Greaseproof paper and method for producing the same
By adjusting the formation index of oil-resistant paper to 4.0 to 8.0 with a non-fluorine-based layer, the paper achieves both high oil resistance and good air permeability, addressing the limitations of non-fluorine-based agents.
Patent Information
- Application Number
- JP2023082025
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-18
- Publication Date
- 2024-11-28
AI Technical Summary
Non-fluorine-based oil resistance agents provide inferior oil resistance compared to fluorine-based agents, leading to thicker layers that compromise air permeability in oil-resistant paper.
Adjusting the formation index of oil-resistant paper to a range of 4.0 to 8.0, using a non-fluorine-based oil-resistant layer with specific pulp and coating methods, ensures both high oil resistance and good air permeability.
The oil-resistant paper achieves both high oil resistance and desirable air permeability, suitable for applications requiring breathability.
Smart Images

Figure 2024165659000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a paper having excellent oil resistance. In particular, the present invention relates to an oil-resistant paper that is required to have good breathability. For example, the oil-resistant paper of the present invention can be used as a packaging material for foods that contain oil, such as fast food, or as a packaging material filled with an oxygen agent to prevent oxidation of foods or medicines. [Background technology]
[0002] Conventionally, plastic films have been used as such packaging materials, for example, laminates of porous films made of polyester or nylon. However, there is a social demand to move away from plastics in consideration of the environment, and expectations are growing for paper packaging materials.
[0003] Greaseproof paper containing fluorine-based oil-proofing agents is known as a paper packaging material that also has oil resistance. However, it has been pointed out that fluorine-based oil-proofing agents may lead to environmental and health problems. For example, compounds containing fluorine are difficult to decompose in the environment and are thought to accumulate in ecosystems over a long period of time. In addition, some compounds containing fluorine are known to pose health risks to the human body. For this reason, a shift to non-fluorine-based oil-proofing agents is being promoted.
[0004] For example, Patent Document 1 proposes an invention in which a paper substrate is provided with an intermediate layer containing polyvinyl alcohol as a non-fluorinated oil-resistant agent and a surface layer containing a styrene-(meth)acrylic copolymer resin and a sizing agent. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent Publication No. 2022-85465 Summary of the Invention [Problem to be solved by the invention]
[0006] In general, non-fluorinated oil-proofing agents have inferior oil resistance compared to fluorinated oil-proofing agents. Therefore, in order to obtain a certain level of oil resistance using a non-fluorinated oil-proofing agent, it is necessary to apply a large amount of the non-fluorinated oil-proofing agent, which results in a thick oil-resistant layer. If the oil-resistant layer becomes thick, the breathability of the grease-resistant paper decreases, making it difficult to obtain the desired breathability.
[0007] In addition, oil resistance is required for grease-resistant paper.
[0008] An object of the present invention is to solve the above problems, specifically to provide a non-fluorine-based greaseproof paper that has both good breathability and high oil resistance. [Means for solving the problem]
[0009] Therefore, after extensive research, the inventors discovered that by adjusting the formation index of the grease-resistant paper to fall within a certain range, it is possible to provide a non-fluorine-based grease-resistant paper with good breathability and high oil resistance, and thus completed the present invention.
[0010] The present invention relates to an greaseproof paper in which a pulp-containing substrate is provided with a non-fluorine-based oil-resistant layer and has a formation index of 4.0 to 8.0.
[0011] The Oken air permeability is preferably 1400 seconds or less. Effect of the Invention
[0012] The grease-resistant paper of the present invention has good breathability and high oil resistance, and can therefore be suitably used as grease-resistant paper that requires breathability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The present invention is characterized in that the greaseproof paper has a pulp-containing substrate provided with a non-fluorine-based oil-resistant layer and has a formation index of 4.0 to 8.0.
[0014] The present invention will now be described.
[0015] (base material) The greaseproof paper of the present invention has a substrate containing pulp. The substrate is preferably a paper layer. The substrate may be a single layer or multiple layers.
[0016] Examples of pulp include wood pulps such as softwood bleached kraft pulp (NBKP), hardwood bleached kraft pulp (LBKP), softwood bleached sulfite pulp (NBSP), and thermomechanical pulp (TMP); non-wood pulps such as hemp, bamboo, straw, kenaf, mitsumata, kozo, and cotton; modified pulps such as cationic pulp and mercerized pulp; cellulose fibers or regenerated cellulose fibers derived from rayon, etc., and waste paper pulp obtained from waste paper. These can be used alone or in combination of two or more.
[0017] The type of pulp affects the formation of the resulting greaseproof paper, so it is advisable to select an appropriate type of pulp so that the formation index falls within the range specified in the present invention. For example, it is preferable to mix NPKP and LBKP in a mass ratio of 90:10 to 50:50, and more preferably 80:20 to 60:40.
[0018] The base material may contain other components besides pulp, such as synthetic fibers made of resins such as polyethylene, polypropylene, and polyethylene terephthalate; paper strength agents or fixing agents such as starch, polyacrylamide, and polyamine polyamide epichlorohydrin; sizing agents, fillers, retention aids, dyes, coloring pigments, fixing agents, defoamers, and slime control agents, and these may be used alone or in combination of two or more.
[0019] The method for producing the base material (papermaking) is not particularly limited, and the base material can be produced by a known production (papermaking) method using a known papermaking machine such as a Fourdrinier papermaking machine or a cylinder papermaking machine. It is preferable to add components other than the pulp to the pulp slurry.
[0020] The basis weight of the substrate is not particularly limited, but is preferably 20 g / m 2 ~200g / m 2 is preferred, and 25 g / m 2 ~120g / m 2 More preferably, 30 g / m 2 ~80g / m 2 is even more preferred, and 30 g / m 2 ~60g / m 2 In addition, the thickness of the substrate is not particularly limited, but is preferably from 30 μm to 180 μm, more preferably from 35 μm to 120 μm, and even more preferably from 40 μm to 80 μm.
[0021] The degree of beating of the pulp is not particularly limited, but as the beating of the pulp proceeds, the entanglement of the cellulose fibers increases and the fibers tend to become uniform, which is expected to improve the formation. Therefore, the degree of beating may be appropriately adjusted so that the formation index falls within the range of the present invention. The degree of beating is preferably more than 100 to 400 mLcsf, more preferably 150 to 300 mLcsf.
[0022] (Non-fluorinated oil-resistant layer) The grease-resistant paper of the present invention has at least one non-fluorine-based oil-resistant layer. The non-fluorine-based oil-resistant layer may be composed of a single layer or multiple layers. In addition, the oil-resistant layer of the present invention may be provided on one surface of the substrate, or on both sides of the substrate. In particular, it is preferable that the non-fluorine-based oil-resistant layer is provided on both sides of the substrate. When the non-fluorine-based oil-resistant layer is provided on one surface of the substrate, it is preferable that the non-fluorine-based oil-resistant layer is provided on the side that requires the oil-resistant effect. It is not necessary for the non-fluorine-based oil-resistant layer to form a complete "layer", and at least a part of the contact surface with the substrate surface may be mixed with the substrate. For example, a part of the non-fluorine-based oil-resistant layer may be included inside the substrate, and the interface between a part of the non-fluorine-based oil-resistant layer and the substrate may not be clear. However, it is preferable that the amount of the non-fluorine-based oil-resistant layer included inside the substrate is small, in other words, it is preferable that the amount of the non-fluorine-based oil-resistant layer present on the surface of the substrate is large. It is not necessary for the non-fluorine-based oil-resistant layer and the substrate to be in contact with each other, and another layer may be provided between them.
[0023] The non-fluorine-based oil-resistant layer is a layer containing an agent having at least oil resistance, and the content of the fluorine-based oil-resistant agent in the entire layer is 5% by mass or less. This content is preferably 3% by mass or less, more preferably 1% by mass or less, and even more preferably 0% by mass. There are no particular limitations on the fluorine-based oil-resistant agent, including known ones, and examples thereof include various compounds having a perfluoroalkyl group (polyfluoroalkyl group), other resins containing fluorine, etc.
[0024] Known components can be used as components constituting the non-fluorine-based oil-resistant layer. Examples include starch, styrene-acrylic copolymer resin, paraffin wax, polyvinyl alcohol, and acrylic resin emulsion, and these can be used alone or in combination of two or more. Examples of starch that can be used include modified starches such as corn starch, potato starch, tapioca starch, oxidized starch, starch phosphate, etherified starch, dialdehyde starch, and esterified starch. Modified starch is more preferred. Starch is preferably mixed with fatty acid, alkyl ketene dimer, alkenyl succinic anhydride, sodium sulfate, and acrylic resin, as appropriate, to improve oil resistance.
[0025] The non-fluorinated oil-resistant layer may contain various additives in addition to the oil-resistant agent, such as dispersants, wetting agents, water retention agents, defoaming agents, water-resistant agents, fluorescent dyes, coloring dyes, coloring pigments, surfactants, pH adjusters, cationic resins, anionic resins, ultraviolet absorbers, and metal salts.
[0026] The method of forming the non-fluorine-based oil-resistant layer (and, if necessary, the intermediate layer or additional layer) on the substrate is not particularly limited, and for example, it can be formed on the substrate by coating using a known coating device and coating system. The non-fluorine-based oil-resistant layer is preferably a coating layer. Examples of the coating device include a blade coater, a bar coater, an air knife coater, a curtain coater, a spray coater, a roll coater, a reverse roll coater, a size press coater, and a gate roll coater. Examples of the coating system include water-based coating using a solvent such as water, and solvent-based coating using a solvent such as an organic solvent. The viscosity, solid content, and the like of the composition for forming the non-fluorine-based oil-resistant layer (and, if necessary, the intermediate layer or additional layer), for example, the coating liquid, can be appropriately adjusted according to the coating device, coating system, and the like used. After coating, it is preferable to heat-dry. As a method of heating and drying, for example, a normal method such as a steam heater, a gas heater, an infrared heater, an electric heater, a hot air heater, a microwave, and a cylinder dryer is used.
[0027] The amount of the non-fluorinated oil-resistant layer may be designed in consideration of the balance between the oil resistance and breathability. In particular, the thicker the layer, the worse the breathability tends to be. For example, the amount of the non-fluorinated oil-resistant layer is 0.5 to 5.0 g / m 2 is preferable, and 1.0 to 4.5 g / m 2 More preferably, 1.2 to 4.2 g / m 2 is even more preferred.
[0028] (2) Formation index The greaseproof paper of the present invention has a formation index of 4.0 to 8.0. The lower limit of the formation index is preferably 4.1, more preferably 4.2. The upper limit of the formation index is preferably 7.8, more preferably 7.6, more preferably 7.0, and even more preferably 5.0.
[0029] By setting the formation index of the grease-resistant paper within the above-mentioned specified range, it is possible to obtain the desired breathability while ensuring a certain level of oil resistance by providing a non-fluorine-based oil-resistant layer. When the formation index is high, breathability tends to be obtained but oil resistance is poor. In this case, it is possible to increase the amount of the non-fluorine-based oil-resistant layer in order to improve the oil resistance, but this will result in a corresponding decrease in breathability. On the other hand, if the formation index is too low, the quality (physical properties of paper including air permeability and oil resistance) of the grease-resistant paper as a whole will vary greatly, and there is a high risk of the strength of the paper decreasing and the quality decreasing during printing.
[0030] The formation index is measured by using a point light source drum scan type optical transmission meter to convert the light intensity fluctuations in the amount of transmitted light into numerical values and evaluate it. The measurement is performed using the "3D Sheet Analyzer" manufactured by M / K Systems. In this measurement, the light source intensity is automatically calibrated according to the thickness of the paper, and it is known that the evaluation can be performed regardless of differences in basis weight, etc. The higher the formation index value, the better the formation. For the measurement, greaseproof paper is used as A4 size and wrapped around the device so that the paper does not float. Then, the transmitted light formation index is measured with a measurement range of 1 (standard sensitivity) and a light source aperture of 0.5 mm. The specific calculation of the formation index is as follows, with the peak class P being 32. The measurement area is 10 cm x 10 cm. A = P / (N 100) A: Formation index P: Number of peaks (number of transmitted light intensity classes) N: The number of classes in which 0.1% or more of pixels are distributed + the number of the class with the largest number of counts less than 0.1%, rounded to the nearest tenths place
[0031] In order to design the formation index of the grease-resistant paper to be within the above range, a known method can be adopted. That is, it is possible to appropriately adjust the selection of pulp and papermaking conditions, etc. Specifically, the mixing ratio of softwood pulp and hardwood pulp, the selection of tree species, the degree of beating, the papermaking speed during papermaking, the suction conditions, the jet wire ratio of the wire part, the adjustment of the wire shaker, the tension, the use of a dandy roll, the press pressure, the drying conditions, the coating conditions of the non-fluorine-based oil-resistant layer, etc. may be appropriately adjusted.
[0032] The greaseproof paper of the present invention is also breathable. As an index of breathability, the Oken air permeability measured in accordance with JIS P8117:2009 is preferably 1400 seconds or less, more preferably 1000 seconds or less, even more preferably 800 seconds or less, even more preferably 600 seconds or less, even more preferably 400 seconds or less, and even more preferably 200 seconds or less. The lower the Oken air permeability value, the better the breathability.
[0033] The oil-resistant paper of the present invention preferably has an oil resistance of 2 or more, more preferably 2.5 or more, even more preferably 3 or more, and still more preferably 4 or more, as measured by a kit method in accordance with TAPPI UM-557 as its oil resistance performance. [Industrial Applicability]
[0034] The greaseproof paper of the present invention can be suitably used in applications requiring grease resistance. It is particularly suitable for use as greaseproof paper that requires breathability, and can be used, for example, as a packaging material for foods that contain oil, such as fast food, or as a packaging material filled with an oxygen agent to prevent oxidation of foods or medicines.
[0035] The grease-resistant paper obtained by the present invention has a non-fluorine-based grease-resistant layer, and therefore can be used without causing various problems caused by fluorine.
[0036] Since the greaseproof paper of the present invention is made of pulp, which is a carbon-neutral material, it has a small environmental impact and can suppress the overall increase in the amount of carbon dioxide in the atmosphere even when incinerated. EXAMPLES
[0037] The present invention will be described in more detail below using examples and comparative examples, but the scope of the present invention is not limited to the examples.
[0038] (Non-fluorinated oil-resistant fluid) Hydrophobized starch (Filmkote 370, manufactured by Ingredion) and Glauber's salt were mixed with water to give concentrations of 7.2% by mass and 0.2% by mass, respectively, to prepare a non-fluorinated oil-resistant liquid.
[0039] Example 1 A mixture of 67 parts by mass of bleached softwood kraft pulp and 33 parts by mass of bleached hardwood kraft pulp was disintegrated to prepare a pulp slurry with a beating degree of 270 mlc.sf. To the pulp slurry, 1.3 parts by mass of kaolin (manufactured by Shiraishi Calcium Co., Ltd., product name "Kaobrite"), 0.3 parts by mass of polyamide-epichlorohydrin resin (manufactured by Seiko PMC Co., Ltd., product name "WS4024"), and 4.0 parts by mass of aluminum sulfate were added per 100 parts by mass of pulp solids to prepare a papermaking stock. When making paper using this papermaking stock on a Fourdrinier papermaking machine, the non-fluorinated oil-resistant liquid was applied at a solid content of 3.6 g / m using a size press coater. 2 This resulted in a 40g / m2 sheet with a non-fluorine-based oil-resistant layer. 2 As a result, greaseproof paper of
[0040] Example 2 Non-fluorinated oil-resistant liquid with a solid content of 3.0 g / m 2 Except for the above change, the same procedure as in Example 1 was followed to obtain an grease-resistant paper having a non-fluorine-based oil-resistant layer.
[0041] Example 3 A mixture of 67 parts by mass of bleached softwood kraft pulp and 33 parts by mass of bleached hardwood kraft pulp was disintegrated to prepare a pulp slurry with a beating degree of 200 mlc.sf. To the pulp slurry, 1.3 parts by mass of kaolin (Shiraishi Calcium Co., Ltd., product name "Kaobrite"), 0.3 parts by mass of polyamide-epichlorohydrin resin (Seiko PMC Co., Ltd., product name "WS4024"), and 4.0 parts by mass of aluminum sulfate were added per 100 parts by mass of pulp solids to prepare a papermaking stock. When this papermaking stock was used to make paper on a Fourdrinier papermaking machine, a dandy roll was installed at the wet end so that the wet paper would pass through, and the non-fluorinated oil-resistant liquid was applied to the paper at a solid content of 1.5 g / m using a size press coater. 2 This resulted in a 40g / m2 sheet with a non-fluorine-based oil-resistant layer. 2 As a result, greaseproof paper of
[0042] Example 4 Non-fluorinated oil-resistant liquid with solid content of 3.6 g / m 2 An oil-resistant paper having a non-fluorine-based oil-resistant layer was obtained in the same manner as in Example 3, except that the oil-resistant layer was provided so as to be as shown in FIG.
[0043] Comparative Example 1 Paper not having a non-fluorine-based oil-resistant layer was obtained in the same manner as in Example 1, except that the non-fluorine-based oil-resistant liquid was not applied and dried.
[0044] Comparative Example 2 The pulp used was a mixture of 19 parts by mass of softwood bleached kraft pulp and 81 parts by mass of hardwood bleached kraft pulp. The beating degree was 430 mlc.sf, and the non-fluorinated oil-resistant liquid was 6.0 g / m2 in solid content. 2 An oil-resistant paper having a non-fluorine-based oil-resistant layer was obtained in the same manner as in Example 1, except that the coating and drying were performed so that the above-mentioned
[0045] Comparative Example 3 An oil-resistant paper having a non-fluorine-based oil-resistant layer was obtained in the same manner as in Example 1, except that a mixture of 19 parts by mass of softwood bleached kraft pulp and 81 parts by mass of hardwood bleached kraft pulp was used as the pulp.
[0046] Comparative Example 4 An grease-resistant paper having a non-fluorine-based oil-resistant layer was obtained in the same manner as in Example 1, except that 100 parts by mass of softwood bleached kraft pulp was used as the pulp and the beating degree was 200 mlc.sf.
[0047] Comparative Example 5 The beating degree was set to 100 mlc.sf, and a dandy roll was installed to process the wet paper. A non-fluorine-based oil-resistant liquid was applied to the wet paper at a solid content of 0.7 g / m 2 An oil-resistant paper having a non-fluorine-based oil-resistant layer was obtained in the same manner as in Example 1, except that the coating and drying were performed so that the above-mentioned
[0048] Comparative Example 6 Non-fluorinated oil-resistant liquid with solid content of 3.6 g / m 2 An oil-resistant paper having a non-fluorine-based oil-resistant layer was obtained in the same manner as in Comparative Example 5, except that the coating and drying were performed so that the above-mentioned
[0049] The formation index, air permeability, and oil resistance of each of the greaseproof papers of the Examples and Comparative Examples were measured. The methods for measuring each property were as follows.
[0050] Formation index: Measured using a "3D Sheet Analyzer" manufactured by M / K Systems. Air permeability: Evaluated by Oken air permeability measured in accordance with JIS P8117:2009. Oil resistance: Evaluated by the oil resistance kit method measured in accordance with TAPPI UM-557.
[0051] The results are shown in Table 1 below.
[0052] [Table 1]
[0053] The air permeability and oil resistance of the grease-resistant papers obtained in Examples 1 to 4 and Comparative Examples 1 to 6 were confirmed. Comparative Example 1 did not have a non-fluorine-based oil-resistant layer, so it had good air permeability but no oil resistance. The grease-resistant papers of Comparative Examples 2 and 3 had a high formation index and good air permeability, but no oil resistance was obtained. The grease-resistant paper of Comparative Example 4, which had a low formation index, had good oil resistance but poor air permeability. The grease-resistant paper of Comparative Example 5 had a high formation index and good air permeability, but no oil resistance was obtained. Comparative Example 6, in which the amount of the oil-resistant layer was increased compared to Comparative Example 5, had oil resistance but poor air permeability. On the other hand, the grease-resistant papers of Examples 1 to 4 had both air permeability and oil resistance.
Claims
1. The grease-resistant paper has a pulp-containing substrate provided with a non-fluorine-based oil-resistant layer and has a formation index of 4.0 to 8.
0.
2. 2. The greaseproof paper according to claim 1, having an Oken air permeability of 1,400 seconds or less.
Citation Information
Patent Citations
Oil resistant paper
JP2022085465A
Cited By
Laminate, and packaging paper, packaging bag, and packaging body made of the laminate
JP7829092B1