Molding

By laminating resin-impregnated veneers with melamine, urethane, and phenolic resins, the method addresses interfacial strength issues, achieving high interlaminar strength and flexibility in molded products, particularly for chair seats, with improved tactile properties.

JP2024165595APending Publication Date: 2024-11-28SANKEI CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023081913
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-17
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Existing methods of laminating wood materials using different resin types result in reduced adhesive strength at the interface due to lower chemical affinity, leading to issues like peeling and difficulty in achieving desired strength and flexibility in molded products, particularly in applications like chair seats that require high interlaminar strength and tactile characteristics.

Method used

A method involving the use of multiple resin-impregnated veneers, such as those impregnated with melamine, urethane, and phenolic resins, stacked and laminated without adhesives to create a three-layer integral structure that enhances interlayer strength and flexibility, allowing for three-dimensional shaping and improved tactile properties.

Benefits of technology

The method ensures high interlaminar strength, flexibility, and comfortable seating by optimizing resin combinations, enabling the production of molded products with enhanced adhesive strength and wood-like texture, suitable for applications like chair seats.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024165595000001_ABST
    Figure 2024165595000001_ABST
Patent Text Reader

Abstract

To form an unconventional molding utilizing features of an impregnation resin by forming resin-impregnated veneers by being impregnated with different kinds of resins and stacking the veneers.SOLUTION: A first resin-impregnated veneer is formed by impregnating a woody material with a melamine-based resin and an urethane-based resin, a second resin-impregnated veneer is formed by impregnating a woody material with a melamine-based resin, a third resin-impregnated veneer is formed by impregnating a woody material with a phenolic resin, and a fourth resin-impregnated veneer is formed by impregnating a woody material with an urethane-based resin. The first resin-impregnated veneer and the second resin-impregnate veneer are stacked with one another so that their surfaces are closely contacted to each other, any one of the second resin-impregnated veneer, the third resin-impregnated veneer and the fourth resin-impregnated veneer are stacked and pressurized on any one side of the stacked laminate, and are integrally constituted and formed into a molding.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a molded article comprising a laminate of resin-impregnated veneers, each of which is made by impregnating a veneer with a resin, and which is characterized in that each resin-impregnated veneer is impregnated with a different resin. [Background technology]

[0002] Conventionally, various proposals have been made to impregnate wood with resin to make the most of the properties of the wood itself while adding various functions.

[0003] For example, Patent Document 1 describes a plywood made by bonding multiple wood veneers together with an adhesive to greatly improve the bending strength and elastic modulus of the plywood, which is used for architectural flooring, wall materials, roofing, etc. The adhesive is made by impregnating a fiber reinforcement material with an adhesive composition. It is described that the resin composition is composed of a phenolic resin composition, a melamine resin composition, a urethane resin composition, and a urea resin composition alone or a co-condensation resin composition of these, but an example is described in which the adhesive is composed of only one selected type of resin composition. In this case, the wood veneer is not impregnated with resin. In addition, in Patent Document 2, a proposal is made to form a laminate for musical instruments by coating or impregnating a resin on a wood veneer, laminating it, and thermocompressing it without using an adhesive between wood elements, in order to make rare natural materials for musical instruments less likely to crack, increase the freedom of appearance design, and make it easier to manufacture. The resin used here is melamine resin, but it is described that urea resin, phenolic resin, etc. can also be used as long as it is a resin used for wood adhesives (paragraph number 0015 of Patent Document 2), but an example is described in which the adhesive is formed from only one selected type of resin composition. In this case, it is described that the laminate is sliced, impregnated with melamine resin as a laminated veneer, and hot platen press is used to obtain a wood material for musical instruments (paragraph number 0026 of Patent Document 2). However, there is no description of forming an uneven shape by hot platen press. Also, in the cited document 3, a sheet having many ridges and depressions for use on the facades and walls of buildings is described, which is intended to be easily manufactured by pressing without adhesive bonding or removal of material by cutting. The sheet is constructed by arranging parts on the surface of a flat core sheet having a thickness of about 8 to 12 mm. Here, the parts have ridges made of wood fiber material to form a curved surface. Here, the parts (ridges) are thermally bonded or thermoformed to the core sheet under pressure (paragraph 0035 of the cited document 3), and it is also described that the parts have a melamine resin-treated decorative paper layer formed on the curved surface (paragraph 0038 of the cited document 3). It is also described that the decorative layer formed on one or both sides of the sheet may be composed of crosslinked acrylic, urethane, epoxy, or melamine resin (paragraph 0038 of the cited document 3). It is also stated that the core is made of kraft paper, wood fiber, cellulose fiber, etc. impregnated with thermosetting phenol-formaldehyde resin (paragraphs 0020 and 0026 of cited document 3). Furthermore, Patent Document 4 proposes a method for producing reinforced wood by combining a technique for softening wood by impregnating it with phenolic resin with steam treatment of wood to form reinforced wood, with the aim of obtaining high-strength reinforced wood at a relatively low pressure. More specifically, it describes that a veneer that has been steam-treated is impregnated with low-molecular-weight phenolic resin for three days under a reduced pressure of 0.5 atm, and then air-dried to form a veneer, and four veneers are stacked with the grain aligned, and compressed using a hot plate at 150°C to obtain a test panel. In addition, in Patent Document 5, when constructing a chair or the like from laminated materials, a reinforcing layer and a permeation prevention layer made by impregnating a carbon fiber sheet with carbon fiber reinforced resin are provided between a core material and a wood-based surface material. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 7-214506 [Patent Document 2] JP 2004-58416 A [Patent Document 3] JP 2003-220652 A [Patent Document 4] JP 2006-240032 A [Patent Document 5] JP 2016-199003 A Summary of the Invention [Problem to be solved by the invention]

[0005] Resins such as acrylic, urethane, epoxy, or melamine resins have been used as adhesives for wood (Patent Document 1), and these resins are impregnated into wood and laminated without the use of adhesives to form plywood (Patent Documents 2 to 4). However, although each document describes that different impregnating resins can be used, only one type of resin material is impregnated into each laminated wooden material, and there have been no examples of studies on a configuration in which different resin materials are actually impregnated into wooden materials and then impregnated with the wooden materials themselves. This is generally believed to be because when different types of compounds are brought into contact with each other and laminated, the chemical affinity at the interface is lower than that of a single compound, so the adhesive strength at the laminate interface is significantly reduced, and many defects such as peeling at the laminate interface occur, making it difficult to achieve the desired results. In other words, in conventional inventions, various properties of molded bodies were achieved by devising the adhesive itself or the adhesive layer structure without selecting laminate layers made of different types of compounds, and by solving defects such as adhesive strength at the laminate interface. The devising of adhesive layers is described in Patent Documents 1, 2, 5, etc. Furthermore, although Patent Document 3 describes forming a molded body with a curved shape, the core sheet that serves as the core is not bent, but rather protrusions made from parts are attached to the core sheet to form an externally curved shape.

[0006] Therefore, in this invention, when forming a resin-impregnated veneer by impregnating a wood material (wood) with resin and laminating a plurality of such veneers without using adhesive to form a molded body, the object is to realize a combination of resin-impregnated veneers that exhibits a desired strength without peeling off the laminated surfaces of the resin-impregnated veneers in the molded body by impregnating each resin-impregnated veneer with a different resin. This is expected to produce a molded body that fully exhibits the characteristics (strength, softness, etc.) of each resin-impregnated veneer, such as when molding the molded body into a folded shape. Furthermore, when applying this molded body to various products such as furniture, the objective is to realize a resin-impregnated veneer configuration that can exhibit the visual and tactile characteristics of wood materials, particularly on the surface of the resin-impregnated veneer that comes into contact with the human body, such as on chairs. In particular, when applying it to the seat of a chair, it is necessary to select a material with a high wood-like texture (softness and wood grain) for the surface that comes into contact with the human body in addition to the three-dimensional shaping, and the molded body is required to have different properties, such as sufficient strength and thickness change for attaching legs to the underside of the molded body. There are no examples of using such laminated resin-impregnated veneers for chair seats, etc. Furthermore, this invention aims to apply this molded body to the seat and back of a chair, thereby ensuring strength (because it is a laminated material, interlayer strength is important), while providing a comfortable seating experience, freedom of shape (the ability to freely mold curves, bumps, etc.), and a moderate softness of the surface (wood-like texture). [Means for solving the problem]

[0007] In this invention, a number of resin-impregnated veneers with different properties are prepared, and various combinations of these resin-impregnated veneers are examined, taking into consideration factors such as the affinity at the adhesive interface when stacked. As a result, two or three of a first resin-impregnated veneer formed by impregnating a wood material with melamine-based resin and urethane-based resin, a second resin-impregnated veneer formed by impregnating a wood material with melamine-based resin, and a third resin-impregnated veneer formed by impregnating a plate-shaped base material with phenol-based resin are selected and laminated directly together on the surfaces to form a molded body with a new structure that solves the above-mentioned problems.

[0008] That is, the first invention is a molded article characterized in that a plurality of sheets are selected from the first resin-impregnated veneer to the fourth resin-impregnated veneer, and are stacked together with their surfaces in direct contact with each other to form an integrated body. (1) The first resin-impregnated veneer is a resin-impregnated veneer in which a wood material is impregnated with a melamine-based resin and a urethane-based resin. (2) The second resin-impregnated veneer is a resin-impregnated veneer in which a wood material is impregnated with a melamine-based resin. (3) The third resin-impregnated veneer is a resin-impregnated veneer in which a wood material is impregnated with a phenolic resin. (4) The fourth resin-impregnated veneer is a resin-impregnated veneer in which a wood material is impregnated with a urethane-based resin.

[0009] The second invention is a molded body characterized in that a first resin-impregnated veneer and a second resin-impregnated veneer are stacked with their surfaces in close contact with each other, and then either a second resin-impregnated veneer, a third resin-impregnated veneer or a fourth resin-impregnated veneer is stacked and pressed onto either side of the stacked laminate, forming a three-layer structure. (1) The first resin-impregnated veneer is a resin-impregnated veneer in which a wood material is impregnated with a melamine-based resin and a urethane-based resin. (2) The second resin-impregnated veneer is a resin-impregnated veneer in which a wood material is impregnated with a melamine-based resin. (3) The third resin-impregnated veneer is a resin-impregnated veneer in which a wood material is impregnated with a phenolic resin. (4) The fourth resin-impregnated veneer is a resin-impregnated veneer in which a wood material is impregnated with a urethane-based resin.

[0010] In the second invention, a first resin-impregnated veneer and a second resin-impregnated veneer are stacked together with their surfaces directly in contact with each other, and further, a surface of a third resin-impregnated veneer is in contact with the other surface of the second resin-impregnated veneer and laminated and pressed together to form a molded body having three integral layers.

[0011] Furthermore, the first resin-impregnated veneer and the second resin-impregnated veneer are stacked on top of each other with their surfaces directly in contact with each other, and the surface of a third resin-impregnated veneer is laminated on the other surface of the second resin-impregnated veneer with its surface in contact with each other, resulting in a molded body having curved surfaces and uneven portions, which is composed of three integrated layers.

[0012] Furthermore, an invention in which the second invention is applied to a chair seat or the like is a molded body in which a first resin-impregnated veneer and a second resin-impregnated veneer are layered with their surfaces directly in contact with each other, and the following A or B is then laminated and pressed into three layers, resulting in a molded body having curved surfaces and uneven portions in accordance with the shape of the seat or back of the chair, constituted as a three-layer integral body. (A) The surface of a third resin-impregnated veneer is closely attached to the other surface of the second resin-impregnated veneer, and the first resin-impregnated veneer is laminated so as to be positioned on the surface that comes into contact with the user. (B) The surface of a fourth resin-impregnated veneer is adhered to the other surface of the first resin-impregnated veneer, and the fourth resin-impregnated veneer is laminated so as to be positioned on the surface that comes into contact with the user.

[0013] Furthermore, the above-mentioned molded article is a molded article according to claim 5, in which the surface on the side that comes into contact with the user's buttocks or back is heat-treated, and the molded article has curved surfaces and uneven parts according to the shape of the seat or back of the chair, and is constructed in three integrated layers.

[0014] The term "three layers" mentioned above is not limited to three layers, but also includes a molded product having four or five layers formed by laminating other resin-impregnated veneers or the like. Effect of the Invention

[0015] In this invention, a molded body with a new structure is constructed by directly laminating two or three of the following: a first resin-impregnated veneer formed by impregnating a wood material with a melamine-based resin and a urethane-based resin, a second resin-impregnated veneer formed by impregnating a wood material with a melamine-based resin, and a third resin-impregnated veneer formed by impregnating a plate-shaped substrate with a phenol-based resin. This makes it possible to construct an integrated molded body with the same interlayer strength as when the same resin-impregnated veneers are laminated together without using adhesives. Furthermore, in the present invention, the first resin-impregnated veneer, the second resin-impregnated veneer, and the third resin-impregnated veneer can be selected according to the purpose of use, and the range of applications of the molded body can be expanded by utilizing the differences in the properties of each resin-impregnated veneer and further applying surface treatment as necessary. In particular, if a first resin-impregnated veneer and a second resin-impregnated veneer are stacked with their surfaces in close contact with each other and used as a core to form a laminate, the affinity of the adhesive interface is further increased, and the strength between the layers and various properties required of the molded product can be ensured even in the case of bending molding. In particular, by applying this molded product to the seat of a chair, it is possible to improve the comfort of sitting while maintaining strength, and to form a curved surface that matches the shape of the person's lower back. Furthermore, by reheating the surface of the resin-impregnated veneer on the topmost layer, it is possible to achieve an appropriate softness and improve the texture. [Brief description of the drawings]

[0016] [Figure 1] Graph showing experimental results of apparent interlaminar shear strength of a two-layer laminated wood molding. [Diagram 2] Graph showing experimental results of apparent interlaminar shear strength of a three-layer laminated wood molding. [Diagram 3] Graph showing experimental results of the Brinell hardness of the surface of the three-layer laminated wood molding in Examples 7 and 8. [Figure 4] Photograph of the exterior showing the three-dimensional shape of the "laminated wood molding UM-MP" in Example 9. [Diagram 5] Photograph of the exterior showing the three-dimensional shape of the "laminated wood molding UM-PM" in Example 10. [Figure 6] An exterior photograph showing the design surface of the "laminated wood molding U-UM-M" in Example 11. [Figure 7] An exterior photograph showing the design surface of the reheated "laminated wood molding U-UM-M" in Example 12. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] The present invention is as described in the above section "Means for solving the problems", and one example of a specific embodiment will be described below.

[0018] The veneer used for the impregnated veneer of the present invention is usually made of wood. The wood material is derived from a plant having a cell wall, such as wood (coniferous trees such as cedar, cypress, and pine; broad-leaved trees such as poplar, beech, oak, and birch), bamboo, hemp (jute, kenaf, flax, hemp, ramie, sisal, and the like), and herbaceous plants, and may be either the plant itself, its waste material, or a chemically treated product thereof. The shape and thickness of the veneer of the present invention are not particularly limited, but the thickness is 0.1 mm to 10 mm, more preferably 0.5 mm to 5 mm, and even more preferably 1 mm to 5 mm. The veneer may be either sawn board or veneer, and may be in the form of a board having the above-mentioned thickness, and the processing form is not particularly limited.

[0019] The melamine resin, urethane resin, and phenol resin used in the present invention are not particularly limited, but are preferably resins or precursors thereof. The precursors may be either low molecular weight compounds or high molecular weight compounds. The weight average molecular weight of each resin is not particularly limited, but is preferably 100 to 200,000, more preferably 100 to 20,000. When using a melamine resin or a phenol resin with a molecular weight that can penetrate into the cell walls of a wood material, a curing agent can be used in combination.

[0020] Each of the above resins may further contain a plasticizer, an antioxidant, an ultraviolet absorber, an antiaging agent, a filler, an antibacterial agent, an antiseptic, an antistatic agent, and the like.

[0021] The method for producing the resin-impregnated veneer of the present invention is not particularly limited, but may be a method including a step of impregnating the veneer with resin (hereinafter, referred to as "impregnation step"). The manufacturing method of the present invention including this impregnation step will be described below.

[0022] In the method for producing the resin-impregnated veneer of the present invention, for example, in the impregnation step, as long as the resin is impregnated into the wood material, any of the following can be used: (1) resin only, (2) a liquid containing resin and a medium that dissolves the resin, or (3) a liquid containing resin and a medium that disperses the resin without dissolving it. Of these, it is preferable to use the liquids (2) and (3). Note that the medium of the resin-containing liquids (2) and (3) preferably contains water in terms of permeability to cell walls, but if the resin does not dissolve in water, a medium that dissolves the resin can be appropriately selected.

[0023] In the above impregnation step, the resin-impregnated veneer is dehydrated by air drying, vacuum drying, high-temperature drying, etc., to a moisture content of, for example, 10% by mass or less, and then, for example, immersed in a resin-containing liquid, and if necessary, under vacuum conditions, pressurized conditions, cooling / heating conditions, etc., to inject the liquid into the resin-impregnated veneer, allowing the resin-containing liquid to penetrate into the cell walls, and then the medium of the resin-containing liquid is removed to obtain a resin-impregnated veneer containing resin in the cell walls. Methods for removing the medium include air drying, vacuum drying, high-temperature drying, etc. Water or the medium used may be contained (remained) in the produced resin-impregnated veneer.

[0024] The molded body of the present invention is constructed by selecting a plurality of resin-impregnated veneers from the first resin-impregnated veneer to the fourth resin-impregnated veneer, stacking them together with their surfaces in direct contact with each other, and the number of resin-impregnated veneers selected and the number of layers are not particularly limited. The molded body may also include the same type of resin-impregnated veneers, and for example, in the case of a three-layer structure, the molded body may be formed by stacking the second resin-impregnated veneers on both sides of the first resin-impregnated veneer. The number of laminated sheets may be increased or decreased in one molded product. For example, a molded product may be obtained by laminating a first resin-impregnated veneer and a second resin-impregnated veneer, and further laminating a third resin-impregnated veneer in a portion of the laminated product. Conversely, a molded product may be obtained by laminating a first resin-impregnated veneer and a second resin-impregnated veneer, and a portion may be formed of only the first resin-impregnated veneer, in which no second resin-impregnated veneer is present, and further, a molded product may be obtained by laminating another resin-impregnated veneer, such as a third resin-impregnated veneer, in the portion of only the first resin-impregnated veneer.

[0025] The number of resin-impregnated veneers of the same type, from the first resin-impregnated veneer to the fourth resin-impregnated veneer, to be laminated is not particularly limited, but is preferably 2 to 10, more preferably 2 to 5, and even more preferably 1 to 3, and the number may be varied depending on the type of resin-impregnated veneer, or the number may be increased or decreased in some areas to change the thickness of the molded body.

[0026] The order of lamination of the resin-impregnated veneers of the present invention is not particularly limited, but it is preferable to place a veneer impregnated with a urethane resin with a high wood-like texture on the surface of the molded body (the design surface, or the surface that people come into contact with in the case of a seat surface). In addition, when providing curved or uneven surfaces such as ribs or reinforcing parts on the back surface of the molded body, high fluidity is required, so it is preferable to place a veneer impregnated with a phenolic resin. In addition, when high strength characteristics are required or when metal fittings are attached to the back surface, it is preferable to use a veneer impregnated with a melamine and / or phenolic resin on the back surface.

[0027] The molded body of the present invention, which is made by laminating the resin-impregnated veneers, is produced by hot pressing using a press. The laminated resin-impregnated veneers are placed in a preheated mold, and pressure is applied in the lamination direction to bond the layers of the veneers together. The pressing temperature is not particularly limited, but is 40 to 220°C, preferably 60 to 200°C, and more preferably 120 to 180°C. In order to suppress thermal decomposition of wood, it is preferable to set the temperature to less than 200°C. The pressing pressure can be selected according to the shape of the molded body and the desired surface properties. For example, when the shape of the molded body is not complicated (when the amount of deformation is not large), the surface pressure applied to the molded body is selected to be 1 to 100 MPa, preferably 1 to 50 MPa. When the grain of the material is required on the surface of the molded body, it is appropriate to perform pressing at a low pressure of 50 MPa or less (preferably 20 MPa or less) in order to suppress fiber breakage of the wood. On the other hand, by pressing at high pressure, a shear force is applied to the wood and plastic flow due to intercellular slippage is generated, and the cells are moved to a predetermined free space in the mold, filling the free space and shaping the wood, thereby obtaining a molded body having the desired shape, size and surface properties similar to those obtained using resin or metal. In this case, the preferred pressure is 1 to 500 MPa, more preferably 5 to 200 MPa. In this way, when producing a molded body, the molding temperature and pressure during pressing can be appropriately set, and other factors such as the moisture content of the raw material and the molding time can also be set to control the properties of the molded body.

[0028] The mold used for producing the molded article in the present invention is not particularly limited, but includes molds used for general metal and resin molding. The mold surface forming the surface of the molded article may be flat or may include a curved surface or a shape such as an uneven portion.

[0029] In the present invention, in the case of a molded body having a thermoplastic urethane resin disposed on the surface, reheating the molded body increases the voids on the surface of the wood-based molded body, and a softer texture of wood material is obtained. The method and conditions (temperature, pressure, etc.) of reheating are not particularly limited, but it is preferable to perform the reheating at a temperature equal to or higher than the softening temperature of the urethane resin. In addition, by reheating the molded body with a mold (regardless of whether it is flat or curved) in contact with the surface of the molded body, the surface of the molded body can be formed to match the surface shape of the mold. EXAMPLES

[0030] The present invention will be described in more detail below with reference to examples. However, since these examples merely show some embodiments of the present invention, the present invention should not be interpreted as being limited to these examples.

[0031] 1. Wood material A used

[0032] Several board-shaped wood samples measuring approximately 200 mm (in the direction of the grain: L) and approximately 300 mm (in the direction perpendicular to the grain: T) in length were cut from a cypress veneer approximately 4 mm thick, and dried at 105°C for more than four hours in a constant temperature, forced-air dryer.

[0033] 2. Impregnating resin used

[0034] (1) Blocked isocyanate compound (MOI) 2-[0-(1'-methylpropylideneamino)carboxyamino]ethyl methacrylate "Karenz MOI-BM" (trade name) manufactured by Showa Denko KK was used. This compound is deblocked, that is, the methyl ethyl ketone oxime group is dissociated, by heating to about 120° C. or higher.

[0035] (2) Polyethylene glycol 1540 (PEG1540) The polyethylene glycol used was "Polyethylene Glycol 1,540" (trade name) manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. The molecular weight was approximately 1,500.

[0036] (3) Melamine resin The melamine / formaldehyde resin "Amidair M-3(60)" (trade name) manufactured by DIC Corporation was used. This is a water-soluble resin.

[0037] (4) Phenol resin A phenol / formaldehyde resin "PX-341" (trade name) manufactured by Aica Kogyo Co., Ltd. was used. This is a water-soluble resin.

[0038] 3. Preparation of Resin-impregnated Wood Samples

[0039] (1) Wood-based material containing polyurethane precursor An aqueous polyethylene glycol solution obtained by dissolving polyethylene glycol previously melted at 60° C. in water and an ethanol solution of a blocked isocyanate compound obtained by dissolving the polyethylene glycol in ethanol were mixed, Polyethylene glycol 1540 (PEG1540):blocked isocyanate compound (MOI) = 1:1 (mass ratio) An aqueous 35% ethanol solution with a solid content of 20 wt % was used as an impregnation liquid (hereinafter referred to as "impregnation liquid L1"). Next, the wood material A was immersed in "impregnation liquid L1" at about 20°C, and in that state, the pressure was reduced (0.01 MPa, 1 hour) at room temperature (about 20°C), and then pressurized (0.8 MPa, about 18 hours).The wood material impregnated with impregnation liquid L1 was then removed from impregnation liquid L1, placed on a wire rack, and air-dried at room temperature (about 20°C) for 2 days, and then dried in a 35°C air dryer for about 3 days and further in a 35°C vacuum dryer for at least 2 days, to obtain a polyurethane precursor-containing wood material that was a soluble matter. The weight increase rate of the obtained polyurethane precursor-containing wood material (hereinafter referred to as "impregnated wood U") compared to the weight of the wood material A before contact with the "impregnation liquid L1" was calculated to be 42%.

[0040] (2) Wood-based materials containing melamine-added polyurethane precursors Polyethylene glycol that has been melted at 60°C is dissolved in water to prepare an aqueous polyethylene glycol solution, and the aqueous polyethylene glycol solution is cooled to room temperature, and then a melamine resin is added to the aqueous polyethylene glycol solution to prepare a mixed liquid. The mixed liquid is mixed with an ethanol solution obtained by dissolving a blocked isocyanate compound in ethanol, Polyethylene glycol 1540 (PEG1540):blocked isocyanate compound (MOI):melamine resin=1:1:1 (mass ratio), A 35% aqueous ethanol solution with a solid content of 20% was used as an impregnation liquid (hereinafter referred to as "impregnation liquid L2"). Next, the wood material A was immersed in impregnation liquid L2 at about 20° C., and the same operation as for the polyurethane precursor-containing wood material was carried out to obtain a melamine-added polyurethane precursor-containing wood material, which was a dissolved product. The weight increase rate of the obtained melamine-added polyurethane precursor-containing wood material (hereinafter referred to as "impregnated wood UM") compared to the wood material A before contact with the impregnation liquid L2 was measured and calculated to be 43%.

[0041] (3) Wood materials containing melamine resin A melamine resin-containing wood material was obtained by carrying out the same operations as for the polyurethane precursor-containing wood material, except that an aqueous melamine resin solution (hereinafter referred to as "impregnation solution L3") was used in which the solid content concentration of the melamine / formaldehyde resin "Amidia M-3" (trade name) manufactured by DIC Corporation was used instead of impregnation solution L1, and the solid content concentration of the melamine / formaldehyde resin was set to 20%. The weight increase rate of the obtained melamine resin-containing wood material (hereinafter referred to as "impregnated wood M") compared to the wood material A before contact with the impregnation liquid L3 was measured and calculated to be 42%.

[0042] (4) Wood materials containing phenolic resin A phenolic resin-containing wood material was obtained by carrying out the same operations as for the polyurethane precursor-containing wood material, except that an aqueous phenolic resin solution (hereinafter referred to as "impregnation solution L4") was used in which the solid content concentration of the phenolic / formaldehyde resin "PX-341" (product name) manufactured by Aica Kogyo Co., Ltd. was adjusted to 20% instead of the impregnation solution L1. The weight increase rate of the obtained phenolic resin-containing wood material (hereinafter referred to as "impregnated wood P") compared to the wood material A before contact with the impregnation liquid L4 was measured and calculated to be 53%.

[0043] 4. Preparation and evaluation of two-layer laminated wood moldings

[0044] (1) Example 1 One piece each of "Impregnated Wood M" and "Impregnated Wood U" cut to 49mm (L) x 50mm (T) (total of two pieces) were stacked directly with the fibers aligned in the same direction, placed in a closed mold with a flat plate with a punch area of ​​52mm x 50mm set at a temperature of 170°C, and pressed under a load of 2.5 tons (approximately 10MPa). After holding the pressure for five minutes, the closed mold was cooled to below 50°C and a 3.0mm thick "laminated wood molded body MU" was produced. Naturally, no adhesive was used between the "Impregnated Wood M" and the "Impregnated Wood U" (as in each example). Six rectangular test pieces measuring 11 mm wide and 20 mm long were cut out from the "laminated wood molding MU" in the fiber direction, and the apparent interlaminar shear strength was evaluated in accordance with JIS K7078 (interlaminar shear test method for carbon fiber reinforced plastics). The results are shown in Figure 1.

[0045] (2) Example 2 A "laminated wood molding PU" having a thickness of 2.5 mm was produced by carrying out the same operations as in Example 1, except that one piece each of "impregnated wood P" and "impregnated wood U" cut to 49 mm (L) x 50 mm (T) was used. The "laminated wood molded body PU" was subjected to the same procedure as in Example 1 to evaluate the apparent interlaminar shear strength, and the results are shown in FIG.

[0046] (3) Example 3 A 3.2 mm thick "laminated wood molding M-UM" was produced by the same procedure as in Example 1, except that one piece each of impregnated wood M and impregnated wood UM, each cut to 49 mm (L) x 50 mm (T), was used. The "laminated wood molded body M-UM" was subjected to the same procedure as in Example 1 to evaluate the apparent interlaminar shear strength, and the results are shown in FIG.

[0047] (4) Example 4 A "laminated wood molding P-UM" having a thickness of 2.7 mm was produced by the same procedure as in Example 1, except that one piece each of "impregnated wood P" and "impregnated wood UM" cut to 49 mm (L) x 50 mm (T) was used. The "laminated wood molded body M-UM" was subjected to the same procedure as in Example 1 to evaluate the apparent interlaminar shear strength, and the results are shown in FIG.

[0048] (5) Comparative Example 1 A laminated wood molding UU having a thickness of 2.8 mm was produced in the same manner as in Example 1, except that two pieces of "impregnated wood U" cut to 49 mm (L) x 50 mm (T) were used. The "laminated wood molded body UU" was subjected to the same procedure as in Example 1, and the apparent interlaminar shear strength was evaluated. The results are shown in FIG.

[0049] (6) Comparative Example 2 Except for using two pieces of "impregnated wood UM" cut to 49 mm (L) x 50 mm (T), the same procedure as in Example 1 was carried out to produce a 2.7 mm thick "laminated wood molding UM-UM." The apparent interlaminar shear strength of the "laminated wood molding UM-UM" was evaluated using the same procedure as in Example 1, and the results are shown in Figure 1.

[0050] (7) Comparative Example 3 A laminated wood molding MM having a thickness of 3.4 mm was produced in the same manner as in Example 1, except that two pieces of impregnated wood M cut to 49 mm (L) x 50 mm (T) were used. The "laminated wood molded body MM" was subjected to the same procedure as in Example 1 to evaluate the apparent interlaminar shear strength, and the results are shown in FIG.

[0051] (8) Comparative Example 4 A 2.7 mm thick "laminated wood molding PP" was produced in the same manner as in Example 1, except that two pieces of "impregnated wood UM" cut to 49 mm (L) x 50 mm (T) were used. The "laminated wood molded body PP" was subjected to the same procedure as in Example 1, and the apparent interlaminar shear strength was evaluated. The results are shown in FIG.

[0052] (9) Evaluation As described above, Figure 1 shows the experimental results comparing the apparent interlaminar shear strength of Examples 1 to 4 with that of Comparative Examples 1 to 4, in which laminated wood moldings made from single pieces of each of the impregnated resin materials used in Examples 1 to 4 were laminated together. As can be seen from FIG. 1, the interlaminar shear strength of Examples 2 to 4 was at the same level as that of Comparative Example 3 (melamine resin-containing wood material "laminated wood molded body MM"). In addition, in FIG. 1, the "diamond plot" in the bar graph of Example 1 (MU) represents the average value of the two constituent laminated wood moldings (Comparative Example 1 "UU" and Comparative Example 3 "MM"). Similarly, the bar graph plot of Example 2 (PU) represents the average value of the two constituent laminated wood moldings (Comparative Example 1 "UU" and Comparative Example 4 "PP"). Similarly, Example 2 (M-UM) represents the average value of Comparative Example 3 and Comparative Example 2, and Example 4 (P-UM) represents the average value of Comparative Example 4 and Comparative Example 2. In particular, it is shown that the interlaminar shear strength of Example 3 is greater than the average value of the constituent laminated wood moldings (Comparative Examples 2 and 3). In other words, it was suggested that the "laminated wood molding (M-UM)" which combines a melamine resin-containing wood material and a melamine-added polyurethane precursor-containing wood material has better interlaminar affinity than each of the laminated wood moldings alone.

[0053] 5. Preparation and evaluation of three-layer laminated wood moldings

[0054] (1) Example 5 Impregnated wood U, impregnated wood M, and impregnated wood P, each cut to 49 mm (L) x 50 mm (T), were stacked one by one in that order for a total of three pieces (stacked with the same fiber direction), and placed in a closed mold with a flat plate with a punch area of ​​52 mm x 50 mm set at a temperature of 170°C. Press-molded under a load of 2.5 tons (approximately 10 MPa). After holding the pressure for five minutes, the closed mold was cooled to below 50°C and a 4.2 mm thick "laminated wood molded body UMP" was produced. Three rectangular test pieces measuring 10 mm wide and 35 mm long were cut out from the "laminated wood molding UMP" in the fiber direction, and the apparent interlaminar shear strength was evaluated in accordance with JIS / K7078 (interlaminar shear test method for carbon fiber reinforced plastics). The results are shown in Figure 2.

[0055] (2) Example 6 A 4.4 mm thick "laminated wood molding UPM" was produced in the same manner as in Example 5, except that a total of three pieces of "impregnated wood U," "impregnated wood P," and "impregnated wood M," cut to 49 mm (L) x 50 mm (T), were stacked in that order. The "UPM laminated wood molded body" was subjected to the same procedure as in Example 5 to evaluate the apparent interlaminar shear strength, and the results are shown in FIG.

[0056] (3) Example 7 A "laminated wood molding UM-MP" with a thickness of 4.1 mm was produced by the same procedure as in Example 5, except that a total of three pieces of "impregnated wood UM," "impregnated wood M," and "impregnated wood P," each cut to 49 mm (L) x 50 mm (T), were stacked in that order. The "laminated wood molded body UM-MP" was subjected to the same procedure as in Example 5 to evaluate the apparent interlaminar shear strength, and the results are shown in FIG. Next, the Brinell hardness of both surfaces of the laminated wood molding (the "impregnated wood UM" molding surface and the "impregnated wood P" molding surface) was evaluated in accordance with JIS / Z2101 (testing method for wood) using both end portions (undamaged portions) of the sample after the interlaminar shear test of the "laminated wood molding UM-MP." The results are shown in Figure 3.

[0057] (4) Example 8 A "laminated wood molding UM-PM" with a thickness of 4.3 mm was produced by the same procedure as in Example 5, except that a total of three pieces of "impregnated wood UM," "impregnated wood P," and "impregnated wood M," each cut to 49 mm (L) x 50 mm (T), were stacked in that order. The "laminated wood molding UM-PM" was subjected to the same procedure as in Example 5 to evaluate the apparent interlaminar shear strength, and the results are shown in FIG. Next, using the samples of the "laminated wood molding UM-PM" after the interlaminar shear test, the same procedure as in Example 7 was performed to evaluate the Brinell hardness of both surfaces of the laminated wood molding (the "impregnated wood UM molding surface" and the "impregnated wood M molding surface"), and the results are shown in Figure 3.

[0058] (5) Comparative Example 5 A "laminated wood molding UUU" having a thickness of 4.2 mm was produced by the same procedure as in Example 5, except that three sheets of "impregnated wood U" cut to 49 mm (L) x 50 mm (T) were stacked together to form a total of three sheets. The "laminated wood molded body UUU" was subjected to the same procedure as in Example 5 to evaluate the apparent interlaminar shear strength, and the results are shown in FIG.

[0059] (6) Comparative Example 6 A "laminated wood molding UM-UM-UM" having a thickness of 3.9 mm was produced by performing the same procedure as in Example 5, except that three sheets of "impregnated wood UM" cut to 49 mm (L) x 50 mm (T) were stacked together for a total of three sheets. The apparent interlaminar shear strength of the laminated wood molding UM-UM-UM was evaluated in the same manner as in Example 5, and the results are shown in FIG.

[0060] (7) Comparative Example 7 A "laminated wood molding MMM" having a thickness of 4.7 mm was produced by the same procedure as in Example 5, except that three sheets of "impregnated wood M" cut to 49 mm (L) x 50 mm (T) were stacked together for a total of three sheets. The "laminated wood molded body MMM" was subjected to the same procedure as in Example 5 to evaluate the apparent interlaminar shear strength, and the results are shown in FIG.

[0061] (8) Comparative Example 8 A "laminated wood molding PPP" having a thickness of 4.1 mm was produced by the same procedure as in Example 5, except that three sheets of "impregnated wood P" cut to 49 mm (L) x 50 mm (T) were stacked together for a total of three sheets. The "laminated wood molded body PPP" was subjected to the same procedure as in Example 5 to evaluate the apparent interlaminar shear strength, and the results are shown in Figure 2.

[0062] (9) Comparative Example 9 A 4.1 mm-thick "laminated wood molding MUP" was produced by the same procedure as in Example 5, except that a total of three sheets of "impregnated wood M," "impregnated wood U," and "impregnated wood P," cut to 49 mm (L) x 50 mm (T), were stacked in that order. The "laminated wood molded body MUP" was subjected to the same procedure as in Example 5 to evaluate the apparent interlaminar shear strength, and the results are shown in FIG.

[0063] (10) Comparative Example 10 A 4.3 mm thick "laminated wood molding M-UM-P" was produced by the same procedure as in Example 5, except that a total of three sheets of "impregnated wood M," "impregnated wood UM," and "impregnated wood P," cut to 49 mm (L) x 50 mm (T), were stacked in that order. The apparent interlaminar shear strength of the "laminated wood molding M-UM-P" was evaluated in the same manner as in Example 5, and the results are shown in FIG.

[0064] (11) Evaluation As shown in Fig. 2 above, in Examples 6 to 8, failure occurred due to bending failure, and therefore the shear fracture strength was greater than the bending fracture strength. Example 7 ("Laminated wood molding UM-MP") and Example 8 ("Laminated wood molding UM-PM") had the greatest interlaminar shear strength. Therefore, it was found that the preferred stacking order when producing a three-layer laminated wood molding is to place the melamine-added polyurethane precursor-containing wood material (UM) on the surface layer, followed by the melamine resin-containing wood material (M) or the phenol resin-containing wood material (P). Next, the results of evaluating the surface softness of the laminated wood moldings of Examples 7 and 8, which had the highest apparent interlaminar shear strength (MPa), are shown in FIG. In both Example 7 ("Laminated wood molding UM-MP") and Example 8 ("Laminated wood molding UM-PM"), it was found that the "Impregnated wood UM" molded surface had a lower Brinell hardness and was softer than the other side (the "Impregnated wood P" molded surface and the "Impregnated wood M" molded surface). It was found that using the "Impregnated wood UM" molded surface as the product's design surface (the surface showing the molded body, the surface in contact with the molded body) is preferable because it provides a soft wood texture.

[0065] 6. Fabrication of 3D laminated wood compacts

[0066] (1) Approximately 20 g of wood pieces (hereinafter, "wood pieces UM") obtained by cutting the "impregnated wood UM" to approximately 10 mm (L) x 10 mm (T), and "impregnated wood UM" (hereinafter, "board UM"), impregnated wood P (hereinafter, "board P"), and impregnated wood M (hereinafter, "board M"), each cut to 95 mm (L) x 95 mm (T), were used to produce a three-dimensional laminated wood molding as follows. The molded bodies were produced using dies heated to a surface temperature of 160–170°C for the lower die (flat design surface, placed on the lower press plate) and 130–140°C for the upper die (surface with ribs, placed on the upper press plate).

[0067] (2) Example 9 The wood pieces UM, boards UM, boards M, and boards P were arranged and stacked in this order, then inserted into the lower die and pressed at 600kN (surface pressure 75MPa), and the pressure was maintained for 5 minutes.The die was then cooled to below 50°C, and the resulting "laminated wood molding UM-MP" was then removed.A photograph of the appearance of the laminated wood molding UM-MP is shown in Figure 4.In the figure, 1 indicates the entire laminated wood molding, while 2 and 3 indicate the rib section and reinforcing section, respectively, which were flow-formed by backward extrusion.

[0068] (3) Example 10 Except for arranging and stacking the wood pieces UM, board UM, board P, and board M in that order and then putting them into the mold, the same operations as in Example 9 were carried out to produce the laminated wood molded body UM-PM. A photograph of the appearance of the laminated wood molded body UM-PM is shown in Figure 5. In the figure, 1 indicates the entire laminated wood molded body, while 2 and 3 indicate the rib section and reinforcing section, respectively, which were flow-formed by backward extrusion.

[0069] (4) Evaluation 4 and 5, it can be seen that the constituent materials ("Plate UM", "Plate P", and "Plate M") fill the rib section 2 better in "Laminated wood molding UM-MP" than in "Laminated wood molding UM-PM", resulting in a better laminated wood molding 1. In other words, it can be said that the surface of the laminated wood molding 1 that requires a complex shape such as the rib section 2 bent at a nearly right angle (i.e., the surface that is positioned on the concave side when bending) is preferably made of a laminated structure in which a wood material containing phenolic resin is arranged. In addition, when a softer surface is required, the combination with "Laminated wood molding U-UM-M" can also be considered.

[0070] 7. Adding a wood-like texture (appearance, softness) by reheating the design surface

[0071] (1) Example 11 A "laminated wood molding U-UM-M" with a thickness of 4.3 mm was produced by carrying out the same operations as in Example 5, except that a total of three sheets of "impregnated wood U", "impregnated wood UM" and "impregnated wood M" cut to 49 mm (L) x 50 mm (T) were stacked in that order. The "laminated wood molding U-UM-M" with a thickness of 4.3 mm was produced. A photograph of the appearance of the molded surface side (design surface 1a) of "impregnated wood U" of the molded "laminated wood molding U-UM-M" (laminated wood molding 1) is shown in Figure 6. The Brinell hardness of the design surface 1a was measured, and 16.3±3.9N / mm 2 It was.

[0072] (2) Example 12 Using the "laminated wood molding U-UM-M" produced in Example 11, the molded surface side of the "impregnated wood U" (i.e., the top surface of the "laminated wood molding U-UM-M") was placed in contact with a flat hot plate heated to 170°C and heated for 5 minutes while applying a weight of 400g (surface pressure of approximately 1.6kPa) to produce a "reheated laminated wood molding U-UM-M". Figure 7 shows an external photograph of the molded surface side (design surface 1a) of the "impregnated wood U" of the molded "reheated laminated wood molding U-UM-M". The thickness of the "reheated laminated wood molding U-UM-M" was measured to be 4.6mm, which was approximately 7% thicker than the thickness of the "laminated wood molding U-UM-M" before reheating. The Brinell hardness of the design surface 1a was measured to be 3.65±2.8N / mm 2 It was.

[0073] (3) Evaluation The Brinell hardness of Example 12 after reheating was reduced to less than one-quarter of the Brinell hardness of Example 11 before reheating. This shows that a softer wood texture can be obtained by reheating the surface of the "impregnated wood U" that constitutes the laminated wood molding. The thickness of the molding increased due to reheating, which is thought to be due to the voids in the wood near the surface of the "impregnated wood U" being restored by the reheating. Furthermore, when comparing the external photographs in Figures 6 and 7, it can be seen that the reheated laminated wood molding in Figure 7 has surface irregularities that follow the grain of the wood, and that reheating has visually improved the texture of the wood. Therefore, when seeking to improve the texture of wood on surfaces that come into contact with the user's buttocks or back, such as chair seats and backs, "laminated wood molded body UM-MP" (surface UM; also includes heating the surface of surface UM; see Example 9, etc.) or "laminated wood molded body U-UM-M" (surface U; also includes heating the surface of surface U; see Examples 11 and 12, etc.) are considered preferable. At the current stage of molding, "laminated wood molded body UM-MP" (surface UM), which is less likely to produce molding defects, is considered optimal. In particular, since metal fittings for attaching the legs are usually fixed to the bottom of the chair seat (molded body), it is useful to position the "impregnated wood P", which is relatively strong and can easily accommodate uneven thickness (varying wall thickness), at the bottom of the chair seat.

[0074] 8. Other embodiments

[0075] (1) In the above, cypress was used as the wooden material, but of course other types of wood can also be used. (2) Furthermore, the specifications of “melamine-based resin,” “urethane-based resin,” “phenol-based resin,” and “melamine-based resin and urethane-based resin” in the above are not limited to those in the above embodiments, and other resin materials that are considered to be of the same family may also be used. (3) Although an embodiment of the present invention has been described above, the present invention is not limited to the above-described embodiment and can be modified in various ways within the technical scope understood from the description of the claims. [Explanation of symbols]

[0076] 1. Laminated wood molding (molded body) 1a Design surface of laminated wood molding 2. Rib part of laminated wood molding 3 Reinforcement of laminated wood body

Claims

1. A molded body comprising a plurality of selected resin-impregnated veneers from the first resin-impregnated veneer to the fourth resin-impregnated veneer, which are stacked together with their surfaces in direct contact with each other to form an integral body. (1) The first resin-impregnated veneer is a resin-impregnated veneer in which a wood material is impregnated with a melamine-based resin and a urethane-based resin. (2) The second resin-impregnated veneer is a resin-impregnated veneer in which a wood material is impregnated with a melamine-based resin. (3) The third resin-impregnated veneer is a resin-impregnated veneer in which a wood material is impregnated with a phenolic resin. (4) The fourth resin-impregnated veneer is a resin-impregnated veneer in which a wood material is impregnated with a urethane-based resin.

2. A molded body characterized in that a first resin-impregnated veneer and a second resin-impregnated veneer are stacked together with their surfaces in close contact with each other, and either a second resin-impregnated veneer, a third resin-impregnated veneer or a fourth resin-impregnated veneer is stacked and pressed onto either side of the stacked laminate, forming a three-layered integral body. (1) The first resin-impregnated veneer is a resin-impregnated veneer in which a wood material is impregnated with a melamine-based resin and a urethane-based resin. (2) The second resin-impregnated veneer is a resin-impregnated veneer in which a wood material is impregnated with a melamine-based resin. (3) The third resin-impregnated veneer is a resin-impregnated veneer in which a wood material is impregnated with a phenolic resin. (4) The fourth resin-impregnated veneer is a resin-impregnated veneer in which a wood material is impregnated with a urethane-based resin.

3. The molded body according to claim 2, wherein a first resin-impregnated veneer and a second resin-impregnated veneer are stacked with their surfaces directly in contact with each other, and further, a surface of a third resin-impregnated veneer is in contact with the other surface of the second resin-impregnated veneer and laminated and pressed together to form a three-layer integral body.

4. The molded body described in claim 3, wherein a first resin-impregnated veneer and a second resin-impregnated veneer are stacked on top of each other with their surfaces directly in contact with each other, and a third resin-impregnated veneer is laminated on the other surface of the second resin-impregnated veneer with its surface in contact with each other, thereby forming a molded body having curved surfaces and uneven portions, which is constructed as a three-layer integral body.

5. The molded body according to claim 2, characterized in that a first resin-impregnated veneer and a second resin-impregnated veneer are stacked with their surfaces directly in contact with each other, and the following A or B is laminated and pressed into three layers, so that a molded body having curved surfaces and uneven portions according to the shape of the seat or back of a chair is formed as a three-layer integral body. (A) The surface of a third resin-impregnated veneer is adhered to the other surface of the second resin-impregnated veneer, and the first resin-impregnated veneer is laminated so that the surface comes into contact with the user. (B) The surface of a fourth resin-impregnated veneer is adhered to the other surface of the first resin-impregnated veneer, and the fourth resin-impregnated veneer is laminated so that the fourth resin-impregnated veneer is positioned on the surface that comes into contact with the user.

6. The molded body according to claim 5, wherein the surface that comes into contact with the user's buttocks or back is heat-treated, and the molded body is constructed in three integral layers having curved surfaces and uneven portions according to the shape of the seat or back of the chair.

Citation Information

Patent Citations

  • Densified plywood and its production

    JP1995214506A

  • Sheet manufactured from flat core and curved component connected thereto and manufacturing method of the sheet

    JP2003220652A

  • Manufacturing method for woody material for musical instrument, woody material for musical instrument obtained by the method, and musical instrument using the same

    JP2004058416A

  • Compaction of wood by combination treatment of steam treatment and resin impregnation treatment

    JP2006240032A

  • Stuck laminated material, method for producing stuck laminated material, furniture and interior material

    JP2016199003A