Method for producing phenolic compound, method for producing epoxy resin, method for producing composite material, method for producing inorganic fiber, and method for producing inorganic fiber-reinforced resin

By swelling and decomposing cured thermosetting resins with an organic solvent, the method addresses the challenge of crushing and decomposition, enabling the recovery of phenol compounds and production of epoxy resins and composite materials.

JP2024165142APending Publication Date: 2024-11-28MITSUBISHI CHEM CORP

Patent Information

Application Number
JP2023081044
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-16
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

The difficulty in crushing and decomposing cured thermosetting resins, which results in complex mixtures and the inability to obtain monomer raw materials like phenol compounds during chemical recycling.

Method used

A method involving swelling cured thermosetting resins with an organic solvent followed by decomposition, which allows for the production of phenol compounds and inorganic substances, and further processing into epoxy resins and composite materials.

Benefits of technology

Facilitates the easy crushing and decomposition of cured thermosetting resins, enabling the recovery of phenol compounds and inorganic substances, and the production of epoxy resins and composite materials with improved efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024165142000001
    Figure 2024165142000001
  • Figure 2024165142000002
    Figure 2024165142000002
  • Figure 2024165142000003
    Figure 2024165142000003
Patent Text Reader

Abstract

To provide a method for producing a phenolic compound by decomposing a thermosetting cured resin, the method mitigating the problem of crushing difficulty in the thermosetting cured resin.SOLUTION: A method for producing a phenolic compound from a thermosetting cured resin includes: a swelling step for contacting a thermosetting cured resin A with an organic solvent to swell the thermosetting cured resin A, thereby yielding a thermosetting cured resin B; and a decomposition step for decomposing the thermosetting cured resin B.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a phenolic compound, a method for producing an epoxy resin, a method for producing a composite material, a method for producing an inorganic fiber, and a method for producing an inorganic fiber-reinforced resin. [Background technology]

[0002] Thermosetting resins are used in various applications because they can be highly reinforced by blending fillers, additives, etc. Among them, epoxy resins are important materials used in various applications such as adhesives, insulating materials, paints, casting materials, and composite materials because they exhibit excellent adhesive properties, electrical properties, and heat resistance.

[0003] On the other hand, a cured thermosetting resin obtained by curing a thermosetting resin does not melt and is difficult to dissolve in a general-purpose solvent. This is because the cured thermosetting resin has a complex structure that is three-dimensionally crosslinked. Therefore, when chemically recycling a cured thermosetting resin, it is necessary to crush or pulverize the cured thermosetting resin prior to decomposition treatment (see Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 10-024274 Summary of the Invention [Problem to be solved by the invention]

[0005] In the conventional chemical recycling of thermosetting resin cured products, the thermosetting resin cured products are crushed or pulverized before being fed to a decomposition tank, but because the thermosetting resin cured products are hard, crushing or pulverizing them is extremely difficult. In addition, because it takes time to decompose the thermosetting resin cured products, the decomposition products become a complex mixture, making it impossible to obtain monomer raw materials such as phenol compounds.

[0006] The present invention has been made in view of the above circumstances. That is, an object of the present invention is to provide a method for producing a phenol compound by decomposing a cured thermosetting resin material, which reduces the problem of the difficulty of crushing the cured thermosetting resin material. [Means for solving the problem]

[0007] As a result of intensive research to solve the above problems, the present inventors have found that a phenolic compound can be produced by contacting a cured thermosetting resin with an organic solvent to swell it and then decomposing it. They have also found that a phenolic compound and an inorganic substance can be co-produced by using a cured thermosetting resin containing an inorganic substance. They have also found a method for producing an epoxy resin from the obtained phenolic compound, and a method for producing a composite material from the epoxy resin and an inorganic substance recovered from the cured thermosetting resin. That is, the present invention includes the following inventions.

[0008] [1] A method for producing a phenol compound from a cured thermosetting resin, comprising the steps of: a swelling step of contacting a cured thermosetting resin material A with an organic solvent to swell the cured thermosetting resin material A and obtain a cured thermosetting resin material B; a decomposition step of decomposing the thermosetting resin cured material B; A method for producing a phenolic compound, comprising: [2] The method for producing a phenol compound according to [1], wherein in the swelling step, a ratio of the mass of the cured thermosetting resin B to the mass of the cured thermosetting resin A is 1.2 or more. [3] The method for producing a phenol compound according to [1] or [2], wherein the organic solvent is at least one selected from the group consisting of N-methylpyrrolidone and benzyl alcohol. [4] The method for producing a phenol compound according to any one of [1] to [3], wherein the decomposition step is carried out in the presence of one or more decomposition agents selected from the group consisting of bases, acids, and oxidizing agents. The method for producing a phenol compound according to [4], wherein the base is one or more selected from the group consisting of sodium compounds and potassium compounds. [6] The method for producing a phenol compound according to [4] or [5], wherein the acid is one or more selected from the group consisting of sulfuric acid and nitric acid. [7] The method for producing a phenol compound according to any one of [1] to [6], wherein the thermosetting resin cured product A is an epoxy resin cured product. [8] The thermosetting resin cured material A contains an inorganic substance, The method for producing a phenol compound according to any one of [1] to [7], further comprising, after the decomposition step, an inorganic matter recovery step of recovering the inorganic matter. [9] The method for producing a phenol compound according to [8], wherein the inorganic material is at least one type selected from the group consisting of carbon fiber and glass fiber.

[10] A method for producing an epoxy resin, comprising a reaction step of reacting the phenol compound obtained by the method for producing a phenol compound according to any one of [1] to [9] with epihalohydrin.

[11] A method for producing a composite material, comprising a curing step of curing an epoxy resin composition containing the epoxy resin obtained by the method for producing an epoxy resin according to

[10] and the inorganic substance obtained by the method for producing a phenol compound according to [8] or [9].

[12] A method for producing inorganic fibers from an inorganic fiber reinforced resin, comprising the steps of: a swelling step of contacting an inorganic fiber reinforced resin A containing inorganic fibers and a cured thermosetting resin with an organic solvent to swell the inorganic fiber reinforced resin A and obtain an inorganic fiber reinforced resin B; An inorganic fiber recovery step of separating inorganic fibers from the inorganic fiber reinforced resin B; A method for producing inorganic fibers, comprising:

[13] A method for producing an inorganic fiber-reinforced resin, comprising a curing step of curing a thermosetting resin composition containing a thermosetting resin and the inorganic fibers obtained by the method for producing inorganic fibers according to

[12] . Effect of the Invention

[0009] According to the present invention, there can be provided a method for producing a phenol compound by decomposing a cured thermosetting resin, which reduces the problem of the difficulty in crushing the cured thermosetting resin. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The following is a detailed description of the embodiments of the present invention, but the present invention is not limited to the following description, and can be modified as desired without departing from the scope of the present invention. In addition, in this specification, when a numerical value or physical property value is enclosed before and after "~", the values ​​before and after the "~" are included.

[0011] 1. Method for producing phenolic compounds The first embodiment of the present invention is a method for producing a phenol compound from a cured thermosetting resin, which includes a swelling step of bringing a cured thermosetting resin A into contact with an organic solvent to swell the cured thermosetting resin A and obtain a cured thermosetting resin B, and a decomposition step of decomposing the cured thermosetting resin B. The phenol compound produced by the production method according to this embodiment is a compound derived from a monomer, a curing agent, an end-capping agent, etc. of a thermosetting resin.

[0012] 1-1. Swelling process The swelling step is a step of swelling the thermosetting resin cured material A by contacting it with an organic solvent. In the swelling step, the thermosetting resin cured material swells and softens, so that it can be crushed more easily than the thermosetting resin cured material before swelling. That is, while crushing a thermosetting resin cured material has been a difficult task in the past, the manufacturing method of the present embodiment has found that crushing can be easily performed by using a simple operation of contacting a thermosetting resin cured material with an organic solvent, and a phenolic compound can be easily produced from a thermosetting resin cured material. In addition, the thermosetting resin cured material A is easily decomposed by increasing the solid-liquid contact area of ​​the thermosetting resin cured material A due to swelling, so that the decomposition time can be shortened compared to the conventional method.

[0013] 1-1-1. Thermosetting resin cured product A The cured thermosetting resin A that swells in the swelling step is a product of curing a thermosetting resin with or without a curing agent in the presence or absence of a curing accelerator, and is preferably a product of curing a thermosetting resin with a curing agent. The cured thermosetting resin A has a structure derived from a phenol compound in its structure (e.g., a structural unit, a terminal structure, a crosslinked structure, etc.).

[0014] The thermosetting resin is not particularly limited, but preferable examples thereof include a copolymer of a phenolic compound and another monomer, a homopolymer of an epoxidized product of a phenolic compound, and a copolymer of an epoxidized product of a phenolic compound and another monomer, etc. Examples of such thermosetting resins include epoxy resins and phenolic resins.

[0015] The phenol compound is not particularly limited, and may be, for example, a monohydric phenol compound, a dihydric phenol compound, a bisphenol compound, or the like.

[0016] Examples of monovalent phenolic compounds include phenol, o-cresol, m-cresol, p-cresol, p-ethylphenol, p-isopropylphenol, p-tert-butylphenol, p-cumylphenol, p-cyclohexylphenol, p-octylphenol, p-nonylphenol, 2,4-xylenol, p-methoxyphenol, p-hexyloxyphenol, p-decyloxyphenol, o-chlorophenol, m-chlorophenol, p-chlorophenol, p-bromophenol, pentabromophenol, pentachlorophenol, o-nitrophenol, m-nitrophenol, p-nitrophenol, 2,4,6-trinitrophenol, o-phenolsulfonic acid, m-phenolsulfonic acid, p-phenolsulfonic acid, p-phenylphenol, p-isopropenylphenol, 2,4-di(1'-methyl-1'-phenylethyl)phenol, β-naphthol, α-naphthol, p-(2',4',4'-trimethylchromanyl ... 2-(4'-methoxyphenyl)-2-(4''-hydroxyphenyl)propane and the like.

[0017] Examples of the divalent phenol compound include hydroquinone, resorcinol, and 2-methylresorcinol.

[0018] Examples of bisphenol compounds include 2,2'-biphenol, 4,4'-biphenol, 1,5-naphthalenediol, 2,7-naphthalenediol, bis(4-hydroxyphenyl)methane (i.e., bisphenol F), bis{(4-hydroxy-3,5-dimethyl)phenyl}methane, 1,1-bis(4-hydroxyphenyl)ethane (i.e., bisphenol E), 1,1-bis(4-hydroxyphenyl)-1-phenylethane (i.e., bisphenol AP), and 2,2-bis(4-hydroxyphenyl)hexafluoropropane. (i.e., bisphenol AF), 2,2-bis(4-hydroxyphenyl)propane (i.e., bisphenol A), 2,2-bis{(4-hydroxy-3-methyl)phenyl}propane (i.e., bisphenol C), 2,2-bis{(4-hydroxy-3,5-dimethyl)phenyl}propane, 2,2-bis{(3,5-dibromo-4-hydroxy)phenyl}propane, 2,2-bis{(3-isopropyl-4-hydroxy)phenyl}propane, 2,2-bis{(4-hydroxy-3-phenyl)phenyl}propane, 2-(4-hydroxyphenyl)phenyl Bisphenol B, 1,1-bis(4-hydroxyphenyl)-1,1-diphenylmethane (i.e., bisphenol B), 2-(2-hydroxyphenyl)-2-(4-hydroxyphenyl)propane, 1-(4-hydroxyphenyl)-1,3,3-trimethyl-5-hydroxyindan, 2-(4-hydroxyphenyl)-[3-{2-(4-hydroxyphenyl)propan-2-yl}-4-hydroxyphenyl]propane, 2,2-bis(4-hydroxyphenyl)butane (i.e., bisphenol B), 1,1-bis(4-hydroxyphenyl)-1,1-diphenylmethane (i.e., , bisphenol BP), 4,4′-isopropylidenebis(2-methyl-phenol) (i.e., bisphenol C), 2,2-bis(4-hydroxy-3-isopropylphenyl)propane (i.e., bisphenol G), 2,2-bis(4-hydroxyphenyl)-3-methylbutane, 2,2-bis(4-hydroxyphenyl)-3,3-dimethylbutane, 2,4-bis(4-hydroxyphenyl)-2-methylbutane, 2,2-bis(4-hydroxyphenyl)pentane, 2,2-bis(4-hydroxyphenyl)-4-methylpentane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)-4-isopropylcyclohexane, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, 9,9-bis(4-hydroxyphenyl)fluorene, 9,9-bis{(4-hydroxy-3-methyl)phenyl}fluorene, α,α'-bis(4-hydroxyphenyl)-o-diisopropylbenzene, α,α'-bis(4-hydroxyphenyl)-m-diisopropylbenzene benzene, α,α'-bis(4-hydroxyphenyl)-p-diisopropylbenzene, 1,3-bis(4-hydroxyphenyl)-5,7-dimethyladamantane, 4,4'-dihydroxydiphenyl sulfone (i.e., bisphenol S), 4,4'-dihydroxydiphenyl sulfoxide, 4,4'-dihydroxydiphenyl sulfide, 4,4'-dihydroxydiphenyl ketone, 4,4'-dihydroxydiphenyl ether, and 4,4'-dihydroxydiphenyl ester.

[0019] Of these, the phenol compound is preferably a bisphenol compound, and examples of the phenol compound include 2,2-bis(4-hydroxyphenyl)propane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, 2,2-bis(4-hydroxyphenyl)hexafluoropropane, 2,2-bis(4-hydroxyphenyl)butane, 1,1-bis(4-hydroxyphenyl)-1,1-diphenylmethane, 4,4'-isopropylidenebis(2-methylphenol), 1,1-bis(4-hydroxyphenyl)ethane, ... More preferably, the aryl group is selected from 2,2-bis(4-hydroxyphenyl)methane, 2,2-bis(4-hydroxy-3-isopropylphenyl), and 4,4'-dihydroxydiphenyl sulfone, and further preferably, is 2,2-bis(4-hydroxyphenyl)propane.

[0020] The epoxy resin is not particularly limited, and examples thereof include diglycidyl ethers of the above-mentioned bisphenol compounds; bisphenol type epoxy resins such as bisphenol A type epoxy resin, bisphenol F type epoxy resin, and bisphenol S type epoxy resin; novolac epoxy resins such as phenol novolac type epoxy resin, cresol novolac type epoxy resin, and bisphenol A novolac type epoxy resin; biphenyl type epoxy resin; glycidyl ester type epoxy resin; glycidyl amine type epoxy resin; linear aliphatic epoxy resin; alicyclic epoxy resin; heterocyclic epoxy resin; and alkyl substituted products, halides, and hydrogenated products thereof.

[0021] In the technical field of the present invention, "epoxy resin" includes polymers containing repeating units and epoxy compounds with a monomolecular structure (i.e., non-polymer compounds), both of which are sometimes expressed and sold as "epoxy resins". A mixture of two or more epoxy resins may also be simply called "epoxy resin". In this specification, "epoxy resin" refers to any of polymers containing repeating units, epoxy compounds with a monomolecular structure, and mixtures thereof.

[0022] The cured thermosetting resin may be a cured product of one type of thermosetting resin, or a cured product of a mixture of two or more types of thermosetting resins in any combination and ratio.

[0023] In this specification, a curing agent means a substance that contributes to the crosslinking reaction and / or chain extension reaction of a thermosetting resin. Even substances that are usually called "curing accelerators" are considered to be curing agents as long as they contribute to the crosslinking reaction and / or chain extension reaction of a thermosetting resin.

[0024] Examples of the curing agent for the thermosetting resin include a phenol-based curing agent, a polyisocyanate-based curing agent, an amine-based curing agent, an acid anhydride-based curing agent, an imidazole-based curing agent, an amide-based curing agent, a mercaptan-based curing agent, a cationic polymerization initiator, an organic phosphine-based curing agent, a phosphonium salt-based curing agent, and a tetraphenyl boronate-based curing agent. Of these, the curing agent is preferably one or more selected from the group consisting of an amine-based curing agent, an acid anhydride-based curing agent, and a phenol-based curing agent.

[0025] In view of the above, the thermosetting resin cured material A is preferably an epoxy resin cured material, more preferably an epoxy resin cured with one or more curing agents selected from the group consisting of an amine-based curing agent, an acid anhydride-based curing agent, and a phenol-based curing agent, and even more preferably an epoxy resin cured with an amine-based curing agent, an acid anhydride-based curing agent, or a phenol-based curing agent.

[0026] Examples of phenol-based curing agents include bisphenols such as bisphenol A, bisphenol F, bisphenol S, bisphenol B, bisphenol AD, bisphenol Z, and tetrabromobisphenol A; biphenols such as 4,4'-biphenol and 3,3',5,5'-tetramethyl-4,4'-biphenol; benzenediols such as catechol, resorcin, and hydroquinone; and polyfunctional phenols such as naphthalenediols. The hydrogen atoms bonded to the aromatic rings of these compounds may be substituted with non-interfering substituents, such as halogeno groups, alkyl groups, aryl groups, ether groups, ester groups, and organic substituents containing heteroelements such as sulfur, phosphorus, and silicon. In this specification, the term "benzenediols" refers to compounds having one benzene ring with two hydroxyl groups directly bonded to this benzene ring.

[0027] The phenol-based curing agent may be novolak resins and resol resins which are polycondensates of the above-mentioned polyfunctional phenols and aldehydes, and novolak resins and resol resins which are polycondensates of monofunctional phenols such as phenol, cresol, and alkylphenol and aldehydes.

[0028] Examples of polyisocyanate-based curing agents include tolylene diisocyanate, methylcyclohexane diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate, xylylene diisocyanate, hydrogenated xylylene diisocyanate, dimer acid diisocyanate, trimethylhexamethylene diisocyanate, and lysine triisocyanate.

[0029] The polyisocyanate-based curing agent may be a polyisocyanate compound obtained by reacting the above-mentioned polyisocyanate compound with a compound having at least two active hydrogen atoms such as an amino group, a hydroxyl group, a carboxyl group, or water; or a trimer to pentamer of the above-mentioned polyisocyanate compound; or the like.

[0030] Examples of the amine-based curing agent include aliphatic primary amines, aliphatic secondary amines, aliphatic tertiary amines, aromatic primary amines, aromatic secondary amines, aromatic tertiary amines, cyclic amines, guanidines, and urea derivatives. More specific examples of the amine-based curing agent include triethylenetetramine, diaminodiphenylmethane, diaminodiphenylether, metaxylenediamine, dicyandiamide (DICY), 1,8-diazabicyclo(5,4,0)-7-undecene, 1,5-diazabicyclo(4,3,0)-5-nonene, dimethylurea, and guanylurea.

[0031] Examples of acid anhydride curing agents include condensates of maleic anhydride and unsaturated compounds, phthalic anhydride, 4-methylhexahydrophthalic anhydride, hexahydrophthalic anhydride, and trimellitic anhydride.

[0032] Examples of imidazole-based curing agents include 1-isobutyl-2-methylimidazole, 2-methylimidazole, 1-benzyl-2-methylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, and benzimidazole. Although imidazole-based curing agents also function as curing accelerators, they are classified as curing agents in this embodiment.

[0033] Examples of the amide-based curing agent include polyamide resins.

[0034] Examples of the mercaptan curing agent include polysulfide type mercaptan compounds, thioester type mercaptan compounds, and thioether type mercaptan compounds.

[0035] The cationic polymerization initiator generates cations by heat or irradiation with active energy rays, and examples of the initiator include aromatic onium salts. Specifically, SbF 6- , B.F. 4 -, AsF 6- , P.F. 6- , C.F. 3 SO 3 2 - and B(C 6 F 5 ) 4- and an aromatic cation component containing an atom selected from iodine, sulfur, nitrogen, and phosphorus. The aromatic onium salt is preferably one or more salts selected from the group consisting of diaryliodonium salts and triarylsulfonium salts.

[0036] Examples of the organic phosphine curing agent include tributylphosphine, methyldiphenylphosphine, triphenylphosphine, diphenylphosphine, and phenylphosphine.

[0037] Examples of phosphonium salt curing agents include tetraphenylphosphonium tetraphenylborate, tetraphenylphosphonium ethyltriphenylborate, and tetrabutylphosphonium tetrabutylborate.

[0038] Examples of the tetraphenylborate-based curing agent include 2-ethyl-4-methylimidazole·tetraphenylborate, and N-methylmorpholine·tetraphenylborate.

[0039] The curing agent may be used alone or as a mixture of two or more kinds in any combination and in any ratio.

[0040] The thermosetting resin cured material A may be a product obtained by curing a thermosetting resin using a curing accelerator. The curing accelerator is not particularly limited, and known curing accelerators for epoxy resins, such as urea compounds such as 3-(3,4-dichlorophenyl)-1,1-dimethylurea (DCMU), alkali metal compounds, imidazole compounds, tertiary amine compounds, quaternary ammonium salts, and organic phosphorus compounds, can be used. The curing accelerator may be used alone or as a mixture of two or more kinds in any combination and in any ratio.

[0041] The cured thermosetting resin may be mixed with other components to form a composite material, as long as the effects of the present invention are not impaired. Examples of the other components include inorganic substances and thermoplastic resins. The other components may be used alone or as a mixture of two or more kinds in any combination and ratio.

[0042] The inorganic substance is not particularly limited, but examples thereof include carbon, glass, metal, and metal compounds such as fused silica, crystalline silica, alumina, calcium carbonate, calcium sulfate, talc, and boron nitride. The inorganic substance may be in the form of fiber, particle, foil, etc., and is preferably fiber. Among these, the inorganic substance is preferably one or more types selected from the group consisting of carbon fiber and glass fiber, and more preferably carbon fiber.

[0043] The fibers may be in the form of a nonwoven fabric or a woven fabric. If in the form of a woven fabric, it may be a cross material made by weaving fiber bundles, or a UD (Uni-Directional) material in which fiber bundles are arranged in one direction.

[0044] Examples of the thermoplastic resin include polyethylene and polypropylene.

[0045] 1-1-2. Organic solvents The organic solvent is not particularly limited as long as it can swell the cured thermosetting resin A, but since the swelling step is preferably carried out under heating conditions, the organic solvent has a boiling point of 120° C. or more at atmospheric pressure, and more preferably an organic solvent has a boiling point of 150° C. or more at atmospheric pressure. The upper limit of the boiling point of the organic solvent at atmospheric pressure is not particularly limited, but is preferably 300° C. or less, and more preferably 280° C. or less. The organic solvent may be used alone or in any combination and ratio of two or more kinds. This is also fine.

[0046] Preferred examples of such organic solvents include alcohol-based solvents, amide-based solvents, and aminoalcohol-based solvents.

[0047] As the alcohol-based solvent, the same as those exemplified as the alcohol-based solvent, which is one type of organic solvent that can be used in the decomposition step described below, can be used, and benzyl alcohol is preferred.

[0048] Examples of amide solvents include N-methylpyrrolidone (NMP), diethylformamide (DEF), N,N-dimethylacetamide (DMA), N,N-dimethylformamide (DMF), tetramethylurea (TMU), and hexamethylphosphoric acid triamide (HMPA).

[0049] Aminoalcohol solvents include 2-aminoethanol, 2-amino-2-methyl-1-propanol, 2-(methylamino)ethanol, 2-(ethylamino)ethanol, 2-(butylamino)ethanol, and diethanolamine.

[0050] Among these, the organic solvent is preferably one or more selected from the group consisting of N-methylpyrrolidone, benzyl alcohol, and 2-aminoethanol, more preferably one or more selected from the group consisting of N-methylpyrrolidone and benzyl alcohol, and particularly preferably benzyl alcohol, from the viewpoint that the organic solvent used in the swelling step can be used as it is as the solvent in the decomposition step.

[0051] The amount of the organic solvent used in the swelling step is not particularly limited as long as it can swell the cured thermosetting resin A, but is preferably at least 0.2 times, more preferably at least 0.5 times, and even more preferably at least 1 time the volume of the cured thermosetting resin A. The upper limit of the amount of the organic solvent is not particularly limited, but is preferably at most 1,000 times, more preferably at most 500 times, and even more preferably at most 100 times the volume of the cured thermosetting resin A, so that the decomposition step can be carried out in the next step without distilling off the excess organic solvent.

[0052] 1-1-3. Swelling As a method for contacting the thermosetting resin cured material A with an organic solvent, it is preferable to adopt a method of immersing the thermosetting resin cured material A in an organic solvent from the viewpoint of swelling efficiency. The conditions for immersing the thermosetting resin cured material A in an organic solvent are not particularly limited, but it is preferable to perform the immersion under heating conditions. Specifically, the immersion temperature is preferably 80°C or more and 250°C or less, more preferably 100°C or more and 220°C or less, and even more preferably 150°C or more and 200°C or less. In addition, the immersion time is preferably 0.1 hours or more and 24 hours or less, more preferably 0.1 hours or more and 12 hours or less, and even more preferably 0.1 hours or more and 6 hours or less.

[0053] Whether or not the cured thermosetting resin A has swelled can be evaluated based on the ratio of the mass of the cured thermosetting resin B to the mass of the cured thermosetting resin A (hereinafter, sometimes referred to as "swelling ratio"). The swelling ratio is usually more than 1.0, preferably 1.1 or more, more preferably 1.2 or more, and even more preferably 1.4 or more. The upper limit of the swelling ratio is not particularly limited, and may be preferably 10.0 or less, 8.0 or less, or 5.0 or less.

[0054] If the swelling ratio is within the above range, the thermosetting resin cured product B is in a sufficiently softened state and can be easily crushed and decomposed, so that the cured product B can be sufficiently crushed and decomposed in a shorter time than in the conventional method. It can decompose the cured thermosetting resin material in small amounts.

[0055] In the swelling step, since the base may make it difficult for the thermosetting resin cured material A to swell, it is preferable to contact the thermosetting resin cured material A with the organic solvent in the absence of a base. When contacting the thermosetting resin cured material A with an organic solvent containing a base, the lower the base concentration, the more preferable. When the organic solvent contains a base, the specific base concentration depends on the type of base, but is preferably 0.10N or less, more preferably 0.05N or less, and even more preferably 0.01N or less.

[0056] 1-2. Decomposition process The decomposition step is a step of decomposing the thermosetting resin cured material B obtained in the swelling step. The method of decomposing the thermosetting resin cured material B is not particularly limited as long as it is a method capable of producing a phenolic compound or a salt thereof as a decomposition product, and a known decomposition method or a decomposition method similar to a known decomposition method can be appropriately adopted. As a known method, for example, a method of decomposing a thermosetting resin cured material in the presence of a decomposing agent can be preferably mentioned. In this method, the decomposition reaction is generally carried out in a treatment liquid containing a decomposing agent and an organic solvent.

[0057] The decomposition agents preferably include bases, acids, and oxidizing agents. The decomposing agent may be used alone or as a mixture of two or more kinds in any combination and ratio.

[0058] Examples of the base include metal compounds such as metal hydrides, metal hydroxides, metal borohydride salts, metal carbonates, and metal alkoxides. Of these, the base is preferably one or more selected from the group consisting of metal hydroxides and metal alkoxides, and more preferably a metal alkoxide. In addition, examples of the metal in the base include alkali metals such as lithium, sodium, and potassium, and are preferably at least one of sodium and potassium, and more preferably sodium. Therefore, the base is preferably one or more selected from the group consisting of sodium compounds and potassium compounds, and is more preferably one or more selected from the group consisting of sodium hydroxide, potassium hydroxide, sodium alkoxide, and potassium alkoxide, and is even more preferably sodium alkoxide.

[0059] Examples of the acid include inorganic acids such as sulfuric acid, nitric acid, and phosphoric acid; and organic acids such as methanesulfonic acid and toluenesulfonic acid. Preferably, the acid is one or more selected from the group consisting of inorganic acids, and more preferably sulfuric acid and nitric acid.

[0060] Examples of oxidizing agents include air, oxygen, and hydrogen peroxide.

[0061] Among the above compounds, the decomposing agent is preferably a metal alkoxide. A metal alkoxide is a compound in which the hydrogen atom of a hydroxyl group of an alcohol is substituted with a metal, and can be obtained by adding a metal to an alcohol.

[0062] The alcohol used to obtain the metal alkoxide is not particularly limited, and examples thereof include methanol, ethanol, 1-butanol, 2-butanol, 2-methyl-1-propanol, 2-methyl-2-propanol, 1-pentanol, 2-pentanol, 3-pentanol, 2-methyl-1-butanol, 2-methyl-2-butanol, 3-methyl-1-butanol, 3-methyl-2-butanol, 2,2-dimethyl-1-propanol, 1-hexanol, 2-hexanol, 3-hexanol, 2-methyl-1-pentanol, 4-methyl-2-pentanol, 2-ethyl-1-butanol, 1-heptanol, 2-heptanol, 3-heptanol, 2-ethylhexanol, dodecanol, cyclohexanol, and the like. Examples of the alcohol include ethanol, 1-methylcyclohexanol, 2-methylcyclohexanol, 3-methylcyclohexanol, 4-methylcyclohexanol, benzyl alcohol, phenoxyethanol, 1-(2-hydroxyethyl)-2-pyrrolidone, diacetone alcohol, ethylene glycol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monobutyl ether, diethylene glycol, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monopropyl ether, diethylene glycol monobutyl ether, triethylene glycol, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, tetraethylene glycol, polyethylene glycol (molecular weight 200 to 400), 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, 1,5-pentanediol, glycerin, and dipropylene glycol. These alcohols may be used alone or in any combination of two or more in any ratio.

[0063] The metal alkoxide may be in a solid state or a solution state. From the viewpoint of the decomposition efficiency of the thermosetting resin cured material B, the metal alkoxide is preferably at least one selected from the group consisting of sodium methoxide, sodium ethoxide, sodium propoxide, sodium isopropoxide, sodium benzyl alkoxide (sodium benzyl oxide), potassium methoxide, potassium ethoxide, potassium propoxide, isopropoxide, and potassium benzyl alkoxide (potassium benzyl oxide).

[0064] The organic solvent is not particularly limited, and examples thereof include alcohol-based solvents, ether-based solvents, aromatic solvents, etc. Among these, the organic solvent is preferably an alcohol-based solvent because it has excellent solubility for the decomposition product of the cured thermosetting resin B. The organic solvent may be used alone or as a mixture of two or more kinds in any combination and in any ratio.

[0065] Examples of alcohol-based solvents include 1-butanol, 2-butanol, 2-methyl-1-propanol, 2-methyl-2-propanol, 1-pentanol, 2-pentanol, 3-pentanol, 2-methyl-1-butanol, 2-methyl-2-butanol, 3-methyl-1-butanol, 3-methyl-2-butanol, 2,2-dimethyl-1-propanol, 1-hexanol, 2-hexanol, 3-hexanol, 2-methyl-1- Examples of the alcohol include pentanol, 4-methyl-2-pentanol, 2-ethyl-1-butanol, 1-heptanol, 2-heptanol, 3-heptanol, 2-ethylhexanol, dodecanol, cyclohexanol, 1-methylcyclohexanol, 2-methylcyclohexanol, 3-methylcyclohexanol, 4-methylcyclohexanol, benzyl alcohol, and phenoxyethanol, and benzyl alcohol is preferred.

[0066] Examples of ether solvents include diethyl ether, dipropyl ether, dibutyl ether, butyl methyl ether, butyl ethyl ether, diisoamyl ether, hexyl methyl ether, octyl methyl ether, cyclopentyl methyl ether, and dicyclopentyl ether.

[0067] Examples of aromatic solvents include benzene, toluene, xylene, alkylbenzenes such as trimethylbenzene and ethylbenzene, and alkylnaphthalenes such as methylnaphthalene, ethylnaphthalene, and dimethylnaphthalene.

[0068] Since the decomposition of the cured thermosetting resin B is usually carried out under heating conditions, the boiling point of the organic solvent under atmospheric pressure is preferably 100° C. or higher, and more preferably 120° C. or higher. It is more preferable that the temperature is not lower than 150° C. In addition, it is also preferable to use the organic solvent used in the swelling step as it is as the solvent in the decomposition step, in terms of improving the work efficiency and suppressing the cost. From these viewpoints as well, benzyl alcohol (boiling point 205° C.) is a preferred organic solvent.

[0069] The treatment liquid containing the decomposing agent and the organic solvent may further contain other components as necessary, such as a surfactant and a low-viscosity solvent.

[0070] From the viewpoint of improving the efficiency of decomposition of the cured thermosetting resin B, the concentration of the decomposing agent in the treatment liquid is preferably 0.001 mol / L or more and 100 mol / L or less, more preferably 0.005 mol / L or more and 50 mol / L or less, and even more preferably 0.01 mol / L or more and 20 mol / L or less. By setting the concentration of the decomposing agent to the above lower limit or more, the cured thermosetting resin B can be efficiently decomposed. By setting the concentration of the decomposing agent to the above upper limit or less, the cured thermosetting resin B can be decomposed without increasing the viscosity of the treatment liquid.

[0071] In preparing the treatment liquid, the decomposing agent may be mixed with the organic solvent in a solid state or in a solution state. In preparing the treatment liquid, there is no need to perform heating, and the treatment liquid can be prepared by mixing the organic solvent and the decomposing agent at room temperature of about 5° C. or higher and 35° C. or lower.

[0072] The reaction vessel is not particularly limited as long as it is capable of contacting the treatment liquid with the cured thermosetting resin B. As long as the vessel can be used as a decomposition tank, it may be box-shaped, cylindrical, mesh-like cage-shaped, or made of a porous material. The ratio (filling rate) of the volume of the cured thermosetting resin B placed in the container to the volume of the container is preferably within the range of 5% to 25% from the viewpoint of dissolution efficiency.

[0073] The temperature of the treatment liquid when contacting the treatment liquid with the cured thermosetting resin B is preferably 100° C. or higher, more preferably 130° C. or higher, and even more preferably 150° C. or higher, from the viewpoint of improving the decomposition efficiency of the cured thermosetting resin B. On the other hand, from the viewpoint of suppressing the denaturation of the organic solvent and the decomposition products, this temperature is preferably 300° C. or lower, more preferably 250° C. or lower, and even more preferably 200° C. or lower.

[0074] The contact time between the treatment liquid and the cured thermosetting resin B may be any time that allows the cured thermosetting resin B to be sufficiently decomposed and dissolved, and varies depending on the type of thermosetting resin, the type and concentration of the decomposer and organic solvent, and the treatment temperature, but is preferably from 1 hour to 50 hours.

[0075] 1-3. Inorganic matter recovery process When the thermosetting resin cured material A contains an inorganic substance, the production method according to the present embodiment may include an inorganic substance recovery step of separating the phenol compound or its salt from the inorganic substance after the decomposition step and recovering the inorganic substance, thereby obtaining each of the phenol compound and the inorganic substance.

[0076] The method for recovering the inorganic substances is not particularly limited, and can be carried out by a known separation method such as filtration, sedimentation separation, stretching separation, etc. The recovered inorganic substances can be recycled.

[0077] 2. Epoxy resin manufacturing method The second embodiment of the present invention is a phenotype obtained by the production method according to the first embodiment of the present invention. The method for producing an epoxy resin includes a reaction step of reacting a phenol compound with epihalohydrin. Since the production method according to this embodiment uses a phenol compound obtained by decomposing a cured thermosetting resin as a raw material, hereinafter, the epoxy resin produced by the production method according to this embodiment may be referred to as a "recycled epoxy resin."

[0078] In the reaction step, a recycled epoxy resin is produced by a known one-step method for producing a recycled epoxy resin or a method similar thereto. The one-step method for producing a recycled epoxy resin is a method for obtaining a recycled epoxy resin by reacting a hydroxy compound raw material with epihalohydrin. In this embodiment, the hydroxy compound raw material contains a phenol compound obtained by the production method according to the first embodiment of the present invention, and may contain a polyhydric hydroxy compound (hereinafter, sometimes referred to as a "polyhydric hydroxy compound") as necessary.

[0079] The term "polyhydric hydroxy compound" is a general term for dihydric or higher phenol compounds and dihydric or higher alcohol compounds, and may be the same compound as the phenol compound obtained by the production method according to the first embodiment of the present invention. In the one-stage method for producing recycled epoxy resin, the "hydroxy compound raw material" is the total hydroxy compound including the phenol compound obtained by the production method according to the first embodiment of the present invention and the polyhydric hydroxy compound used as needed.

[0080] Examples of polyhydric hydroxy compounds include various polyhydric phenols such as bisphenol A, tetramethyl bisphenol A, bisphenol F, tetramethyl bisphenol F, bisphenol S, bisphenol C, bisphenol AD, bisphenol AF, hydroquinone, resorcin, methyl resorcin, biphenol, tetramethyl biphenol, dihydroxynaphthalene, dihydroxydiphenyl ether, thiodiphenols, phenol novolac resins, cresol novolac resins, phenol aralkyl resins, biphenyl aralkyl resins, naphthol aralkyl resins, terpene phenol resins, dicyclopentadiene phenol resins, bisphenol A novolac resins, naphthol novolac resins, brominated bisphenol A, and brominated phenol novolac resins; various phenols and benzaldehyde, hydroxybenzaldehyde, etc. polyhydric phenol resins obtained by a condensation reaction of xylene resin with phenols; various phenol resins such as co-condensation resins of heavy oils or pitches with phenols and formaldehydes; chain aliphatic diols such as ethylene glycol, trimethylene glycol, propylene glycol, 1,3-butanediol, 1,4-butanediol, 1,3-pentanediol, 1,4-pentanediol, 1,5-pentanediol, and 1,6-hexanediol; cyclic aliphatic diols such as cyclohexanediol and cyclodecanediol; and polyalkylene ether glycols such as polyethylene ether glycol, polyoxytrimethylene ether glycol, and polypropylene ether glycol.

[0081] In the reaction step, a phenol compound and a polyhydric hydroxy compound are dissolved in epihalohydrin to form a homogeneous solution, and the reaction is allowed to proceed.

[0082] Examples of epihalohydrin include epichlorohydrin, β-methylepichlorohydrin, epibromohydrin, etc. Among these, epihalohydrin is particularly preferably epichlorohydrin from the viewpoints of reactivity, availability of raw materials, and versatility of the resulting epoxy resin. The epihalohydrin may be used alone or in any combination of two or more kinds in any ratio.

[0083] The amount of epihalohydrin used is usually 1.0 equivalent or more and 14.0 equivalent or less, and preferably 2.0 equivalent or more and 10.0 equivalent or less, per equivalent of the total hydroxyl group of the hydroxy compound raw material (total hydroxy compounds). By setting the amount of epihalohydrin to the above lower limit or more, it is easy to control the polymerizing reaction, and the obtained recycled epoxy resin can have an appropriate epoxy equivalent. In addition, by setting the amount of epihalohydrin to the above upper limit or less, production efficiency tends to be improved.

[0084] Next, while stirring the solution, an alkali metal hydroxide is added in an amount of preferably 0.1 to 3.0 equivalents, more preferably 0.8 to 2.0 equivalents per equivalent of the total hydroxyl groups of the hydroxy compound raw material, in the form of a solid or aqueous solution, to react. By setting the amount of alkali metal hydroxide to the above lower limit or more, the unreacted hydroxyl groups and the generated epoxy resin are less likely to react, and therefore the polymerizing reaction can be easily controlled. In addition, by setting the amount of alkali metal hydroxide to the above upper limit or less, the generation of impurities due to side reactions can be suppressed. Examples of alkali metal hydroxides include sodium hydroxide and potassium hydroxide.

[0085] The reaction can be carried out under normal pressure or under reduced pressure. The reaction temperature is preferably 20° C. or higher and 200° C. or lower, more preferably 40° C. or higher and 150° C. or lower. By setting the reaction temperature to the above lower limit or higher, the reaction can be easily progressed and controlled. In addition, by setting the reaction temperature to the above upper limit or lower, side reactions can be suppressed and the amount of by-products can be reduced.

[0086] The reaction is carried out while dehydrating the reaction liquid by azeotroping while maintaining a predetermined temperature as necessary, cooling the volatilized steam, separating the condensate obtained, and returning the oil content without moisture to the reaction system. In order to suppress a rapid reaction, the alkali metal hydroxide is added intermittently or continuously in small amounts over a period of preferably 0.1 to 24 hours, more preferably 0.5 to 10 hours. By setting the addition time of the alkali metal hydroxide to the above lower limit or more, the reaction can be prevented from proceeding rapidly, making it easier to control the reaction temperature. In addition, by setting the addition time of the alkali metal hydroxide to the above upper limit or less, the amount of by-products can be reduced.

[0087] The reaction may be carried out in the presence of a catalyst, such as quaternary ammonium salts, such as tetramethylammonium chloride and tetraethylammonium bromide; tertiary amines, such as benzyldimethylamine and 2,4,6-tris(dimethylaminomethyl)phenol; imidazoles, such as 2-ethyl-4-methylimidazole and 2-phenylimidazole; phosphonium salts, such as ethyltriphenylphosphonium iodide; and phosphines, such as triphenylphosphine.

[0088] The reaction may be carried out in an inert organic solvent, such as alcohols, such as ethanol and isopropanol; ketones, such as acetone, methyl ethyl ketone, and methyl isobutyl ketone; ethers, such as dioxane and ethylene glycol dimethyl ether; glycol ethers, such as methoxypropanol; and aprotic polar solvents, such as dimethylsulfoxide and dimethylformamide.

[0089] After the reaction is completed, a typical post-treatment in the field of organic synthesis may be carried out, such as removing insoluble by-product salts by filtration or washing with water, followed by distilling off unreacted epihalohydrin by heating and / or distillation under reduced pressure.

[0090] 3. Manufacturing method of composite materials The third embodiment of the present invention is a regenerated energy storage device obtained by the manufacturing method according to the second embodiment of the present invention. The present invention relates to a method for producing a composite material, the method including a curing step of curing an epoxy resin composition containing an epoxy resin and an inorganic material (hereinafter, sometimes referred to as "recycled inorganic material") recovered in the inorganic material recovery step of the production method according to the first embodiment of the present invention.

[0091] In this embodiment, the epoxy resin composition may contain, as necessary, an epoxy resin other than the recycled epoxy resin obtained by the production method according to the second embodiment of the present invention, a curing agent, a curing accelerator, a release agent, a coupling agent, and the like.

[0092] 3-1. Recycled epoxy resin The content of the recycled epoxy resin in the epoxy resin composition is not particularly limited, but the content of the recycled epoxy resin relative to 100 parts by mass of the total epoxy resin components is preferably 40 parts by mass or more, and more preferably 60 parts by mass or more, from the viewpoint of environmental harmony. When the epoxy resin composition contains other epoxy resins, the content of the recycled epoxy resin in 100 parts by mass of the total epoxy resin components is preferably 40 parts by mass or more and 99 parts by mass or less, and more preferably 60 parts by mass or more and 99 parts by mass or less. Note that the "total epoxy resin components" corresponds to the amount of all epoxy resins contained in the epoxy resin composition, and is the total of the recycled epoxy resin and other epoxy resins used as necessary.

[0093] 3-2.Other epoxy resins The epoxy resin composition may further contain other epoxy resins (hereinafter, sometimes referred to as "other epoxy resins") in addition to the recycled epoxy resin obtained by the production method according to the second embodiment of the present invention. By containing other epoxy resins, various physical properties can be improved.

[0094] The other epoxy resin corresponds to all epoxy resins other than the recycled epoxy resin obtained by the production method according to the second embodiment of the present invention, and may be the same type of epoxy resin as the recycled epoxy resin. The other epoxy resins may be used alone or in any combination of two or more in any ratio.

[0095] Other epoxy resins include, for example, bisphenol A type epoxy resins, bisphenol C type epoxy resins, trisphenolmethane type epoxy resins, anthracene type epoxy resins, phenol-modified xylene resin type epoxy resins, bisphenol cyclododecyl type epoxy resins, bisphenol diisopropylidene resorcin type epoxy resins, bisphenol F type epoxy resins, bisphenol AD ​​type epoxy resins, bisphenol AF type epoxy resins, hydroquinone type epoxy resins, methyl hydroquinone type epoxy resins, dibutyl hydroquinone type epoxy resins, resorcin type epoxy resins, methyl resorcin type epoxy resins, biphenol type epoxy resins, tetramethyl biphenol type epoxy resins, tetramethyl bisphenol F type epoxy resins, dihydroxy diphenyl ether type epoxy resins, epoxy resins derived from thiodiphenols, dihydroxy naphthalene type Epoxy resins, dihydroxyanthracene type epoxy resins, dihydroxydihydroanthracene type epoxy resins, dicyclopentadiene type epoxy resins, epoxy resins derived from dihydroxystilbenes, phenol novolac type epoxy resins, cresol novolac type epoxy resins, bisphenol A novolac type epoxy resins, naphthol novolac type epoxy resins, phenol aralkyl type epoxy resins, naphthol aralkyl type epoxy resins, biphenyl aralkyl type epoxy resins, terpene phenol type epoxy resins, dicyclopentadiene phenol type epoxy resins, epoxy resins derived from phenol-hydroxybenzaldehyde condensates, epoxy resins derived from phenol-crotonaldehyde condensates, epoxy resins derived from phenol-glyoxal condensates, epoxy resins derived from co-condensation resins of heavy oils or pitches with phenols and formaldehydes Examples of epoxy resins that can be used include epoxy resins derived from dimethylaminophenylamine, epoxy resins derived from diaminodiphenylmethane, epoxy resins derived from aminophenol, epoxy resins derived from xylenediamine, epoxy resins derived from methylhexahydrophthalic acid, and epoxy resins derived from dimer acid.

[0096] When the epoxy resin composition contains other epoxy resins, the content of the other epoxy resins in 100 parts by mass of the total epoxy resin components is preferably 1 part by mass or more and 60 parts by mass or less, and more preferably 1 part by mass or more and 40 parts by mass or less.

[0097] 3-3.Inorganic substances The epoxy resin composition contains a recycled inorganic material, and may further contain a known inorganic filler for plastics. The recycled inorganic material is preferably one or more selected from the group consisting of carbon fiber and glass fiber, and more preferably carbon fiber. The known inorganic filler for plastics may be the same type of inorganic material as the recycled inorganic material.

[0098] The total content of the recycled inorganic material and the known inorganic filler for plastics in the epoxy resin composition is preferably 10% by mass or more and 95% by mass or less.

[0099] Furthermore, when the epoxy resin composition contains a known inorganic filler for plastics, the content of the recycled inorganic material when the total amount of the recycled inorganic material and the known inorganic filler for plastics is taken as 100 parts by mass, from the viewpoint of environmental friendliness, is preferably 40 parts by mass or more and 99 parts by mass or less, and more preferably 60 parts by mass or more and 99 parts by mass or less.

[0100] 3-4. Hardener The epoxy resin composition preferably contains a curing agent. As the curing agent, a known epoxy resin curing agent, for example, the curing agent described in the above section "1-1-1. Cured thermosetting resin A" can be used. The curing agent may be used alone or as a mixture of two or more kinds in any combination and in any ratio.

[0101] When the epoxy resin composition contains a curing agent, the content of the curing agent relative to 100 parts by mass of the total epoxy resin components is not particularly limited, but is preferably from 0.1 to 1,000 parts by mass, more preferably from 0.1 to 500 parts by mass, and even more preferably from 0.5 to 100 parts by mass.

[0102] When the curing agent is an amine-based curing agent or an acid anhydride-based curing agent, the content of the curing agent in the epoxy resin composition is preferably an amount such that the equivalent ratio of the functional groups in the curing agent to the epoxy groups in the total epoxy resin component is 0.1 or more and 2.0 or less, and more preferably an amount such that the equivalent ratio is 0.8 or more and 1.2 or less. By setting the content of the curing agent within the above range, the remaining amount of unreacted epoxy groups in the epoxy resin and unreacted functional groups in the curing agent can be reduced.

[0103] When the curing agent is an amide-based curing agent or an imidazole-based curing agent, the content of the curing agent relative to the total amount of all epoxy resin components and the curing agent in the epoxy resin composition is preferably 0.1 mass % or more and 20 mass % or less.

[0104] 3-5. Hardening accelerator The epoxy resin composition preferably contains a curing accelerator. By containing the curing accelerator, it is possible to shorten the curing time and lower the curing temperature, and it is possible to easily obtain a desired cured product.

[0105] As the curing accelerator, a known curing accelerator for epoxy resins, for example, the curing accelerators explained in the above section "1-1-1. Cured thermosetting resin A" can be used. The curing accelerator may be used alone or as a mixture of two or more kinds in any combination and in any ratio.

[0106] When the epoxy resin composition contains a curing accelerator, the content of the curing accelerator relative to 100 parts by mass of the total epoxy resin components is not particularly limited, but is preferably 0.1 parts by mass or more and 20 parts by mass or less. By making the content of the curing accelerator equal to or more than the above lower limit, a good curing acceleration effect can be obtained. In addition, by making the content of the curing accelerator equal to or less than the above upper limit, the desired curing properties can be easily obtained.

[0107] 3-6. Release agent The epoxy resin composition may contain a mold release agent. Examples of the mold release agent that can be used include natural waxes such as carnauba wax, synthetic waxes such as polyethylene wax, higher fatty acids such as stearic acid and zinc stearate, metal salts of the higher fatty acids, and hydrocarbon-based mold release agents such as paraffin. The release agent may be used alone or as a mixture of two or more kinds in any combination and in any ratio.

[0108] When the epoxy resin composition contains a mold release agent, the content of the mold release agent relative to 100 parts by mass of the total epoxy resin components is not particularly limited, but is preferably 0.001 parts by mass or more and 10.0 parts by mass or less. By setting the content of the mold release agent within the above range, it is possible to exhibit good mold releasability while maintaining the curing characteristics.

[0109] 3-7. Coupling agents The epoxy resin composition preferably contains a coupling agent, which can improve the adhesion between the epoxy resin matrix and inorganic substances.

[0110] The coupling agent includes a silane coupling agent and a titanate coupling agent. The coupling agent may be used alone or as a mixture of two or more kinds in any combination and in any ratio.

[0111] Examples of the silane coupling agent include epoxy silane coupling agents such as γ-glycidyloxypropyltrimethoxysilane, γ-glycidyloxypropyltriethoxysilane, and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; amino silane coupling agents such as γ-aminopropyltriethoxysilane, N-β(aminoethyl)γ-aminopropyltrimethoxysilane, N-β(aminoethyl)γ-aminopropylmethyldimethoxysilane, γ-aminopropyltrimethoxysilane, and γ-ureidopropyltriethoxysilane; mercapto silane coupling agents such as 3-mercaptopropyltrimethoxysilane; and vinyl silane coupling agents such as p-styryltrimethoxysilane, vinyltrichlorosilane, vinyltris(β-methoxyethoxy)silane, vinyltrimethoxysilane, vinyltriethoxysilane, and γ-methacryloxypropyltrimethoxysilane.

[0112] Examples of titanate coupling agents include isopropyl triisostearoyl titanate, isopropyl tri(N-aminoethyl aminoethyl) titanate, diisopropyl bis(dioctyl phosphate) titanate, tetraisopropyl bis(dioctyl phosphite) titanate, and tetraoctyl bis(ditridecyl phosphite) titanate. bis(dioctylpyrophosphate) ethylene titanate, tetra(2,2-diallyloxymethyl-1-butyl)bis(ditridecyl)phosphite titanate, bis(dioctylpyrophosphate) oxyacetate titanate, and bis(dioctylpyrophosphate) ethylene titanate.

[0113] When the epoxy resin composition contains a coupling agent, the content of the coupling agent relative to 100 parts by mass of the total epoxy resin components is not particularly limited, but is preferably 0.001 parts by mass or more and 10.0 parts by mass or less. By making the content of the coupling agent equal to or more than the above lower limit, the adhesiveness between the epoxy resin matrix and the inorganic material tends to be further improved. In addition, by making the content of the coupling agent equal to or less than the above upper limit, the coupling agent is less likely to bleed out from the obtained composite material.

[0114] 3-8.Other additives The epoxy resin composition may contain additives other than the above components, as necessary. Examples of the additives include flame retardants, plasticizers, reactive diluents, and pigments.

[0115] Examples of the flame retardant include halogen-based flame retardants such as brominated epoxy resins and brominated phenol resins; antimony compounds such as antimony trioxide; phosphorus-based flame retardants such as red phosphorus, phosphate esters, and phosphines; nitrogen-based flame retardants such as melamine derivatives; and inorganic flame retardants such as aluminum hydroxide and magnesium hydroxide.

[0116] 3-9.Curing process The curing step is a step of curing the above-mentioned epoxy resin composition, and a composite material can be obtained by this. The method of curing the epoxy resin composition is not particularly limited, but it is preferable to adopt a curing method by a thermosetting reaction. During the thermosetting reaction, it is preferable to appropriately select the curing temperature depending on the type of curing agent. For example, when an amine-based curing agent is used, the curing temperature is usually 80°C or higher and 250°C or lower. In addition, it is also possible to lower the curing temperature by adding a curing accelerator to these curing agents.

[0117] The reaction time is preferably 0.01 hours or more and 20 hours or less. By setting the reaction time to the above lower limit or more, the epoxy resin composition tends to be sufficiently cured. In addition, by setting the reaction time to the above upper limit or less, deterioration due to heating and energy loss during heating tend to be reduced.

[0118] 4. Manufacturing method of inorganic fibers A fourth embodiment of the present invention is a method for producing inorganic fibers from inorganic fiber reinforced resin, which includes a swelling step of contacting inorganic fiber reinforced resin A containing inorganic fibers and a cured thermosetting resin with an organic solvent to swell the inorganic fiber reinforced resin A to obtain inorganic fiber reinforced resin B, and an inorganic fiber recovery step of separating inorganic fibers from the inorganic fiber reinforced resin B.

[0119] In the manufacturing method according to the present embodiment, the inorganic fiber reinforced resin A swells and softens in the swelling step, so that fraying occurs in the inorganic fiber reinforced resin B, and the swollen mass of the inorganic fiber reinforced resin B can be torn with less force than the crushing performed in the conventional method. Then, in the inorganic fiber recovery step, the inorganic fibers can be easily separated from the cured thermosetting resin from the fraying or torn surface. At this time, since there is no need to decompose and / or dissolve the cured thermosetting resin, in a preferred embodiment of the present embodiment, the problem of the high viscosity substance generated by the decomposition and / or dissolution of the cured thermosetting resin becoming entangled with the inorganic fibers is reduced, and inorganic fibers with a small amount of foreign matter attached can be recovered.

[0120] In addition, in the conventional recycling method of inorganic fiber reinforced resin, the inorganic fiber reinforced resin is crushed or pulverized. However, according to the manufacturing method of the present embodiment, there is no need to crush or pulverize the inorganic fiber reinforced resin. Therefore, in a preferred embodiment of the present embodiment, reusable inorganic fibers of approximately the same quality and shape as when they were contained in the inorganic fiber reinforced resin can be recovered.

[0121] 4-1. Swelling process The swelling step in this embodiment is the same as the swelling step in the method for producing a phenolic compound according to the first embodiment of the present invention, except that the thermosetting resin cured material A is replaced with inorganic fiber reinforced resin A. Therefore, the organic solvent, swelling conditions, and the definition of swelling are as described in the above section "1-1. Swelling step", and the description in this section is incorporated by reference.

[0122] The inorganic fiber reinforced resin A that swells in the swelling step is a cured thermosetting resin composition containing inorganic fibers and a thermosetting resin, and contains inorganic fibers and a cured thermosetting resin.

[0123] The inorganic fibers are not particularly limited, and examples thereof include carbon fibers, glass fibers, metal fibers such as stainless steel, and ceramic fibers such as alumina fibers and silica fibers. Of these, the inorganic fibers are preferably one or more types selected from the group consisting of carbon fibers and glass fibers, and more preferably carbon fibers. The fibers may be in the form of a nonwoven fabric or a woven fabric. In the case of a woven fabric, the fibers may be a cloth material made by weaving fiber bundles, or a UD (Uni-Directional) material in which fiber bundles are arranged in one direction.

[0124] The thermosetting resin cured product is obtained by curing a thermosetting resin in the presence or absence of a curing accelerator, without using a curing agent or using a curing agent, and preferably by curing a thermosetting resin using a curing agent. The thermosetting resin, the curing agent, and the curing accelerator are the same as the thermosetting resin, the curing agent, and the curing accelerator described in the above section "1-1-1. Cured Thermosetting Resin A", respectively, and the description in that section is incorporated by reference. The thermosetting resin may also contain other epoxy resins described in the above section "3-2. Other Epoxy Resins".

[0125] 4-2. Inorganic fiber recovery process The inorganic fiber recovery step is a step of separating inorganic fibers from the inorganic fiber reinforced resin B. The method of separating inorganic fibers from the inorganic fiber reinforced resin B is not particularly limited, and examples thereof include a method of breaking the inorganic fiber reinforced resin B into small pieces as necessary, and pulling out the inorganic fibers exposed from the surface or the fracture surface of the inorganic fiber reinforced resin B.

[0126] 5. Manufacturing method of inorganic fiber reinforced resin The fifth embodiment of the present invention is a method for producing an inorganic fiber reinforced resin, which includes a curing step of curing a thermosetting resin composition containing a thermosetting resin and inorganic fibers (hereinafter, sometimes referred to as "recycled inorganic fibers") obtained by the method for producing inorganic fibers according to the fourth embodiment of the present invention. The manufacturing method according to this embodiment allows the recycled inorganic fibers to be reused.

[0127] The thermosetting resin contained in the thermosetting resin composition is not particularly limited, and in addition to known thermosetting resins, epoxy resins obtained by the epoxy resin manufacturing method according to the second embodiment of the present invention can be used. In addition, the thermosetting resin composition may be appropriately blended with a curing agent, a curing accelerator, a mold release agent, a coupling agent, etc., as necessary. The curing method of the thermosetting resin composition is not particularly limited, but it is preferable to adopt a curing method by a thermosetting reaction. In the thermosetting reaction, the curing conditions may be appropriately selected according to the composition of the thermosetting resin composition. EXAMPLES

[0128] The present invention will be described in more detail below with reference to examples and comparative examples. The present invention is not limited to the following examples unless it goes beyond the scope of the present invention. In addition, the various manufacturing conditions and evaluation result values ​​in the following examples have the meaning of preferred upper or lower limit values ​​in the embodiment of the present invention, and the preferred range may be a range defined by a combination of the above-mentioned upper or lower limit value and the values ​​of the following examples or values ​​between the examples. In the following examples, "room temperature" refers to a temperature range of 15°C or higher and 35°C or lower.

[0129] [Raw materials and reagents] The bisphenol A type epoxy resin (epoxy equivalent: 950 g / eq or 183 g / eq) used was a product of Mitsubishi Chemical Corporation. The Rikacid (acid anhydride) M-700 used was a product of New Japan Chemical Co., Ltd. Curesol 2E4MZ (curing catalyst) was a product of Shikoku Chemical Industry Co., Ltd. The phenol novolac resin (PSM-4261) used was a product of Gun-ei Chemical Industry Co., Ltd. The 48% by mass aqueous sodium hydroxide solution, disilenediamide (DICY), 3-(3,4-dichlorophenyl)-1,1-dimethylurea (DCMU), hydrochloric acid, toluene, acetonitrile, and N-methylpyrrolidone were products of Fujifilm Wako Pure Chemical Industries, Ltd. Benzyl alcohol used was a product of Sankyo Chemical Co., Ltd. The carbon fiber used was 3mm chopped carbon fiber manufactured by Yoshino Co., Ltd.

[0130] [analysis] The production and quantification of bisphenol A were carried out by high performance liquid chromatography according to the following procedures and conditions. ·Device: High-performance liquid chromatograph (Shimadzu Corporation) Pump: LC-20AD (Shimadzu Corporation) Column oven: CTO-20AC (Shimadzu Corporation) Detector: SPD-20A (Shimadzu Corporation) Column: 3 μm 250 mm × 4.6 mm ID (Intact Co., Ltd.) Method: Low pressure gradient method ·Analysis temperature: 40℃ ·Eluent composition: Solution A: Acetonitrile B liquid water At 0 min of analysis time, the eluent composition was A:B = 30:70 (volume ratio, same below), and from 0 to 5 min of analysis time the eluent composition was A:B = 30:70, then from 5 to 20 min of analysis time it gradually became A:B = 100:0, and from 20 to 35 min of analysis time it was A:B = 100:0. ·Flow rate: 1mL / min Detection wavelength: 280nm

[0131] [Swelling rate] The swelling ratio was calculated according to the following procedure. First, the mass I of the resin sample before swelling was measured. Then, the resin sample was immersed in a predetermined organic solvent as a swelling liquid and swollen under predetermined conditions. The liquid adhering to all surfaces of the swollen resin sample was removed with a Kimtowel, and the mass II of the resin sample after swelling was measured. The ratio of the mass II of the resin sample after swelling to the mass I of the resin sample before swelling was calculated as the swelling ratio according to the following formula. Swelling ratio = mass of resin sample after swelling II ÷ mass of resin sample before swelling I

[0132] [Easy to handle] The handleability was evaluated according to the following criteria. S: Easily bendable by hand A: Can be bent using radio pliers B: The surface is softened, but it cannot be bent with pliers. C: The surface is not softened and cannot be bent with radio pliers.

[0133] [Epoxy equivalent] The epoxy equivalent of the epoxy resin was measured based on JIS K 7236:2009 (revised on January 20, 2009).

[0134] Reference Example 1: Preparation of amine cured product 280g of bisphenol A type epoxy resin (epoxy equivalent: 183g / eq), 2g of DICY, and 3g of DCMU were mixed thoroughly in an aluminum cup to obtain a mixture. The mixture was heated at 150°C for 3 hours to obtain an amine cured product.

[0135] Reference Example 2: Preparation of acid anhydride cured product 300g of bisphenol A type epoxy resin (epoxy equivalent 183g / eq), 270g of Rikacid, and 3g of Curesol 2E4MZ were mixed well in an aluminum cup to obtain a mixture. The mixture was heated at 100℃ for 3 hours, and then heated at 140℃ for 3 hours to obtain a hardened acid anhydride material.

[0136] Reference Example 3: Preparation of phenolic cured material 280g of bisphenol A type epoxy resin (epoxy equivalent 183g / eq), 172g of phenol novolac resin (PSM-4261), and 2g of Curesol 2E4MZ were placed in an aluminum cup and mixed thoroughly to obtain a mixture. The mixture was heated at 120°C for 2 hours and then at 175°C for 6 hours to obtain a phenol cured material.

[0137] Reference Example 4: Preparation of amine-cured CFRP 100 g of bisphenol A type epoxy resin (epoxy equivalent: 183 g / eq), 1 g of DICY, and 1 g of DCMU were placed in an aluminum cup and mixed thoroughly to obtain mixture 1. 100 g of carbon fiber was added to the obtained mixture 1 and mixed to obtain mixture 2. The obtained mixture 2 was poured into a flat mold and heated at 150°C for 3 hours to obtain an amine-cured carbon fiber composite material.

[0138] Example 1 In a 100 mL Schlenk flask, 2.77 g of the amine cured product obtained in Reference Example 1 and 50 g of benzyl alcohol (BnOH) as an organic solvent were placed. The Schlenk flask was immersed in an oil bath at 110°C and then left to stand for 2 hours. When the amine cured product was then removed from the Schlenk flask, it was found to have swollen and softened. The benzyl alcohol adhering to the softened amine cured product was wiped off with a Kimtowel, and the weight was measured to be 4.51 g. The swelling ratio was 4.51 g ÷ 2.77 g = 1.63. The softened amine cured product could be easily bent by hand.

[0139] Example 2 In a 100 mL Schlenk flask, 2.58 g of the amine cured product obtained in Reference Example 1 and 40 g of N-methylpyrrolidone (NMP) and 10 g of benzyl alcohol (BnOH) (NMP:BnOH=4:1) were placed as organic solvents. The Schlenk flask was immersed in an oil bath at 110° C. and allowed to stand for 2 hours. When the amine cured product was then removed from the Schlenk flask, it was found to have swollen and softened. The liquid adhering to the softened amine cured product was removed by quenching. The weight was measured and found to be 3.72 g. The swelling ratio was 3.72 g ÷ 2.58 g = 1.44. The softened amine-cured product could be easily bent by hand.

[0140] Example 3 In a 100 mL Schlenk flask, 3.44 g of the amine cured product obtained in Reference Example 1 and 45 g of N-methylpyrrolidone (NMP) and 5 g of 2-aminoethanol (AE) (NMP:AE=9:1) were placed as organic solvents. The Schlenk flask was immersed in an oil bath at 110°C and then allowed to stand for 2 hours. The amine cured product was then removed from the Schlenk flask and found to have swollen and softened. The liquid adhering to the softened amine cured product was wiped off with a Kimtowel and the weight was measured to be 5.21 g. The swelling ratio was 5.21 g ÷ 3.65 g = 1.43. The softened amine cured product could be easily bent by hand.

[0141] Comparative Example 1 In a 100 mL Schlenk flask, 3.01 g of the amine cured product obtained in Reference Example 1, 50 g of benzyl alcohol (BnOH) as an organic solvent, and 2.41 g of 25% by mass aqueous sodium hydroxide solution were placed. The Schlenk flask was immersed in an oil bath at 110°C and then allowed to stand for 2 hours. The amine cured product was then removed from the Schlenk flask to obtain a treated amine cured product. The benzyl alcohol and aqueous sodium hydroxide solution adhering to the treated amine cured product were wiped off with a Kimtowel, and the weight was measured to be 3.04 g. The swelling ratio was 3.04 g ÷ 3.01 g = 1.01. The surface of the treated amine cured product was not softened, and it was impossible to bend it with radio pliers.

[0142] Table 1 shows the organic solvents used, the oil bath temperatures, swelling ratios, and handleability in Examples 1 to 3 and Comparative Example 1. Table 1 shows that the handleability is improved by immersing the cured product in only an organic solvent without adding an alkali.

[0143] [Table 1]

[0144] Example 4 In a 100 mL Schlenk flask, 2.35 g of the amine cured product obtained in Reference Example 1 and 50 g of benzyl alcohol (BnOH) as an organic solvent were placed. The Schlenk flask was immersed in an oil bath at 170°C and then allowed to stand for 2 hours. The amine cured product was then removed from the Schlenk flask, and found to have swollen and softened. The benzyl alcohol adhering to the softened amine cured product was wiped off with a Kimtowel, and the weight was measured to be 4.56 g. The swelling ratio was 4.56 g ÷ 2.35 g = 1.94. The softened amine cured product could be easily bent by hand.

[0145] Example 5 In Example 1, instead of 2.35 g of the amine cured product obtained in Reference Example 1, The same procedure as in Example 1 was repeated, except that 3.44 g of the acid anhydride cured product obtained in step 1 was used instead. The swelling ratio was 1.44, and the obtained softened acid anhydride cured product could be easily bent by hand.

[0146] Example 6 The same procedure as in Example 1 was repeated, except that 4.31 g of the phenol cured product obtained in Reference Example 3 was used instead of 2.35 g of the amine cured product obtained in Reference Example 1. The swelling ratio was 1.40, and the softened phenol cured product obtained could be easily bent by hand.

[0147] Example 7 The same procedure as in Example 1 was repeated, except that 10.04 g of the amine-cured carbon fiber composite material obtained in Reference Example 4 was used instead of 2.35 g of the amine-cured product obtained in Reference Example 1. The swelling ratio was 1.42, and the softened amine-cured carbon fiber composite material obtained could be easily bent by hand.

[0148] The cured thermosetting resin and carbon fiber composite materials used in Examples 4 to 7, their swelling ratios, and handleability are summarized in Table 2. It can be seen from Table 2 that any material containing a cured thermosetting resin can swell and be easily handled.

[0149] [Table 2]

[0150] Example 8 A stirrer, 1 g of the amine cured product obtained in Example 1, 5 g of benzyl alcohol, and 1 g of a 28% by mass solution of sodium methoxide in methanol were placed in a 100 mL Schlenk. The Schlenk was immersed in an oil bath at 180°C, and the liquid inside was stirred for 2 hours. The amine cured product was not observed in the resulting decomposition liquid, and was completely dissolved. A portion of the resulting decomposition liquid was extracted and subjected to high performance liquid chromatography, revealing that 0.8% by mass of bisphenol A was produced.

[0151] Comparative Example 2 Example 8 was carried out in the same manner as in Example 8, except that 1 g of the amine cured product obtained in Reference Example 1 was used instead of 1 g of the amine cured product obtained in Example 1. The obtained decomposition liquid contained solids of the amine cured product. In addition, a portion of the obtained decomposition liquid was extracted and subjected to high performance liquid chromatography, but no bisphenol A was detected (detection limit <0.001% by mass).

[0152] In Example 8 and Comparative Example 2, the presence or absence of swelling, the presence or absence of solid content after decomposition, and the presence or absence of production of bisphenol A are summarized in Table 3. From Table 3, it can be seen that by swelling the resin, the solid and liquid components disappear after decomposition, allowing the resin to be completely dissolved and bisphenol A is produced.

[0153] [Table 3]

[0154] Example 9 14 g of the amine-cured carbon fiber composite material obtained in Example 7, 90 g of benzyl alcohol, and 14 g of a 28% by mass solution of sodium methoxide in methanol were placed in a stainless steel separable flask equipped with a cooling tube, a thermometer, and a stirrer, and a nitrogen atmosphere was created. The separable flask was immersed in an oil bath heated to 185°C, and the mixture was stirred for 4 hours to obtain a decomposition liquid. A portion of the obtained decomposition liquid was extracted and subjected to high performance liquid chromatography, which revealed that 0.4% by mass of bisphenol A was produced.

[0155] The separable flask was removed from the oil bath and cooled to room temperature. The decomposition liquid was then filtered under reduced pressure to separate the crude carbon fiber and the filtrate into a solid-liquid separation. The crude carbon fiber obtained was washed with acetone and water, and then dried at 170°C for 5 hours under reduced pressure of 10 kPa to obtain 5 g of recycled carbon fiber.

[0156] Example 10 In a stainless steel separable flask equipped with a distillation tube, a thermometer, and a stirrer, 100 g of the amine cured product obtained in Reference Example 1 and 500 g of benzyl alcohol were placed and a nitrogen atmosphere was created. The separable flask was immersed in an oil bath heated to 185°C and then stirred for 2 hours. The separable flask was removed from the oil bath and cooled to room temperature. When the inside of the separable flask was checked, the amine cured product was found to be swollen. The separable flask was placed in a 28% by mass methanol solution of sodium methoxide and a nitrogen atmosphere was created. The flask was immersed in an oil bath heated to 185°C, and after the distillation of methanol ceased, the mixture was stirred for 5 hours to obtain a decomposition liquid. No undissolved amine cured product was found in the obtained decomposition liquid. The separable flask was again removed from the oil bath and cooled to room temperature.

[0157] The entire amount of the decomposition liquid obtained and 500 g of water were placed in a jacketed separable flask equipped with a Dimroth condenser, a stirring blade, and a thermometer, and mixed for 1 hour under a nitrogen atmosphere. After that, the mixture was left to stand to separate organic phase 1 and aqueous phase 1 into oil and water, and aqueous phase 1 was extracted. 500 g of water was added again to the obtained organic phase 1, and the mixture was mixed for 1 hour. After that, the mixture was left to stand to separate organic phase 2 and aqueous phase 2 into oil and water, and aqueous phase 2 was extracted.

[0158] The aqueous phase 1 and the aqueous phase 2 were placed in a jacketed separable flask equipped with a Dimroth condenser, a stirring blade, and a thermometer under a nitrogen atmosphere, and then 150 g of toluene was added and mixed, and the internal temperature was raised to 80 ° C. The aqueous phase was neutralized with hydrochloric acid while maintaining the internal temperature at 80 ° C. Then, the mixture was left to stand for oil-water separation, and the aqueous phase 3 was extracted to obtain an organic phase 3. 150 g of water was added to the obtained organic phase 3, and the mixture was mixed while maintaining the internal temperature at 80 ° C. Then, the mixture was left to stand for oil-water separation, and the aqueous phase 4 was extracted to obtain an organic phase 4. The obtained organic phase 4 was cooled to 10 ° C. to obtain a slurry liquid. The obtained slurry liquid was filtered by reduced pressure filtration to obtain a cake. The entire cake was dried using an evaporator equipped with an oil bath at an oil bath temperature of 85 ° C. and 15 Torr for 3 hours, and 16 g of solid was obtained. The obtained solid was confirmed by high performance liquid chromatography to be bisphenol A and had a purity of 99%.

[0159] In a 0.5L four-neck flask equipped with a thermometer, a stirrer, and a cooling tube, 15g of the obtained bisphenol A, 84g of epichlorohydrin, 32g of isopropanol, and 13g of water were charged, and the temperature was raised to 40°C to dissolve uniformly, and then 12g of 48.5% by mass aqueous sodium hydroxide solution was added dropwise over 90 minutes. At the same time as the dropwise addition, the temperature was raised from 40°C to 65°C over 90 minutes. Then, the reaction was completed by holding at 65°C for 30 minutes, and the reaction liquid was transferred to a 1L separatory funnel, and 23g of water at 65°C was added to the separatory funnel and allowed to stand at 65°C for 1 hour. After standing, the aqueous phase was extracted from the separated oil phase and aqueous phase, and by-product salt and excess sodium hydroxide were removed. Then, epichlorohydrin was completely removed from the oil phase under reduced pressure at 150°C to obtain a residue.

[0160] Then, 35 g of methyl isobutyl ketone was added to the obtained residue, and the temperature was raised to 65° C. to dissolve the residue uniformly, and then the mixture was mixed with 0.5 g of a 48.5% by mass aqueous sodium hydroxide solution and reacted for 60 minutes. The reaction liquid was then mixed with 19 g of methyl isobutyl ketone, and washed four times with 100 g of water. Thereafter, methyl isobutyl ketone was completely removed under reduced pressure at 150° C. to obtain an epoxy resin. The epoxy equivalent of the obtained epoxy resin was 210 g / eq.

[0161] Example 11 5 g of the epoxy resin (epoxy equivalent: 210 g / eq) obtained in Example 10, 0.05 g of DICY, and 0.05 g of DCMU were placed in an aluminum cup and mixed thoroughly to obtain mixture 1. 5 g of the recycled carbon fiber obtained in Example 9 was placed therein and mixed thoroughly to obtain mixture 2. The obtained mixture 2 was poured into a flat mold and heated at 150°C for 3 hours to obtain a recycled amine-cured carbon fiber composite material.

[0162] Example 12 10 g of the amine-cured CFRP obtained in Reference Example 4 and 50 g of benzyl alcohol were placed in a 100 mL Schlenk flask and placed in a nitrogen atmosphere. The Schlenk flask was immersed in an oil bath at 180°C and stirred for 2 hours. The flask was then cooled to room temperature, taken out with tweezers, and the adhering benzyl alcohol was wiped off with a Kimtowel to obtain a swollen amine-cured CFRP. Carbon fibers were pulled out from the frayed portions found in the resulting swollen amine-cured CFRP, yielding 5 g of carbon fibers.

[0163] Example 13 5 g of bisphenol A type epoxy resin (epoxy equivalent: 183 g / eq), 0.05 g of DICY, and 0.05 g of DCMU were placed in an aluminum cup and mixed thoroughly to obtain mixture 1. 5 g of the carbon fiber obtained in Example 12 was placed therein and mixed thoroughly to obtain mixture 2. The obtained mixture 2 was poured into a flat mold and heated at 150°C for 3 hours to obtain an inorganic carbon fiber reinforced resin.

Claims

1. A method for producing a phenol compound from a cured thermosetting resin, comprising the steps of: a swelling step of contacting the cured thermosetting resin A with an organic solvent to swell the cured thermosetting resin A and obtain a cured thermosetting resin B; a decomposition step of decomposing the thermosetting resin cured material B; A method for producing a phenolic compound, comprising:

2. 2. The method for producing a phenol compound according to claim 1, wherein in the swelling step, a ratio of a mass of the cured thermosetting resin B to a mass of the cured thermosetting resin A is 1.2 or more.

3. The method for producing a phenol compound according to claim 1, wherein the organic solvent is at least one selected from the group consisting of N-methylpyrrolidone and benzyl alcohol.

4. The method for producing a phenol compound according to claim 1, wherein the decomposition step is carried out in the presence of one or more decomposition agents selected from the group consisting of bases, acids, and oxidizing agents.

5. The method for producing a phenol compound according to claim 4, wherein the base is at least one selected from the group consisting of sodium compounds and potassium compounds.

6. The method for producing a phenol compound according to claim 4, wherein the acid is at least one selected from the group consisting of sulfuric acid and nitric acid.

7. The method for producing a phenolic compound according to claim 1 , wherein the thermosetting resin cured product A is an epoxy resin cured product.

8. The thermosetting resin cured material A contains an inorganic substance, The method for producing a phenolic compound according to claim 1 , further comprising, after the decomposition step, an inorganic matter recovery step of recovering the inorganic matter.

9. The method for producing a phenol compound according to claim 8, wherein the inorganic material is at least one selected from the group consisting of carbon fiber and glass fiber.

10. A method for producing an epoxy resin, comprising a reaction step of reacting the phenol compound obtained by the method for producing a phenol compound according to any one of claims 1 to 9 with epihalohydrin.

11. A method for producing a composite material, comprising a curing step of curing an epoxy resin composition containing the epoxy resin obtained by the method for producing an epoxy resin according to claim 10 and the inorganic substance obtained by the method for producing a phenol compound according to claim 8 or 9.

12. A method for producing inorganic fibers from an inorganic fiber reinforced resin, comprising the steps of: a swelling step of contacting an inorganic fiber reinforced resin A containing inorganic fibers and a cured thermosetting resin with an organic solvent to swell the inorganic fiber reinforced resin A and obtain an inorganic fiber reinforced resin B; An inorganic fiber recovery step of separating inorganic fibers from the inorganic fiber reinforced resin B; A method for producing inorganic fibers, comprising:

13. A method for producing an inorganic fiber-reinforced resin, comprising: a curing step of curing a thermosetting resin composition containing a thermosetting resin and the inorganic fibers obtained by the method for producing inorganic fibers according to claim 12.

Citation Information

Patent Citations

  • Method for decomposing and recycling thermosetting resin

    JP1998024274A

Cited By

  • Method for manufacturing fibrous filler and reaction apparatus

    JP2026144018A