Method for producing phenolic compound, method for producing epoxy resin, and method for producing composite material

The method of swelling and decomposing cured thermosetting resins with an organic solvent addresses the difficulty in recycling by producing phenol compounds and epoxy resins efficiently, while recovering inorganic substances.

JP2024165141APending Publication Date: 2024-11-28MITSUBISHI CHEM CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023081043
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-16
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Conventional chemical recycling of cured thermosetting resins is difficult due to their hardness, requiring crushing and resulting in complex mixtures that hinder the recovery of monomer raw materials like phenol compounds.

Method used

A method involving swelling cured thermosetting resins with an organic solvent to break them into small pieces, followed by drying and decomposition, which allows for the production of phenol compounds and co-production of inorganic substances, and further processing into epoxy resins and composite materials.

Benefits of technology

This method simplifies the decomposition of cured thermosetting resins, enabling efficient production of phenol compounds and epoxy resins, and facilitates the recovery of inorganic substances, thus overcoming the challenges of hardness and complex mixtures in conventional recycling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024165141000001
    Figure 2024165141000001
Patent Text Reader

Abstract

To provide a method for producing a phenolic compound by decomposing a thermosetting cured resin, the method mitigating the problem of crushing difficulty in the thermosetting cured resin.SOLUTION: A method for producing a phenolic compound from a thermosetting cured resin includes: a swelling step for contacting a thermosetting cured resin A with an organic solvent to swell and fragment the thermosetting cured resin A, thereby yielding a thermosetting cured resin B; a drying step for drying the thermosetting cured resin B to provide a thermosetting cured resin C; and a decomposition step for decomposing the thermosetting cured resin C.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a phenolic compound, a method for producing an epoxy resin, and a method for producing a composite material. [Background technology]

[0002] Thermosetting resins are used in various applications because they can be highly reinforced by blending fillers, additives, etc. Among them, epoxy resins are important materials used in various applications such as adhesives, insulating materials, paints, casting materials, and composite materials because they exhibit excellent adhesive properties, electrical properties, and heat resistance.

[0003] On the other hand, a cured thermosetting resin obtained by curing a thermosetting resin does not melt and is difficult to dissolve in a general-purpose solvent. This is because the cured thermosetting resin has a complex structure that is three-dimensionally crosslinked. Therefore, when chemically recycling a cured thermosetting resin, it is necessary to crush or pulverize the cured thermosetting resin prior to decomposition treatment (see Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 10-024274 Summary of the Invention [Problem to be solved by the invention]

[0005] In the conventional chemical recycling of thermosetting resin cured products, the thermosetting resin cured products are crushed or pulverized before being fed to a decomposition tank, but because the thermosetting resin cured products are hard, crushing or pulverizing them is extremely difficult. In addition, because it takes time to decompose the thermosetting resin cured products, the decomposition products become a complex mixture, making it impossible to obtain monomer raw materials such as phenol compounds.

[0006] The present invention has been made in view of the above circumstances. That is, an object of the present invention is to provide a method for producing a phenol compound by decomposing a cured thermosetting resin material, which reduces the problem of the difficulty of crushing the cured thermosetting resin material. [Means for solving the problem]

[0007] As a result of intensive research to solve the above problems, the present inventors have found that a phenolic compound can be produced by contacting a cured thermosetting resin with an organic solvent to swell and break it into small pieces, and then drying and decomposing the pieces. They have also found that a phenolic compound and an inorganic substance can be co-produced by using a cured thermosetting resin containing an inorganic substance. They have also found a method for producing an epoxy resin from the obtained phenolic compound, and a method for producing a composite material from the epoxy resin and an inorganic substance recovered from the cured thermosetting resin. That is, the present invention includes the following inventions.

[0008] [1] A method for producing a phenol compound from a cured thermosetting resin, comprising the steps of: a swelling step of contacting the cured thermosetting resin A with an organic solvent to swell and fragment the cured thermosetting resin A to obtain a cured thermosetting resin B; A drying step of drying the thermosetting resin cured material B to obtain a thermosetting resin cured material C; and A decomposition step of decomposing the thermosetting resin cured material C. A method for producing a phenolic compound, comprising: [2] The method for producing a phenol compound according to [1], wherein the boiling point of the organic solvent under atmospheric pressure is 150° C. or lower. [3] The method for producing a phenol compound according to [1] or [2], wherein the organic solvent is formic acid. [4] The method for producing a phenol compound according to any one of [1] to [3], wherein the thermosetting resin cured product A is an epoxy resin cured with an amine-based curing agent. [5] The method for producing a phenol compound according to any one of [1] to [4], wherein the decomposition step is carried out in the presence of one or more decomposition agents selected from the group consisting of bases, acids, and oxidizing agents. The method for producing a phenol compound according to [5], wherein the base is one or more selected from the group consisting of sodium compounds and potassium compounds. [7] The method for producing a phenol compound according to [5] or [6], wherein the acid is one or more selected from the group consisting of sulfuric acid and nitric acid. [8] The thermosetting resin cured material A contains an inorganic substance, The method for producing a phenol compound according to any one of [1] to [7], further comprising, after the decomposition step, an inorganic matter recovery step of recovering the inorganic matter. [9] The method for producing a phenol compound according to [8], wherein the inorganic material is at least one type selected from the group consisting of carbon fiber and glass fiber.

[10] A method for producing an epoxy resin, comprising a reaction step of reacting the phenol compound obtained by the method for producing a phenol compound according to any one of [1] to [9] with epihalohydrin.

[11] A method for producing a composite material, comprising a curing step of curing an epoxy resin composition containing the epoxy resin obtained by the method for producing an epoxy resin according to

[10] and the inorganic substance obtained by the method for producing a phenol compound according to [8] or [9]. Effect of the Invention

[0009] According to the present invention, it is possible to provide a method for producing a phenol compound by decomposing a cured thermosetting resin material, which reduces the problem of the difficulty in crushing the cured thermosetting resin material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The following is a detailed description of the embodiments of the present invention, but the present invention is not limited to the following description, and can be modified as desired without departing from the scope of the present invention. In addition, in this specification, when a numerical value or physical property value is enclosed before and after "~", the values ​​before and after the "~" are included.

[0011] 1. Method for producing phenolic compounds The first embodiment of the present invention is a method for producing a phenolic compound from a cured thermosetting resin, comprising the steps of: a swelling step of contacting a cured thermosetting resin A with an organic solvent to swell and fragment the cured thermosetting resin A to obtain a cured thermosetting resin B; The method includes a drying step of drying the cured material B to obtain a thermosetting resin cured material C, and a decomposition step of decomposing the thermosetting resin cured material C. The phenol compound produced by the production method according to this embodiment is a compound derived from a monomer, a curing agent, an end-capping agent, etc. of a thermosetting resin.

[0012] 1-1. Swelling process The swelling step is a step of swelling and fragmenting the thermosetting resin cured material A by contacting the thermosetting resin cured material A with an organic solvent. In the swelling step, the thermosetting resin cured material swells and softens, and is fragmented to a size that can be easily decomposed without going through a step of crushing or pulverizing the thermosetting resin cured material. That is, the manufacturing method of this embodiment realizes fragmentation of the thermosetting resin cured material by performing a simple operation of contacting the thermosetting resin cured material with an organic solvent instead of crushing the thermosetting resin cured material, which was difficult in the past, and can easily produce a phenol compound. In addition, since the thermosetting resin cured material A becomes easily decomposed by swelling and fragmenting, in a preferred embodiment of this embodiment, the decomposition time can be shortened compared to the conventional method.

[0013] 1-1-1. Thermosetting resin cured product A The cured thermosetting resin A swelled and fragmented in the swelling step is a thermosetting resin cured with or without a curing agent in the presence or absence of a curing accelerator, preferably a thermosetting resin cured with a curing agent. The cured thermosetting resin A has a structure derived from a phenol compound in its structure (e.g., a structural unit, a terminal structure, a crosslinked structure, etc.).

[0014] The thermosetting resin is not particularly limited, but preferable examples thereof include a copolymer of a phenolic compound and another monomer, a homopolymer of an epoxidized product of a phenolic compound, and a copolymer of an epoxidized product of a phenolic compound and another monomer, etc. Examples of such thermosetting resins include epoxy resins and phenolic resins.

[0015] The phenol compound is not particularly limited, and may be, for example, a monohydric phenol compound, a dihydric phenol compound, a bisphenol compound, or the like.

[0016] Examples of monovalent phenolic compounds include phenol, o-cresol, m-cresol, p-cresol, p-ethylphenol, p-isopropylphenol, p-tert-butylphenol, p-cumylphenol, p-cyclohexylphenol, p-octylphenol, p-nonylphenol, 2,4-xylenol, p-methoxyphenol, p-hexyloxyphenol, p-decyloxyphenol, o-chlorophenol, m-chlorophenol, p-chlorophenol, p-bromophenol, pentabromophenol, and penta Examples of such phenols include chlorophenol, o-nitrophenol, m-nitrophenol, p-nitrophenol, 2,4,6-trinitrophenol, o-phenolsulfonic acid, m-phenolsulfonic acid, p-phenolsulfonic acid, p-phenylphenol, p-isopropenylphenol, 2,4-di(1'-methyl-1'-phenylethyl)phenol, β-naphthol, α-naphthol, p-(2',4',4'-trimethylchromanyl)phenol, and 2-(4'-methoxyphenyl)-2-(4''-hydroxyphenyl)propane.

[0017] Examples of the divalent phenol compound include hydroquinone, resorcinol, and 2-methylresorcinol.

[0018] Examples of bisphenol compounds include 2,2'-biphenol, 4,4'-biphenol, 1,5-naphthalenediol, 2,7-naphthalenediol, bis(4-hydroxyphenyl)methane (i.e., bisphenol F), bis{(4-hydroxy-3, 5-dimethyl)phenyl}methane, 1,1-bis(4-hydroxyphenyl)ethane (i.e., bisphenol E), 1,1-bis(4-hydroxyphenyl)-1-phenylethane (i.e., bisphenol AP), 2,2-bis(4-hydroxyphenyl)hexafluoropropane (i.e., bisphenol AF), 2,2-bis(4-hydroxyphenyl)propane (i.e., bisphenol A), 2,2-bis{(4-hydroxy-3-methyl)phenyl}propane (i.e., bisphenol C), 2,2-bis{ ... 2,2-bis{(3,5-dibromo-4-hydroxy)phenyl}propane, 2,2-bis{(3-isopropyl-4-hydroxy)phenyl}propane, 2,2-bis{(4-hydroxy-3-phenyl)phenyl}propane, 2-(4-hydroxyphenyl)-2-(3-carboxy-4-hydroxyphenyl)propane, 2-(2-hydroxyphenyl)-2-(4-hydroxyphenyl)propane, 1-(4-hydroxyphenyl)-1,3,3-trimethyl-5-hydroxyindan , 2-(4-hydroxyphenyl)-[3-{2-(4-hydroxyphenyl)propan-2-yl}-4-hydroxyphenyl]propane, 2,2-bis(4-hydroxyphenyl)butane (i.e., bisphenol B), 1,1-bis(4-hydroxyphenyl)-1,1-diphenylmethane (i.e., bisphenol BP), 4,4′-isopropylidenebis(2-methyl-phenol) (i.e., bisphenol C), 2,2-bis(4-hydroxy-3-isopropylphenyl)propane (i.e., bisphenol G), 2, 2-bis(4-hydroxyphenyl)-3-methylbutane, 2,2-bis(4-hydroxyphenyl)-3,3-dimethylbutane, 2,4-bis(4-hydroxyphenyl)-2-methylbutane, 2,2-bis(4-hydroxyphenyl)pentane, 2,2-bis(4-hydroxyphenyl)-4-methylpentane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)-4-isopropylcyclohexane, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, 9,Examples of the fluorene include 9-bis(4-hydroxyphenyl)fluorene, 9,9-bis{(4-hydroxy-3-methyl)phenyl}fluorene, α,α'-bis(4-hydroxyphenyl)-o-diisopropylbenzene, α,α'-bis(4-hydroxyphenyl)-m-diisopropylbenzene, α,α'-bis(4-hydroxyphenyl)-p-diisopropylbenzene, 1,3-bis(4-hydroxyphenyl)-5,7-dimethyladamantane, 4,4'-dihydroxydiphenyl sulfone (i.e., bisphenol S), 4,4'-dihydroxydiphenyl sulfoxide, 4,4'-dihydroxydiphenyl sulfide, 4,4'-dihydroxydiphenyl ketone, 4,4'-dihydroxydiphenyl ether, and 4,4'-dihydroxydiphenyl ester.

[0019] Of these, the phenol compound is preferably a bisphenol compound, more preferably selected from 2,2-bis(4-hydroxyphenyl)propane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, 2,2-bis(4-hydroxyphenyl)hexafluoropropane, 2,2-bis(4-hydroxyphenyl)butane, 1,1-bis(4-hydroxyphenyl)-1,1-diphenylmethane, 4,4'-isopropylidenebis(2-methyl-phenol), 1,1-bis(4-hydroxyphenyl)ethane, bis(4-hydroxyphenyl)methane, 2,2-bis(4-hydroxy-3-isopropylphenyl), and 4,4'-dihydroxydiphenylsulfone, and even more preferably 2,2-bis(4-hydroxyphenyl)propane.

[0020] The epoxy resin is not particularly limited, and examples thereof include diglycidyl ethers of the above bisphenol compounds; bisphenol type epoxy resins such as bisphenol A type epoxy resins, bisphenol F type epoxy resins, and bisphenol S type epoxy resins; phenol novolac type epoxy resins, cresol novolac type epoxy resins, and bisphenol Examples of epoxy resins include novolac epoxy resins such as A novolac epoxy resins; biphenyl epoxy resins; glycidyl ester epoxy resins; glycidyl amine epoxy resins; linear aliphatic epoxy resins; alicyclic epoxy resins; heterocyclic epoxy resins; and alkyl substituted, halides, and hydrogenated versions of these epoxy resins.

[0021] In the technical field of the present invention, "epoxy resin" includes polymers containing repeating units and epoxy compounds with a monomolecular structure (i.e., non-polymer compounds), both of which are sometimes expressed and sold as "epoxy resins". A mixture of two or more epoxy resins may also be simply called "epoxy resin". In this specification, "epoxy resin" refers to any of polymers containing repeating units, epoxy compounds with a monomolecular structure, and mixtures thereof.

[0022] The cured thermosetting resin may be a cured product of one type of thermosetting resin, or a cured product of a mixture of two or more types of thermosetting resins in any combination and ratio.

[0023] In this specification, a curing agent means a substance that contributes to the crosslinking reaction and / or chain extension reaction of a thermosetting resin. Even substances that are usually called "curing accelerators" are considered to be curing agents as long as they contribute to the crosslinking reaction and / or chain extension reaction of a thermosetting resin.

[0024] Examples of the curing agent for the thermosetting resin include phenol-based curing agents, polyisocyanate-based curing agents, amine-based curing agents, acid anhydride-based curing agents, imidazole-based curing agents, amide-based curing agents, mercaptan-based curing agents, cationic polymerization initiators, organic phosphine-based curing agents, phosphonium salt-based curing agents, and tetraphenyl boronate-based curing agents. Of these, the curing agent is preferably an amine-based curing agent. When the thermosetting resin is an epoxy resin, the curing agent is particularly preferably an amine-based curing agent, and therefore, the thermosetting resin cured material A is particularly preferably an epoxy resin cured by an amine-based curing agent.

[0025] Examples of phenol-based curing agents include bisphenols such as bisphenol A, bisphenol C, bisphenol F, bisphenol S, bisphenol B, bisphenol AD, bisphenol Z, and tetrabromobisphenol A; biphenols such as 4,4'-biphenol and 3,3',5,5'-tetramethyl-4,4'-biphenol; benzenediols such as catechol, resorcin, and hydroquinone; and polyfunctional phenols such as naphthalenediols. The hydrogen atoms bonded to the aromatic rings of these compounds may be substituted with non-interfering substituents, such as halogeno groups, alkyl groups, aryl groups, ether groups, ester groups, sulfur, phosphorus, and organic substituents containing heteroelements such as silicon. In this specification, "benzenediols" refers to compounds having one benzene ring and two hydroxyl groups directly bonded to this benzene ring.

[0026] The phenol-based curing agent may be novolak resins and resol resins which are polycondensates of the above-mentioned polyfunctional phenols and aldehydes, and novolak resins and resol resins which are polycondensates of monofunctional phenols such as phenol, cresol, and alkylphenol and aldehydes.

[0027] Examples of polyisocyanate-based curing agents include tolylene diisocyanate, methylcyclohexane diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate, xylylene diisocyanate, hydrogenated xylylene diisocyanate, dimer acid diisocyanate, trimethylhexamethylene diisocyanate, and lysine triisocyanate.

[0028] The polyisocyanate-based curing agent may be a polyisocyanate compound obtained by reacting the above-mentioned polyisocyanate compound with a compound having at least two active hydrogen atoms such as an amino group, a hydroxyl group, a carboxyl group, or water; or a trimer to pentamer of the above-mentioned polyisocyanate compound; or the like.

[0029] Examples of the amine-based curing agent include aliphatic primary amines, aliphatic secondary amines, aliphatic tertiary amines, aromatic primary amines, aromatic secondary amines, aromatic tertiary amines, cyclic amines, guanidines, and urea derivatives. More specific examples of the amine-based curing agent include triethylenetetramine, diaminodiphenylmethane, diaminodiphenylether, metaxylenediamine, dicyandiamide (DICY), 1,8-diazabicyclo(5,4,0)-7-undecene, 1,5-diazabicyclo(4,3,0)-5-nonene, dimethylurea, and guanylurea.

[0030] Examples of acid anhydride curing agents include condensates of maleic anhydride and unsaturated compounds, phthalic anhydride, 4-methylhexahydrophthalic anhydride, hexahydrophthalic anhydride, and trimellitic anhydride.

[0031] Examples of imidazole-based curing agents include 1-isobutyl-2-methylimidazole, 2-methylimidazole, 1-benzyl-2-methylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, and benzimidazole. Although imidazole-based curing agents also function as curing accelerators, they are classified as curing agents in this embodiment.

[0032] Examples of the amide-based curing agent include polyamide resins.

[0033] Examples of the mercaptan curing agent include polysulfide type mercaptan compounds, thioester type mercaptan compounds, and thioether type mercaptan compounds.

[0034] The cationic polymerization initiator generates cations by heat or irradiation with active energy rays, and examples of the initiator include aromatic onium salts. Specifically, SbF 6- , B.F. 4 -, AsF 6- , P.F. 6- , CF3SO3 2 - and B(C6F5) 4- and an aromatic cation component containing an atom selected from iodine, sulfur, nitrogen, and phosphorus. The aromatic onium salt is preferably one or more salts selected from the group consisting of diaryliodonium salts and triarylsulfonium salts.

[0035] Examples of the organic phosphine curing agent include tributylphosphine, methyldiphenylphosphine, triphenylphosphine, diphenylphosphine, and phenylphosphine.

[0036] Examples of phosphonium salt curing agents include tetraphenylphosphonium tetraphenylborate, tetraphenylphosphonium ethyltriphenylborate, and tetrabutylphosphonium tetrabutylborate.

[0037] Examples of the tetraphenylborate-based curing agent include 2-ethyl-4-methylimidazole·tetraphenylborate, and N-methylmorpholine·tetraphenylborate.

[0038] The curing agent may be used alone or in any combination and ratio of two or more kinds. Good too.

[0039] The thermosetting resin cured material A may be a product obtained by curing a thermosetting resin using a curing accelerator. The curing accelerator is not particularly limited, and known curing accelerators for epoxy resins, such as urea compounds such as 3-(3,4-dichlorophenyl)-1,1-dimethylurea (DCMU), alkali metal compounds, imidazole compounds, tertiary amine compounds, quaternary ammonium salts, and organic phosphorus compounds, can be used. The curing accelerator may be used alone or as a mixture of two or more kinds in any combination and in any ratio.

[0040] The cured thermosetting resin may be mixed with other components to form a composite material, as long as the effects of the present invention are not impaired. Examples of the other components include inorganic substances and thermoplastic resins. The other components may be used alone or as a mixture of two or more kinds in any combination and ratio.

[0041] The inorganic substance is not particularly limited, but examples thereof include carbon, glass, metal, and metal compounds such as fused silica, crystalline silica, alumina, calcium carbonate, calcium sulfate, talc, and boron nitride. The inorganic substance may be in the form of fiber, particle, foil, etc., and is preferably fiber. Among these, the inorganic substance is preferably one or more types selected from the group consisting of carbon fiber and glass fiber, and more preferably carbon fiber.

[0042] The fibers may be in the form of a nonwoven fabric or a woven fabric. If in the form of a woven fabric, it may be a cross material made by weaving fiber bundles, or a UD (Uni-Directional) material in which fiber bundles are arranged in one direction.

[0043] Examples of the thermoplastic resin include polyethylene and polypropylene.

[0044] 1-1-2. Organic solvents The organic solvent is not particularly limited as long as it can swell and fragment the cured thermosetting resin A, but in order to facilitate removal in the drying step, it is preferable for the organic solvent to have a boiling point of 150° C. or less under atmospheric pressure, and more preferably an organic solvent having a boiling point of 120° C. or less under atmospheric pressure. The lower limit of the boiling point of the organic solvent under atmospheric pressure is not particularly limited, but in order to facilitate the existence of the organic solvent in a liquid state under swelling conditions, it is preferably 20° C. or more, and more preferably 30° C. or more. The organic solvent may be used alone or as a mixture of two or more kinds in any combination and in any ratio.

[0045] Examples of organic solvents having a boiling point of 150° C. or less under atmospheric pressure include formic acid, acetic acid, propionic acid, ammonia solution (e.g., ammonia in ethanol and ammonia in tetrahydrofuran), diethylamine, triethylamine, propylamine, dipropylamine, tripropylamine, butylamine, pyridine, etc. Among these, the organic solvent is preferably formic acid from the viewpoint of swelling property.

[0046] The amount of organic solvent used in the swelling step is not particularly limited as long as it can swell and fragment the thermosetting resin cured material A, but since it becomes easier to transport the cured thermosetting resin A as a solid and liquid slurry after swelling and fragmentation, the amount is preferably at least twice the volume of the cured thermosetting resin A, more preferably at least five times, and even more preferably at least ten times. The upper limit of the amount of organic solvent is not particularly limited, but increasing the amount of organic solvent too much may cause the thermosetting resin to deteriorate. Since the time required for swelling and fragmentation of the cured thermosetting resin A will not be shortened, which would result in inefficiency, the volume of the cured thermosetting resin A is preferably 1,000 times or less, more preferably 500 times or less, and even more preferably 100 times or less, the volume of the cured thermosetting resin A.

[0047] 1-1-3. Swelling and fragmentation As a method for contacting the thermosetting resin cured material A with the organic solvent, it is preferable to adopt a method of immersing the thermosetting resin cured material A in the organic solvent from the viewpoint of swelling efficiency. The conditions for immersing the thermosetting resin cured material A in the organic solvent are not particularly limited, but the immersion temperature is preferably 10°C or more and 100°C or less, more preferably 20°C or more and 80°C or less, and even more preferably 25°C or more and 60°C or less. The immersion time is preferably 0.1 days or more and 28 days or less, more preferably 0.2 days or more and 21 days or less, and even more preferably 0.3 days or more and 14 days or less. In order to shorten the immersion time, ultrasonic or microwave irradiation may be used in combination.

[0048] "Swelling and fragmentation" in the swelling step refers to a state in which the cured thermosetting resin A swells, softens, and crumbles to a size smaller than that before contacting with the organic solvent. From the viewpoint of shortening the decomposition time, the length x width x thickness size of the cured thermosetting resin B obtained by swelling and fragmentation is preferably 15 mm or less x 15 mm or less x 15 mm or less, more preferably 10 mm or less x 10 mm or less x 10 mm or less, and even more preferably 3 mm or less x 3 mm or less x 2 mm or less.

[0049] The swelling and fragmentation of the cured thermosetting resin A can also be evaluated by conducting a swelling test in which a test piece of the cured thermosetting resin A having dimensions of 20 mm x 20 mm x 2 mm is contacted with an organic solvent. If the dimensions of the test piece are 10 mm or less x 10 mm or less x 2 mm or less, it can be evaluated that the cured thermosetting resin fragments under the test conditions.

[0050] In addition, the case where an external force is applied to the swollen material when the organic solvent is removed from the swollen material by filtration, decantation, or the like after contact with the organic solvent, causing the swollen material to break into small pieces, is also included in the "swelling and fragmentation" in the swelling process.

[0051] 1-2.Drying process The drying step is a step of drying the cured thermosetting resin B obtained in the swelling step to obtain a cured thermosetting resin C.

[0052] The drying conditions in the drying step are not particularly limited as long as the organic solvent adhering to the surface of the cured thermosetting resin B can be evaporated, and may be appropriately selected depending on the type of organic solvent and the amount of organic solvent adhering to the surface of the cured thermosetting resin B, etc., but drying under reduced pressure is preferred. For example, when one or more organic solvents selected from the group consisting of formic acid and acetic acid are selected, drying may be performed under reduced pressure conditions of 1 kPa to 20 kPa at a temperature of 50° C. to 150° C. for 1 hour to 20 hours.

[0053] 1-3. Decomposition process The decomposition step is a step of decomposing the thermosetting resin cured material C obtained in the drying step. The method of decomposing the thermosetting resin cured material C is not particularly limited as long as it is a method capable of producing a phenol compound or a salt thereof as a decomposition product, and a known decomposition method or a decomposition method similar to a known decomposition method can be appropriately adopted. As a known method, for example, a method of decomposing a thermosetting resin cured material in the presence of a decomposing agent can be preferably mentioned. In this method, a decomposition reaction is generally carried out in a treatment liquid containing a decomposing agent and an organic solvent.

[0054] The decomposition agents preferably include bases, acids, and oxidizing agents. The decomposing agent may be used alone or as a mixture of two or more kinds in any combination and ratio.

[0055] Examples of the base include metal compounds such as metal hydrides, metal hydroxides, metal borohydride salts, metal carbonates, and metal alkoxides. Of these, the base is preferably one or more selected from the group consisting of metal hydroxides and metal alkoxides, and more preferably metal alkoxides. In addition, examples of the metal in the base include alkali metals such as lithium, sodium, and potassium, and is preferably at least one of sodium and potassium, and more preferably sodium. Therefore, the base is preferably one or more selected from the group consisting of sodium compounds and potassium compounds, and more preferably one or more selected from the group consisting of sodium hydroxide, potassium hydroxide, sodium alkoxide, and potassium alkoxide.

[0056] Examples of the acid include inorganic acids such as sulfuric acid, nitric acid, and phosphoric acid; and organic acids such as methanesulfonic acid and toluenesulfonic acid. In view of their oxidizing effect at high concentrations, preferred are inorganic acids, and more preferred are one or more acids selected from the group consisting of sulfuric acid and nitric acid.

[0057] Examples of oxidizing agents include air, oxygen, and hydrogen peroxide.

[0058] Among the above compounds, the decomposing agent is preferably a metal alkoxide. A metal alkoxide is a compound in which the hydrogen atom of a hydroxyl group of an alcohol is substituted with a metal, and can be obtained by adding a metal to an alcohol.

[0059] The alcohol used to obtain the metal alkoxide is not particularly limited, and examples thereof include methanol, ethanol, 1-butanol, 2-butanol, 2-methyl-1-propanol, 2-methyl-2-propanol, 1-pentanol, 2-pentanol, 3-pentanol, 2-methyl-1-butanol, 2-methyl-2-butanol, 3-methyl-1-butanol, 3-methyl-2-butanol, 2,2-dimethyl-1-propanol, 1-hexanol, 2-Hexanol, 3-Hexanol, 2-Methyl-1-pentanol, 4-Methyl-2-pentanol, 2-Ethyl-1-butanol, 1-Heptanol, 2-Heptanol, 3-Heptanol, 2-Ethylhexanol, Dodecanol, Cyclohexanol, 1-Methylcyclohexanol, 2-Methylcyclohexanol, 3-Methylcyclohexanol, 4-Methylcyclohexanol, Benzyl alcohol, Phenoxyethanol, 1-(2-Hydroxyethyl) Examples of the alcohols include (2-pyrrolidone), diacetone alcohol, ethylene glycol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monobutyl ether, diethylene glycol, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monopropyl ether, diethylene glycol monobutyl ether, triethylene glycol, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, tetraethylene glycol, polyethylene glycol (molecular weight 200 to 400), 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, 1,5-pentanediol, glycerin, and dipropylene glycol. These alcohols may be used alone or in any combination and ratio of two or more.

[0060] The metal alkoxide may be in a solid state or in a solution state. From the viewpoint of the decomposition efficiency of the thermosetting resin cured material C, the metal alkoxide may be, for example, sodium methoxide, sodium ethoxide, sodium propoxide, sodium isopropoxide, sodium benzyl alkoxide (sodium benzyl oxide), potassium methoxide, potassium ethoxide, etc. It is preferable that the alkoxide is at least one selected from the group consisting of potassium alkoxide, potassium propoxide, isopropoxide, and potassium benzyl alkoxide (potassium benzyl oxide).

[0061] The organic solvent is not particularly limited, and examples thereof include alcohol-based solvents, ether-based solvents, aromatic solvents, etc. Among these, the organic solvent is preferably an alcohol-based solvent because it has excellent solubility for the decomposition product of the cured thermosetting resin C. The organic solvent may be used alone or as a mixture of two or more kinds in any combination and in any ratio.

[0062] Examples of alcohol-based solvents include 1-butanol, 2-butanol, 2-methyl-1-propanol, 2-methyl-2-propanol, 1-pentanol, 2-pentanol, 3-pentanol, 2-methyl-1-butanol, 2-methyl-2-butanol, 3-methyl-1-butanol, 3-methyl-2-butanol, 2,2-dimethyl-1-propanol, 1-hexanol, 2-hexanol, 3-hexanol, 2-methyl-1- Examples of the alcohol include pentanol, 4-methyl-2-pentanol, 2-ethyl-1-butanol, 1-heptanol, 2-heptanol, 3-heptanol, 2-ethylhexanol, dodecanol, cyclohexanol, 1-methylcyclohexanol, 2-methylcyclohexanol, 3-methylcyclohexanol, 4-methylcyclohexanol, benzyl alcohol, and phenoxyethanol, and benzyl alcohol is preferred.

[0063] Examples of ether solvents include diethyl ether, dipropyl ether, dibutyl ether, butyl methyl ether, butyl ethyl ether, diisoamyl ether, hexyl methyl ether, octyl methyl ether, cyclopentyl methyl ether, and dicyclopentyl ether.

[0064] Examples of aromatic solvents include benzene, toluene, xylene, alkylbenzenes such as trimethylbenzene and ethylbenzene, and alkylnaphthalenes such as methylnaphthalene, ethylnaphthalene, and dimethylnaphthalene.

[0065] Since the decomposition of the cured thermosetting resin C is usually carried out under heating conditions, the boiling point of the organic solvent under atmospheric pressure is preferably 100°C or higher, more preferably 120°C or higher, and even more preferably 150°C or higher. From this viewpoint, benzyl alcohol (boiling point: 205° C.) is a preferred organic solvent.

[0066] The treatment liquid containing the decomposing agent and the organic solvent may further contain other components as necessary, such as a surfactant and a low-viscosity solvent.

[0067] From the viewpoint of improving the decomposition efficiency of the cured thermosetting resin C, the concentration of the decomposing agent in the treatment liquid is preferably 0.001 mol / L or more and 100 mol / L or less, more preferably 0.005 mol / L or more and 50 mol / L or less, and even more preferably 0.01 mol / L or more and 20 mol / L or less. By setting the concentration of the decomposing agent to the above lower limit or more, the cured thermosetting resin B can be efficiently decomposed. By setting the concentration of the decomposing agent to the above upper limit or less, the cured thermosetting resin B can be decomposed without increasing the viscosity of the treatment liquid.

[0068] In preparing the treatment liquid, the decomposing agent may be mixed with the organic solvent in a solid state or in a solution state. In preparing the treatment liquid, there is no need to perform heating, and the treatment liquid can be prepared by mixing the organic solvent and the decomposing agent at room temperature of about 5° C. or higher and 35° C. or lower.

[0069] The reaction vessel is not particularly limited as long as it is capable of contacting the treatment liquid with the cured thermosetting resin C. As long as the vessel can be used as a decomposition tank, it may be box-shaped, cylindrical, mesh-like cage-shaped, or made of a porous material. From the viewpoint of dissolution efficiency, the ratio of the volume of the cured thermosetting resin C placed in the container to the volume of the container (filling rate) is preferably within the range of 5% to 50%.

[0070] The temperature of the treatment liquid when contacting the treatment liquid with the cured thermosetting resin C is preferably 100° C. or higher, more preferably 130° C. or higher, and even more preferably 150° C. or higher, from the viewpoint of improving the decomposition efficiency of the cured thermosetting resin C. On the other hand, from the viewpoint of suppressing denaturation of the organic solvent and the decomposition products, this temperature is preferably 300° C. or lower, more preferably 250° C. or lower, and even more preferably 200° C. or lower.

[0071] The contact time between the treatment liquid and the cured thermosetting resin C may be any time required for the cured thermosetting resin C to be sufficiently decomposed and dissolved, and varies depending on the type of thermosetting resin, the type and concentration of the decomposer and organic solvent, and the treatment temperature, but is preferably from 1 hour to 50 hours.

[0072] 1-4. Inorganic matter recovery process When the thermosetting resin cured material A contains an inorganic substance, the production method according to the present embodiment may include an inorganic substance recovery step of separating the phenol compound or its salt from the inorganic substance after the decomposition step and recovering the inorganic substance, thereby obtaining each of the phenol compound and the inorganic substance.

[0073] The method for recovering the inorganic substances is not particularly limited, and can be carried out by a known separation method such as filtration, sedimentation separation, stretching separation, etc. The recovered inorganic substances can be recycled.

[0074] 2. Epoxy resin manufacturing method The second embodiment of the present invention is a method for producing an epoxy resin, which includes a reaction step of reacting the phenol compound obtained by the production method according to the first embodiment of the present invention with epihalohydrin. Since the production method according to this embodiment uses, as a raw material, a phenol compound obtained by decomposing a cured thermosetting resin, hereinafter, the epoxy resin produced by the production method according to this embodiment may be referred to as a "recycled epoxy resin."

[0075] In the reaction step, a recycled epoxy resin is produced by a known one-step method for producing a recycled epoxy resin or a method similar thereto. The one-step method for producing a recycled epoxy resin is a method for obtaining a recycled epoxy resin by reacting a hydroxy compound raw material with epihalohydrin. In this embodiment, the hydroxy compound raw material contains a phenol compound obtained by the production method according to the first embodiment of the present invention, and may contain a polyhydric hydroxy compound (hereinafter, sometimes referred to as a "polyhydric hydroxy compound") as necessary.

[0076] The term "polyhydric hydroxy compound" is a general term for dihydric or higher phenol compounds and dihydric or higher alcohol compounds, and may be the same compound as the phenol compound obtained by the production method according to the first embodiment of the present invention. In the one-stage method for producing recycled epoxy resin, the "hydroxy compound raw material" is the total hydroxy compound including the phenol compound obtained by the production method according to the first embodiment of the present invention and the polyhydric hydroxy compound used as needed.

[0077] Polyhydric hydroxy compounds include bisphenol A, tetramethylbisphenol A, bisphenol F, tetramethylbisphenol F, bisphenol S, and bisphenol Various polyhydric phenols such as C, bisphenol AD, bisphenol AF, hydroquinone, resorcin, methylresorcin, biphenol, tetramethylbiphenol, dihydroxynaphthalene, dihydroxydiphenyl ether, thiodiphenols, phenol novolac resins, cresol novolac resins, phenol aralkyl resins, biphenyl aralkyl resins, naphthol aralkyl resins, terpene phenol resins, dicyclopentadiene phenol resins, bisphenol A novolac resins, naphthol novolac resins, brominated bisphenol A, and brominated phenol novolac resins; condensation reactions of various phenols with various aldehydes such as benzaldehyde, hydroxybenzaldehyde, crotonaldehyde, and glyoxal. polyhydric phenol resins obtained by a condensation reaction of xylene resin and phenols; various phenol resins such as co-condensation resins of heavy oils or pitches, phenols and formaldehydes; chain aliphatic diols such as ethylene glycol, trimethylene glycol, propylene glycol, 1,3-butanediol, 1,4-butanediol, 1,3-pentanediol, 1,4-pentanediol, 1,5-pentanediol, and 1,6-hexanediol; cyclic aliphatic diols such as cyclohexanediol and cyclodecanediol; and polyalkylene ether glycols such as polyethylene ether glycol, polyoxytrimethylene ether glycol, and polypropylene ether glycol.

[0078] In the reaction step, a phenol compound and a polyhydric hydroxy compound are dissolved in epihalohydrin to form a homogeneous solution, and the reaction is allowed to proceed.

[0079] Examples of epihalohydrin include epichlorohydrin, β-methylepichlorohydrin, epibromohydrin, etc. Among these, epihalohydrin is particularly preferably epichlorohydrin from the viewpoints of reactivity, availability of raw materials, and versatility of the resulting epoxy resin. The epihalohydrin may be used alone or in any combination of two or more kinds in any ratio.

[0080] The amount of epihalohydrin used is usually 1.0 equivalent or more and 14.0 equivalent or less, and preferably 2.0 equivalent or more and 10.0 equivalent or less, per equivalent of the total hydroxyl group of the hydroxy compound raw material (total hydroxy compounds). By setting the amount of epihalohydrin to the above lower limit or more, it is easy to control the polymerizing reaction, and the obtained recycled epoxy resin can have an appropriate epoxy equivalent. In addition, by setting the amount of epihalohydrin to the above upper limit or less, production efficiency tends to be improved.

[0081] Next, while stirring the solution, an alkali metal hydroxide is added in an amount of preferably 0.1 to 3.0 equivalents, more preferably 0.8 to 2.0 equivalents per equivalent of the total hydroxyl groups of the hydroxy compound raw material, in the form of a solid or aqueous solution, to react. By setting the amount of alkali metal hydroxide to the above lower limit or more, the unreacted hydroxyl groups and the generated epoxy resin are less likely to react, and therefore the polymerizing reaction can be easily controlled. In addition, by setting the amount of alkali metal hydroxide to the above upper limit or less, the generation of impurities due to side reactions can be suppressed. Examples of alkali metal hydroxides include sodium hydroxide and potassium hydroxide.

[0082] The reaction can be carried out under normal pressure or under reduced pressure. The reaction temperature is preferably 20° C. or higher and 200° C. or lower, more preferably 40° C. or higher and 150° C. or lower. By setting the reaction temperature to the above lower limit or higher, the reaction can be easily progressed and controlled. In addition, by setting the reaction temperature to the above upper limit or lower, side reactions can be suppressed and the amount of by-products can be reduced.

[0083] The reaction is carried out while dehydrating the reaction liquid by azeotroping while maintaining a predetermined temperature as necessary, cooling the volatilized steam, separating the condensate obtained, and returning the oil content without moisture to the reaction system. In order to suppress a rapid reaction, the alkali metal hydroxide is added intermittently or continuously in small amounts over a period of preferably 0.1 to 24 hours, more preferably 0.5 to 10 hours. By setting the addition time of the alkali metal hydroxide to the above lower limit or more, the reaction can be prevented from proceeding rapidly, making it easier to control the reaction temperature. In addition, by setting the addition time of the alkali metal hydroxide to the above upper limit or less, the amount of by-products can be reduced.

[0084] The reaction may be carried out in the presence of a catalyst, such as quaternary ammonium salts, such as tetramethylammonium chloride and tetraethylammonium bromide; tertiary amines, such as benzyldimethylamine and 2,4,6-tris(dimethylaminomethyl)phenol; imidazoles, such as 2-ethyl-4-methylimidazole and 2-phenylimidazole; phosphonium salts, such as ethyltriphenylphosphonium iodide; and phosphines, such as triphenylphosphine.

[0085] The reaction may be carried out in an inert organic solvent, such as alcohols, such as ethanol and isopropanol; ketones, such as acetone, methyl ethyl ketone, and methyl isobutyl ketone; ethers, such as dioxane and ethylene glycol dimethyl ether; glycol ethers, such as methoxypropanol; and aprotic polar solvents, such as dimethylsulfoxide and dimethylformamide.

[0086] After the reaction is completed, a typical post-treatment in the field of organic synthesis may be carried out, such as removing insoluble by-product salts by filtration or washing with water, followed by distilling off unreacted epihalohydrin by heating and / or distillation under reduced pressure.

[0087] 3. Manufacturing method of composite materials A third embodiment of the present invention is a method for producing a composite material, comprising a curing step of curing an epoxy resin composition containing the recycled epoxy resin obtained by the production method according to the second embodiment of the present invention and the inorganic material recovered in the inorganic material recovery step of the production method according to the first embodiment of the present invention (hereinafter sometimes referred to as "recycled inorganic material").

[0088] In this embodiment, the epoxy resin composition may contain, as necessary, an epoxy resin other than the recycled epoxy resin obtained by the production method according to the second embodiment of the present invention, a curing agent, a curing accelerator, a release agent, a coupling agent, and the like.

[0089] 3-1. Recycled epoxy resin The content of the recycled epoxy resin in the epoxy resin composition is not particularly limited, but the content of the recycled epoxy resin relative to 100 parts by mass of the total epoxy resin components is preferably 40 parts by mass or more, and more preferably 60 parts by mass or more, from the viewpoint of environmental harmony. When the epoxy resin composition contains other epoxy resins, the content of the recycled epoxy resin in 100 parts by mass of the total epoxy resin components is preferably 40 parts by mass or more and 99 parts by mass or less, and more preferably 60 parts by mass or more and 99 parts by mass or less. Note that the "total epoxy resin components" corresponds to the amount of all epoxy resins contained in the epoxy resin composition, and is the total of the recycled epoxy resin and other epoxy resins used as necessary.

[0090] 3-2.Other epoxy resins The epoxy resin composition may further contain other epoxy resins (hereinafter referred to as "other epoxy resins") in addition to the recycled epoxy resin obtained by the production method according to the second embodiment of the present invention. By including other epoxy resins, various physical properties can be improved.

[0091] The other epoxy resin corresponds to all epoxy resins other than the recycled epoxy resin obtained by the production method according to the second embodiment of the present invention, and may be the same type of epoxy resin as the recycled epoxy resin. The other epoxy resins may be used alone or in any combination of two or more in any ratio.

[0092] Other epoxy resins include, for example, bisphenol A type epoxy resins, bisphenol C type epoxy resins, trisphenolmethane type epoxy resins, anthracene type epoxy resins, phenol-modified xylene resin type epoxy resins, bisphenol cyclododecyl type epoxy resins, bisphenol diisopropylidene resorcin type epoxy resins, bisphenol F type epoxy resins, bisphenol AD ​​type epoxy resins, bisphenol AF type epoxy resins, hydroquinone type epoxy resins, methyl hydroquinone type epoxy resins, dibutyl hydroquinone type epoxy resins, resorcin type epoxy resins, methyl resorcin type epoxy resins, biphenol type epoxy resins, tetramethyl biphenol type epoxy resins, tetramethyl bisphenol F type epoxy resins, dihydroxy diphenyl ether type epoxy resins, epoxy resins derived from thiodiphenols, dihydroxy naphthalene type epoxy resins, dihydroxy anthracene type epoxy resins, dihydroxy dihydro anthracene type epoxy resins, dicyclopentadiene type epoxy resins, Examples of epoxy resins include epoxy resins derived from dihydroxystilbenes, phenol novolac type epoxy resins, cresol novolac type epoxy resins, bisphenol A novolac type epoxy resins, naphthol novolac type epoxy resins, phenol aralkyl type epoxy resins, naphthol aralkyl type epoxy resins, biphenyl aralkyl type epoxy resins, terpene phenol type epoxy resins, dicyclopentadiene phenol type epoxy resins, epoxy resins derived from a condensate of phenol and hydroxybenzaldehyde, epoxy resins derived from a condensate of phenol and crotonaldehyde, epoxy resins derived from a condensate of phenol and glyoxal, epoxy resins derived from a co-condensation resin of heavy oil or pitches, phenols, and formaldehydes, epoxy resins derived from diaminodiphenylmethane, epoxy resins derived from aminophenols, epoxy resins derived from xylylenediamine, epoxy resins derived from methylhexahydrophthalic acid, and epoxy resins derived from dimer acids.

[0093] When the epoxy resin composition contains other epoxy resins, the content of the other epoxy resins in 100 parts by mass of the total epoxy resin components is preferably 1 part by mass or more and 60 parts by mass or less, and more preferably 1 part by mass or more and 40 parts by mass or less.

[0094] 3-3.Inorganic substances The epoxy resin composition contains a recycled inorganic material, and may further contain a known inorganic filler for plastics. The recycled inorganic material is preferably one or more selected from the group consisting of carbon fiber and glass fiber, and more preferably carbon fiber. The known inorganic filler for plastics may be the same type of inorganic material as the recycled inorganic material.

[0095] The total content of the recycled inorganic material and the known inorganic filler for plastics in the epoxy resin composition is preferably 10% by mass or more and 95% by mass or less.

[0096] In addition, when the epoxy resin composition contains a known inorganic filler for plastics, the content of the recycled inorganic material is preferably 40 parts by mass or more and 99 parts by mass or less when the total amount of the recycled inorganic material and the known inorganic filler for plastics is 100 parts by mass, from the viewpoint of environmental friendliness. , more preferably 60 parts by mass or more and 99 parts by mass or less.

[0097] 3-4. Hardener The epoxy resin composition preferably contains a curing agent. As the curing agent, a known epoxy resin curing agent, for example, the curing agent described in the above section "1-1-1. Cured thermosetting resin A" can be used. The curing agent may be used alone or as a mixture of two or more kinds in any combination and in any ratio.

[0098] When the epoxy resin composition contains a curing agent, the content of the curing agent relative to 100 parts by mass of the total epoxy resin components is not particularly limited, but is preferably from 0.1 to 1,000 parts by mass, more preferably from 0.1 to 500 parts by mass, and even more preferably from 0.5 to 100 parts by mass.

[0099] When the curing agent is an amine-based curing agent or an acid anhydride-based curing agent, the content of the curing agent in the epoxy resin composition is preferably an amount such that the equivalent ratio of the functional groups in the curing agent to the epoxy groups in the total epoxy resin component is 0.1 or more and 2.0 or less, and more preferably an amount such that the equivalent ratio is 0.8 or more and 1.2 or less. By setting the content of the curing agent within the above range, the remaining amount of unreacted epoxy groups in the epoxy resin and unreacted functional groups in the curing agent can be reduced.

[0100] When the curing agent is an amide-based curing agent or an imidazole-based curing agent, the content of the curing agent relative to the total amount of all epoxy resin components and the curing agent in the epoxy resin composition is preferably 0.1 mass % or more and 20 mass % or less.

[0101] 3-5. Hardening accelerator The epoxy resin composition preferably contains a curing accelerator. By containing the curing accelerator, it is possible to shorten the curing time and lower the curing temperature, and it is possible to easily obtain a desired cured product.

[0102] As the curing accelerator, a known curing accelerator for epoxy resins, for example, the curing accelerators explained in the above section "1-1-1. Cured thermosetting resin A" can be used. The curing accelerator may be used alone or as a mixture of two or more kinds in any combination and in any ratio.

[0103] When the epoxy resin composition contains a curing accelerator, the content of the curing accelerator relative to 100 parts by mass of the total epoxy resin components is not particularly limited, but is preferably 0.1 parts by mass or more and 20 parts by mass or less. By making the content of the curing accelerator equal to or more than the above lower limit, a good curing acceleration effect can be obtained. In addition, by making the content of the curing accelerator equal to or less than the above upper limit, the desired curing properties can be easily obtained.

[0104] 3-6. Release agent The epoxy resin composition may contain a mold release agent. Examples of the mold release agent that can be used include natural waxes such as carnauba wax, synthetic waxes such as polyethylene wax, higher fatty acids such as stearic acid and zinc stearate, metal salts of the higher fatty acids, and hydrocarbon-based mold release agents such as paraffin. The release agent may be used alone or as a mixture of two or more kinds in any combination and in any ratio.

[0105] When the epoxy resin composition contains a mold release agent, the content of the mold release agent relative to 100 parts by mass of the total epoxy resin components is not particularly limited, but is preferably 0.001 parts by mass or more and 10.0 parts by mass or less. By setting the content of the release agent within the above range, it is possible to exhibit good releasability while maintaining the curing characteristics.

[0106] 3-7. Coupling agents The epoxy resin composition preferably contains a coupling agent, which can improve the adhesion between the epoxy resin matrix and inorganic substances.

[0107] The coupling agent includes a silane coupling agent and a titanate coupling agent. The coupling agent may be used alone or as a mixture of two or more kinds in any combination and in any ratio.

[0108] Examples of the silane coupling agent include epoxy silane coupling agents such as γ-glycidyloxypropyltrimethoxysilane, γ-glycidyloxypropyltriethoxysilane, and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; amino silane coupling agents such as γ-aminopropyltriethoxysilane, N-β(aminoethyl)γ-aminopropyltrimethoxysilane, N-β(aminoethyl)γ-aminopropylmethyldimethoxysilane, γ-aminopropyltrimethoxysilane, and γ-ureidopropyltriethoxysilane; mercapto silane coupling agents such as 3-mercaptopropyltrimethoxysilane; and vinyl silane coupling agents such as p-styryltrimethoxysilane, vinyltrichlorosilane, vinyltris(β-methoxyethoxy)silane, vinyltrimethoxysilane, vinyltriethoxysilane, and γ-methacryloxypropyltrimethoxysilane.

[0109] Examples of titanate coupling agents include isopropyl triisostearoyl titanate, isopropyl tri(N-aminoethyl aminoethyl) titanate, diisopropyl bis(dioctyl phosphate) titanate, tetraisopropyl bis(dioctyl phosphite) titanate, tetraoctyl bis(ditridecyl phosphite) titanate, tetra(2,2-diallyloxymethyl-1-butyl)bis(ditridecyl)phosphite titanate, bis(dioctyl pyrophosphate)oxyacetate titanate, and bis(dioctyl pyrophosphate)ethylene titanate.

[0110] When the epoxy resin composition contains a coupling agent, the content of the coupling agent relative to 100 parts by mass of the total epoxy resin components is not particularly limited, but is preferably 0.001 parts by mass or more and 10.0 parts by mass or less. By making the content of the coupling agent equal to or more than the above lower limit, the adhesiveness between the epoxy resin matrix and the inorganic material tends to be further improved. In addition, by making the content of the coupling agent equal to or less than the above upper limit, the coupling agent is less likely to bleed out from the obtained composite material.

[0111] 3-8.Other additives The epoxy resin composition may contain additives other than the above components, as necessary. Examples of the additives include flame retardants, plasticizers, reactive diluents, and pigments.

[0112] Examples of the flame retardant include halogen-based flame retardants such as brominated epoxy resins and brominated phenol resins; antimony compounds such as antimony trioxide; phosphorus-based flame retardants such as red phosphorus, phosphate esters, and phosphines; nitrogen-based flame retardants such as melamine derivatives; and inorganic flame retardants such as aluminum hydroxide and magnesium hydroxide.

[0113] 3-9.Curing process The curing step is a step of curing the above-mentioned epoxy resin composition, and a composite material can be obtained by this. The method of curing the epoxy resin composition is not particularly limited, but it is preferable to adopt a curing method by a thermosetting reaction. During the thermosetting reaction, it is preferable to appropriately select the curing temperature depending on the type of curing agent. For example, when an amine-based curing agent is used, the curing temperature is usually 80°C or higher and 250°C or lower. In addition, it is also possible to lower the curing temperature by adding a curing accelerator to these curing agents.

[0114] The reaction time is preferably 0.01 hours or more and 20 hours or less. By setting the reaction time to the above lower limit or more, the epoxy resin composition tends to be sufficiently cured. In addition, by setting the reaction time to the above upper limit or less, deterioration due to heating and energy loss during heating tend to be reduced. EXAMPLES

[0115] The present invention will be described in more detail below with reference to examples and comparative examples. However, the present invention is not limited to the following examples as long as it does not depart from the gist of the present invention. In addition, the various manufacturing conditions and evaluation result values ​​in the following examples have the meaning of preferred upper or lower limit values ​​in the embodiment of the present invention, and the preferred range may be a range defined by a combination of the above-mentioned upper or lower limit value and the values ​​of the following examples or values ​​between the examples. In the following examples, "room temperature" refers to a temperature range of 15°C or higher and 35°C or lower.

[0116] [Raw materials and reagents] The bisphenol A type epoxy resin (epoxy equivalent: 183 g / eq or 215 g / eq) used was a product of Mitsubishi Chemical Corporation. The 48% by mass aqueous sodium hydroxide solution, disilenediamide (DICY), 3-(3,4-dichlorophenyl)-1,1-dimethylurea (DCMU), hydrochloric acid, toluene, and acetonitrile were all products of Fujifilm Wako Pure Chemical Industries, Ltd. Benzyl alcohol used was a product of Sankyo Chemical Co., Ltd. The carbon fiber used was 3mm chopped carbon fiber manufactured by Yoshino Co., Ltd.

[0117] [analysis] The production and quantification of bisphenol A were carried out by high performance liquid chromatography according to the following procedures and conditions. ·Device: High-performance liquid chromatograph (Shimadzu Corporation) Pump: LC-20AD (Shimadzu Corporation) Column oven: CTO-20AC (Shimadzu Corporation) Detector: SPD-20A (Shimadzu Corporation) Column: 3 μm 250 mm × 4.6 mm ID (Intact Co., Ltd.) Method: Low pressure gradient method ·Analysis temperature: 40℃ ·Eluent composition: Solution A: Acetonitrile B liquid water At 0 min of analysis time, the eluent composition was A:B = 30:70 (volume ratio, same below), and from 0 to 5 min of analysis time the eluent composition was A:B = 30:70, then gradually changed to A:B = 0:100 from 5 to 20 min of analysis time, and from 20 to 35 min of analysis time it was A:B = 0:100. ·Flow rate: 1mL / min Detection wavelength: 280nm

[0118] [Swelling and fragmentation] Swelling and fragmentation refers to the fact that when a test piece of a cured thermosetting resin (length x width x thickness = 20 mm x 20 mm x 2 mm) was immersed in an organic solvent, the test piece swelled and became small pieces (length x width x thickness = 10 mm or less x 10 mm or less x 2 mm or less). The swelling and fragmentation were evaluated by immersing a test piece of length x width x thickness = 20 mm x 20 mm x 2 mm in an organic solvent and measuring the size of the fragments (or the test piece if it was not fragmented) after leaving it at room temperature for 3 days. The evaluation criteria are as follows: S: Length x Width x Thickness = 3mm or less x 3mm or less x 2mm or less A: Length x width x thickness = 3~10mm x 3~10mm x 2mm or less B: Length x width x thickness = 10~20mm x 10~20mm x 2mm or less C: Length x width x thickness = 20 mm x 20 mm x 2 mm (no change due to immersion in organic solvent)

[0119] [Epoxy equivalent] The epoxy equivalent of the epoxy resin was measured based on JIS K 7236:2009 (revised on January 20, 2009).

[0120] Reference Example 1: Preparation of amine cured product 280g of bisphenol A type epoxy resin (epoxy equivalent: 183g / eq), 2g of DICY, and 3g of DCMU were mixed thoroughly in an aluminum cup to obtain a mixture. The mixture was heated at 150°C for 3 hours to obtain an amine cured product.

[0121] Reference Example 2: Preparation of amine-cured CFRP 100 g of bisphenol A type epoxy resin (epoxy equivalent: 183 g / eq), 1 g of DICY, and 1 g of DCMU were placed in an aluminum cup and mixed thoroughly to obtain mixture 1. 100 g of carbon fiber was added to the obtained mixture 1 and mixed to obtain mixture 2. The obtained mixture 2 was poured into a flat mold and heated at 150°C for 3 hours to obtain an amine-cured carbon fiber composite material.

[0122] Example 1 About 10 g of the amine cured product obtained in Reference Example 1 (10 test pieces each measuring about 20 mm x 20 mm x 2 mm, each measuring about 1 g) and 50 g of formic acid were placed in a 100 mL glass bottle and allowed to stand for 3 days. After that, when the bottle was filtered using filter paper, the amine cured product swelled and softened, shrinking to small pieces measuring about 2 mm x 2 mm x 2 mm.

[0123] The obtained amine cured product was placed in a 100 mL Schlenk flask, and the internal pressure was adjusted to 10 kPa. The Schlenk flask was then immersed in an oil bath at 100° C. and dried by heating for 5 hours. After drying, the pressure inside the Schlenk flask was restored with nitrogen, the Schlenk flask was removed from the oil bath, and cooled to room temperature.

[0124] A stirrer, 50 g of benzyl alcohol, and 10 g of a 28% by mass solution of sodium methoxide in methanol were placed in the Schlenk flask containing the dried amine cured product. The Schlenk flask was then immersed in an oil bath at 185°C and decomposed for 2 hours. After decomposition, the amine cured product in the Schlenk flask disappeared and a homogeneous solution was formed. A portion of the decomposition liquid obtained was extracted and analyzed by high performance liquid chromatography, revealing that 0.5% by mass of bisphenol A was produced.

[0125] Comparative Example 1 In a Schlenk flask, a stirrer and 10 g of the amine cured product obtained in Reference Example 1 (approximately 20 mm × 20 Ten test pieces (approximately 1 g, 2 mm x 2 mm), 50 g of benzyl alcohol, and 10 g of a 28% by mass solution of sodium methoxide in methanol were placed in the flask. The flask was then immersed in an oil bath at 185°C and decomposed for 2 hours. After decomposition, an amine hardened product was observed in the flask. A portion of the decomposition liquid was extracted and analyzed by high performance liquid chromatography, revealing that 0.01% by mass of bisphenol A had been produced.

[0126] Comparative Example 2 About 10 g of the amine cured product obtained in Reference Example 1 (10 test pieces each measuring about 20 mm x 20 mm x 2 mm, each measuring about 1 g) and 50 g of formic acid were placed in a 100 mL glass bottle and allowed to stand for 3 days. After that, when the bottle was filtered using filter paper, the amine cured product swelled and softened, shrinking to small pieces measuring about 2 mm x 2 mm x 2 mm.

[0127] A stirrer, 50 g of benzyl alcohol, and 10 g of a 28% by mass solution of sodium methoxide in methanol were placed in the Schlenk flask containing the obtained amine cured product. The Schlenk flask was then immersed in an oil bath at 185°C and decomposed for 2 hours. After the decomposition, the amine cured product in the Schlenk flask was observed. A portion of the decomposition liquid obtained was extracted and analyzed by high performance liquid chromatography, but no generation of bisphenol A was observed.

[0128] Table 1 summarizes the presence or absence of immersion of the amine cured product in formic acid, the size of the amine cured product before decomposition, the presence or absence of distillation of formic acid, the presence or absence of the amine cured product after decomposition, and the amount of bisphenol A produced in Example 1 and Comparative Examples 1 and 2. Table 1 shows that by immersing the amine cured product in formic acid, the amine cured product swells and breaks into small pieces, and decomposition easily proceeds, allowing bisphenol A to be produced efficiently.

[0129] [Table 1]

[0130] Example 2 The same procedure as in Example 1 was repeated, except that 10 g of the 28 mass % sodium methoxide methanol solution was replaced with 4.3 g of a 48 mass % sodium hydroxide aqueous solution. After decomposition, 0.3 mass % of bisphenol A was produced.

[0131] Example 3 The same procedure as in Example 1 was repeated, except that 6 g of 8 mol / L potassium hydroxide solution was used instead of 10 g of the 28 mass % sodium methoxide methanol solution in Example 1. After decomposition, 0.2 mass % of bisphenol A was produced.

[0132] Example 4 200 g of the amine-cured carbon fiber composite obtained in Reference Example 2 and 500 g of formic acid were placed in a glass bottle and left to stand at room temperature for one week. After that, the formic acid was removed by filtration to obtain a swollen and fragmented amine-cured carbon fiber composite. The size of the fragments of the obtained carbon fiber composite was 1 mm or less × 1 mm or less × 1 mm or less. The obtained amine-cured carbon fiber composite was placed in a 500 mL eggplant-shaped flask and the internal pressure was set to 10 kPa. Then, the eggplant-shaped flask was immersed in an oil bath at 100°C and dried by heating for 5 hours. After drying, the pressure inside the Schlenk flask was restored with nitrogen, the eggplant-shaped flask was removed from the oil bath, and cooled to room temperature to obtain a dried amine-cured carbon fiber composite.

[0133] The obtained amine-cured carbon fiber composite, 500 g of benzyl alcohol, and 200 g of a 28% by mass solution of sodium methoxide in methanol were placed in a stainless steel separable flask equipped with a cooling tube, a thermometer, and a stirrer, and a nitrogen atmosphere was created. The separable flask was immersed in an oil bath heated to 185°C, and the mixture was stirred for 3 hours to obtain a decomposition liquid. A portion of the obtained decomposition liquid was extracted and subjected to high performance liquid chromatography, revealing that 0.2% by mass of bisphenol A was produced.

[0134] The separable flask was removed from the oil bath and cooled to room temperature. The decomposition liquid was then filtered under reduced pressure to separate the crude carbon fiber and the filtrate into a solid-liquid separation. The crude carbon fiber obtained was washed with acetone and water, and then dried at 170°C for 5 hours under reduced pressure of 10 kPa to obtain 95 g of recycled carbon fiber.

[0135] The entire amount of the decomposition liquid obtained and 600 g of water were placed in a jacketed separable flask equipped with a Dimroth condenser, stirring blade, and thermometer under a nitrogen atmosphere and mixed for 1 hour. After that, the mixture was left to stand to separate organic phase 1 and aqueous phase 1 into oil and water, and aqueous phase 1 was extracted. 600 g of water was added again to the obtained organic phase 1 and mixed for 1 hour. After that, the mixture was left to stand to separate organic phase 2 and aqueous phase 2 into oil and water, and aqueous phase 2 was extracted.

[0136] The aqueous phase 1 and the aqueous phase 2 were placed in a jacketed separable flask equipped with a Dimroth condenser, a stirring blade, and a thermometer under a nitrogen atmosphere, and then 200 g of toluene was added and mixed, and the internal temperature was raised to 80 ° C. The aqueous phase was neutralized with hydrochloric acid while maintaining the internal temperature at 80 ° C. Then, the mixture was left to stand for oil-water separation, and the aqueous phase 3 was extracted to obtain an organic phase 3. 200 g of water was added to the obtained organic phase 3, and the mixture was mixed while maintaining the internal temperature at 80 ° C. Then, the mixture was left to stand for oil-water separation, and the aqueous phase 4 was extracted to obtain an organic phase 4. The obtained organic phase 4 was cooled to 10 ° C. to obtain a slurry liquid. The obtained slurry liquid was filtered by reduced pressure filtration to obtain a cake. The entire cake was dried using an evaporator equipped with an oil bath at an oil bath temperature of 85 ° C. and 15 Torr for 3 hours, and 11 g of solid was obtained. The obtained solid was confirmed by high performance liquid chromatography to be bisphenol A and had a purity of 99%.

[0137] In a 0.5L four-neck flask equipped with a thermometer, a stirrer, and a cooling tube, 11g of the obtained bisphenol A, 84g of epichlorohydrin, 26g of isopropanol, and 13g of water were charged, and the temperature was raised to 40°C to dissolve uniformly, and then 10g of 48% by mass aqueous sodium hydroxide solution was dropped over 90 minutes. At the same time as the dropwise addition, the temperature was raised from 40°C to 65°C over 90 minutes. Then, the reaction was completed by holding at 65°C for 30 minutes, and the reaction liquid was transferred to a 1L separatory funnel, and 23g of water at 65°C was added to the separatory funnel and left to stand at 65°C for 1 hour. After standing, the aqueous phase was extracted from the separated oil phase and aqueous phase, and by-product salt and excess sodium hydroxide were removed. Then, epichlorohydrin was completely removed from the oil phase under reduced pressure at 150°C to obtain a residue.

[0138] Then, 35 g of methyl isobutyl ketone was added to the resulting residue, and the temperature was raised to 65°C. After uniformly dissolving, the mixture was mixed with 0.4 g of a 48% by mass aqueous solution of sodium hydroxide and reacted for 60 minutes. Thereafter, the reaction solution was mixed with 15 g of methyl isobutyl ketone and washed four times with 100 g of water. Thereafter, methyl isobutyl ketone was completely removed under reduced pressure at 150° C. to obtain an epoxy resin. The epoxy equivalent of the obtained epoxy resin was 215 g / eq.

[0139] 5 g of the obtained epoxy resin (epoxy equivalent: 215 g / eq), 0.05 g of DICY, and 0.05 g of DCMU were placed in an aluminum cup and mixed thoroughly to obtain mixture 1. 5 g of the obtained recycled carbon fiber was placed therein and mixed thoroughly to obtain mixture 2. The obtained mixture 2 was poured into a flat mold and heated at 150°C for 3 hours to obtain a recycled amine cured carbon fiber composite material.

Claims

1. A method for producing a phenol compound from a cured thermosetting resin, comprising the steps of: a swelling step of contacting the cured thermosetting resin A with an organic solvent to swell and fragment the cured thermosetting resin A to obtain a cured thermosetting resin B; A drying step of drying the thermosetting resin cured material B to obtain a thermosetting resin cured material C; and A decomposition step of decomposing the thermosetting resin cured material C. A method for producing a phenolic compound, comprising:

2. The method for producing a phenol compound according to claim 1, wherein the organic solvent has a boiling point of 150° C. or lower under atmospheric pressure.

3. The method for producing a phenolic compound according to claim 1 , wherein the organic solvent is formic acid.

4. The method for producing a phenolic compound according to claim 1 , wherein the thermosetting resin cured product A is an epoxy resin cured with an amine-based curing agent.

5. The method for producing a phenol compound according to claim 1, wherein the decomposition step is carried out in the presence of one or more decomposition agents selected from the group consisting of bases, acids, and oxidizing agents.

6. The method for producing a phenol compound according to claim 5, wherein the base is one or more selected from the group consisting of sodium compounds and potassium compounds.

7. The method for producing a phenol compound according to claim 5, wherein the acid is at least one selected from the group consisting of sulfuric acid and nitric acid.

8. The thermosetting resin cured material A contains an inorganic substance, The method for producing a phenolic compound according to claim 1 , further comprising, after the decomposition step, an inorganic matter recovery step of recovering the inorganic matter.

9. The method for producing a phenol compound according to claim 8, wherein the inorganic material is at least one selected from the group consisting of carbon fiber and glass fiber.

10. A method for producing an epoxy resin, comprising a reaction step of reacting the phenol compound obtained by the method for producing a phenol compound according to any one of claims 1 to 9 with epihalohydrin.

11. A method for producing a composite material, comprising a curing step of curing an epoxy resin composition containing the epoxy resin obtained by the method for producing an epoxy resin according to claim 10 and the inorganic substance obtained by the method for producing a phenol compound according to claim 8 or 9.

Citation Information

Patent Citations

  • Method for decomposing and recycling thermosetting resin

    JP1998024274A