing step of curing an epoxy resin composition containing recycled epoxy resin obtained by the production method according to the third embodiment of the present invention and inorganic matter recovered in the inorganic matter recovery step of the production method according to the second embodiment of the present invention (hereinafter sometimes referred to as "recycled inorganic matter").

[0081] In this embodiment, the epoxy resin composition may contain, as necessary, an epoxy resin other than the recycled epoxy resin obtained by the production method according to the third embodiment of the present invention, a curing agent, a curing accelerator, a release agent, a coupling agent, and the like.

[0082] 4-1. Recycled epoxy resin The content of the recycled epoxy resin in the epoxy resin composition is not particularly limited, but the content of the recycled epoxy resin relative to 100 parts by mass of the total epoxy resin components is preferably 40 parts by mass or more, and more preferably 60 parts by mass or more, from the viewpoint of environmental harmony. When the epoxy resin composition contains other epoxy resins, the content of the recycled epoxy resin in 100 parts by mass of the total epoxy resin components is preferably 40 parts by mass or more and 99 parts by mass or less, and more preferably 60 parts by mass or more and 99 parts by mass or less. Note that the "total epoxy resin components" corresponds to the amount of all epoxy resins contained in the epoxy resin composition, and is the total of the recycled epoxy resin and other epoxy resins used as necessary.

[0083] 4-2.Other epoxy resins The epoxy resin composition may further contain other epoxy resins (hereinafter, sometimes referred to as "other epoxy resins") in addition to the recycled epoxy resin obtained by the manufacturing method according to the third embodiment of the present invention. By containing other epoxy resins, various physical properties can be improved.

[0084] The other epoxy resin corresponds to all epoxy resins other than the recycled epoxy resin obtained by the production method according to the third embodiment of the present invention, and may be the same type of epoxy resin as the recycled epoxy resin. The other epoxy resins may be used alone or in any combination of two or more in any ratio.

[0085] Other epoxy resins include, for example, bisphenol A type epoxy resins, bisphenol C type epoxy resins, trisphenolmethane type epoxy resins, anthracene type epoxy resins, phenol-modified xylene resin type epoxy resins, bisphenol cyclododecyl type epoxy resins, bisphenol diisopropylidene resorcin type epoxy resins, bisphenol F type epoxy resins, bisphenol AD ​​type epoxy resins, bisphenol AF type epoxy resins, hydroquinone type epoxy resins, methyl hydroquinone type epoxy resins, dibutyl hydroquinone type epoxy resins, resorcin type epoxy resins, methyl resorcin type epoxy resins, biphenol type epoxy resins, tetramethyl biphenol type epoxy resins, tetramethyl bisphenol F type epoxy resins, dihydroxy diphenyl ether type epoxy resins, epoxy resins derived from thiodiphenols, dihydroxy naphthalene type epoxy resins, dihydroxy anthracene type epoxy resins, dihydroxy dihydro anthracene type epoxy resins, dicyclopentadiene type epoxy resins, Examples of epoxy resins include epoxy resins derived from dihydroxystilbenes, phenol novolac type epoxy resins, cresol novolac type epoxy resins, bisphenol A novolac type epoxy resins, naphthol novolac type epoxy resins, phenol aralkyl type epoxy resins, naphthol aralkyl type epoxy resins, biphenyl aralkyl type epoxy resins, terpene phenol type epoxy resins, dicyclopentadiene phenol type epoxy resins, epoxy resins derived from a condensate of phenol and hydroxybenzaldehyde, epoxy resins derived from a condensate of phenol and crotonaldehyde, epoxy resins derived from a condensate of phenol and glyoxal, epoxy resins derived from a co-condensation resin of heavy oil or pitches, phenols, and formaldehydes, epoxy resins derived from diaminodiphenylmethane, epoxy resins derived from aminophenols, epoxy resins derived from xylylenediamine, epoxy resins derived from methylhexahydrophthalic acid, and epoxy resins derived from dimer acids.

[0086] When the epoxy resin composition contains another epoxy resin, the content of the other epoxy resin in 100 parts by mass of the total epoxy resin components is preferably 1 part by mass or more and 60 parts by mass or less, It is more preferable that the content is from 1 part by mass to 40 parts by mass.

[0087] 4-3.Inorganic substances The epoxy resin composition contains a recycled inorganic material, and may further contain a known inorganic filler for plastics. The recycled inorganic material is preferably one or more selected from the group consisting of carbon fiber and glass fiber, and more preferably carbon fiber. The known inorganic filler for plastics may be the same type of inorganic material as the recycled inorganic material.

[0088] The total content of the recycled inorganic material and the known inorganic filler for plastics in the epoxy resin composition is preferably 10% by mass or more and 95% by mass or less.

[0089] Furthermore, when the epoxy resin composition contains a known inorganic filler for plastics, the content of the recycled inorganic material when the total amount of the recycled inorganic material and the known inorganic filler for plastics is taken as 100 parts by mass, from the viewpoint of environmental friendliness, is preferably 40 parts by mass or more and 99 parts by mass or less, and more preferably 60 parts by mass or more and 99 parts by mass or less.

[0090] 4-4. Hardener The epoxy resin composition preferably contains a curing agent. As the curing agent, a known epoxy resin curing agent, for example, the curing agent described in the above section "1-4. Cured thermosetting resin product" can be used. The curing agent may be used alone or as a mixture of two or more kinds in any combination and in any ratio.

[0091] When the epoxy resin composition contains a curing agent, the content of the curing agent relative to 100 parts by mass of the total epoxy resin components is not particularly limited, but is preferably from 0.1 to 1,000 parts by mass, more preferably from 0.1 to 500 parts by mass, and even more preferably from 0.5 to 100 parts by mass.

[0092] When the curing agent is an amine-based curing agent or an acid anhydride-based curing agent, the content of the curing agent in the epoxy resin composition is preferably an amount such that the equivalent ratio of the functional groups in the curing agent to the epoxy groups in the total epoxy resin component is 0.1 or more and 2.0 or less, and more preferably an amount such that the equivalent ratio is 0.8 or more and 1.2 or less. By setting the content of the curing agent within the above range, the remaining amount of unreacted epoxy groups in the epoxy resin and unreacted functional groups in the curing agent can be reduced.

[0093] When the curing agent is an amide-based curing agent or an imidazole-based curing agent, the content of the curing agent relative to the total amount of all epoxy resin components and the curing agent in the epoxy resin composition is preferably 0.1 mass % or more and 20 mass % or less.

[0094] 4-5. Hardening accelerator The epoxy resin composition preferably contains a curing accelerator. By containing the curing accelerator, it is possible to shorten the curing time and lower the curing temperature, and it is possible to easily obtain a desired cured product.

[0095] As the curing accelerator, a known curing accelerator for epoxy resins, for example, the curing accelerators explained in the above section "1-4. Cured thermosetting resin" can be used. The curing accelerator may be used alone or as a mixture of two or more kinds in any combination and in any ratio.

[0096] When the epoxy resin composition contains a curing accelerator, the content of the curing accelerator per 100 parts by mass of the total epoxy resin components is not particularly limited, but is preferably 0.1 parts by mass or more and 20 parts by mass or less. It is preferable that the content of the curing accelerator is equal to or more than the lower limit, so that a good curing acceleration effect can be obtained. Also, by setting the content of the curing accelerator to equal to or less than the upper limit, it is possible to easily obtain the desired curing properties.

[0097] 4-6. Release agent The epoxy resin composition may contain a mold release agent. Examples of the mold release agent that can be used include natural waxes such as carnauba wax, synthetic waxes such as polyethylene wax, higher fatty acids such as stearic acid and zinc stearate, metal salts of the higher fatty acids, and hydrocarbon-based mold release agents such as paraffin. The release agent may be used alone or as a mixture of two or more kinds in any combination and in any ratio.

[0098] When the epoxy resin composition contains a mold release agent, the content of the mold release agent relative to 100 parts by mass of the total epoxy resin components is not particularly limited, but is preferably 0.001 parts by mass or more and 10.0 parts by mass or less. By setting the content of the mold release agent within the above range, it is possible to exhibit good mold releasability while maintaining the curing characteristics.

[0099] 4-7. Coupling agents The epoxy resin composition preferably contains a coupling agent, which can improve the adhesion between the epoxy resin matrix and inorganic substances.

[0100] The coupling agent includes a silane coupling agent and a titanate coupling agent. The coupling agent may be used alone or as a mixture of two or more kinds in any combination and in any ratio.

[0101] Examples of the silane coupling agent include epoxy silane coupling agents such as γ-glycidyloxypropyltrimethoxysilane, γ-glycidyloxypropyltriethoxysilane, and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; amino silane coupling agents such as γ-aminopropyltriethoxysilane, N-β(aminoethyl)γ-aminopropyltrimethoxysilane, N-β(aminoethyl)γ-aminopropylmethyldimethoxysilane, γ-aminopropyltrimethoxysilane, and γ-ureidopropyltriethoxysilane; mercapto silane coupling agents such as 3-mercaptopropyltrimethoxysilane; and vinyl silane coupling agents such as p-styryltrimethoxysilane, vinyltrichlorosilane, vinyltris(β-methoxyethoxy)silane, vinyltrimethoxysilane, vinyltriethoxysilane, and γ-methacryloxypropyltrimethoxysilane.

[0102] Examples of titanate coupling agents include isopropyl triisostearoyl titanate, isopropyl tri(N-aminoethyl aminoethyl) titanate, diisopropyl bis(dioctyl phosphate) titanate, tetraisopropyl bis(dioctyl phosphite) titanate, tetraoctyl bis(ditridecyl phosphite) titanate, tetra(2,2-diallyloxymethyl-1-butyl)bis(ditridecyl)phosphite titanate, bis(dioctyl pyrophosphate)oxyacetate titanate, and bis(dioctyl pyrophosphate)ethylene titanate.

[0103] When the epoxy resin composition contains a coupling agent, the content of the coupling agent relative to 100 parts by mass of the total epoxy resin components is not particularly limited, but is preferably 0.001 parts by mass or more and 10.0 parts by mass or less. In addition, by controlling the content of the coupling agent to the above upper limit or less, the coupling agent is less likely to bleed out from the obtained composite material.

[0104] 4-8.Other additives The epoxy resin composition may contain additives other than the above components, as necessary. Examples of the additives include flame retardants, plasticizers, reactive diluents, and pigments.

[0105] Examples of the flame retardant include halogen-based flame retardants such as brominated epoxy resins and brominated phenol resins; antimony compounds such as antimony trioxide; phosphorus-based flame retardants such as red phosphorus, phosphate esters, and phosphines; nitrogen-based flame retardants such as melamine derivatives; and inorganic flame retardants such as aluminum hydroxide and magnesium hydroxide.

[0106] 4-9.Curing process The curing step is a step of curing the above-mentioned epoxy resin composition, and a composite material can be obtained by this. The method of curing the epoxy resin composition is not particularly limited, but it is preferable to adopt a curing method by a thermosetting reaction. During the thermosetting reaction, it is preferable to appropriately select the curing temperature depending on the type of curing agent. For example, when an amine-based curing agent is used, the curing temperature is usually 80°C or higher and 250°C or lower. In addition, it is also possible to lower the curing temperature by adding a curing accelerator to these curing agents.

[0107] The reaction time is preferably 0.01 hours or more and 20 hours or less. By setting the reaction time to the above lower limit or more, the epoxy resin composition tends to be sufficiently cured. In addition, by setting the reaction time to the above upper limit or less, deterioration due to heating and energy loss during heating tend to be reduced. EXAMPLES

[0108] The present invention will be described in more detail below with reference to examples and comparative examples. However, the present invention is not limited to the following examples as long as it does not depart from the gist of the present invention. In addition, the various manufacturing conditions and evaluation result values ​​in the following examples have the meaning of preferred upper or lower limit values ​​in the embodiment of the present invention, and the preferred range may be a range defined by a combination of the above-mentioned upper or lower limit value and the values ​​of the following examples or values ​​between the examples. In the following examples, "room temperature" refers to a temperature range of 15°C or higher and 35°C or lower.

[0109] [Raw materials and reagents] The bisphenol A type epoxy resin (epoxy equivalent: 950 g / eq or 183 g / eq) used was a product of Mitsubishi Chemical Corporation. The Rikacid (acid anhydride) M-700 used was a product of New Japan Chemical Co., Ltd. Curesol 2E4MZ (curing catalyst) was a product of Shikoku Chemical Industry Co., Ltd. The 48 mass% aqueous sodium hydroxide solution, disilenediamide (DICY), 3-(3,4-dichlorophenyl)-1,1-dimethylurea (DCMU), hydrochloric acid, methanol, toluene, and acetonitrile were all products of Fujifilm Wako Pure Chemical Industries, Ltd. Benzyl alcohol used was a product of Sankyo Chemical Co., Ltd. The carbon fiber used was 3mm chopped carbon fiber manufactured by Yoshino Co., Ltd.

[0110] [analysis] The production and quantification of bisphenol A was confirmed by high performance liquid chromatography as follows: The procedure and conditions were followed. ·Device: High-performance liquid chromatograph (Shimadzu Corporation) Pump: LC-20AD (Shimadzu Corporation) Column oven: CTO-20AC (Shimadzu Corporation) Detector: SPD-20A (Shimadzu Corporation) Column: 3 μm 250 mm × 4.6 mm ID (Intact Co., Ltd.) Method: Low pressure gradient method ·Analysis temperature: 40℃ ·Eluent composition: Solution A: Acetonitrile B liquid water At 0 min of analysis time, the eluent composition was A:B = 30:70 (volume ratio, same below), and from 0 to 5 min of analysis time the eluent composition was A:B = 30:70, then from 5 to 20 min of analysis time it gradually became A:B = 100:0, and from 20 to 35 min of analysis time it was A:B = 100:0. ·Flow rate: 1mL / min Detection wavelength: 280nm

[0111] [Carbon fiber evaluation] The carbon fibers recovered from the composite material consisting of an inorganic substance and an acid anhydride cured product were evaluated according to the following criteria. S: All carbon fibers are unraveled one by one. A: When pulled, the carbon fiber unravels, leaving a single carbon fiber. B: Some of the resin has melted and some of the carbon fiber has come loose, but even when pulled, a single carbon fiber cannot be obtained. C: The resin does not dissolve at all, and the carbon fiber does not dissolve at all.

[0112] Reference Example 1: Preparation of acid anhydride cured product 300g of bisphenol A type epoxy resin (epoxy equivalent 183g / eq), 270g of Rikacid, and 3g of Curesol 2E4MZ were mixed well in an aluminum cup to obtain a mixture. The mixture was heated at 100℃ for 3 hours, and then heated at 140℃ for 3 hours to obtain a hardened acid anhydride material.

[0113] Reference example 2: Preparation of acid anhydride cured product CFRP 100g of bisphenol A type epoxy resin (epoxy equivalent 183g / eq), 90g of Rikacid, and 1g of Curesol 2E4MZ were placed in an aluminum cup and mixed well to obtain mixture 1. 100g of carbon fiber was added to the obtained mixture 1 and mixed to obtain mixture 2. The obtained mixture 2 was poured into a flat mold and heated at 100℃ for 3 hours, and then heated at 140℃ for 3 hours to obtain a carbon fiber composite material of an acid anhydride cured product.

[0114] Example 1 50 g of benzyl alcohol and 10 g of the acid anhydride cured product obtained in Reference Example 1 were placed in a 100 mL three-neck flask equipped with a stirrer, a thermometer, and a dropping funnel. The three-neck flask was immersed in an oil bath at 120°C, and 4.3 g of a 48% aqueous sodium hydroxide solution was then added from the dropping funnel. The internal temperature was then raised to 200°C. When the internal temperature reached 200°C and the reaction was continued for 1 hour, the solid content of the acid anhydride cured product disappeared and dissolved. In addition, a portion of the decomposition liquid was extracted and analyzed by high performance liquid chromatography, and it was found that 0.71% by mass of bisphenol A was produced.

[0115] Comparative Example 1 50g of benzyl alcohol and 4.3g of 48% aqueous sodium hydroxide solution were placed in a 100mL three-neck flask equipped with a stirrer, a thermometer, and a dropping funnel. The three-neck flask was immersed in an oil bath at 120°C, and then 10g of the acid anhydride cured product obtained in Reference Example 1 was placed in the flask. The internal temperature was then raised to 200°C. The reaction was continued for 1 hour after the internal temperature reached 200°C, but the solid content of the acid anhydride cured product remained. In addition, a portion of the decomposition liquid was extracted and analyzed by high performance liquid chromatography, and it was found that 0.08% by mass of bisphenol A was produced.

[0116] Table 1 summarizes the mixing order of benzyl alcohol, the cured acid anhydride product, and the aqueous sodium hydroxide solution, the presence or absence of solids after the reaction, and the amount of bisphenol A produced in Example 1 and Comparative Example 1. Table 1 shows that by mixing benzyl alcohol and the cured acid anhydride product and then mixing with sodium hydroxide, the dissolution time of the cured acid anhydride product can be shortened and the amount of bisphenol A produced can be increased.

[0117] [Table 1]

[0118] Example 2 The same procedure as in Example 1 was repeated, except that 10 g of the acid anhydride cured product obtained in Reference Example 1 was replaced with 10 g of the carbon fiber composite of the acid anhydride cured product obtained in Reference Example 2. After decomposition, the carbon fibers were in a state in which all the carbon fibers had been dissolved one by one. In addition, a portion of the decomposition liquid was extracted and analyzed by high performance liquid chromatography, and it was found that 0.51 mass% of bisphenol A was produced.

[0119] Comparative Example 2 Comparative Example 2 was carried out in the same manner as Comparative Example 2, except that 10 g of the acid anhydride cured product obtained in Reference Example 1 was replaced with 10 g of the carbon fiber composite of the acid anhydride cured product obtained in Reference Example 2. After decomposition, the carbon fiber was in a state in which some of the resin had dissolved and some of the carbon fiber had unraveled, but no single carbon fiber could be obtained even when pulled. In addition, a portion of the decomposition liquid was extracted and analyzed by high performance liquid chromatography, and it was found that 0.05 mass% of bisphenol A was produced.

[0120] Table 2 shows the mixing order of benzyl alcohol, the carbon fiber composite material of a cured acid anhydride, and the aqueous sodium hydroxide solution, the appearance of the carbon fiber, and the amount of bisphenol produced in Example 2 and Comparative Example 2. Table 2 shows that by mixing benzyl alcohol and the carbon fiber composite material of a cured acid anhydride, and then mixing with sodium hydroxide, the cured acid anhydride can be dissolved in a short time, the carbon fiber can be recovered, and a large amount of bisphenol A is produced.

[0121] [Table 2]

Claims

1. A method for decomposing a cured thermosetting resin, comprising the steps of: a first mixing step of mixing a cured thermosetting resin with an organic solvent to obtain a mixed liquid; a second mixing step of mixing the mixed solution with an alkaline compound after the first mixing step; and a decomposition step of decomposing the cured thermosetting resin material after the second mixing step. The decomposition method of the cured thermosetting resin, comprising the steps of:

2. The method for decomposing a cured thermosetting resin material according to claim 1 , wherein the alkali compound is an alkali metal compound.

3. 3. The method for decomposing a cured thermosetting resin material according to claim 2, wherein the alkali metal compound is at least one selected from the group consisting of alkali metal hydroxides, alkali metal phosphates, alkali metal carbonates, and metal alkoxides.

4. The method for decomposing a cured thermosetting resin according to claim 1 , wherein the cured thermosetting resin is a cured epoxy resin.

5. A method for producing a phenol compound from a cured thermosetting resin, comprising the steps of: The thermosetting resin cured product contains an inorganic substance, The method for decomposing a cured thermosetting resin according to claim 1, further comprising the steps of: decomposing the cured thermosetting resin; The method for producing a phenol compound includes, after the decomposition step, an inorganic matter recovery step of recovering the inorganic matter.

6. The method for producing a phenol compound according to claim 5, wherein the inorganic material is at least one selected from the group consisting of carbon fiber and glass fiber.

7. The method for producing a phenolic compound according to claim 5 , wherein the cured thermosetting resin is a cured phenolic epoxy resin.

8. The method for producing a phenolic compound according to claim 5, wherein the phenolic compound is a bisphenol.

9. A method for producing an epoxy resin, comprising a reaction step of reacting a phenol compound obtained by the method for producing a phenol compound according to any one of claims 5 to 8 with epihalohydrin.

10. A method for producing a composite material, comprising a step of curing an epoxy resin composition containing an epoxy resin obtained by the method for producing an epoxy resin according to claim 9 and the inorganic substance obtained by the method for producing a phenol compound according to any one of claims 5 to 8.

Citation Information

Patent Citations

  • Dissolution treatment liquid of epoxy resin cured article

    JP2019099734A