Adsorbent and treatment method
A dolomite-based adsorbent with phosphate and iron ions effectively removes heavy metals by forming stable compounds, addressing the inefficiencies of existing adsorbents in treating contaminated water.
Patent Information
- Application Number
- JP2023081895
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-17
- Publication Date
- 2024-11-28
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing adsorbents struggle to efficiently remove heavy metals like chromium and arsenic, and they often face issues with re-dissolution in alkaline solutions, limiting their effectiveness in treating contaminated water.
An adsorbent composed of dolomites, phosphate ions, and iron ions, where phosphate ions chemically bond with calcium and magnesium in dolomites to form calcium and magnesium phosphate compounds, enhancing heavy metal removal efficiency.
The adsorbent achieves high removal rates for chromium and arsenic, with phosphate and iron ions being stably immobilized, preventing re-dissolution and improving durability and efficiency.
Smart Images

Figure 2024165588000001 
Figure 2024165588000002 
Figure 2024165588000003
Abstract
Description
[Technical field]
[0001] The present invention relates to adsorbents and treatment methods. [Background technology]
[0002] Water used in factories and mines can contain many contaminants such as heavy metals. When such contaminated water is to be discharged, the contaminants must be thoroughly removed.
[0003] Furthermore, well water from contaminated soil may contain contaminants such as heavy metals, and if it is to be used for drinking water or other daily life purposes, it is necessary to thoroughly remove the contaminants.
[0004] Conventionally, large amounts of adsorbents have been used to remove pollutants (see, for example, Patent Document 1). However, when treatment with an adsorbent is performed in an alkaline liquid, heavy metals cannot be sufficiently adsorbed, or the adsorbed heavy metals are re-dissolved, making it difficult to sufficiently remove pollutants.
[0005] Adsorbents made from MgO-based or CaO-based materials have also been proposed (see, for example, Patent Document 2). However, it has been difficult to sufficiently remove heavy metals such as chromium (Cr) and arsenic (As). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2013-696 A [Patent Document 2] JP 2014-97477 A Summary of the Invention [Problem to be solved by the invention]
[0007] An object of the present invention is to provide an adsorbent capable of efficiently removing heavy metals, and to provide a treatment method capable of efficiently removing heavy metals from a material to be treated. [Means for solving the problem]
[0008] Such an object can be achieved by the present invention described below. The adsorbent of the present invention contains dolomite, phosphate ions, and iron ions, At least a portion of the phosphate ions is chemically bonded to at least one of Ca and Mg constituting the dolomite to form at least one of a calcium phosphate compound and a magnesium phosphate compound.
[0009] In the adsorbent of the present invention, the dolomite is preferably dolomite hydroxide. In the adsorbent of the present invention, the dolomite is preferably burnt dolomite.
[0010] In the adsorbent of the present invention, the dolomite-based material is preferably dolomite. In the adsorbent of the present invention, it is preferable that at least a portion of the iron ions form Fe2O3.
[0011] In the adsorbent of the present invention, it is preferable that at least a portion of the iron ions form iron phosphate.
[0012] In the adsorbent of the present invention, it is preferable that the content of the phosphate ions relative to the dolomites is 0.1% by mass or more and 10.0% by mass or less. In the adsorbent of the present invention, it is preferable that the content of the iron ions in the dolomites is 0.1% by mass or more and 10.0% by mass or less.
[0013] In the adsorbent of the present invention, when the content of the phosphate ions in the dolomites is X1 [mass%] and the content of the iron ions in the dolomites is X2 [mass%], it is preferable that the adsorbent satisfies the relationship 0.01≦X1 / X2≦100.
[0014] In the adsorbent of the present invention, when 1 g of the adsorbent is mixed with 100 mL of water at 25° C., the amount of phosphate ions eluted is 100 ppm or less; When 1 g of the adsorbent is mixed with 100 mL of 1N hydrochloric acid at 25° C., the amount of phosphate ions eluted is preferably 30% or more of the amount adsorbed.
[0015] In the adsorbent of the present invention, when 1 g of the adsorbent is mixed with 100 mL of water at 25° C., the amount of leaching of iron ions is 500 ppm or less, When 1 g of the adsorbent is mixed with 100 mL of 1N hydrochloric acid at 25° C., the amount of leaching of iron ions is preferably 30% or more of the adsorbed amount.
[0016] The adsorbent of the present invention has a BET specific surface area of 10 m 2 / g or more 1000m 2 It is preferable that the molecular weight is not more than 1 / g. In the adsorbent of the present invention, the average pore diameter is preferably 1 nm or more and 200 nm or less.
[0017] The treatment method of the present invention is characterized in that the adsorbent of the present invention is brought into contact with a material to be treated that contains heavy metals, and the heavy metals contained in the material to be treated are removed.
[0018] In the treatment method of the present invention, it is preferable to contact the adsorbent with the material to be treated under conditions of a pH of 2.0 or more and 12.0 or less. Effect of the Invention
[0019] According to the present invention, it is possible to provide an adsorbent capable of efficiently removing heavy metals, and also to provide a treatment method capable of efficiently removing heavy metals from a material to be treated. [Brief description of the drawings]
[0020] [Figure 1] FIG. 1 is a graph showing the results of X-ray diffraction (XRD) of the adsorbent of Example 1 and the dolomite of Comparative Example 1. [Diagram 2] FIG. 2(A) is an electron microscope photograph (SEM) of the dolomite of Comparative Example 1, and FIG. 2(B) is an electron microscope photograph of the adsorbent of Example 1. [Diagram 3] FIG. 3 is a diagram showing the relationship between the phosphorus content and the chromium (VI) removal rate when the firing temperature is changed. [Figure 4] FIG. 4 is a diagram showing the relationship between the iron content and the chromium (VI) removal rate when the firing temperature is changed. [Diagram 5] FIG. 5 is a graph showing the relationship between the calcination temperature and the removal rate and adsorption amount of chromium (VI). [Figure 6] FIG. 6 is a graph showing the relationship between the pH of the standard solution and the amount of chromium (VI) adsorption when an adsorbent dried at 80° C. and an adsorbent calcined at 450° C. are used. [Figure 7] FIG. 7 shows the results of X-ray powder diffraction when the firing temperature was changed. [Figure 8] FIG. 8 is a diagram showing the pore volume distribution when the firing temperature is changed. [Figure 9] FIG. 9 is a diagram showing the crystallite size of hydroxyapatite (HAP) when the firing temperature is changed. [Figure 10] FIG. 10 is a diagram showing the crystallite size of MgO when the firing temperature is changed. [Figure 11] FIG. 11 is a TG-DTA curve of the adsorbent of Example 1 on which iron and phosphorus are adsorbed. [Figure 12] FIG. 12 is a graph showing the relationship between the calcination temperature and the BET specific surface area of the adsorbent when the calcination temperature is changed between 450° C. and 700° C. [Figure 13] FIG. 13 is a graph showing the relationship between the pore size and the pore volume of the adsorbent when the firing temperatures were 450° C. and 700° C. [Figure 14] FIG. 14 is a diagram showing the pore volume distribution when the composition of the atmosphere in the firing step is changed. [Figure 15] FIG. 15 is a graph showing the amount of chromium (VI) removed for each adsorbent produced by changing the calcination temperature and the composition of the calcination atmosphere. [Figure 16] FIG. 16 is a graph showing the relationship between pH and the chromium (VI) removal rate when the pH of the standard solution was changed in the range of 2 to 9 using the adsorbents of Example 1 and Comparative Example 1. [Figure 17] FIG. 17 is a graph showing the relationship between the dosage of adsorbent for the standard solution and the chromium (VI) removal rate. [Figure 18] FIG. 18 is a graph showing the relationship between the treatment time and the chromium (VI) removal rate when the initial chromium (VI) concentration of the standard solution is changed. [Figure 19] FIG. 19 is a graph showing the adsorption isotherm when the adsorbent of Example 1 is used. [Figure 20] FIG. 20 is a diagram showing the results of quantitative analysis of each crystal phase by the RIR (Reference Intensity Ratio) method for dolomite rough and fired dolomite obtained by firing the dolomite rough at a predetermined firing temperature. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] [1] Adsorbent First, the adsorbent of the present invention will be described.
[0022] The adsorbent of the present invention is characterized in that it contains dolomite, phosphate ions, and iron ions, and at least a portion of the phosphate ions are chemically bonded to at least one of Ca and Mg that constitute the dolomite, forming at least one of a calcium phosphate compound and a magnesium phosphate compound. This makes it possible to provide an adsorbent capable of efficiently removing heavy metals.
[0023] It is believed that the adsorbent contains iron ions in addition to phosphate ions, which increases the specific surface area, thereby increasing the amount of heavy metal adsorbed.
[0024] In particular, the adsorbent of the present invention can remove chromium (Cr) and arsenic (As) at a high removal rate, which have been particularly difficult to remove at a high removal rate in the past.
[0025] Thus, the reason why the adsorbent of the present invention can remove heavy metals (particularly chromium (VI)) at a high removal rate is believed to be that by adding phosphorus ions and iron ions to dolomites, the amount of heavy metals adsorbed can be increased, and the adsorbed heavy metals can be fixed and insolubilized in the adsorbent by chemical bonds, and thus re-dissolving in water, etc. can be suitably prevented.
[0026] Furthermore, in the adsorbent of the present invention, the phosphate ions and iron ions adsorbed to the dolomites are preferably fixed and insolubilized in the dolomites and are preferably prevented from dissolving in water, etc., and therefore it is believed that the above-mentioned excellent effects can be stably obtained.
[0027] Examples of dolomites include dolomite, dolomite hydroxide (slaked dolomite, including dolomite plaster), lightly burned dolomite (including burned dolomite), and dolomite clinker. One or a combination of two or more selected from these can be used.
[0028] In particular, when the dolomite is dolomite hydroxide, the chemical bond between the phosphate ion and Ca constituting the dolomite becomes strong.
[0029] In addition, since the dolomite is burnt dolomite, the chemical bond between the phosphate ion and Ca constituting the dolomite becomes stronger.
[0030] In addition, since the dolomite is dolomite, the conditions of the adsorbent such as the particle size and pore size can be suitably adjusted. In addition, since dolomite as a raw material is cheaper, it is also advantageous from the viewpoint of further reducing the production cost of the adsorbent.
[0031] The content of phosphate ions in the dolomites is preferably 0.1% by mass or more and 10.0% by mass or less, more preferably 1.0% by mass or more and 4.5% by mass or less, even more preferably 1.1% by mass or more and 3.0% by mass or less, and most preferably 1.2% by mass or more and 2.0% by mass or less. This can further improve the efficiency of removing heavy metals by the adsorbent.
[0032] The content of the iron ions in the dolomites is preferably 0.1% by mass or more and 10.0% by mass or less, more preferably 1.0% by mass or more and 4.5% by mass or less, even more preferably 1.5% by mass or more and 4.0% by mass or less, and most preferably 2.0% by mass or more and 3.8% by mass or less. This can further improve the efficiency of removing heavy metals by the adsorbent.
[0033] In the adsorbent, when the content of phosphate ions relative to the dolomites is X1 [mass%] and the content of iron ions relative to the dolomites is X2 [mass%], it is preferable to satisfy the relationship of 0.01≦X1 / X2≦100, it is more preferable to satisfy the relationship of 0.40≦X1 / X2≦0.80, it is even more preferable to satisfy the relationship of 0.41≦X1 / X2≦0.78, and it is most preferable to satisfy the relationship of 0.42≦X1 / X2≦0.76. This can further improve the efficiency of removing heavy metals by the adsorbent.
[0034] The adsorbent of the present invention may be produced by any method, but the adsorbent of the present invention can be produced efficiently by using the method for producing an adsorbent described below.
[0035] In the adsorbent of the present invention, it is preferable that the majority of phosphate ions are chemically bonded to Ca constituting the dolomite.
[0036] When 1 g of the adsorbent is mixed with 100 mL of water at 25° C., the amount of phosphate ions eluted is preferably 100 ppm or less, more preferably 50 ppm or less, and even more preferably 30 ppm or less.
[0037] When these conditions are satisfied, phosphorus is fixed more stably in the adsorbent, and heavy metals can be removed stably and with excellent efficiency even when the adsorbent is used for a long period of time or when a large amount of material is treated (when a large amount of material is brought into contact with the adsorbent).
[0038] The amount of phosphate ions eluted when the adsorbent is mixed with water can be determined, for example, by mixing the adsorbent with water, stirring for one hour, and then measuring.
[0039] The fact that phosphate ions are chemically bonded to Ca constituting the dolomites can be confirmed, for example, by a significant increase in the amount of phosphate ions eluted when the adsorbent is brought into contact with water as described above and then with a low pH liquid.
[0040] More specifically, when 1 g of the adsorbent is mixed with 100 mL of 1N hydrochloric acid at 25° C., the amount of phosphate ions dissolved increases significantly.
[0041] When 1 g of the adsorbent is mixed with 100 mL of 1N hydrochloric acid at 25°C, the amount of phosphate ions eluted is preferably 30% or more of the total phosphorus (adsorbed amount) contained in the adsorbent, more preferably 60% or more, and even more preferably 80% or more.
[0042] When these conditions are satisfied, a large amount of phosphorus is fixed in the adsorbent, and particularly excellent heavy metal removal capability is obtained. Therefore, even when the adsorbent is used for a long period of time or when a large amount of material is treated (when a large amount of material is brought into contact with the adsorbent), heavy metals can be removed stably and efficiently.
[0043] The amount of phosphate ions eluted when the adsorbent is mixed with 1N hydrochloric acid can be determined, for example, by mixing the adsorbent with 1N hydrochloric acid, stirring for 1 hour, and then measuring.
[0044] In particular, in the adsorbent of the present invention, it is preferable that the amount of phosphate ion eluted when 1 g of the adsorbent is mixed with 100 mL of water at 25° C. and the amount of phosphate ion eluted when 1 g of the adsorbent is mixed with 100 mL of 1N hydrochloric acid at 25° C. both satisfy the above-mentioned conditions. That is, it is preferable that the amount of phosphate ion eluted when 1 g of the adsorbent is mixed with 100 mL of water at 25° C. is 100 ppm or less, and that the amount of phosphate ion eluted when 1 g of the adsorbent is mixed with 100 mL of 1N hydrochloric acid at 25° C. is 30% or more of the adsorbed amount. This allows the above-mentioned effects to act synergistically, resulting in better results.
[0045] In the adsorbent of the present invention, at least a portion of the iron ions is Fe x O y and preferably satisfies the relationship 0.01≦y / x≦2, and more preferably, at least a portion of the iron ions forms Fe2O3.
[0046] Fe x O y (In particular, Fe2O3) is generally produced in the pores of the adsorbent, which is finely porous and has a high specific surface area, and therefore can further improve the efficiency of heavy metal removal by the adsorbent.
[0047] Such Fe2O3 is produced, for example, when iron hydroxide is dehydrated in the calcination step during production, or when the iron component in the adsorbent is oxidized, as described below.
[0048] In the adsorbent of the present invention, at least a portion of the iron ions preferably forms iron phosphate.
[0049] By chemically bonding at least a portion of the iron ions to phosphate, a larger amount of iron is fixed in the adsorbent, and the efficiency of removing heavy metals by the adsorbent can be further improved.
[0050] When 1 g of the adsorbent is mixed with 100 mL of water at 25° C., the amount of leaching of iron ions is preferably 500 ppm or less, more preferably 400 ppm or less, and even more preferably 300 ppm or less.
[0051] When these conditions are satisfied, iron is fixed more stably in the adsorbent, and heavy metals can be removed stably and with excellent efficiency even when the adsorbent is used for a long period of time or when a large amount of material is treated (when a large amount of material is brought into contact with the adsorbent).
[0052] The amount of iron ions eluted when the adsorbent is mixed with water can be determined, for example, by mixing the adsorbent with water, stirring for one hour, and then measuring.
[0053] When 1 g of the adsorbent is mixed with 100 mL of 1 N hydrochloric acid at 25°C, the amount of leached iron ions is preferably 30% or more of the total iron ions (adsorbed amount) contained in the adsorbent, more preferably 60% or more, and even more preferably 80% or more.
[0054] When these conditions are satisfied, a large amount of iron is fixed in the adsorbent, and particularly excellent heavy metal removal capability is obtained. Therefore, even when the adsorbent is used for a long period of time or when a large amount of material is treated (when a large amount of material is brought into contact with the adsorbent), heavy metals can be removed stably and efficiently.
[0055] The amount of iron ions eluted when the adsorbent is mixed with 1N hydrochloric acid can be determined, for example, by mixing the adsorbent with 1N hydrochloric acid, stirring for 1 hour, and then measuring.
[0056] In particular, in the adsorbent of the present invention, it is preferable that the amount of eluted iron ions when 1 g of the adsorbent is mixed with 100 mL of water at 25° C. and the amount of eluted iron ions when 1 g of the adsorbent is mixed with 100 mL of 1N hydrochloric acid at 25° C. both satisfy the above-mentioned conditions. That is, it is preferable that the amount of eluted iron ions when 1 g of the adsorbent is mixed with 100 mL of water at 25° C. is 500 ppm or less, and that the amount of eluted iron ions when 1 g of the adsorbent is mixed with 100 mL of 1N hydrochloric acid at 25° C. is 30% or more of the adsorbed amount. This allows the above-mentioned effects to act synergistically, resulting in better results.
[0057] The adsorbent is usually a porous body. This makes it possible to increase the surface area per unit mass (unit volume) of the adsorbent, thereby further improving the efficiency of removing heavy metals.
[0058] The average pore size in the adsorbent is not particularly limited, but is preferably from 1 nm to 200 nm, more preferably from 2 nm to 100 nm, and even more preferably from 3 nm to 30 nm.
[0059] This makes it possible to further improve the efficiency of removing heavy metals by the adsorbent while ensuring the durability of the adsorbent.
[0060] The BET specific surface area of the adsorbent is 10 m 2 / g or more 1000m 2 / g or less, and 2 / g or more is more preferable, and 30m 2 It is more preferable that the molecular weight is 1 / g or more. This further improves the efficiency of removing heavy metals by the adsorbent.
[0061] The shape and size of the adsorbent are not particularly limited, but when the adsorbent is particulate, the average particle size is preferably 0.5 μm or more and 20,000 μm or less, more preferably 1 μm or more and 1,500 μm or less, and even more preferably 50 μm or more and 1,000 μm or less.
[0062] This makes it possible to increase the particle surface area per unit mass (unit volume) of the adsorbent and to uniformly adsorb phosphorus and iron components to the adsorbent, while effectively preventing the particulate adsorbent from unintentionally agglomerating, thereby improving the fluidity and ease of handling of the adsorbent. In addition, the fillability into a container (ease of filling, ability to follow the shape of the container) can be improved, making it easy to mold into a desired shape.
[0063] [2] Manufacturing method of adsorbent Next, a method for producing the adsorbent will be described.
[0064] The method for producing an adsorbent of the present embodiment includes a phosphorus adsorption step of contacting dolomites with a phosphorus solution containing a dissolved phosphorus compound to adsorb phosphorus components to the dolomites, an iron adsorption step of contacting dolomites with an iron solution containing a dissolved iron compound to adsorb iron components to the dolomites, and a calcination step of calcining the dolomites that have been contacted with the phosphorus solution and the iron solution.
[0065] This provides a method for producing an adsorbent capable of efficiently removing heavy metals, and in particular, an adsorbent capable of efficiently removing heavy metals such as chromium (Cr) and arsenic (As) can be produced inexpensively and with good productivity.
[0066] In addition, the manufacturing method of this embodiment can produce an adsorbent that can remove arsenic and chromium (Cr(IV)) at a high removal rate, which have been particularly difficult to remove at a high removal rate in the past.
[0067] In this embodiment, the order of the phosphorus adsorption step and the iron adsorption step is not particularly limited. For example, the phosphorus adsorption step may be performed first, and then the iron adsorption step may be performed on the dolomite having the phosphorus component adsorbed therein in the phosphorus adsorption step, or the iron adsorption step may be performed first, and then the phosphorus adsorption step may be performed on the dolomite having the iron component adsorbed therein in the iron adsorption step.Furthermore, the phosphorus adsorption step and the iron adsorption step may be performed simultaneously.
[0068] In the following description, as an example, a phosphorus adsorption process is performed first, and then an iron adsorption process is performed on the dolomite having phosphorus components adsorbed thereon in the phosphorus adsorption process.
[0069] By first allowing phosphorus to be adsorbed onto the dolomite, and then forming at least one of a calcium phosphate compound and a magnesium phosphate compound with at least one of the Ca and Mg that constitute the dolomite, and then adding iron ions, it is possible to suitably adsorb the iron ions onto the dolomite, since phosphorus and iron react easily.
[0070] Furthermore, by carrying out the reaction in a solution, production costs can be kept low, and conditions such as particle size, pore size, and surface area of the adsorbent can be suitably adjusted.
[0071] [2-1] Phosphorus adsorption process In the phosphorus adsorption step, the dolomites are brought into contact with a solution containing a dissolved phosphorus compound, whereby the phosphorus component contained in the solution is adsorbed onto the dolomites.
[0072] As the dolomite used in this step, the dolomites described above can be used. The dolomites used in this step (dolomites as a raw material) are usually porous. This makes it possible to increase the surface area per unit mass (unit volume) of the adsorbent, thereby further improving the efficiency of removing heavy metals. Furthermore, the specific surface area can be increased by the calcination process.
[0073] The average pore size of the dolomite as the raw material is not particularly limited, but is preferably 1 nm or more and 200 nm or less, more preferably 2 nm or more and 100 nm or less, and even more preferably 5 nm or more and 30 nm or less.
[0074] This makes it possible to further improve the efficiency of removing heavy metals by the adsorbent while ensuring the durability of the adsorbent. The average pore size can be adjusted, for example, by the firing conditions in the firing step.
[0075] The dolomite as the raw material may be calcined prior to the phosphorus adsorption step to form lightly calcined dolomite.
[0076] Dolomite is converted into the following formula by calcination: CaMg(CO3)2 → MgO + CaO + 2CO2 The decomposition reaction shown below is shown.
[0077] It is believed that the pyrolysis caused by calcining dolomite results in the formation of CaO, which enables phosphorus to be more suitably adsorbed in the phosphorus adsorption step.
[0078] The calcination temperature of dolomite is preferably 650°C or higher and 1000°C or lower. This makes it possible to make the above-mentioned effects more pronounced.
[0079] As the lightly burned dolomite, commercially available lightly burned dolomite may be used. The phosphorus compound (phosphorus component to be adsorbed to dolomites) to be brought into contact with dolomites in the phosphorus adsorption step may be at least partially dissolved in a solvent, and for example, another part of the phosphorus compound may be in a dispersed state in the solution. In other words, the solvent constituting the solution may also function as a dispersion medium.
[0080] The solution is preferably an aqueous solution containing at least water as a solvent, but may contain a solvent other than water. Furthermore, the solvent may contain components other than the phosphorus compound as solutes or dispersoids.
[0081] Examples of the phosphorus compound to be contacted with the dolomite in this step include phosphoric acid and its salts (e.g., ammonium phosphate, diammonium hydrogen phosphate, ammonium dihydrogen phosphate, trisodium phosphate, disodium hydrogen phosphate, sodium dihydrogen phosphate, tripotassium phosphate, dipotassium hydrogen phosphate, potassium dihydrogen phosphate, calcium dihydrogen phosphate, etc.), phosphorous acid and its salts, peroxomonophosphoric acid and its salts, phosphonic acid and its salts, phosphinic acid and its salts, phosphorus oxides such as diphosphorus pentoxide, phosphorus halides such as phosphorus pentachloride, phosphoryl halides such as phosphoryl chloride, calcium phosphides such as calcium monophosphide and tricalcium diphosphide, etc.
[0082] Of these, phosphoric acid and its salts are preferred. This allows the formation of chemical bonds between phosphate ions and Ca constituting the dolomite to proceed more suitably during the firing process.
[0083] The concentration of the phosphorus compound in the solution is preferably from 0.01% by mass to 80% by mass, more preferably from 0.1% by mass to 10% by mass, and even more preferably from 1% by mass to 2% by mass.
[0084] This makes it possible to increase the amount of phosphorus compounds adsorbed to the dolomites while suppressing the amount of phosphorus compounds remaining unadsorbed on the dolomites, thereby further improving the efficiency of heavy metal removal by the adsorbent.
[0085] Any phosphorus compound may be used, including, for example, synthetic products, ore-derived products, activated sludge-derived products, and steel slag-derived products, with sludge ash-derived products being preferred.
[0086] In this way, by using a material derived from sludge ash, which is an industrial waste, as phosphorus, which is a valuable resource, resources can be effectively utilized, and it is also preferable from the viewpoint of reducing the amount of industrial waste, etc. It is also preferable from the viewpoint of reducing the cost of the adsorbent.
[0087] The ratio of dolomites and the phosphorus compound is not particularly limited, but the adsorption amount of the phosphorus compound to the dolomites, in terms of the amount of phosphate ions, is preferably 0.1 parts by mass or more and 20 parts by mass or less per 100 parts by mass (%) of dolomites, and more preferably 1 part by mass or more and 2 parts by mass or less.
[0088] This makes it possible to increase the amount of phosphorus compounds adsorbed to dolomites while suppressing the amount of phosphorus compounds remaining unadsorbed on dolomites, thereby saving phosphorus, which is more expensive than dolomite, and further improving the efficiency of removing heavy metals by the adsorbent.
[0089] This step is preferably carried out under conditions in which the pH of the mixture containing the dolomites and the solution containing the phosphorus compound is 2 or more and 12 or less, more preferably 3 or more and 8 or less, and even more preferably 4 or more and 6 or less.
[0090] This allows the phosphorus compounds to be more efficiently adsorbed onto the dolomites, and the efficiency of removing heavy metals by the adsorbent can be further improved.
[0091] In addition, this step is preferably carried out while stirring the mixture. This allows the phosphorus compound to come into contact with the dolomites more efficiently, and the phosphorus compound can be adsorbed by the dolomites more efficiently. In particular, the phosphorus compound can be adsorbed by the dolomites more efficiently even in the pores of the dolomites. As a result, the efficiency of removing heavy metals by the adsorbent can be further improved. For mixing the mixture, various stirring devices and various mixing devices can be used.
[0092] The treatment time in this step (contact time between the dolomite and the solution containing the dissolved phosphorus compound) is preferably from 1 minute to 180 minutes, and more preferably from 10 minutes to 60 minutes.
[0093] This makes it possible to effectively prevent a decrease in the productivity of the adsorbent and to further improve the efficiency of removing heavy metals by the adsorbent.
[0094] The treatment temperature in this step is preferably from 0°C to 100°C, more preferably from 10°C to 80°C, and even more preferably from 20°C to 60°C.
[0095] This allows the amount of energy required for producing the adsorbent to be reduced, while the phosphorus compound can be efficiently adsorbed onto the dolomite, and this step can be carried out efficiently in a short period of time.
[0096] In the phosphorus adsorption step, phosphorus may be adsorbed onto dolomites in an aqueous solution in which a phosphorus component is dissolved, and then solid-liquid separation may be carried out (solid-liquid separation step).
[0097] In addition, the phosphorus-adsorbed dolomite, which is a solid obtained in the solid-liquid separation step, may be subjected to a drying treatment (drying step).
[0098] [2-2] Iron adsorption process In the iron adsorption step, the dolomites having adsorbed phosphorus compounds obtained in the phosphorus adsorption step (hereinafter referred to as phosphorus-adsorbed dolomites) are brought into contact with a solution containing dissolved iron compounds, thereby allowing the iron components contained in the solution to be adsorbed by the dolomites.
[0099] The iron compound (iron component to be adsorbed to the phosphorus-adsorbed dolomites) to be brought into contact with the phosphorus-adsorbed dolomites in the iron adsorption step may be at least partially dissolved in a solvent, and for example, another part of the iron compound may be in a dispersed state in the solution. In other words, the solvent constituting the solution may also function as a dispersion medium.
[0100] The solution is preferably an aqueous solution containing at least water as a solvent, but may contain a solvent other than water. Furthermore, the solvent may contain components other than the iron compound as solutes or dispersoids.
[0101] Examples of iron compounds to be contacted with the phosphorus-adsorbed dolomites in this step include iron chloride (II), iron chloride (III), iron hydroxide (II), iron hydroxide (III), iron sulfate (II), iron sulfate (III), and iron phosphate (III).
[0102] Among these, iron(III) chloride and iron(III) hydroxide are preferred, but any other iron compound that can ionize iron may be used.
[0103] This allows the iron ions to be favorably adsorbed onto the phosphorus-adsorbed dolomites in the adsorption step, and also allows the formation of chemical bonds between the iron ions and phosphoric acid to proceed more favorably in the firing step.
[0104] The concentration of the iron compound in the solution is preferably 0.01% by mass or more and 80.0% by mass or less, more preferably 0.1% by mass or more and 10.0% by mass or less, and even more preferably 1.0% by mass or more and 2.0% by mass or less.
[0105] This makes it possible to control the amount of iron compounds adsorbed to the dolomite while suppressing the amount of iron compounds remaining unadsorbed on the dolomite, thereby further improving the efficiency of heavy metal removal by the adsorbent.
[0106] The ratio of dolomites and iron compounds is not particularly limited, but the adsorption amount of iron compounds on dolomites, converted into the amount of iron ions, is preferably 0.1 parts by mass or more and 20.0 parts by mass or less per 100 parts by mass (%) of dolomites, and more preferably 1.0 parts by mass or more and 2.0 parts by mass or less.
[0107] This makes it possible to more suitably control the amount of iron compounds adsorbed to the phosphorus-adsorbed dolomites while suppressing the amount of iron compounds remaining unadsorbed on the phosphorus-adsorbed dolomites, and further improve the efficiency of removing heavy metals by the adsorbent.
[0108] This step is preferably carried out under conditions in which the pH of the mixture containing the phosphorus-adsorbed dolomites and the solution containing an iron compound is 2 or more and 10 or less, and more preferably 4 or more and 6 or less.
[0109] This allows the iron compounds to be efficiently adsorbed by the phosphorus-adsorbed dolomites, and the efficiency of removing heavy metals by the adsorbent can be further improved.
[0110] In addition, this step is preferably carried out while stirring the mixture. This allows the iron compounds to come into contact with the phosphorus-adsorbed dolomites more efficiently, and allows the iron compounds to be adsorbed by the phosphorus-adsorbed dolomites more efficiently. In particular, the iron compounds can be adsorbed by the phosphorus-adsorbed dolomites more efficiently even in the pores of the phosphorus-adsorbed dolomites. As a result, the efficiency of removing heavy metals by the adsorbent can be further improved. For mixing the mixture, various stirring devices and various mixing devices can be used.
[0111] The treatment time in this step (contact time between the phosphorus-adsorbed dolomites and the solution containing the dissolved iron compound) is preferably from 1 minute to 180 minutes, and more preferably from 10 minutes to 60 minutes.
[0112] This makes it possible to effectively prevent a decrease in the productivity of the adsorbent and to further improve the efficiency of removing heavy metals by the adsorbent.
[0113] The treatment temperature in this step is preferably from 0°C to 100°C, more preferably from 10°C to 80°C, and even more preferably from 20°C to 60°C.
[0114] This allows the amount of energy required to produce the adsorbent to be reduced while the iron compounds can be adsorbed more efficiently by dolomite, and the process can be carried out efficiently in a short time.
[0115] In the iron adsorption process, iron is adsorbed onto phosphorus-adsorbed dolomite in an aqueous solution in which iron components are dissolved, and then solid-liquid separation is carried out (solid-liquid separation process).
[0116] In addition, the phosphorus- and iron-adsorbed dolomite, which is the solid obtained in the solid-liquid separation process, is subjected to a drying treatment (drying process).
[0117] The treatment temperature in the drying step is not particularly limited, but is preferably 300°C or lower, and more preferably 70°C or higher and 300°C or lower.
[0118] Thereafter, the dried phosphorus- and iron-adsorbed dolomites are subjected to a firing process, which will be described in detail below.
[0119] [2-3] Firing process In the calcination step, the dolomites that have been brought into contact with the phosphorus-containing solution and the iron-containing solution (dolomites that have adsorbed phosphorus and iron components) are calcined.
[0120] This fixes the phosphoric acid component in the adsorbent (dolomite), improving its ability to adsorb heavy metals compared to the raw material dolomite, and in particular, its ability to adsorb heavy metals under alkaline conditions is significantly improved.
[0121] In addition, the calcination process causes the Ca that constitutes the dolomites to chemically bond (ionically bond) with Pa to form a calcium phosphate compound, which effectively prevents the phosphorus components from being released when the adsorbent comes into contact with the material to be treated over a wide pH range (especially in the pH range of 5 or higher), and ensures stable and excellent adsorption capacity. Moreover, not only heavy metals but also F (fluorine) can be suitably removed.
[0122] The above-mentioned excellent effects are obtained by adsorbing the phosphorus component to the adsorbent (dolomite) in the calcination process and immobilizing it, but not by simply mixing the dolomite with the phosphorus compound and bringing the solids into contact with each other. More specifically, for example, even if the dolomite and the phosphorus compound are simply brought into contact with each other in a phosphorus-containing aqueous solution, the reactivity is poor, and if the calcination process is not performed, the phosphoric acid component is easily eluted when the material to be treated is treated under high-concentration alkaline conditions, and the effect of improving the efficiency of removing heavy metals cannot be stably obtained.
[0123] Examples of calcium phosphate compounds include calcium phosphate (Ca(H2PO4)2 and its hydrates), anhydrous calcium hydrogen phosphate (CaHPO4), hydroxyapatite (HAP) (Ca 10 Examples of compounds that contain phosphate ions and calcium ions include compounds such as (PO4)6(OH)2).
[0124] In addition, by firing, iron ions chemically bond with phosphate ions to form iron phosphate, which fixes the iron components in the phosphorus-adsorbing dolomite, improving the heavy metal adsorption capacity compared to the raw material dolomite.
[0125] In addition, through calcination, some of the iron ions that are chemically bonded to phosphate ions become iron oxide (Fe2O3) at approximately 450°C, improving the adsorption capacity for Cr(IV) ions and increasing the surface area of the adsorbent, further improving the adsorption capacity for heavy metals.
[0126] The treatment temperature (maximum firing temperature) in the firing step is preferably 300°C or higher and 1000°C or lower, more preferably 340°C or higher and 800°C or lower, and even more preferably 400°C or higher and 600°C or lower. This makes it possible to make the above-mentioned effects more pronounced.
[0127] This makes it possible to reduce the amount of energy required to produce the adsorbent while more efficiently forming chemical bonds between phosphate ions and Ca that constitutes the dolomites, and between iron and phosphate ions, and thus makes it possible to carry out this process efficiently in a short period of time.
[0128] The treatment time in the firing step (heating time at a temperature of 200°C or higher) is not particularly limited, but is preferably from 0.3 hours to 10 hours, more preferably from 0.4 hours to 5 hours, and even more preferably from 0.5 hours to 3 hours.
[0129] This makes it possible to effectively prevent a decrease in the productivity of the adsorbent and to further improve the efficiency of removing heavy metals by the adsorbent.
[0130] The heating in the firing step may be performed by maintaining the temperature at a substantially constant level, or by maintaining the temperature at a plurality of different levels. The heating in the firing step may be performed at a substantially constant temperature increase rate and a substantially constant temperature decrease rate, or at least one of the temperature increase rate during the temperature increase and the temperature decrease rate during the temperature decrease may be changed over time.
[0131] The firing step may be carried out in any atmosphere, but is preferably carried out in air. This allows the use of an apparatus with a relatively simple configuration in the firing step, eliminates the need to adjust the composition of the atmosphere, etc., and improves the productivity of the adsorbent. Even if a phosphorus compound other than phosphoric acid (including a salt of phosphoric acid) is used as a raw material, the oxidation number of phosphorus can be adjusted in this step to efficiently form a calcium phosphate-based compound.
[0132] Furthermore, even when an iron compound other than iron(III) (including a salt of iron(III)) is used as a raw material, the oxidation number of iron can be adjusted in this process to efficiently form an iron-based compound.
[0133] [2-4] Hydration process The calcined product obtained in the calcination step as described above may be used as an adsorbent as it is, but a hydration step of hydrating the product may be further carried out after the calcination step.
[0134] This improves the chemical stability of the adsorbent. In addition, the hydrophilicity of the adsorbent is improved, and for example, when the material to be treated with the adsorbent contains water, the affinity between the adsorbent and the material to be treated (wettability of the material to the adsorbent) can be further improved. As a result, for example, the material to be treated can be suitably introduced into the pores of the adsorbent, and the efficiency of removing heavy metals by the adsorbent is further improved.
[0135] The hydration step can be carried out by contacting the fired product with water, for example, by immersing the fired product in a liquid containing water, spraying the fired product with a liquid containing water, or placing the fired product in water vapor.
[0136] According to the above-mentioned method for producing an adsorbent, an adsorbent capable of efficiently removing heavy metals can be efficiently produced in a simple manner.
[0137] In the above-mentioned production method, the ease of adsorption of each heavy metal can be adjusted by adjusting the production conditions, more specifically, for example, the ratio of phosphorus compounds and iron compounds to dolomites, the ratio of phosphorus compounds and iron compounds, the heat treatment conditions in the firing step, etc. This makes it possible to increase the selectivity of a specific type of heavy metal, for example, and to suitably apply the method to the recovery, purification, etc. of the specific heavy metal.
[0138] In the above explanation, an example was given in which the dolomites that have adsorbed phosphorus in the phosphorus adsorption process (phosphorus-adsorbed dolomites) were subjected to a solid-liquid separation process and a drying process before being subjected to an iron adsorption process. However, the phosphorus-adsorbed dolomites may also be subjected to a further firing process before being subjected to the iron adsorption process.
[0139] In addition, the phosphorus-adsorbed dolomites may be subjected to the iron adsorption step without undergoing the solid-liquid separation step or the drying step. In this case, a separately prepared iron solution containing dissolved iron compounds may be added to the mixture of the dolomites and the phosphorus solution containing dissolved phosphorus compounds after the phosphorus adsorption step is completed, or the iron compounds may be directly added to the mixture and at least a part of them may be dissolved.
[0140] In addition, when the phosphorus adsorption process and the iron adsorption process are performed at the same time, they can be performed, for example, by contacting dolomite with a solution containing a dissolved phosphorus compound and a dissolved iron compound.
[0141] [3] Processing method Next, the processing method of the present invention will be described.
[0142] The treatment method of the present invention is characterized in that the adsorbent according to the present invention is brought into contact with a material to be treated that contains heavy metals, and the heavy metals contained in the material to be treated are removed.
[0143] This makes it possible to provide a treatment method capable of efficiently removing heavy metals from the material to be treated.
[0144] The form of the material to be treated when carrying out the treatment method of the present invention is not particularly limited, but it usually has fluidity, for example, liquid (including paste and slurry) or gaseous form.
[0145] In particular, the material to be treated is preferably in a liquid form, so that the material to be treated can be in good contact with the adsorbent (e.g., good penetration into the pores of the adsorbent) and the heavy metals can be removed more efficiently.
[0146] When the adsorbent is brought into contact with the material to be treated, the pH (hydrogen ion exponent) of the mixture of the adsorbent and the material to be treated is preferably 2.0 or more and 12.0 or less, more preferably 2.5 or more and 10.0 or less, and even more preferably 3.0 or more and 8.0 or less. This can further improve the efficiency of removing heavy metals by the adsorbent.
[0147] The material to be treated may be anything that may contain the heavy metals to be removed, but examples include wastewater from factories, laboratories, power plants, building demolition sites, mines, sewage sludge combustion ash and liquids containing it, well water, etc.
[0148] The material to be treated may be any material that may possibly contain heavy metals to be removed, regardless of whether or not it actually contains heavy metals.
[0149] However, the heavy metal content in the treated material (if multiple types of heavy metals are contained, the total content of these heavy metals) is not particularly limited, but is preferably 10 ppm or more and 10,000 ppm or less, more preferably 10 ppm or more and 1,000 ppm or less, and even more preferably 10 ppm or more and 100 ppm or less.
[0150] This makes it possible to particularly increase the removal rate (adsorption rate) of heavy metals while particularly reducing the content of heavy metals in the treated material after treatment, thereby making the effects of the present invention more pronounced.
[0151] When the material to be treated is liquid, the amount of adsorbent administered to the material to be treated is not particularly limited, but is preferably 0.5 g / L to 4 g / L, and more preferably 1.5 g / L to 3 g / L.
[0152] This allows the heavy metals to be removed by the adsorbent more efficiently in a shorter adsorption time.
[0153] The treatment time (contact time between the adsorbent and the heavy metal-containing material to be treated) is preferably 1 minute or more and 120 minutes or less, and more preferably 10 minutes or more and 60 minutes or less. This allows the adsorbent to remove heavy metals more efficiently.
[0154] Although the preferred embodiments of the present invention have been described above, the present invention is not limited to these.
[0155] For example, the adsorbent of the present invention may contain dolomites, phosphate ions, and iron ions, and at least a portion of the phosphate ions may be chemically bonded to at least one of Ca and Mg constituting the dolomites to form at least one of a calcium phosphate compound and a magnesium phosphate compound, and is not limited to those produced by the methods described above.
[0156] The method for producing an adsorbent may also include steps other than those described above (e.g., a pretreatment step, an intermediate treatment step, a post-treatment step, etc.). For example, the method may include a step of pulverizing or crushing the fired product or a step of classifying the fired product after the firing step. The method may also include a molding step for obtaining an adsorbent molded into a predetermined shape.
[0157] Furthermore, in the above-described embodiment, a case has been representatively described in which a hydration step is performed after the calcination step, but the method for producing an adsorbent does not necessarily have to include a hydration step. EXAMPLES
[0158] The present invention will be described in detail below based on specific examples, but the present invention is not limited thereto.
[0159] [4] Manufacturing of adsorbents Example 1 As the dolomite, domestic dolomite from Gifu Prefecture was prepared. This dolomite was crushed and classified to a particle size of 75 μm to 150 μm. After that, this dolomite was dried at 105 °C for 24 hours and then fired at 800 °C to obtain lightly fired dolomite.
[0160] Separately, 100 mL of hydrochloric acid adjusted to 1 mol / L was placed in a 300 mL Erlenmeyer flask and heated to 80°C. 1 g of sludge ash was placed in the flask and stirred for 50 minutes while maintaining the temperature using a magnetic stirrer to dissolve the phosphorus compounds contained in the sludge ash. Note that 80 mass% or more of the phosphorus compounds eluted from the sludge ash were phosphoric acid or its salts.
[0161] After the stirring was completed, solid-liquid separation was performed, and the separated liquid phase (filtrate) was diluted to 500 mL. The concentration of phosphorus compounds in the diluted solution was determined by the molybdenum blue method, and the phosphorus elution rate was 90 mass%. The phosphoric acid concentration in the solution was 2000 ppm.
[0162] Next, a 1 mol / L aqueous solution of sodium hydroxide was added to the solution to adjust the pH to 12.
[0163] Next, the temperature of the solution of the phosphorus compound whose pH had been adjusted as described above was brought to room temperature (25°C), and then 5 g of the lightly burned dolomite was added to 500 mL of the solution, and the mixture was stirred for 1 hour to adsorb the phosphorus compound onto the burned dolomite (phosphorus adsorption process). After the stirring was completed, solid-liquid separation was performed to separate the phosphorus-adsorbed dolomite, which was then naturally dried and then fired at 800°C.
[0164] On the other hand, a 1 mol / L aqueous solution of iron chloride (III) (FeCl3) was prepared as an iron compound. 5 g of the phosphorus-adsorbed dolomite was added to 500 mL of this aqueous solution, and the mixture was stirred for 1 hour to allow the phosphorus-adsorbed dolomite to further adsorb the iron compound (iron adsorption step).
[0165] After the stirring was completed, solid-liquid separation was performed, and the dolomite with the phosphorus compounds and iron compounds adsorbed thereon was subjected to a firing treatment at 450°C (maximum firing temperature) for 30 minutes in a nitrogen atmosphere (firing step).
[0166] Next, the fired product obtained as described above was immersed in water to perform a hydration treatment, and then the solid-liquid separation was performed and the product was naturally dried.Then, the product was ground in a mortar to obtain a powdered adsorbent.
[0167] On the other hand, the liquid phase (filtrate) after the phosphorus and iron compounds were adsorbed on the dolomite was made up to 1000 mL, and the concentration of the phosphorus compounds was then determined by the molybdenum blue method. From the results, the amount of phosphorus adsorbed on the dolomite (i.e., the phosphorus content in the adsorbent) was determined. Also, the amount of iron (i.e., the iron content in the adsorbent) was determined by ICP mass spectrometry (Inductively Coupled Plasma Mass Spectrometry). From the results, it was found that the highest Cr(VI) removal rate was achieved when the phosphorus content in the adsorbent was 1.5 mass% and the iron content in the adsorbent was 3.5 mass% relative to the dolomite.
[0168] Comparative Example 1 In this comparative example, the burnt dolomite used as the raw material in the above-mentioned Example 1 was used as it is as the adsorbent.
[0169] FIG. 1 is a graph showing the results of X-ray diffraction (XRD) of the adsorbent of Example 1 and the dolomite of Comparative Example 1 on which iron (Fe(III)) ions are adsorbed.
[0170] In the adsorbent of Example 1, a peak derived from Fe2O3 was confirmed, which was not observed in the dolomite of Comparative Example 1. This confirmed that at least a part of the iron component in the adsorbent of Example 1 exists as Fe2O3.
[0171] Fe2O3 is the adsorbent in Example 1, which adsorbs iron on the surface of the fine pores, and is generated by oxidation during resintering. The surface area is expected to increase because the surface of the pores is covered with Fe2O3. This is expected to improve the removal efficiency of heavy metals, especially Cr(III).
[0172] 2(A) is an electron microscope (SEM) photograph of the dolomite before calcination used in Comparative Example 1, and FIG. 2(B) is an electron microscope photograph of the adsorbent of Example 1.
[0173] Dolomite has a round or flower-like particle shape, but when phosphorus and iron are adsorbed, the shape changes to a needle shape or a mass of fine particles. This is thought to be the reason why the specific surface area of the adsorbent of Example 1 is significantly increased compared to that of the dolomite of Comparative Example 1.
[0174] [5] Evaluation In the evaluation experiment described below, the manufacturing conditions and adsorption conditions of the adsorbent were evaluated based on the removal rate of chromium (VI) from a standard solution containing chromium (VI).
[0175] <Chromium (VI) removal experiment> First, a standard solution was prepared that contained 10 ppm chromium (VI) and was substantially free of other heavy metals and had a pH of 4.
[0176] Next, for the adsorbent of Example 1, 2 g of the adsorbent was added to 1 L of the standard solution and stirred at room temperature (25° C.) for 2 hours. After that, solid-liquid separation was performed, and the content of chromium (VI) in the liquid phase was determined by ICP mass spectrometry (Inductively Coupled Plasma Mass Spectrometry), and the removal rate by the adsorbent was calculated from the content value.
[0177] [5-1] Study on the optimal phosphorus content Adsorbents were produced in the same manner as in Example 1, except that the iron (III) content in dolomite was fixed at 2 mass%, the phosphorus content was varied between 1 mass% and 4.5 mass%, and the calcination temperature was changed to 450°C or 550°C, or a drying treatment was performed at 80°C instead of calcination. The obtained adsorbent was used to carry out a chromium (VI) removal experiment in the same manner as described above.
[0178] FIG. 3 is a diagram showing the relationship between the phosphorus content and the chromium removal rate when the firing temperature is changed.
[0179] Regarding the calcination temperature of the adsorbent containing 2.0% Fe by mass, the highest chromium (VI) removal rate (adsorption rate) was obtained at 450°C. When only drying treatment was performed without calcination, a sufficient removal rate was not obtained. In addition, at each calcination temperature, the highest chromium removal rate was obtained when the phosphorus content was 1.5% by mass.
[0180] In this case, when the phosphorus content was 1.5 mass % and the firing temperature was 450° C., the highest chromium removal rate of 81.59% was obtained.
[0181] [5-2] Study on the optimum iron content Adsorbents were produced in the same manner as in Example 1, except that the phosphorus content relative to the dolomite was fixed at 1.5% by mass, the iron (III) content was varied between 1% by mass and 4.5% by mass, and the calcination temperature was changed to 450°C or 550°C, or a drying treatment was performed at 80°C instead of calcination. The obtained adsorbent was used to carry out a chromium (VI) removal experiment in the same manner as described above.
[0182] FIG. 4 is a diagram showing the relationship between the iron content and the chromium (VI) removal rate when the firing temperature is changed.
[0183] Concerning the firing temperature, the results showed that the chromium (VI) removal rate was the highest at 450°C. When only drying treatment was performed without firing, a sufficient removal rate was not obtained. In addition, regardless of the firing temperature, the results showed that the chromium removal rate was the highest when the iron content was 3.5 mass%.
[0184] In this case, when the iron content was 3.5 mass % and the firing temperature was 450°C, the highest chromium removal rate of 92.19% was obtained.
[0185] In the following, the phosphorus content in dolomite was fixed at 1.5 mass% and the iron (III) content was fixed at 3.5 mass%, and the manufacturing conditions for the adsorbent were examined.
[0186] [5-3] Examination of firing temperature Except for changing the calcination temperature between 120°C and 800°C, the adsorbent was produced in the same manner as in Example 1. The obtained adsorbent was used to carry out a chromium (VI) removal experiment in the same manner as described above.
[0187] Figure 5 is a graph showing the relationship between the firing temperature and the removal rate and adsorption amount of chromium (VI). In both cases, the removal rate and adsorption amount of chromium (VI) were highest when the firing temperature was 450°C.
[0188] In addition, chromium (VI) removal experiments were conducted in the same manner as above, except that adsorbents dried at 80°C and calcined at 450°C were used and the pH of the standard solution was varied between 2 and 12.
[0189] FIG. 6 is a graph showing the relationship between the pH of the standard solution and the amount of chromium (VI) adsorption. When only drying treatment was performed without calcination, a sufficient removal rate was not obtained. The adsorbent calcined at 450°C showed good chromium (VI) adsorption characteristics at treatment solution pH values from 2 to 12. The highest chromium (VI) adsorption amount of 4.49 mg / g was obtained when the standard solution pH was 4.
[0190] From the above results, it was found that good chromium (VI) adsorption characteristics were obtained when the calcination temperature of the adsorbent was 450°C and the pH of the standard solution was 4.
[0191] FIG. 7 shows the results of X-ray powder diffraction when the firing temperature was changed. From FIG. 7, it can be seen that as the firing temperature increases, the crystallinity improves and approaches the peak of the stoichiometric ratio of hydroxyapatite (HAP).
[0192] FIG. 8 is a diagram showing the pore volume distribution when the firing temperature is changed. From FIG. 8, it can be seen that in a nitrogen atmosphere, when the firing temperature is in the range of 400° C. or more and 500° C. or less, the number of fine mesopores increases and the specific surface area increases.
[0193] FIG. 9 is a diagram showing the crystallite diameter of hydroxyapatite (HAP) when the firing temperature is changed, and FIG. 10 is a diagram showing the crystallite diameter of MgO when the firing temperature is changed.
[0194] [5-4] Study on firing temperature and BET specific surface area FIG. 11 is a TG-DTA curve of the adsorbent of Example 1 on which iron and phosphorus are adsorbed. The decomposition of the adsorbent occurred in four different stages according to the DTA peaks. First, the peak near 141°C is believed to be due to the removal of moisture. The peak near 380°C is believed to be due to the dehydration of Mg(OH)2. The peak near 460°C is believed to be due to the dehydration of Fe(OH)3. The peak near 680°C is believed to be due to the decomposition of Ca(CO)3. These results indicate that Fe(OH)3 is dehydrated at approximately 450°C.
[0195] Except for changing the calcination temperature between 400°C and 700°C, the adsorbent was produced in the same manner as in Example 1.
[0196] FIG. 12 is a graph showing the relationship between the calcination temperature and the BET specific surface area of the adsorbent. The BET specific surface area increases rapidly when the firing temperature is 450°C, reaching a maximum of 50m 2 If the calcination temperature is too high, the BET specific surface area decreases. The BET specific surface area is a value determined by measurement using a surface area measuring device (TriStarII3020, manufactured by Mircometrics).
[0197] FIG. 13 is a graph showing the relationship between the pore size and the pore volume of the adsorbent when the firing temperatures were 450° C. and 700° C.
[0198] It can be seen that when the firing temperature is 450°C, the pore volume is largest when a large amount of pores with a pore diameter of 3.74 nm are generated. This is thought to be because Fe2O3 and MgO contribute to the fine porosity.
[0199] From the results shown in Figures 12 and 13, it is believed that Fe(OH)3 adsorbed on dolomite is dehydrated at approximately 450°C by firing and becomes finely porous Fe2O3, which leads to an increase in the BET specific surface area.
[0200] [5-5] Consideration of firing atmosphere An adsorbent was produced in the same manner as in Example 1, except that the firing temperature was set to 400° C. and the composition of the firing atmosphere was changed from nitrogen to air and carbon dioxide. For each of the obtained adsorbents, the pore volume distribution was determined.
[0201] FIG. 14 is a diagram showing the pore volume distribution when the composition of the atmosphere in the firing step is changed. From FIG. 14, it can be seen that at a firing temperature of 400° C., firing in a nitrogen atmosphere increases the number of fine mesopores and the specific surface area.
[0202] In addition, a chromium (VI) removal experiment was carried out in the same manner as above using an adsorbent produced in the same manner as in Example 1, except that the calcination temperature and the composition of the calcination atmosphere were changed.
[0203] FIG. 15 is a graph showing the amount of chromium (VI) removed for each adsorbent produced by changing the calcination temperature and the composition of the calcination atmosphere.
[0204] In the following experiment, the adsorption conditions for chromium (VI) using an adsorbent were investigated. [5-6] Study on the effect of pH during adsorption treatment A chromium (VI) removal experiment was carried out in the same manner as above, except that the adsorbent of Comparative Example 1 (dolomite) and the adsorbent of Example 1 were used and the pH of the standard solution was changed between 2 and 9.
[0205] FIG. 16 is a graph showing the relationship between pH and the chromium (VI) removal rate when the pH of the above standard solution is changed in the range of 2 to 9.
[0206] It can be seen that the adsorbent of Example 1 achieved a much higher chromium (VI) removal rate than that of Comparative Example 1. Moreover, the highest chromium (VI) removal rate of 90% was obtained when the standard solution had a pH of 4.
[0207] Chromium(VI) forms the hydrogen chromate anion (HCrO4 - ) and its acidic nature was found to be favorable for the removal of chromium(VI). HCrO4 - ⇔CrO4 2- +H + pKa=5.9 H2CrO4⇔HCrO4 - +H + pKa=4.1 Cr2O7 2- +H2O⇔2HCrO4 - pKa=2.2
[0208] [5-7] Consideration of the dosage of adsorbent A chromium (VI) removal experiment was carried out in the same manner as above, except that the adsorbent of Example 1 was used and the dosage of the adsorbent to the standard solution was changed between 0.5 g / L and 4 g / L.
[0209] FIG. 17 is a graph showing the relationship between the dosage of adsorbent for the standard solution and the chromium (VI) removal rate.
[0210] Increasing the dosage of adsorbent improved the removal rate but decreased the adsorption amount, which is likely due to the increased surface area, which results in a larger number of vacant adsorption sites.
[0211] The best result was obtained when the dosage of adsorbent for the standard solution was 2 g / L, with a chromium (VI) removal rate of 90.032%.
[0212] [5-8] Study on initial concentration of chromium(VI) and treatment time A chromium (VI) removal experiment was carried out in the same manner as above, except that the adsorbent of Example 1 was used and the initial concentration of chromium (VI) in the standard solution was changed to 10 ppm, 20 ppm, and 50 ppm.
[0213] FIG. 18 is a graph showing the relationship between the treatment time and the chromium (VI) removal rate when the initial concentration of chromium (VI) in the standard solution is changed.
[0214] As the initial concentration of chromium (VI) increased, the amount of adsorption itself increased, but the removal rate decreased. This is thought to be because the surface sites of the adsorbent were covered by adsorbing chromium (VI), limiting the number of active sites available for adsorption.
[0215] The adsorption rate was fast at all initial concentrations, proceeding rapidly within the first 10 minutes and approaching equilibrium in about 1 hour.
[0216] FIG. 19 is a graph showing the adsorption isotherm when a chromium (VI) removal experiment was carried out in the same manner as described above using the adsorbent of Example 1. In addition, the figure also shows model isotherms based on the Langmuir equation and the Freundlich equation. The experimental results were well fitted to the model isotherm by the Langmuir equation.
[0217] From the above results, it was found that the present invention was able to remove (adsorb) chromium (VI), a heavy metal, with a high removal rate (adsorption rate).
[0218] In addition, in Example 1, the amount of phosphate ion elution determined by mixing 1 g of the adsorbent with 100 mL of water at 25° C. and stirring for 1 hour and then measuring was 10 ppm or less in all cases. Furthermore, when 1 g of the adsorbent was then further separated into solid and liquid, mixed with 100 mL of 1N hydrochloric acid at 25° C. and stirred for 1 hour, the amount of phosphate ion elution was 80% or more of the total phosphorus (adsorbed amount) contained in the adsorbent in all cases.
[0219] From this result, it is understood that in Example 1, most of the phosphate ions in the adsorbent are chemically bonded to Ca constituting the dolomites to form calcium phosphate compounds.
[0220] In Example 1, the amounts of eluted iron ions obtained by mixing 1 g of the adsorbent with 100 mL of water at 25° C. and stirring for 1 hour and then measuring the amounts were all 10 ppm or less. Furthermore, when 1 g of the adsorbent was then further separated into solid and liquid and mixed with 100 mL of 1 N hydrochloric acid at 25° C. and stirred for 1 hour, the amounts of eluted iron ions obtained by mixing the adsorbent with 100 mL of 1 N hydrochloric acid at 25° C. and stirring for 1 hour were all 80% or more of the total iron contained in the adsorbent (adsorbed amount).
[0221] From this result, it is understood that in Example 1, most of the iron ions in the adsorbent are chemically bonded to phosphoric acid to form iron phosphate.
[0222] Furthermore, when the components of the adsorbent of Example 1 were analyzed by X-ray diffraction (XRD), it was confirmed that the adsorbent contained calcium phosphate compounds (calcium phosphate, anhydrous calcium hydrogen phosphate, and hydroxyapatite).
[0223] An adsorbent was produced in the same manner using dolomite hydroxide instead of dolomite, and various evaluation experiments were carried out, with the same results as above being obtained.
[0224] In addition, the same evaluation as above was carried out, except that a liquid prepared in the same manner as the above standard solution was used instead of chromium (VI), and chromium (III) was used as the standard solution. As a result, chromium (III) was also able to be removed at a high removal rate, just like in the case of chromium (VI).
[0225] In addition, the same evaluation was carried out as above, except that liquids prepared in the same manner as the above standard solution were used instead of chromium (VI), using arsenic, nickel, cadmium, and lead.As a result, as with chromium (VI), these heavy metals were also able to be removed at high removal rates.
[0226] FIG. 20 is a diagram showing the results of quantitative analysis of each crystal phase by the RIR (Reference Intensity Ratio) method for dolomite rough and fired dolomite obtained by firing the dolomite rough at a predetermined firing temperature. [Industrial Applicability]
[0227] The adsorbent of the present invention contains dolomites, phosphate ions, and iron ions, and at least a part of the phosphate ions is chemically bonded to at least one of Ca and Mg constituting the dolomites to form at least one of a calcium phosphate compound and a magnesium phosphate compound. Therefore, an adsorbent capable of efficiently removing heavy metals can be provided. In addition, the treatment method of the present invention contacts the adsorbent according to the present invention with a material to be treated that contains heavy metals, and removes the heavy metals contained in the material to be treated. Therefore, a treatment method capable of efficiently removing heavy metals from the material to be treated can be provided. Therefore, the adsorbent and treatment method of the present invention have industrial applicability.
Claims
1. Contains dolomite, phosphate ions, and iron ions; An adsorbent characterized in that at least a portion of the phosphate ions are chemically bonded to at least one of Ca and Mg that constitute the dolomites, forming at least one of a calcium phosphate compound and a magnesium phosphate compound.
2. 2. The adsorbent according to claim 1, wherein the dolomite is dolomite hydroxide.
3. 2. The adsorbent according to claim 1, wherein the dolomite is calcined dolomite.
4. The adsorbent according to claim 1 or 2, wherein the dolomite-based material is dolomite.
5. At least a portion of the iron ions is Fe 2 O 3 The adsorbent according to claim 1 or 2, which is formed as follows:
6. 3. The adsorbent according to claim 1, wherein at least a portion of the iron ions forms iron phosphate.
7. 3. The adsorbent according to claim 1, wherein a content of the phosphate ions relative to the dolomite is 0.1% by mass or more and 10.0% by mass or less.
8. The adsorbent according to claim 1 or 2, wherein a content of the iron ions in the dolomite is 0.1% by mass or more and 10.0% by mass or less.
9. The content of the phosphate ion in the dolomite is X 1 [mass%], and the content of the iron ions in the dolomite is X 2 When expressed as [mass %], 0.01≦X 1 / X 2 The adsorbent according to claim 1 or 2, which satisfies the relationship ≦100.
10. When 1 g of the adsorbent is mixed with 100 mL of water at 25° C., the amount of phosphate ions eluted is 100 ppm or less; 3. The adsorbent according to claim 1, wherein when 1 g of the adsorbent is mixed with 100 mL of 1N hydrochloric acid at 25° C., the amount of phosphate ions eluted is 30% or more of the adsorbed amount.
11. When 1 g of the adsorbent is mixed with 100 mL of water at 25° C., the amount of iron ions eluted is 500 ppm or less; 3. The adsorbent according to claim 1, wherein when 1 g of the adsorbent is mixed with 100 mL of 1N hydrochloric acid at 25° C., the amount of iron ions eluted is 30% or more of the adsorbed amount.
12. BET specific surface area is 10m 2 / g or more 1000m 2 The adsorbent according to claim 1 or 2, wherein the adsorbent has a molecular weight of 1 / g or less.
13. 3. The adsorbent according to claim 1, having an average pore diameter of 1 nm or more and 200 nm or less.
14. 3. A treatment method comprising contacting a material to be treated containing heavy metals with the adsorbent according to claim 1 or 2, and removing the heavy metals contained in the material to be treated.
15. The treatment method according to claim 14, wherein the adsorbent is contacted with the material to be treated under conditions of a pH of 2.0 or more and 12.0 or less.
Citation Information
Patent Citations
Water purification method
JP2013000696A
Harmful substance insolubilizing material and insolubilizing method of harmful substance
JP2014097477A