Nonwoven fabric laminate and bag-like article using the same

A nonwoven fabric laminate with specific polyethylene terephthalate content and mechanical entanglement addresses recyclability and strength issues, enabling high-shrinkable and recyclable bag-like articles with strong bonding and heat-shrinkable properties.

JP2024165349APending Publication Date: 2024-11-28TOYOBO MC CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023081475
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-17
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Nonwoven fabrics with polyethylene terephthalate blends are difficult to recycle and short fiber nonwoven fabrics lack the strength of long fiber counterparts, limiting their applications and recyclability.

Method used

A nonwoven fabric laminate composed of at least a first and second long fiber nonwoven fabric, where the second fabric has a dry heat area shrinkage rate of 30% or more, containing 99% polyethylene terephthalate, and is mechanically entangled, allowing for thermocompression bonding and heat shrinkage.

Benefits of technology

The laminate achieves high shrinkability, excellent mechanical strength, and recyclability, enabling the production of a bag-like article with strong bonding and close contact with contents upon heat shrinkage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024165349000001
    Figure 2024165349000001
Patent Text Reader

Abstract

To provide a nonwoven fabric laminate having high shrinkability.SOLUTION: A nonwoven fabric laminate of the invention is formed by laminating at least a first long fiber nonwoven fabric and a second long fiber nonwoven fabric having a dry heat area shrinkage percentage higher by 30% or more than that of the first long fiber nonwoven fabric. The constituent fiber of the second long fiber nonwoven fabric includes resin having 99 mass% or more of polyethylene terephthalate component. The second long fiber nonwoven fabric has 30% or more of the dry heat area shrinkage percentage. The constituent fiber has 10×10-3 to 60×10-3 of double refractive index (Δn) and 1.335 to 1.340 g / cm3 of density.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to nonwoven laminates and pouches. [Background technology]

[0002] There is a technology for shrinking nonwoven fabrics by heating. For example, Patent Document 1 discloses a technology that can shrink at low temperatures by blending amorphous polyester, which reduces the thermal energy required for shrinking processing and contributes to energy saving. Patent Document 2 discloses a high-shrinkage nonwoven fabric containing short fibers of isophthalic acid copolymerized polyethylene terephthalate. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent Publication No. 2014-240531 [Patent Document 2] JP2003-336151A Summary of the Invention [Problem to be solved by the invention]

[0004] However, the nonwoven fabric in Patent Document 1 is difficult to recycle because it is a blend rather than a single polyethylene terephthalate, and the nonwoven fabric in Patent Document 2 is a short fiber nonwoven fabric, which is inferior in strength to a long fiber nonwoven fabric.

[0005] The present invention has been made in consideration of the problems with the prior art described above, and an object of the present invention is to provide a nonwoven fabric laminate having high shrinkability, and further to provide a bag-shaped article which can be heat-pressed using the same. [Means for solving the problem]

[0006] The present inventors have conducted intensive research to solve the above problems and have finally completed the present invention. 1. A nonwoven fabric laminate comprising at least a first long-fiber nonwoven fabric and a second long-fiber nonwoven fabric having a dry heat areal shrinkage rate 30% or more higher than that of the first long-fiber nonwoven fabric, the second long-fiber nonwoven fabric having constituent fibers containing a resin with a polyethylene terephthalate component of 99% by mass or more, a dry heat areal shrinkage rate of 30% or more, and a birefringence index (Δn) of the constituent fibers of 10×10 -3 ~60×10 -3 and the density of the constituent fibers is 1.335 to 1.340 g / cm 3 The nonwoven fabric laminate according to claim 1, 2. The nonwoven fabric laminate according to the above item 1, wherein the second long-fiber nonwoven fabric has a ratio of dry heat areal shrinkage rate in the longitudinal direction to that in the transverse direction of 0.95 to 1.05. 3. The nonwoven fabric laminate according to claim 1 or 2, wherein the nonwoven fabric laminate is mechanically entangled. 4. The nonwoven fabric laminate according to any one of 1 to 3 above, wherein the first long-fiber nonwoven fabric is made of fibers made of a resin having a polyethylene terephthalate content of 99% by mass or more. 5. A bag-shaped product using the nonwoven fabric laminate according to any one of 1 to 4 above, the bag-shaped product having a joint where the first long-fiber nonwoven fabrics are joined together by thermocompression bonding. 6. The bag-like article according to 5 above, wherein the bonding strength at the joint is not more than one-third of the strength of the base fabric of the nonwoven fabric laminate. 7. A bag as described in 5 or 6 above, which is sealed to the contents placed in the bag by heat shrinkage. Effect of the Invention

[0007] According to the present invention, a nonwoven fabric laminate having excellent shrinkability can be obtained, and heat compression bonding can be performed satisfactorily. Furthermore, since the present invention uses a resin containing 99% by mass or more of a polyethylene terephthalate component, it is possible to provide a nonwoven fabric laminate with good recyclability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The present invention will be described in detail below, but the present invention is not limited to the following and can be practiced with appropriate modifications within the scope of the above and below described intent, and all such modifications are included in the technical scope of the present invention.

[0009] [Nonwoven fabric laminate] The present invention is a nonwoven fabric laminate having at least a first long-fiber nonwoven fabric and a second long-fiber nonwoven fabric laminated thereto, the second long-fiber nonwoven fabric having a dry heat areal shrinkage rate 30% or more higher than that of the first long-fiber nonwoven fabric. When the dry heat areal shrinkage rates of the first long-fiber nonwoven fabric and the second long-fiber nonwoven fabric differ by 30% or more, the effect of increasing the elongation of the nonwoven fabric laminate obtained by heat treatment is easily achieved. Here, in the present invention, the dry heat areal shrinkage rate refers to the areal shrinkage rate when heat treated at 100°C for 3 minutes. The nonwoven fabric laminate of the present invention is sufficient as long as at least a first long-fiber nonwoven fabric and a second long-fiber nonwoven fabric are laminated together, and other nonwoven fabrics may also be laminated thereto.

[0010] The first long-fiber nonwoven fabric in the present invention preferably has a dry heat areal shrinkage of 10% or less, more preferably 5% or less. The second long-fiber nonwoven fabric in the present invention preferably has a dry heat areal shrinkage of 25% or more, more preferably 30% or more, and even more preferably 40% or more. The dry heat areal shrinkage is the dry heat areal shrinkage at 100°C for 3 minutes measured separately for each of the first and second long-fiber nonwoven fabrics before laminating them to form a nonwoven fabric laminate.

[0011] The first long-fiber nonwoven fabric of the present invention will be described. The resin used for the first long-fiber nonwoven fabric is preferably polyester, and particularly preferably polyethylene terephthalate (PET), which is a general-purpose thermoplastic resin and inexpensive. Other examples of the resin used include homopolyesters such as polybutylene terephthalate (PBT), polybutylene naphthalate (PBN), polyethylene naphthalate (PEN), polycyclohexane dimethyl terephthalate (PCHT), and polytrimethylene terephthalate (PTT). In the present invention, PET is used. This is because PET has excellent properties such as strength and heat resistance. Note that polyesters other than PET may be blended. In addition, the first long-fiber nonwoven fabric of the present invention may contain commonly used additives, such as paints, pigments, matting agents, antistatic agents, flame retardants, and reinforcing particles.

[0012] The method for producing the first long-fiber nonwoven fabric in the present invention is not particularly limited, but it is preferably produced by a spunbond method from the viewpoint of the productivity and ease of obtaining mechanical strength properties as a long-fiber nonwoven fabric. The average fiber diameter of the long fibers (single fibers) constituting the first long-fiber nonwoven fabric is preferably about 1 to 10 dtex. The basis weight of the first long-fiber nonwoven fabric may be set in consideration of the mechanical strength properties required for the final product, and in consideration of not inhibiting the shrinkage when the second long-fiber nonwoven fabric, which has a high dry heat areal shrinkage rate, is shrunk by heat treatment.

[0013] The second long-fiber nonwoven fabric of the present invention will be described. The resin used for the second long-fiber nonwoven fabric is preferably polyester, and particularly preferably polyethylene terephthalate (PET), which is a general-purpose thermoplastic resin and inexpensive. Other examples of the resin that can be used include homopolyesters such as polybutylene terephthalate (PBT), polybutylene naphthalate (PBN), polyethylene naphthalate (PEN), polycyclohexane dimethyl terephthalate (PCHT), and polytrimethylene terephthalate (PTT). In the present invention, PET is used. This is because PET has excellent properties such as strength and heat resistance. Note that polyesters other than PET may be blended as long as the amount is less than 1% by mass. In addition, in the present invention, The second long fiber nonwoven fabric may contain commonly used additives, such as paints, pigments, matting agents, antistatic agents, flame retardants, and reinforcing particles.

[0014] A method for obtaining the second long-fiber nonwoven fabric in the present invention will be described. The method for producing the second long-fiber nonwoven fabric is not particularly limited, but it is preferable to produce it by the spunbond method from the viewpoint of productivity and easy mechanical strength properties as a long-fiber nonwoven fabric. In order to obtain a second long-fiber nonwoven fabric with a high dry heat areal shrinkage rate by this method, a method is used in which the resin used is fiberized at a spinning speed lower than the condition under which stable filaments are obtained by oriented crystallization, and then sheeted. The spinning speed needs to be appropriately changed depending on the resin used, and when PET is used, the spinning speed is preferably 2000 to 3500 m / min, and more preferably 2000 to 3000 m / min. The average fiber diameter of the long fibers (single fibers) constituting the second long-fiber nonwoven fabric is preferably about 1 to 20 dtex, and more preferably about 2 to 15 dtex. The basis weight of the second long-fiber nonwoven fabric can be set in consideration of the mechanical strength properties required for the final product, but it is preferably 80 g / m in order to obtain the stress to shrink by heat treatment. 2 The above is preferable. In consideration of the processability in the mechanical entangling step after obtaining the second long-fiber nonwoven fabric, it is preferable to limit the compression of the second long-fiber nonwoven fabric to an extent that allows transportability. If the average fiber diameter and basis weight are within the above ranges, each property such as strength, processability, flexibility, etc. can be well-balanced and excellent.

[0015] The birefringence (Δn) of the constituent fibers of the second long fiber nonwoven fabric in the present invention is 60×10 -3 It is preferably 55×10 or less. -3 Less than 50×10, more preferably -3 The birefringence of the fiber is 60×10 or less. -3 If the shrinkage rate exceeds 100%, the polymer molecules are oriented and crystallized, inhibiting shrinkage and resulting in a low shrinkage rate. The birefringence can be controlled by the discharge conditions, cooling conditions, and stretching conditions during fiberization. When a particularly high shrinkage rate is required, a spinning speed of 2000 to 3500 m / min is preferred, and 2500 to 3000 m / min is more preferred.

[0016] The density of the constituent fibers of the second long fiber nonwoven fabric in the present invention is 1.330 to 1.340 g / cm 3 is preferable, and 1.335 to 1.340 g / cm 3 Within the above range, it is possible to obtain a well-balanced and excellent range of properties such as strength, processability, flexibility, etc.

[0017] [Mechanical entanglement] Next, an example of a method for laminating the first long-fiber nonwoven fabric and the second long-fiber nonwoven fabric of the present invention will be described. The first long fiber nonwoven fabric and the second long fiber nonwoven fabric are overlapped, and the fibers are mechanically entangled by needle punching from one or both sides. Methods of mechanical entanglement include needle punching and water punching, but needle punching is preferred because it does not require drying and allows for a high basis weight. Needle punching penetrates the nonwoven fabric with needles to entangle the fibers. The penetration number and needle depth can be set appropriately depending on the type of needle used, the desired mechanical strength properties, and the basis weight.

[0018] [Bag-like items] The nonwoven fabric laminate of the present invention can be easily formed into a bag-like product by bonding the first long-fiber nonwoven fabrics together by thermocompression bonding with the first long-fiber nonwoven fabric on the inside. In the bag-like product, the first long-fiber nonwoven fabric is the side that contacts the contents to be placed inside. The bag-like product using the nonwoven fabric laminate of the present invention is also within the scope of the present invention. The bag-like product of the present invention has a joint where the first long-fiber nonwoven fabrics are bonded together by thermocompression bonding. In the bag-like product of the present invention, the bonding strength of the joint is preferably one-third or less of the strength of the long-fiber nonwoven fabric. In this range, the bag-like product can be easily opened from the joint when it is desired to open the bag-like product from the joint. In addition, the bag-like product can be made to adhere to the contents to be placed in the bag-like product by heat shrinkage. By placing the first long-fiber nonwoven fabric, which has a low dry heat areal shrinkage rate, on the inside, the nonwoven fabric laminate does not fuse to the contents, and therefore can be suitably used as a bag-like product. EXAMPLES

[0019] The present invention will be described in more detail below with reference to examples. However, the following examples do not limit the present invention, and all modifications and variations within the scope of the present invention are included in the technical scope of the present invention. First, the characteristic evaluation method will be described.

[0020] <Dry heat area shrinkage rate> According to JIS L 1913 (2010) 6.10, cut the long fiber nonwoven fabric into 250 mm squares at 10 random locations, and mark 200 mm lengths at 3 locations in each of the warp and weft directions. Heat treat in a thermostatic dryer at 100°C for 3 minutes, and calculate the area shrinkage rate from the dimensional change before and after heat treatment.

[0021] <Birefringence> For a single fiber taken out of the long fiber nonwoven fabric, the retardation and fiber diameter are determined using a polarizing microscope equipped with a Berek compensator, and the average value of n=5 is taken as the birefringence index (Δn) of the fiber.

[0022] <density> The density of the fibers is measured using a density gradient tube (n=4) and the average value is calculated.

[0023] <Ratio of dry heat area shrinkage rate in the vertical and horizontal directions> According to JIS L 1913 (2010) 6.10, a sample of a long fiber nonwoven fabric is cut into 250 mm squares at 10 random locations, and 200 mm long marks are made in 3 locations in each of the warp and weft directions. The sample is heat-treated in a thermostatic dryer at 100°C for 3 minutes, and the ratio of the warp direction to the weft direction is calculated from the change in dimensions before and after the heat treatment.

[0024] <Joining strength> Two samples were cut from the entangled nonwoven fabric laminate, stacked so that the first long fiber nonwoven fabrics were on the inside, and heat sealed in the width direction at 268°C for 2 minutes using a heat sealer (Auto Sealer FA-450-5W series manufactured by Fuji Impulse Co., Ltd.). The heat-sealed sample was spread out and measured in accordance with JIS L 1913 (2010) 6.3 Tensile strength and elongation (ISO method) using a constant-speed extension tensile tester (Tensilon manufactured by Orientec) and the same tester at three sample pieces 50 mm wide and 200 mm long from the product width of the sample, with a grip interval of 100 mm and a speed of 200 mm / min. The average of the obtained tensile strengths was taken as the bonding strength (N / 5 cm).

[0025] <Metsuke> According to the method described in JIS L 1913 (2010), a long fiber nonwoven fabric is measured in a size of 20 cm x 20 cm, and the mass per unit area is measured.

[0026] <Base fabric strength> Using the entangled nonwoven fabric laminate, in accordance with JIS L 1913 (2010) 6.3 Tensile strength and elongation (ISO method), five sample pieces 50 mm wide and 200 mm long from the product width of the nonwoven fabric laminate were measured using a constant speed extension type tensile tester (Orientec Tensilon) and the same tester, with the gripping distance of 100 mm and the measurement speed of 200 mm / min, and the average value of the tensile strength obtained is the base fabric strength (N / 5cm).

[0027] Example 1 The first long fiber nonwoven fabric was produced as follows. The raw material was a polyester having an intrinsic viscosity of 0.63 dl / g. A polyester containing 99% or more ethylene terephthalate was used. The spinning temperature was 285°C, and the spinning was performed from a spinneret with an orifice diameter of φ0.30 mm at a single hole output rate of 1.74 g / min. The spinning was performed while cooling with 20°C air at a wind speed of 0.75 m / sec from 120 mm directly below the spinneret. The spinning was performed at a speed of 2.20 kg / cm from an ejector located 900 mm directly below the spinneret. 2Dry air was supplied at a pressure of 1.00 rpm, stretched in one step, and the fiber bundle was spread onto a conveyor net 1.0 m below, while the speed was adjusted so that the fiber arrangement was random. Next, embossing was performed at 180°C and a linear pressure of 20 kN / m using an embossing roll installed in-line, which had a staggered arrangement of pyramidal frustum-shaped convex parts with a bonding area ratio of 8%. As a result, the single fiber fineness was 2.2 dtex, the converted spinning speed was 4500 m / min, and Δn was 90×10 -3 , density is 1.370g / cm 3 , dry heat area shrinkage rate is 4%, basis weight is 10g / m 2 Thus, a first long fiber nonwoven fabric was obtained.

[0028] The second long fiber nonwoven fabric was manufactured as follows. The raw material was a polyester with an intrinsic viscosity of 0.63 dl / g and 99% by mass or more of polyethylene terephthalate. The fiber was spun from a spinneret with an orifice diameter of φ0.30 mm at a spinning temperature of 285°C at a single hole output rate of 1.74 g / min, and cooled with 20°C air at a wind speed of 0.75 m / sec from 120 mm directly below the spinneret, while being fed at 0.85 kg / cm to an ejector located 900 mm directly below the spinneret. 2 Dry air was supplied at a pressure of 1000 rpm, stretched in one step, and the fiber bundle was spread onto a conveyor net 1.0 m below, while the speed was adjusted so that the fiber arrangement was random, and the fiber bundle was deposited. Next, embossing was performed at 60°C and a linear pressure of 30 kN / m using an embossing roll installed in-line, which had a staggered arrangement of pyramidal frustum-shaped convex parts with a bonding area ratio of 8%. As a result, the single fiber fineness was 6.0 dtex, the converted spinning speed was 2500 m / min, and Δn was 41×10 -3 , density is 1.335g / cm 3 , dry heat area shrinkage rate is 58%, the ratio of dry heat area shrinkage rate in the longitudinal direction to the transverse direction is 1.01, and the basis weight is 100g / m 2 A second long fiber nonwoven fabric was obtained.

[0029] The first long fiber nonwoven fabric and the second long fiber nonwoven fabric are stacked together, and a needle density of 95 / cm is applied to one side. 2 The fibers were then subjected to an entanglement treatment by needle punching at a needle depth of 10 mm to obtain a nonwoven fabric laminate.

[0030] The nonwoven fabric laminate was cut into a length of 25 cm and a width of 10 cm, preheated at 190°C for 10 seconds, folded in half with the first long fiber nonwoven fabric on the inside, and bonded at a temperature of 190°C and a bonding pressure of 15 kg / cm at a point 1 cm from the end of the nonwoven fabric laminate. 2 The bag-like product was then heat-pressed for a bonding time of 5 seconds to obtain a bag-like product with a bonded portion. The entire surface of the heat-pressed portion was bonded to form a bonded portion. Contents were placed in the bag-like product, and heat-treated at 100°C for 3 minutes to obtain a heat-shrunk bag-like product. It was visually confirmed that the bag-like product and the contents had come into close contact with each other due to the heat shrinkage. Furthermore, both ends of the bonded portion of the bag-like product in the vertical direction were cut, and the bonding strength was evaluated using the method described above.

[0031] Example 2

[0032] The first long fiber nonwoven fabric was manufactured as follows. The raw material was a polyester with an intrinsic viscosity of 0.63 dl / g and 99% by mass or more of polyethylene terephthalate. The material was spun from a spinneret with an orifice diameter of φ0.30 mm at a spinning temperature of 285°C at a single hole output rate of 1.74 g / min. The material was cooled with 20°C air at a wind speed of 0.75 m / sec from 120 mm directly below the spinneret, and the material was fed to an ejector located 900 mm directly below the spinneret with a pressure of 2.20 kg / cm. 2 Dry air was supplied at a pressure of 1.00 rpm, stretched in one step, and the fiber bundle was spread onto a conveyor net 1.0 m below, while the speed was adjusted so that the fiber arrangement was random. Next, embossing was performed at 180°C and a linear pressure of 20 kN / m using an embossing roll installed in-line, which had a staggered arrangement of pyramidal frustum-shaped convex parts with a bonding area ratio of 8%. As a result, the single fiber fineness was 2.2 dtex, the converted spinning speed was 4500 m / min, and Δn was 90×10 -3 , density is 1.370g / cm 3 , dry heat area shrinkage rate is 3%, basis weight is 20g / m 2 Thus, a first long fiber nonwoven fabric was obtained.

[0033] The second long fiber nonwoven fabric was manufactured as follows. The raw material was a polyester with an intrinsic viscosity of 0.63 dl / g and 99% by mass or more of polyethylene terephthalate. The fiber was spun from a spinneret with an orifice diameter of φ0.30 mm at a spinning temperature of 285°C at a single hole output rate of 1.74 g / min, and cooled with 20°C air at a wind speed of 0.75 m / sec from 120 mm directly below the spinneret, while being fed at 0.85 kg / cm to an ejector located 900 mm directly below the spinneret. 2 Dry air was supplied at a pressure of 1000 rpm, stretched in one step, and the fiber bundle was spread onto a conveyor net 1.0 m below, while the speed was adjusted so that the fiber arrangement was random, and the fiber bundle was deposited. Next, embossing was performed at 60°C and a linear pressure of 30 kN / m using an embossing roll installed in-line, which had a staggered arrangement of pyramidal frustum-shaped convex parts with a bonding area ratio of 8%. As a result, the single fiber fineness was 6.0 dtex, the converted spinning speed was 2800 m / min, and Δn was 48×10 -3 , density is 1.338g / cm 3 , dry heat area shrinkage rate is 58%, the ratio of dry heat area shrinkage rate in the longitudinal direction to the transverse direction is 1.01, and the basis weight is 100g / m 2 A second long fiber nonwoven fabric was obtained.

[0034] The first long fiber nonwoven fabric and the second long fiber nonwoven fabric are stacked together, and a needle density of 49 / cm is formed on one side. 2 Then, the needle punch is used to entangle the fibers at a needle depth of 8 mm, and the density of the fibers is reduced to 51 fibers / cm from the needle punched surface. 2 The fibers were then subjected to an entanglement treatment by needle punching at a needle depth of 8 mm to obtain a nonwoven fabric laminate.

[0035] The nonwoven fabric laminate was cut into a size of 25 cm length and 10 cm width, preheated at 190°C for 10 seconds, folded in half with the first long fiber nonwoven fabric on the inside, and bonded at a point 1 cm from the edge of the nonwoven fabric laminate at a bonding temperature of 190°C and a bonding pressure of 15 kg / cm. 2The bag-like product was then heat-pressed for a bonding time of 5 seconds to obtain a bag-like product with a bonded portion. The entire surface of the heat-pressed portion was bonded to form a bonded portion. Contents were placed in the bag-like product, and heat-treated at 100°C for 3 minutes to obtain a heat-shrunk bag-like product. It was visually confirmed that the bag-like product and the contents had come into close contact with each other due to the heat shrinkage. Furthermore, both ends of the bonded portion of the bag-like product in the vertical direction were cut, and the bonding strength was evaluated using the method described above.

[0036] Example 3 The first long fiber nonwoven fabric was manufactured as follows. The raw material was a polyester with an intrinsic viscosity of 0.63 dl / g and 99% by mass or more of polyethylene terephthalate. The material was spun from a spinneret with an orifice diameter of φ0.30 mm at a spinning temperature of 285°C at a single hole output rate of 1.74 g / min. The material was cooled with 20°C air at a wind speed of 0.75 m / sec from 120 mm directly below the spinneret, and the material was fed to an ejector located 900 mm directly below the spinneret with a pressure of 2.20 kg / cm. 2 Dry air was supplied at a pressure of 1.00 rpm, stretched in one step, and the fiber bundle was spread onto a conveyor net 1.0 m below, while the speed was adjusted so that the fiber arrangement was random. Next, embossing was performed at 180°C and a linear pressure of 20 kN / m using an embossing roll installed in-line, which had a staggered arrangement of pyramidal frustum-shaped convex parts with a bonding area ratio of 8%. As a result, the single fiber fineness was 2.2 dtex, the converted spinning speed was 4500 m / min, and Δn was 90×10 -3 , density is 1.370g / cm 3 , dry heat area shrinkage rate is 3%, basis weight is 30g / m 2 Thus, a first long fiber nonwoven fabric was obtained.

[0037] The second long fiber nonwoven fabric was manufactured as follows. The raw material was a polyester with an intrinsic viscosity of 0.63 dl / g and 99% by mass or more of polyethylene terephthalate. The fiber was spun from a spinneret with an orifice diameter of φ0.30 mm at a spinning temperature of 285°C at a single hole output rate of 1.74 g / min, and cooled with 20°C air at a wind speed of 0.75 m / sec from 120 mm directly below the spinneret, while being fed at 0.85 kg / cm to an ejector located 900 mm directly below the spinneret. 2Dry air was supplied at a pressure of 1000 rpm, stretched in one step, and the fiber bundle was spread onto a conveyor net 1.0 m below, while the speed was adjusted so that the fiber arrangement was random, and the fiber bundle was deposited. Next, embossing was performed at 60°C and a linear pressure of 30 kN / m using an embossing roll installed in-line, which had a staggered arrangement of pyramidal frustum-shaped convex parts with a bonding area ratio of 8%. As a result, the single fiber fineness was 6.0 dtex, the converted spinning speed was 2800 m / min, and Δn was 48×10 -3 , density is 1.338g / cm 3 , dry heat area shrinkage rate is 61%, and the ratio of dry heat area shrinkage rate in the longitudinal direction to the transverse direction is 1.01 , basis weight is 100g / m 2 A second long fiber nonwoven fabric was obtained.

[0038] The first long fiber nonwoven fabric and the second long fiber nonwoven fabric are stacked together, and a needle density of 49 / cm is formed on one side. 2 Then, the needle punch is used to entangle the fibers at a needle depth of 8 mm, and the density of the fibers is reduced to 51 fibers / cm from the needle punched surface. 2 The fibers were then subjected to an entanglement treatment by needle punching at a needle depth of 8 mm to obtain a nonwoven fabric laminate.

[0039] The nonwoven fabric laminate was cut into a length of 25 cm and a width of 10 cm, preheated at 170°C for 10 seconds, folded in half with the first long fiber nonwoven fabric on the inside, and bonded at a point 1 cm from the edge of the nonwoven fabric laminate at a bonding temperature of 170°C and a bonding pressure of 10 kg / cm. 2 The bag-shaped product was then heat-pressed for a bonding time of 5 seconds to obtain a bag-shaped product with a bonded portion. The entire surface of the heat-pressed portion was bonded to form a bonded portion. Contents were placed in the bag-shaped product, and heat-treated at 100°C for 3 minutes to obtain a heat-shrunk bag-shaped product. It was visually confirmed that the bag-shaped product and the contents had come into close contact with each other due to the heat shrinkage. Furthermore, both ends of the bonded portion of the bag-shaped product in the vertical direction were cut, and the bonding strength was evaluated using the method described above.

[0040] Comparative Example 1 The first long fiber nonwoven fabric was manufactured as follows. The raw material was a polyester with an intrinsic viscosity of 0.63 dl / g and 99% by mass or more of polyethylene terephthalate. The material was spun from a spinneret with an orifice diameter of φ0.30 mm at a spinning temperature of 285°C at a single hole output rate of 1.74 g / min. The material was cooled with 20°C air at a wind speed of 0.75 m / sec from 120 mm directly below the spinneret, and the material was fed to an ejector located 900 mm directly below the spinneret with a pressure of 2.20 kg / cm. 2 Dry air was supplied at a pressure of 1.00 rpm, stretched in one step, and the fiber bundle was spread onto a conveyor net 1.0 m below, while the speed was adjusted so that the fiber arrangement was random. Next, embossing was performed at 180°C and a linear pressure of 20 kN / m using an embossing roll installed in-line, which had a staggered arrangement of pyramidal frustum-shaped convex parts with a bonding area ratio of 8%. As a result, the single fiber fineness was 2.2 dtex, the converted spinning speed was 4500 m / min, and Δn was 90×10 -3 , density is 1.370g / cm 3 , dry heat area shrinkage rate is 4%, basis weight is 10g / m 2 Thus, a first long fiber nonwoven fabric was obtained.

[0041] The second long fiber nonwoven fabric was manufactured as follows. The raw material was a polyester with an intrinsic viscosity of 0.63 dl / g and 99% by mass or more of polyethylene terephthalate. The fiber was spun from a spinneret with an orifice diameter of φ0.30 mm at a spinning temperature of 285°C at a single hole output rate of 1.74 g / min, and cooled with 20°C air at a wind speed of 0.75 m / sec from 120 mm directly below the spinneret, while being fed at 0.85 kg / cm to an ejector located 900 mm directly below the spinneret. 2 Dry air was supplied at a pressure of 1.00 rpm, stretched in one step, and the fiber bundle was spread onto a conveyor net 1.0 m below, while the speed was adjusted so that the fiber arrangement was random. Next, embossing was performed at 180°C and a linear pressure of 20 kN / m using an embossing roll installed in-line, which had a staggered arrangement of pyramidal frustum-shaped convex parts with a bonding area ratio of 8%. As a result, the single fiber fineness was 4.8 dtex, the converted spinning speed was 3800 m / min, and Δn was 70×10 -3 , density is 1.358g / cm 3, dry heat area shrinkage rate is 27%, the ratio of dry heat area shrinkage rate in the longitudinal direction to the transverse direction is 1.05, and the basis weight is 100g / m 2 A second long fiber nonwoven fabric was obtained.

[0042] The first long fiber nonwoven fabric and the second long fiber nonwoven fabric are stacked together, and a needle density of 95 / cm is applied to one side. 2 The fibers were then subjected to an entanglement treatment by needle punching at a needle depth of 10 mm to obtain a nonwoven fabric laminate.

[0043] The nonwoven fabric laminate was cut into a size of 25 cm length and 10 cm width, preheated at 100°C for 10 seconds, folded in half with the first long fiber nonwoven fabric on the inside, and bonded at a point 1 cm from the edge of the nonwoven fabric laminate at a bonding temperature of 100°C and a bonding pressure of 15 kg / cm. 2 The bag was then heat-pressed for 10 seconds to obtain a bag-like product with a bonded portion. The entire surface of the heat-pressed portion was bonded. The contents were placed in the bag-like product, and heat-treated at 100°C for 3 minutes to obtain a heat-shrunk bag-like product. Although the shrinkage was weak, it was visually confirmed that the bag-like object and the contents were in close contact. Furthermore, both ends of the joint in the longitudinal direction of the bag-like object were cut, and the joint strength was evaluated by the above-mentioned method.

[0044] Comparative Example 2 The first long fiber nonwoven fabric was manufactured as follows. The raw material was a polyester with an intrinsic viscosity of 0.63 dl / g and a polyethylene terephthalate component of 99% by mass or more. The material was spun from a spinneret with an orifice diameter of φ0.30 mm at a single hole discharge rate of 1.74 g / min at a spinning temperature of 285°C, cooled with 20°C air at a wind speed of 0.75 m / sec from 120 mm directly below the spinneret, and dried air was supplied to an ejector located 900 mm directly below the spinneret at a pressure of 2.20 kg / cm2 to stretch the fiber bundle in one step, and the speed was adjusted so that the fiber arrangement was random while spreading the fiber bundle on a conveyor net located 1.0 m below. Next, embossing was performed at 180°C and a linear pressure of 20 kN / m using an embossing roll installed inline with a staggered arrangement of pyramidal truncated convex parts with a pressure-bonding area ratio of 8%. As a result, the single yarn fineness was 2.2 dtex, the converted spinning speed was 4500 m / min, Δn was 90 × 10-3, and the density was 1.370 g / cm 3 , dry heat area shrinkage rate is 2%, basis weight is 10g / m 2 Thus, a first long fiber nonwoven fabric was obtained.

[0045] The second long fiber nonwoven fabric was manufactured as follows. The raw material was a polyester with an intrinsic viscosity of 0.63 dl / g and a polyethylene terephthalate content of 99% by mass or more. The material was spun from a spinneret with an orifice diameter of φ0.30 mm at a single hole output rate of 1.74 g / min at a spinning temperature of 285°C, cooled with 20°C air at a wind speed of 0.75 m / sec from 120 mm directly below the spinneret, and dried air was supplied to an ejector located 900 mm directly below the spinneret at a pressure of 2.30 kg / cm2 to stretch the fiber bundle in one step, and deposited on a conveyor net located 1.0 m below, with the speed adjusted so that the fiber arrangement was random while spreading the fiber bundle. The single fiber fineness was 4.7 dtex, the converted spinning speed was 4500 m / min, and Δn103×10 -3 , density 1.370g / cm 3 , dry heat area shrinkage rate is 8%, and the ratio of dry heat area shrinkage rate in the longitudinal and transverse directions is 1.05. 2 A second long fiber nonwoven fabric was obtained.

[0046] The first long fiber nonwoven fabric and the second long fiber nonwoven fabric are stacked together, and a needle density of 95 / cm is applied to one side. 2 The fibers were then subjected to an entanglement treatment by needle punching at a needle depth of 8 mm to obtain a nonwoven fabric laminate.

[0047] The nonwoven fabric laminate was cut into a size of 25 cm length and 10 cm width, preheated at 190°C for 10 seconds, folded in half with the first long fiber nonwoven fabric on the inside, and bonded at a point 1 cm from the edge of the nonwoven fabric laminate at a bonding temperature of 190°C and a bonding pressure of 3 kg / cm. 2 The bag was then heat-pressed for a bonding time of 5 seconds to obtain a bag-like product with a bonded section. Only a portion of the heat-pressed section was bonded to form the bonded section. Contents were placed in the bag-like product, and heat-treated at 100°C for 3 minutes to obtain a heat-shrunk bag-like product. It was not possible to visually confirm that the bag-like product and the contents were in close contact. Furthermore, both vertical ends of the bonded section of the bag-like product were cut, and the bonding strength was evaluated using the method described above.

[0048] Table 1 shows the measurement results of the physical properties of Examples 1 to 3 and Comparative Examples 1 and 2.

[0049] [Table 1]

[0050] From Table 1, it can be seen that in Examples 1 to 3, when made into a bag-like product, the product has excellent adhesion to the contents and excellent bonding strength. In addition, since polyester containing 99% or more by mass of polyethylene terephthalate is used, the product is also easy to recycle. It was also confirmed that in Examples 1 to 3, the bag-like product and the contents are in close contact but are not fused together. [Industrial Applicability]

[0051] INDUSTRIAL APPLICABILITY The present invention makes it possible to provide a nonwoven fabric laminate having high shrinkage properties, excellent mechanical strength properties, light weight and easy to handle, and a bag-like article using the same, which will make a great contribution to the industry.

Claims

1. a nonwoven fabric laminate including at least a first long-fiber nonwoven fabric and a second long-fiber nonwoven fabric having a dry heat areal shrinkage rate 30% or more higher than that of the first long-fiber nonwoven fabric; The second long fiber nonwoven fabric has constituent fibers that contain a resin having a polyethylene terephthalate component of 99% by mass or more, a dry heat areal shrinkage rate of 30% or more, and a birefringence index (Δn) of the constituent fibers of 10×10 -3 ~60 x 10 -3 , and the density of the constituent fibers is 1.335 to 1.340 g / cm 3 The nonwoven fabric laminate according to claim 1,

2. 2. The nonwoven fabric laminate according to claim 1, wherein the second long-fiber nonwoven fabric has a ratio of dry heat areal shrinkage rate in the longitudinal direction to that in the transverse direction of 0.95 to 1.

05.

3. 3. The nonwoven laminate of claim 1 or 2, wherein the nonwoven laminate is mechanically entangled.

4. 3. The nonwoven fabric laminate according to claim 1, wherein the first long-fiber nonwoven fabric is made of resin whose constituent fibers contain 99% or more by mass of a polyethylene terephthalate component.

5. 3. A bag-shaped product using the nonwoven fabric laminate according to claim 1 or 2, characterized in that the bag-shaped product has a joint where the first long-fiber nonwoven fabrics are joined to each other by thermocompression bonding.

6. 6. The bag-like article according to claim 5, wherein the bond strength at the bonded portion is one-third or less of the strength of the base fabric of the nonwoven fabric laminate.

7. 6. The bag-like article according to claim 5, characterized in that the bag-like article and the contents to be placed therein are sealed together by heat shrinkage.

Citation Information

Patent Citations

  • Heat shrinkable nonwoven sheet and its production

    JP1988235560A

  • Manufacturing method of nonwoven fabric of laminated long fiber

    JP2018066069A

  • NONWOVEN SHEET EXCELLENT IN HEAT SEALABILITY AND METHOD FOR MANUFACTURING THE SAME

    JP2713439B2

  • Highly shrinkable nonwoven fabric and method for producing the same

    JP2003336151A

  • Continuous fiber non-woven fabric shrinking largely at low temperature

    JP2014240531A