Control device for acceleration cooling device and control method for acceleration cooling device

The control device for accelerated cooling devices stabilizes material quality in thick steel plates by measuring and adjusting cooling conditions at multiple points along the plate, ensuring uniform cooling stop temperatures and reducing material variations.

JP2024165658AActive Publication Date: 2024-11-28JFE STEEL CORP
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2023082023
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-18
Publication Date
2024-11-28
Estimated Expiration
2043-05-18

AI Technical Summary

Technical Problem

Existing accelerated cooling methods for thick steel plates after hot rolling result in material quality variations due to inconsistent cooling start temperatures along the longitudinal direction, leading to potential decreases in strength and material instability during mass production.

Method used

A control device and method that measures the surface temperature of steel plates at multiple locations before entering the accelerated cooling device, adjusts the cooling conditions, including conveyance speed and cooling fluid application, to achieve uniform cooling stop temperatures across the plate, thereby stabilizing material quality.

Benefits of technology

The solution enhances material uniformity and stability of high-strength steel plates used in applications like ships, bridges, and marine structures by minimizing variations caused by inconsistent cooling start temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024165658000001_ABST
    Figure 2024165658000001_ABST
Patent Text Reader

Abstract

To provide a control device for an acceleration cooling device and a control method for the acceleration cooling device, which can suppress material dispersion caused by dispersion of an acceleration cooling start temperature and can improve material stability during mass production of steel sheets.SOLUTION: A control device 19 of an acceleration cooling device 11 lowers the temperature of a steel sheet 7 to a target acceleration cooling stop temperature by performing acceleration cooling to the steel sheet 7 being conveyed. A target accelerated cooling stop temperature at a measurement point of the temperature of the steel sheet 7 and an accelerated cooling condition at an accelerated cooling device 11 at the measurement point for realizing the target accelerated cooling stop temperature are determined on the basis of a relationship between the accelerated cooling start temperature and the accelerated cooling stop temperature and the temperatures of the steel sheet 7 at least two or more points in the conveying direction T of the steel sheet 7 at a time point before entering the accelerated cooling device 11.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a control device for an accelerated cooling device and a control method for an accelerated cooling device. [Background technology]

[0002] The manufacturing method of high-strength thick steel plate in which accelerated cooling is performed after hot rolling has advantages such as reducing alloy elements of the thick steel plate and omitting heat treatment or reducing the number of times heat treatment is performed, and is widely applied. The accelerated cooling method is generally a pass-through type accelerated cooling method in which the hot-rolled thick steel plate is continuously introduced into an accelerated cooling device from the front end to the tail end, and water is sprayed onto the top and bottom surfaces of the thick steel plate to cool it. The pass-through type accelerated cooling method can make the accelerated cooling device smaller than the simultaneous spray type accelerated cooling method in which accelerated water cooling is started after the entire thick steel plate has completely entered the accelerated cooling device. However, the pass-through type accelerated cooling method may cause material variations in the longitudinal direction of the thick steel plate due to the fact that the accelerated cooling start temperature of the thick steel plate is not constant in the longitudinal direction of the thick steel plate. Generally, from the viewpoint of production efficiency and suppression of deterioration in the strength of the steel plate, the steel plate after completion of hot rolling is transported to the accelerated cooling device over the shortest possible distance, and accelerated cooling is then initiated on the steel plate immediately thereafter.

[0003] In order to solve such problems, various studies have been conducted on a method for manufacturing a steel plate in which accelerated cooling is performed after hot rolling.

[0004] For example, Patent Document 1 describes a method for manufacturing a controlled-cooled steel plate. In this method, between hot rolling and controlled cooling (corresponding to the accelerated cooling described above, hereinafter referred to as accelerated cooling), a shower cooling facility is used to slowly cool the entire length of the thick steel plate before accelerated cooling. Patent Document 2 describes a method for manufacturing a high-strength steel plate, in which tempering is performed by induction heating after accelerated cooling. Patent Documents 3 and 4 describe a method for controlling the cooling of a steel plate. In this method, the speed at which the steel plate passes through the cooling device is adjusted based on the temperature of the steel plate measured by a thermometer installed inside a pass-through cooling device that performs accelerated cooling of the steel plate. Patent Document 5 describes a method for controlling the cooling of a steel plate. In this method, in a pass-through cooling device that performs accelerated cooling of the steel plate, thermometers are placed before and after the cooling device in the passing direction of the steel plate, and the speed at which the steel plate passes through the cooling device is adjusted based on the temperature of the steel plate measured by the thermometers. Patent Document 6 describes a method for controlling the cooling of a pass-through cooling device that performs accelerated cooling of the steel plate. In this method, the accelerated cooling start temperature is measured for each region divided in the longitudinal direction of the steel sheet, and the conveying speed in the pass-through type accelerated cooling device is adjusted based on the measured accelerated cooling start temperature so that the accelerated cooling end temperature of each region becomes the target accelerated cooling end temperature. Patent Document 7 describes a method for reducing the material variation of hot-rolled steel. In this method, when manufacturing a hot-rolled steel sheet, data including the steel sheet components, operating conditions, and material performance values ​​for each hot-rolled steel sheet manufactured in the past are accumulated. Then, based on the accumulated data and the required specifications including the steel sheet components and operating conditions of the hot-rolled steel sheet to be manufactured at the present time, the material quality when the hot-rolled steel sheet to be manufactured at the present time is manufactured is estimated. In addition, operating conditions that satisfy the required specifications are set based on the estimated value and the estimation error of the material quality. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 5-57330 [Patent Document 2] JP 2005-120409 A [Patent Document 3] JP 2006-272395 A [Patent Document 4] JP 2006-281300 A [Patent Document 5] JP2010-167503 Public Relations [Patent Document 6] JP 2010-247234 A [Patent Document 7] JP 2006-239696 A Summary of the Invention [Problem to be solved by the invention]

[0006] The method of Patent Document 1 not only requires shower cooling equipment, but also has the possibility of failing to achieve high strength due to a decrease in the strength of the thick steel plate caused by slow cooling performed before accelerated cooling. In addition, the method of Patent Document 1 cannot suppress the variation in the accelerated cooling start temperature, so there is a possibility that the material variation caused by the variation in the accelerated cooling start temperature cannot be suppressed. Note that Patent Document 2 also has the same problems as Patent Document 1.

[0007] The methods of Patent Documents 3 and 4 improve the accuracy of the accelerated cooling stop temperature of thick steel plates by measuring the surface temperature of the steel plate during accelerated cooling, and may not be able to suppress the material variation caused by the variation in the accelerated cooling start temperature. In the method of Patent Document 5, the accelerated cooling conditions are adjusted after the cooling of the front end of the steel plate is completed, so it may only be applicable when the total length of the steel plate is long or the total length of the accelerated cooling device is short. In addition, the method of Patent Document 5 improves the accuracy of the accelerated cooling stop temperature of the steel plate, and may not be able to suppress the material variation caused by the variation in the accelerated cooling start temperature. The method of Patent Document 6 improves the accuracy of the accelerated cooling stop temperature of thick steel plates, and may not be able to suppress the material variation caused by the variation in the accelerated cooling start temperature. In the method of Patent Document 7, it may not be possible to suppress the material variation caused by the variation in the accelerated cooling start temperature or the accelerated cooling stop temperature of thick steel plates.

[0008] The present invention has been made to solve the above-mentioned problems, and aims to provide a control device for an accelerated cooling device and a control method for an accelerated cooling device that can suppress material quality variations caused by variations in the accelerated cooling start temperature and improve material quality stability during mass production of steel plates. [Means for solving the problem]

[0009] In order to achieve the above object, the present invention provides (1) A control device for an accelerated cooling device that performs accelerated cooling on a steel plate being transported to reduce the temperature of the steel plate to a target accelerated cooling stop temperature, the control device for an accelerated cooling device determining the target accelerated cooling stop temperature at a measurement point of the temperature of the steel plate and the accelerated cooling conditions in the accelerated cooling device at the measurement point for achieving the target accelerated cooling stop temperature, based on the relationship between the accelerated cooling start temperature and the accelerated cooling stop temperature and the temperature of the steel plate at at least two or more points in the transport direction of the steel plate before it enters the accelerated cooling device. (2) The point in time before entering the accelerated cooling device refers to the time when the steel plate enters the accelerated cooling device, and the temperature of the steel plate is the surface temperature of the steel plate when it enters the accelerated cooling device. The control device for an accelerated cooling device described in (1). (3) The control device for an accelerated cooling device described in (1), wherein the temperature of the steel plate is at least one of an actual measured value of the surface temperature of the steel plate at the exit side of the hot rolling device upstream of the accelerated cooling device in the conveying direction, and an estimated value estimated based on the actual measured value and the distance between the accelerated cooling device and the hot rolling device in the conveying direction. (4) A control device for an accelerated cooling device described in (2), wherein the temperature of the steel plate is at least one of an actual measured value of the surface temperature of the steel plate at the exit side of the hot rolling device upstream of the accelerated cooling device in the conveying direction, and an estimated value estimated based on the actual measured value and the distance between the accelerated cooling device and the hot rolling device in the conveying direction. (5) The temperature of the steel plate at at least two points in the conveying direction of the steel plate is at least two points among the leading end, the center, and the trailing end of the steel plate in the conveying direction of the steel plate. (6) A control device for an accelerated cooling device described in any of (1) to (4), wherein the accelerated cooling device includes a plurality of cooling units that supply a cooling fluid to the steel plate, and the accelerated cooling conditions include a conveying speed of the steel plate in the accelerated cooling device and the number of the cooling units that supply the cooling fluid to the steel plate in the accelerated cooling device. (7) A control method for an accelerated cooling device that performs accelerated cooling on a steel plate being transported to reduce a temperature of the steel plate to a target accelerated cooling stop temperature, the control method comprising: a temperature measuring step of determining the temperatures of the steel plate at at least two or more locations in the transport direction of the steel plate before the steel plate enters the accelerated cooling device; and an accelerated cooling condition determining step of determining the target accelerated cooling stop temperature at the temperature measurement locations of the steel plate and the accelerated cooling conditions in the accelerated cooling device at the temperature measurement locations to achieve the target accelerated cooling stop temperature, based on a relationship between the accelerated cooling start temperature and the accelerated cooling stop temperature and the temperature of the steel plate. (8) A method for controlling an accelerated cooling device according to (7), wherein the steel plate is tempered immediately after the temperature of the steel plate is reduced to the accelerated cooling stop temperature, or after the temperature of the steel plate is reduced to the target accelerated cooling stop temperature and further air-cooled. Effect of the Invention

[0010] According to the present invention, it is possible to improve the material uniformity of accelerated cooled steel plates (referred to as high-strength steel plates) used in ships, bridges, buildings, marine structures, line pipes, etc., and the material stability during mass production. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a diagram showing an example of a thick steel plate production line equipped with an accelerated cooling device according to the present invention. [Diagram 2]FIG. 1 is a diagram illustrating an example of the configuration of an accelerated cooling device. [Diagram 3] 4 is a flowchart for explaining an example of control executed by a control device of an accelerated cooling device according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, an embodiment of the present invention will be described. FIG. 1 is a diagram showing an example of a thick steel plate production line equipped with an accelerated cooling device according to the present invention. In the thick steel plate production line 1 shown in FIG. 1, a slab 3 heated in a heating furnace 2 is transported by a transport device 4 to a first rolling mill 5 and a second rolling mill 6 in this order, and the slab 3 is hot-rolled stepwise in each of the rolling mills 5 and 6 to produce a thick steel plate (hereinafter, simply referred to as a steel plate) 7. In the example shown in FIG. 1, the transport device 4 is composed of a plurality of transport rolls. The first rolling mill 5 is a rough rolling mill that roughly rolls the slab 3 to a predetermined thickness. The second rolling mill 6 is a finishing rolling mill that rolls the slab 3 rough-rolled by the first rolling mill 5 to a product thickness to produce a steel plate 7. The above rolling mills 5 and 6 correspond to the hot rolling device in the embodiment of the present invention. The steel plate 7 extends along the transport direction T in the transport device 4. Therefore, the transport direction T of the steel plate 7 and the length direction of the steel plate 7 are substantially parallel to each other.

[0013] A first thermometer 8 is installed on the entrance side of the second rolling mill 6 in the conveying direction T of the steel sheet 7, and a second thermometer 9 is installed on the exit side of the second rolling mill 6. These thermometers 8, 9 may be any conventionally known type as long as they can measure the surface temperature of the steel sheet 7, but are preferably non-contact thermometers such as radiation thermometers.

[0014] A first leveller 10 is provided downstream of the second rolling mill 6 in the conveying direction T of the steel sheet 7. The first leveller 10 corrects the shape of the steel sheet 7 rolled by each of the rolling mills 5 and 6, and may be a conventionally known leveller.

[0015] An accelerated cooling device 11 for controlling the cooling rate in the transformation temperature range of steel to a predetermined accelerated cooling stop temperature (hereinafter simply referred to as the stop temperature) is provided close to the first leveler 10 on the exit side of the first leveler 10. There is a speed difference between the transport speed of the steel sheet 7 in the accelerated cooling device 11 and the transport speed of the steel sheet 7 leaving the second rolling mill 6 and transported to the accelerated cooling device 11. Therefore, a third thermometer 12 is provided on the entry side of the first leveler 10 in order to measure the surface temperature of the steel sheet 7 when it enters the accelerated cooling device 11, that is, just before it. The surface temperature of the steel sheet 7 just before it enters the accelerated cooling device 11 is the accelerated cooling start temperature (hereinafter simply referred to as the start temperature). In addition, in the embodiment of the present invention, the third thermometer 12 is configured to measure the surface temperature of the steel sheet 7 just before it enters the accelerated cooling device 11 at multiple points in the transport direction T of the steel sheet 7 or the length direction of the steel sheet 7. Similarly to the first thermometer 8 and the second thermometer 9, the third thermometer 12 is preferably a non-contact thermometer.

[0016] Fig. 2 is a diagram showing an example of the configuration of an accelerated cooling device 11. The accelerated cooling device 11 shown in Fig. 2 is a so-called pass-through type accelerated cooling device, into which the steel plate 7 is continuously introduced in the longitudinal direction from the leading end to the trailing end. A cooling fluid is sprayed onto each of the upper and lower surfaces of the steel plate 7, thereby cooling the steel plate 7 to a stop temperature set as described later. The above cooling fluid may be liquid-phase cooling water.

[0017] The accelerated cooling device 11 includes a plurality of upper header units 13, 14 that inject cooling water toward the upper surface of the steel plate 7, and a plurality of lower header units 15, 16 that inject cooling water toward the lower surface of the steel plate 7. In order to simplify the drawing, Fig. 2 illustrates only a pair of upper header units 13, 14 and two lower header units 15, 16. Each of the above header units corresponds to a cooling unit in the embodiment of the present invention.

[0018] The first upper header unit 13 is located above the steel plate 7 in the height direction H of the accelerated cooling device 11, and is arranged at a predetermined interval upstream of the second upper header unit 14 in the conveying direction T. The first upper header unit 13 has a plurality of first upper nozzles 13A made of, for example, circular pipes. As shown in Fig. 2, the first upper nozzles 13A are provided at a predetermined angle with respect to the upper surface of the steel plate 7 so as to spray cooling water at an angle from the upstream side to the downstream side in the conveying direction T with respect to the upper surface of the steel plate 7.

[0019] The second upper header unit 14 is located above the steel plate 7 in the height direction H of the accelerated cooling device 11, and has a plurality of second upper nozzles 14A made of, for example, circular pipes. As shown in Fig. 2, the second upper nozzles 14A are provided at a predetermined angle inclined with respect to the upper surface of the steel plate 7 so as to spray cooling water at an angle from the downstream side to the upstream side in the conveying direction T with respect to the upper surface of the steel plate 7. In this way, each of the upper header units 13, 14 is designed to spray cooling water toward a designated location inside the accelerated cooling device 11.

[0020] A first lower header unit 15 is provided on the opposite side to the collision position between the steel sheet 7 and the cooling water sprayed from the first upper header unit 13. The first lower header unit 15 has a plurality of first lower nozzles 15A made of, for example, circular pipes, and these first lower nozzles 15A extend along the height direction H of the accelerated cooling device 11. Note that the interval between the adjacent transport rolls on the opposite side of the collision position is set so that the first lower header unit 15 can be disposed on the opposite side of the above-mentioned collision position.

[0021] A second lower header unit 16 is provided on the opposite side to the collision position between the steel sheet 7 and the cooling water sprayed from the second upper header unit 14. The second lower header unit 16 has a plurality of second lower nozzles 16A made of, for example, circular pipes, and these second lower nozzles 16A extend along the height direction H of the accelerated cooling device 11. Note that the interval between the adjacent transport rolls on the opposite side of the collision position is set so that the second lower header unit 16 can be disposed on the opposite side of the above-mentioned collision position.

[0022] Returning to the explanation of Fig. 1, a fourth thermometer 17 is provided on the outlet side of the accelerated cooling device 11. The fourth thermometer 17 is configured to measure the surface temperature of the steel sheet 7 acceleratedly cooled by the accelerated cooling device 11. Note that the fourth thermometer 17 is preferably a non-contact thermometer, similar to the above-mentioned thermometers 8, 9, and 12.

[0023] A second leveller 18 is provided downstream of the fourth thermometer 17 in the conveying direction T of the steel sheet 7, and the second leveller 18 corrects shape deformation of the steel sheet 7 caused by accelerated cooling. The second leveller 18 may be a conventionally known leveller, similar to the first leveller 10. A tempering device (not shown) is provided downstream of the second leveller 18, and the hardness of the steel sheet 7 is adjusted by the tempering device. The tempering device may be a conventionally known induction heating type tempering device.

[0024] An electronic control unit (hereinafter, referred to as ECU) 19 is provided for controlling the amount of cooling of the steel sheet 7 in the accelerated cooling device 11, i.e., the difference between the start temperature and the stop temperature of the steel sheet 7. The ECU 19 is mainly composed of a microcomputer, and performs calculations based on input data, pre-stored data, and calculation formulas. Then, the calculation results are output as control command signals to the accelerated cooling device 11 and the conveying device 4. Examples of data input to the ECU 19 include the surface temperatures of the steel sheet 7 measured by the thermometers 8, 9, and 12, the conveying speed of the steel sheet 7 in the rolling mills 5 and 6, and the conveying speed of the steel sheet 7 in the accelerated cooling device 11. Examples of control command signals output from the ECU 17 include a signal for controlling the number of upper header units 13 and 14 that spray cooling water onto the steel sheet 7 in the accelerated cooling device 11, a signal for controlling the number of lower header units 15 and 16, and a signal for controlling the conveying speed of the steel sheet 7 in the accelerated cooling device 11.

[0025] Here, the speed difference between the conveying speed of the steel plate 7 in the accelerated cooling device 11 and the conveying speed of the steel plate 7 coming out of the second rolling mill 6 and conveyed to the accelerated cooling device 11 will be described. The conveying speed of the steel plate 7 in the accelerated cooling device 11 is slower than the conveying speed of the steel plate 7 coming out of the second rolling mill 6 and conveyed to the accelerated cooling device 11. Therefore, the front end of the steel plate 7 in the length direction can enter the accelerated cooling device 11 while leaving the second rolling mill 6 and maintaining its temperature. However, the center and the tail end of the steel plate 7 in the length direction are exposed to the outside air on the conveying device 4 between the second rolling mill 6 and the accelerated cooling device 11 while the front end is being cooled in the accelerated cooling device 11, and wait in an air-cooled state. Therefore, the center and the tail end of the steel plate 7 enter the accelerated cooling device 11 in a state where the temperature is lower than that of the front end. Therefore, accelerated cooling is started at the center and the tail end of the steel plate 7 when their respective starting temperatures are lower than the starting temperature at the front end, which may result in material variations in the longitudinal direction of the steel plate 7. Therefore, in the embodiment of the present invention, in order to suppress material variations caused by the variation in the starting temperature in the longitudinal direction of the steel plate 7, the following control is executed.

[0026] FIG. 3 is a flow chart for explaining an example of control executed by the control device of the accelerated cooling device 11 according to the present invention. The control example shown in FIG. 3 is repeatedly executed by the ECU 19 at predetermined short intervals during operation of the thick steel plate production line 1. First, design conditions for a steel plate to be shipped as a product (hereinafter, referred to as a product steel plate) are input to the ECU 19, and a relationship between a start temperature and a stop temperature in the accelerated cooling device 11 for obtaining the product steel plate based on the design conditions is calculated (step S1). Examples of the design conditions mentioned above include the target chemical composition of the product steel plate, the target plate thickness, the target surface temperature of the steel plate 7 immediately after it leaves the second rolling mill 6, the tempering method, and the target tempering temperature. These values ​​are determined in advance as design values ​​of the product steel plate.

[0027] The above-mentioned relationship between the start temperature and the stop temperature is obtained, for example, by first acquiring a plurality of production results of steel sheets aiming at the same chemical composition, the same plate thickness, the same heating temperature, and the same rolling end temperature. From among these production results, for example, a production result with a nearly constant tensile test result is selected, and the start temperature and the stop temperature of the selected production result are obtained. Then, the relationship between the start temperature and the stop temperature thus obtained, that is, a calibration curve, is calculated. Alternatively, the relationship between the start temperature and the stop temperature may be obtained using a machine learning model such as deep learning.

[0028] Following or almost simultaneously with step S1, temperatures at at least two or more locations in the longitudinal direction of the steel plate 7 when it enters the accelerated cooling device 11 are acquired as start temperatures (step S2), and the start temperatures acquired in step S2 are input to the ECU 19. The above-mentioned step S2 corresponds to the temperature measurement step in this embodiment.

[0029] The time of entering the accelerated cooling device 11 means the time when the steel sheet 7 enters the accelerated cooling device 11 or immediately before that. In addition, at least two locations in the length direction of the steel sheet 7 means at least two different locations in the length direction of the steel sheet 7. More specifically, it means at least two locations of the leading end, the center, and the tail end in the length direction of the steel sheet 7. In the embodiment of the present invention, it is preferable to measure the temperatures at the above three locations by the third thermometer 12, and to use at least two or more of the measured values ​​as the start temperatures at the measurement locations of the temperatures. The above-mentioned start temperature may be an actual measurement value by the third thermometer 12. Alternatively, the start temperature may be an estimated value from the surface temperature of the steel sheet 7 measured by the second thermometer 9 immediately after leaving the second rolling mill 6. The estimated value can be calculated based on, for example, the outside air temperature, the distance between the second rolling mill 6 and the accelerated cooling device 11, the time from leaving the second rolling mill 6 to entering the accelerated cooling device 11, and the like.

[0030] Next, the stop temperatures corresponding to the measured or estimated values ​​of each start temperature acquired in step S2 are calculated (step S3). Specifically, in step S3 of FIG. 3, a calibration curve showing the relationship between the start temperature and the stop temperature calculated in step S1 is drawn, and the calibration curve is used to calculate the stop temperature corresponding to the start temperature acquired in step S2. The stop temperature calculated in this way is the target value of the stop temperature at the point where the above-mentioned start temperature is actually measured or estimated (hereinafter, referred to as the target stop temperature), and this is set in the accelerated cooling device 11. In the embodiment of the present invention, as shown in step S3 of FIG. 3, the start temperatures are lower in the order of the front end, the center, and the tail end of the steel plate 7, and the stop temperatures are lower in the order of the front end, the center, and the tail end. Note that the target stop temperature may be calculated for the entire steel plate, but from the viewpoint of reducing the calculation load, it is preferable to calculate it for the point where the temperature of the steel plate 7 is actually measured or estimated, as described above. The above target stop temperature corresponds to the target accelerated cooling stop temperature in the embodiment of the present invention.

[0031] Following step S3, accelerated cooling conditions (hereinafter simply referred to as cooling conditions) for cooling the front end of the steel sheet 7 from the start temperature to the target stop temperature are determined (step S4). Specifically, in step S4, the number of upper header units and the number of lower header units to be used for accelerated cooling of the front end are determined. The amount of cooling water sprayed from each header unit to the steel sheet 7 is almost constant. Therefore, for example, the amount of sprayed cooling water capable of lowering the temperature of the front end of the steel sheet 7 from the start temperature to the target stop temperature, that is, the number of each header unit, is determined. For example, a map or table that defines the relationship between the temperature difference between the start temperature and the stop temperature, and the number of upper header units and the number of lower header units can be prepared in advance, and the number of each header unit described above can be obtained using the map or table. Note that the number of upper header units and the number of lower header units provided in the accelerated cooling device 11 are determined by design. Therefore, the number of upper header units and the number of lower header units to be used for accelerated cooling of the front end are determined with the number of upper header units and the number of lower header units provided in the accelerated cooling device 11 as the upper limit.

[0032] Following step S4, or at approximately the same time, the conveying speed of the steel sheet 7 when the leading end of the steel sheet 7 is acceleratedly cooled by the accelerated cooling device 11 is determined (step S5). When the conveying speed of the leading end is determined in step S5, the time for the leading end to pass through the accelerated cooling device 11 is determined accordingly. This determines the cooling speed of the leading end. Note that the conveying speed of the leading end can be found by using a map or table that is prepared in advance and that defines the relationship between the temperature difference between the start temperature and the stop temperature, the number of upper header units and the number of lower header units, and the conveying speed of the steel sheet 7 in the accelerated cooling device 11, for example.

[0033] Following step S5, the conveying speeds suitable for obtaining the desired metal structure and strength at the center and tail of the steel plate 7 are determined as the cooling conditions for the center and tail of the steel plate 7 (step S6). This is because, as described above, the number of upper header units and the number of lower header units to be used in the accelerated cooling device 11 have already been determined. The conveying speeds of the center and tail of the steel plate 7 are determined, for example, by preparing a map or table in advance that defines the relationship between the temperature difference between the start temperature and the stop temperature, the number of upper header units and the number of lower header units, and the conveying speed of the steel plate 7 in the accelerated cooling device 11. The map or table can then be used to determine the conveying speeds. When the conveying speeds of the center and tail of the steel plate 7 are determined in this way, the time for the center and tail to pass through the accelerated cooling device 11 is determined accordingly. Based on this, the cooling speeds of the center and tail are determined. Note that the cooling speeds of the front, center, and tail of the steel plate 7 may differ from each other.

[0034] Following step S6, equipment constraints on the conveying speed are acquired (step S7). Here, the equipment constraints refer to the limit values ​​of the conveying speed caused by the accelerated cooling device 11. Specifically, the equipment constraints refer to the upper and lower limit values ​​of the conveying speed and the upper and lower limit values ​​of the acceleration determined in the design of the accelerated cooling device 11. Alternatively, in cases where the upper and lower limit values ​​of the conveying speed and the upper and lower limit values ​​of the acceleration are restricted due to maintenance or the like, the equipment constraints refer to those values. Such limit values ​​are stored as data in a storage unit (not shown), and the data is input to the ECU 19.

[0035] Following step S7, it is determined whether or not each of the conveying speeds determined in steps S5 and S6 is equal to or less than the limit value acquired in step S7 (step S8). If each of the conveying speeds exceeds the limit value, that is, if there are equipment constraints and each of the conveying speeds determined in steps S5 and S6 cannot be set, a negative determination is made in step S8 and the process proceeds to step S9. In step S9, the number of header units used for accelerated cooling of the steel sheet 7 in the accelerated cooling device 11 is changed. Thereafter, the process proceeds to step S5, and the previous control is executed.

[0036] On the other hand, if each conveying speed is equal to or lower than the limit value, an affirmative determination is made in step S8 and the process proceeds to step S10. In step S10, the number of header units determined in step S4 and each conveying speed determined in steps S5 and S6 are determined as cooling conditions for the steel sheet 7 to achieve the target stop temperature. The cooling conditions are then set in the accelerated cooling device 11, and the accelerated cooling device 11 is operated under the cooling conditions to accelerate cooling the steel sheet 7. Thereafter, the control shown in the flowchart of FIG. 3 is temporarily terminated. The above-mentioned steps S3 to S10 correspond to the accelerated cooling condition determination process of this embodiment.

[0037] In this manner, in the control device of the accelerated cooling device 11 according to the embodiment of the present invention, the surface temperature (start temperature) of the steel sheet 7 entering the accelerated cooling device 11 is actually measured or estimated at at least two or more points among the leading edge, center, and trailing edge of the steel sheet 7. Then, the stop temperature is set according to these start temperatures. Therefore, even if the variation in the start temperature is unavoidable, the stop temperature is set according to the start temperature, so that the accelerated cooling can be performed in substantially the same manner in each of the above-mentioned portions. As a result, the material variation in the length direction of the steel sheet 7 caused by the variation in the start temperature can be suppressed. This can improve the material uniformity of the accelerated cooled steel sheet 7 and the material stability during mass production of the steel sheet 7.

[0038] In this embodiment, the temperature is measured at three locations, the leading edge, the center, and the tail end of the steel plate 7. Alternatively, the temperature may be measured at at least two locations among the leading edge, the center, and the tail end of the steel plate 7. For example, the leading edge and the center, the leading edge and the tail end, or the center and the tail end of the steel plate 7 may be used. Even in these cases, the material variation in the length direction of the steel plate 7 caused by the variation in the starting temperature can be suppressed compared to the conventional case. That is, the same effects and advantages as those of the above-mentioned embodiment can be obtained. In addition, the amount of cooling water sprayed from each header unit of the accelerated cooling device 11 to the steel plate 7 may be configured to be changeable, and the amount of the cooling water may be included in the cooling conditions. EXAMPLES

[0039] Next, an example will be described that was carried out to confirm the action and effect of the control device of the accelerated cooling device 11 according to the embodiment of the present invention. In this example, a thick steel plate was produced using a thick steel plate production line similar to the thick steel plate production line shown in Fig. 1. That is, a slab having the chemical composition shown in Table 1 was produced by a continuous casting method.

[0040] [Table 1]

[0041] (Examples 1 to 10) After the above-mentioned slab was charged into the heating furnace, hot rolling was performed by the first rolling mill and the second rolling mill. Immediately after the end of rolling by the second rolling mill, the surface temperature of the center of the steel plate in the width direction of the steel plate was measured by the second thermometer. The steel plate was immediately transported to the front of the first leveler, and the surface temperature of the steel plate was measured in the length direction of the steel plate by the third thermometer. Specifically, while the steel plate was continuously introduced (transported) into the first leveler and the accelerated cooling device, the surface temperature of at least two points of the front, center, and tail of the steel plate in the length direction of the steel plate was measured by the third thermometer. These measured values ​​were used as the start temperature of the steel plate, and the cooling conditions of the steel plate were determined by performing the control shown in the flowchart in FIG. 3. That is, the stop temperature was changed according to the start temperature, as in the embodiment of the present invention described above. Then, the accelerated cooling device was operated under the cooling conditions to accelerate cooling the steel plate.

[0042] After the accelerated cooling, the steel sheet was sufficiently reheated and air-cooled for, for example, 50 seconds or more. Thereafter, the surface temperature of the steel sheet was measured with a fourth thermometer while the steel sheet was continuously advanced (conveyed) into a second leveller, and the steel sheet was further air-cooled.

[0043] (Examples 11 to 20) Steel plates were manufactured in the same manner as in Invention Examples 1 to 10, except that the surface temperature of the steel plate entering the accelerated cooling device was estimated using the surface temperature of the center of the steel plate in the width direction of the steel plate measured by the second thermometer.

[0044] (Examples 21 to 30) The steel plates were manufactured in the same manner as in Examples 1 to 10, except that the temperatures of the leading edge and trailing edge of the steel plate were measured, and the steel plates were tempered in an induction heating device after passing through a second leveler.

[0045] (Examples 31 to 40) Steel sheets were produced in the same manner as in Examples 11 to 20, except that after passing through the second leveller, tempering was carried out in an induction heating device.

[0046] (Examples 41 to 50) Steel sheets were produced in the same manner as in Examples 31 to 40, except that tempering was performed in a heating furnace instead of an induction heating device.

[0047] (Comparative Examples 1 to 10) Regardless of the starting temperature, the stop temperature was set to a predetermined temperature and the steel sheet was subjected to accelerated cooling in the accelerated cooling device. In addition, the steel sheet was tempered in an induction heating device installed immediately after the second leveler and then air-cooled. Other than that, the steel sheet was manufactured in the same manner as in Examples 1 to 10.

[0048] (Comparative Examples 11 to 20) The steel plates were produced in the same manner as in Comparative Examples 1 to 10, except that the cooling conditions were determined by the control shown in the flow chart in FIG. 3 only for the front end of the steel plate, and accelerated cooling was performed under those cooling conditions.

[0049] (Comparative Examples 21 to 30) Steel sheets were produced in the same manner as in Comparative Examples 1 to 10, except that after passing through the second leveller, tempering was carried out in an induction heating device.

[0050] (Comparative Examples 31 to 40) Steel sheets were produced in the same manner as in Comparative Examples 21 to 30, except that tempering was performed in a heating furnace instead of an induction heating device.

[0051] (Material evaluation) The material was evaluated by a tensile test. Tensile test specimens were taken from three locations: 250 mm from the leading edge of the steel plate, the center of the steel plate, and 250 mm from the trailing edge of the steel plate. At each location, the tensile test specimen was taken from the center in the width direction of the steel plate. The taking of the tensile test specimens and the tensile test were carried out in accordance with ASTM A370.

[0052] For each of the steel plates of Examples 1 to 50 and Comparative Examples 1 to 40, test pieces were taken from three positions in the length direction of the steel plate, and tensile tests were performed to determine the tensile strength as described above. The standard deviation of the tensile strengths was calculated, and a specimen that was 6 times the standard deviation and was 60 MPa or less was deemed to have passed, and any other specimens were deemed to have failed.

[0053] Table 2 lists the method of determining the stop temperature for each of invention examples 1 to 50 and comparative examples 1 to 40, the manufacturing conditions for each steel plate, and the tensile strength and the standard deviation of the tensile strength multiplied by six for each steel plate. For invention examples and comparative examples in which the stop temperature was determined by the control shown in the flow chart of Fig. 3, "Logic" is listed in the column for the method of determining the target accelerated cooling stop temperature in Table 2. The manufacturing conditions are the slab heating temperature, the final rolling temperature, i.e., the actual measured value of the second thermometer, the start temperature in the accelerated cooling device, the target stop temperature, the actual measured value of the stop temperature, i.e., the actual measured value of the fourth thermometer, the tempering method, and the tempering temperature.

[0054] [Table 2]

[0055] The accelerated cooling start temperature and accelerated cooling stop temperature at the front end listed in Table 2 are the maximum temperature values ​​at a position about 500 mm from the front end of the steel plate entering the accelerated cooling equipment. The accelerated cooling start temperature and accelerated cooling stop temperature at the center are the maximum temperature values ​​near the center in the longitudinal direction of the steel plate. The accelerated cooling start temperature and accelerated cooling stop temperature at the tail end are the maximum temperature values ​​at a position about 500 mm from the tail end in the longitudinal direction of the steel plate.

[0056] As shown in Table 2, inventive examples 1 to 50, the target performance is met. In contrast, comparative examples 1 to 40 do not meet the target performance.

[0057] 1. Thick steel plate production line 2 Furnace 3. Slab 4. Conveyor 5. First rolling mill 6. No. 2 rolling mill 7 Steel plate 8 1st thermometer 9 Second thermometer 10 First Leveler 11 Accelerated cooling device 12 Third thermometer 13 First upper header unit 14 2nd upper header unit 15 1st lower header unit 16 Second lower header unit 17 4th thermometer 18 2nd Leveller 19 Electronic Control Unit (ECU)

Claims

1. A control device for an accelerated cooling device that performs accelerated cooling on a steel plate being transported to reduce the temperature of the steel plate to a target accelerated cooling stop temperature, Based on the relationship between the accelerated cooling start temperature and the accelerated cooling stop temperature and the temperatures of the steel plate at at least two or more points in the conveying direction of the steel plate before the steel plate enters the accelerated cooling device, the target accelerated cooling stop temperature at a measurement point of the temperature of the steel plate and the accelerated cooling conditions in the accelerated cooling device at the measurement point for realizing the target accelerated cooling stop temperature are determined. Control device for accelerated cooling device.

2. The time before entering the accelerated cooling device refers to the time when the material enters the accelerated cooling device, The temperature of the steel plate is the surface temperature of the steel plate when it enters the accelerated cooling device. The control device for an accelerated cooling device according to claim 1 .

3. The temperature of the steel plate is at least one of an actual measured value of a surface temperature of the steel plate at the exit side of the hot rolling mill upstream of the accelerated cooling device in the transport direction and an estimated value estimated based on the actual measured value and a distance between the accelerated cooling device and the hot rolling mill in the transport direction. The control device for an accelerated cooling device according to claim 1 .

4. The temperature of the steel plate is at least one of an actual measured value of a surface temperature of the steel plate at the exit side of the hot rolling mill upstream of the accelerated cooling device in the transport direction and an estimated value estimated based on the actual measured value and a distance between the accelerated cooling device and the hot rolling mill in the transport direction. The control device for an accelerated cooling device according to claim 2.

5. The temperature of the steel plate at at least two points in the conveying direction of the steel plate is at least two points among the leading end, the center, and the trailing end of the steel plate in the conveying direction of the steel plate. The control device for an accelerated cooling device according to any one of claims 1 to 4.

6. The accelerated cooling device includes a plurality of cooling units that supply a cooling fluid to the steel plate, 5. The control device for an accelerated cooling device according to claim 1, wherein the accelerated cooling conditions include a transport speed of the steel plate in the accelerated cooling device and a number of the cooling units that supply the cooling fluid to the steel plate in the accelerated cooling device.

7. A control method for an accelerated cooling device that performs accelerated cooling on a steel plate being transported to reduce a temperature of the steel plate to a target accelerated cooling stop temperature, comprising: A temperature measuring step of determining the temperature of the steel plate at at least two or more points in the conveying direction of the steel plate before the steel plate enters the accelerated cooling device; and an accelerated cooling condition determination step of determining the target accelerated cooling stop temperature at the temperature measurement point of the steel plate and the accelerated cooling conditions in the accelerated cooling device at the temperature measurement point to realize the target accelerated cooling stop temperature, based on a relationship between an accelerated cooling start temperature and an accelerated cooling stop temperature and the temperature of the steel plate. A method for controlling an accelerated cooling device.

8. The steel plate is tempered immediately after the temperature of the steel plate is reduced to the accelerated cooling stop temperature, or after the temperature of the steel plate is reduced to the target accelerated cooling stop temperature and further air-cooled. A method for controlling an accelerated cooling device according to claim 7.

Citation Information

Patent Citations

  • Cooling control method

    JP1988144814A

  • Method and apparatus for heat-treating thick steel plate

    JP2002172411A

  • Method for producing thick steel plate

    JP2005154842A

  • Manufacturing specification determination support device and manufacturing specification determination support method for steel plate, computer program, and computer readable recording medium, and method for manufacturing steel plate

    JP2022014876A

  • Manufacture of steel plat under controlled cooling

    JP1993057330A