Rubber composition and tire

By adding an aromatic phosphate ester metal salt as a nucleating agent to hydrogenated diene rubber compositions, the strength and wear resistance are enhanced through promoted elongation crystallization, addressing the limitations of existing rubber compositions.

JP2024165733APending Publication Date: 2024-11-28TOYO TIRE CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023082198
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-18
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Existing rubber compositions, particularly those containing hydrogenated diene rubbers, lack sufficient strength and wear resistance, despite the potential for hydrogenated styrene-butadiene rubber to exhibit high strength due to unknown mechanisms, and synthetic diene rubbers do not achieve the same level of elongation crystallization as natural rubber.

Method used

Incorporating an aromatic phosphate ester metal salt as a nucleating agent into hydrogenated diene rubber compositions to promote elongation crystallization, thereby enhancing the strength and wear resistance of the rubber.

Benefits of technology

The addition of the nucleating agent leads to improved tensile strength and wear resistance through enhanced elongation crystallization, particularly in hydrogenated styrene-butadiene and acrylonitrile-butadiene rubbers, resulting in higher tensile products and increased durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024165733000001
    Figure 2024165733000001
  • Figure 2024165733000002
    Figure 2024165733000002
  • Figure 2024165733000003
    Figure 2024165733000003
Patent Text Reader

Abstract

To enhance the strength of a rubber composition containing a hydrogenated diene rubber.SOLUTION: A rubber composition according to one embodiment contains a rubber component containing a hydrogenated diene rubber, and a nucleating agent containing an aromatic phosphate metal salt. Relative to 100 pts.mass of the hydrogenated diene rubber, the amount of the nucleating agent is 0.05-10 pts.mass. The hydrogenated diene rubber is preferably a hydrogenated styrene-butadiene rubber and / or a hydrogenated acrylonitrile butadiene rubber. The rubber composition may further contain 10-200 pts.mass of a filler relative to 100 pts.mass of the rubber component.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a rubber composition and a tire using the same. [Background technology]

[0002] Recently, there has been a demand for longer life for rubber products such as tires from the perspective of sustainability, etc. To extend the life of tires, improved abrasion resistance is required, which in turn requires a rubber composition with high strength, i.e., high tensile product.

[0003] Hydrogenated styrene-butadiene rubber has higher strength than non-hydrogenated styrene-butadiene rubber, and it has been reported that this is due to non-uniform crosslinking (see

[0087] of Patent Document 1). However, many aspects of the mechanism by which hydrogenated styrene-butadiene rubber has high strength remain unclear, and there is still room for improvement in terms of increasing strength.

[0004] It is known that natural rubber exhibits high strength properties due to strain-induced crystallization. In contrast, synthetic diene rubber does not exhibit strain-induced crystallization to the same extent as natural rubber. Therefore, it has been proposed to compound a nucleating agent in order to promote the crystallization of synthetic diene rubber and increase its strength.

[0005] For example, Patent Document 2 discloses blending paraffins or higher saturated fatty acids as a crystal nucleating agent and low molecular weight diene polymers or fatty acid esters as a plasticizer into diene rubber. Patent Document 3 discloses blending dimetal tetracarboxylates as a nucleating agent into diene rubber to promote strain-induced crystallization.

[0006] On the other hand, it is known to add a nucleating agent to a resin material. In the case of a resin material, after processing in a molten state, it is necessary to cool it when demolding, and adding a nucleating agent can increase the demolding temperature and improve productivity. In this way, the nucleating agent in a resin material is useful for generating uniform and fine crystals by promoting nucleation in the polymer crystallization process, and its purpose is significantly different from that of a rubber material. For example, Patent Document 4 discloses that a nucleating agent containing an aromatic phosphate metal salt is added to an olefin resin, thereby increasing the crystallization speed of the olefin resin and improving its properties. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2021-138967 A [Patent Document 2] Japanese Patent Application Publication No. 9-31248 [Patent Document 3] Special Publication No. 2017-537176 [Patent Document 4] International Publication No. 2020 / 153343 [Non-patent literature]

[0008] [Non-Patent Document 1] Ryuichi Takagi et al., "ESR Information during Elongation Deformation of Vulcanized Rubber Materials," Journal of the Society of Rubber Science and Technology, Vol. 83, No. 10, pp. 311-317, 2010 Summary of the Invention [Problem to be solved by the invention]

[0009] The present inventors hypothesized that the high strength of hydrogenated diene rubbers such as hydrogenated styrene butadiene rubber is due to strain-induced crystallization, and believed that by applying a nucleating agent that has conventionally been used in olefin resins to hydrogenated diene rubbers, it might be possible to increase strength through strain-induced crystallization.

[0010] Incidentally, Non-Patent Document 1 discloses that hydrogenated acrylonitrile butadiene rubber is strengthened by strain-induced crystallization, but does not disclose the use of an aromatic phosphate metal salt as a nucleating agent for promoting the strain-induced crystallization.

[0011] In view of the above, an object of an embodiment of the present invention is to increase the strength of a rubber composition containing a hydrogenated diene rubber. [Means for solving the problem]

[0012] The present inventors have discovered that by adding an aromatic phosphate metal salt as a nucleating agent to a hydrogenated diene rubber, the strain-induced crystallization of the hydrogenated diene rubber is promoted, and a high-strength rubber composition can be obtained.

[0013] The present invention includes the embodiments set forth below. [1] A rubber composition comprising a rubber component containing a hydrogenated diene rubber and a nucleating agent containing an aromatic phosphate metal salt, wherein the amount of the nucleating agent per 100 parts by mass of the hydrogenated diene rubber is 0.05 to 10 parts by mass. [2] The rubber composition according to [1], wherein the hydrogenated diene rubber is a hydrogenated styrene butadiene rubber and / or a hydrogenated acrylonitrile butadiene rubber. [3] The rubber composition according to [1] or [2], wherein the hydrogenated diene rubber has a hydrogenation rate of 70 to 99 mol %. [4] The rubber composition according to any one of [1] to [3], further comprising a filler, the amount of the filler being 10 to 200 parts by mass per 100 parts by mass of the rubber component. [5] A tire produced using the rubber composition according to any one of [1] to [4]. Effect of the Invention

[0014] According to an embodiment of the present invention, the strength of a rubber composition containing a hydrogenated diene rubber can be increased by adding a nucleating agent containing an aromatic phosphate metal salt. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The rubber composition according to the embodiment includes a rubber component including a hydrogenated diene-based rubber, and a nucleating agent including an aromatic phosphate metal salt.

[0016] Hydrogenated diene rubber is a diene rubber that has been hydrogenated (hydrogenated). Here, diene rubber refers to rubber that has a repeating unit corresponding to a diene monomer that has a conjugated double bond, and examples of such rubber include natural rubber (NR), synthetic isoprene rubber (IR), butadiene rubber (BR), styrene butadiene rubber (SBR), and acrylonitrile butadiene rubber (NBR).

[0017] The hydrogenated diene rubber is preferably a diene rubber containing 1,3-butadiene as a constituent monomer, and more preferably a copolymer rubber of 1,3-butadiene and a vinyl compound. The copolymer rubber is preferably a random copolymer of 1,3-butadiene and a vinyl compound. Specifically, the hydrogenated diene rubber is preferably hydrogenated SBR obtained by hydrogenating styrene-butadiene rubber, or hydrogenated NBR obtained by hydrogenating acrylonitrile-butadiene rubber, and hydrogenated SBR and hydrogenated NBR may be used in combination.

[0018] The hydrogenation rate of the hydrogenated diene rubber is preferably 70 to 99 mol%, more preferably 80 to 98 mol%, and may be 85 to 95 mol%. The hydrogenation rate of the hydrogenated diene rubber is the hydrogenation rate relative to the conjugated diene part (structural unit derived from a conjugated diene monomer), and is the molar ratio of the hydrogenated conjugated diene part when the entire conjugated diene part before hydrogenation is taken as 100 mol%. For example, in the case of a hydrogenated diene rubber obtained by hydrogenating a copolymer rubber of 1,3-butadiene and a vinyl compound, the hydrogenation rate is the molar ratio of the hydrogenated butadiene part when the entire butadiene part (structural unit derived from 1,3-butadiene) is taken as 100 mol%.

[0019] When the hydrogenated diene rubber is a copolymer rubber of a conjugated diene monomer and a vinyl compound, the amount of the conjugated diene portion (a structural unit derived from a conjugated diene monomer) is not particularly limited. The amount of the conjugated diene portion may be, for example, 50 to 95% by mass, 55 to 90% by mass, or 60 to 85% by mass.

[0020] For hydrogenated SBR, the bound styrene content is not particularly limited and may be, for example, 5 to 40% by mass or 10 to 30% by mass. In this case, the amount of butadiene part may be, for example, 60 to 95% by mass or 70 to 90% by mass.

[0021] For hydrogenated NBR, the bound acrylonitrile content is not particularly limited and may be, for example, 15 to 50 mass%, 25 to 45 mass%, or 30 to 40 mass%. In this case, the amount of butadiene part may be, for example, 50 to 85 mass%, 55 to 75 mass%, or 60 to 70 mass%.

[0022] The weight average molecular weight (Mw) of the hydrogenated diene rubber is not particularly limited, and may be, for example, from 200,000 to 2,000,000, or from 300,000 to 1,000,000.

[0023] The rubber component contains the hydrogenated diene rubber, and may contain only the hydrogenated diene rubber, or may contain other diene rubbers together with the hydrogenated diene rubber. The content of the hydrogenated diene rubber in the rubber component is preferably 50 to 100 mass%, more preferably 70 to 100 mass%, and further preferably 80 to 100 mass%, and may be 100 mass%.

[0024] Other diene rubbers that may be used in combination with the hydrogenated diene rubber include non-hydrogenated diene rubbers, such as natural rubber (NR), synthetic isoprene rubber (IR), butadiene rubber (BR), styrene butadiene rubber (SBR), acrylonitrile butadiene rubber (NBR), etc. These other diene rubbers may be used alone or in combination of two or more.

[0025] In this embodiment, an aromatic phosphate metal salt is used as a nucleating agent to be added to the hydrogenated diene rubber. As described above, the aromatic phosphate metal salt is known as a nucleating agent that improves the crystallization rate of olefin resins, but in this embodiment, it is used to promote the stretch crystallization of the hydrogenated diene rubber. In this embodiment, the nucleating agent is a drug that promotes the stretch crystallization of the hydrogenated diene rubber, and is also called a crystal nucleating agent. The stretch crystallization refers to the phase change of an amorphous material when stretched and deformed to approach a crystalline state.

[0026] The aromatic phosphate metal salt is preferably a compound represented by the following general formula (1). [ka] In formula (1), R 1 ~R 4 each independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms; R 5 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, n represents 1 or 2, when n is 1, M represents an alkali metal atom or dihydroxyaluminum, and when n is 2, M represents an alkaline earth metal atom or hydroxyaluminum.

[0027] R 1 ~R 4 Examples of the alkyl group having 1 to 6 carbon atoms represented by the formula (I) include methyl, ethyl, propyl, isopropyl, butyl, sec-butyl, tert-butyl, isobutyl, amyl, isoamyl, tert-amyl, hexyl, 2-hexyl, and 3-hexyl. 1 ~R 4 is preferably tert-butyl or isopropyl.

[0028] R 5 Examples of the alkyl group having 1 to 3 carbon atoms represented by the formula (I) include methyl, ethyl, propyl, and isopropyl. 5 is preferably a hydrogen atom or methyl.

[0029] Examples of the alkali metal atom represented by M include lithium, sodium, and potassium. Examples of the alkaline earth metal atom include magnesium and calcium. M is preferably an alkali metal atom or hydroxyaluminum, and more preferably lithium, sodium, or hydroxyaluminum.

[0030] Specific examples of the aromatic phosphate metal salt represented by the general formula (1) include sodium-2,2'-methylenebis(4,6-di-tert-butylphenyl)phosphate, sodium-2,2'-ethylidenebis(4,6-di-tert-butylphenyl)phosphate, sodium-2,2'-methylenebis(4,6-diisopropylphenyl)phosphate, lithium-2,2'-methylenebis(4,6-di-tert-butylphenyl)phosphate, and lithium-2,2'-ethylidenebis(4,6-di-tert-butylphenyl)phosphate. , lithium-2,2'-methylenebis(4,6-diisopropylphenyl)phosphate, lithium-2,2'-methylenebis(4-methyl-6-tert-butylphenyl)phosphate, hydroxyaluminum bis[2,2'-methylenebis(4,6-di-tert-butylphenyl)phosphate], hydroxyaluminum bis[2,2'-methylenebis(4,6-diisopropylphenyl)phosphate], hydroxyaluminum bis[2,2'-ethylidenebis(4,6-di-tert-butylphenyl)phosphate]. These may be used alone or in combination of two or more.

[0031] The nucleating agent may be an aromatic phosphate metal salt alone, or may contain, together with the aromatic phosphate metal salt, other compounds such as, for example, fatty acid alkali metal salts. The content of the aromatic phosphate metal salt in the nucleating agent is not particularly limited, but is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 95% by mass or more, and may be 100% by mass.

[0032] The amount of the nucleating agent in the rubber composition is preferably 0.05 to 10 parts by mass relative to 100 parts by mass of the hydrogenated diene rubber. By using an amount of the nucleating agent of 0.05 parts by mass or more, the elongation crystallization of the hydrogenated diene rubber is promoted, and the strength of the rubber composition can be increased. The amount of the nucleating agent is preferably 0.1 to 8 parts by mass, more preferably 0.5 to 5 parts by mass, and further preferably 1 to 5 parts by mass.

[0033] The rubber composition according to the present embodiment may contain a filler. As the filler, carbon black and / or silica are preferable.

[0034] The carbon black is not particularly limited, and various known types can be used.Specific examples include SAF grade (N100 series), ISAF grade (N200 series), HAF grade (N300 series), FEF grade (N500 series), GPF grade (N600 series) (all ASTM grades), etc.These grades of carbon black can be used alone or in combination of two or more types.

[0035] The silica is not particularly limited, and examples thereof include wet silica, dry silica, etc. It is preferable to use wet silica such as wet precipitation silica and wet gelation silica.

[0036] The amount of the filler is preferably 10 to 200 parts by mass per 100 parts by mass of the rubber component, and can be appropriately set depending on the application, etc. The amount of the filler is more preferably 40 to 150 parts by mass per 100 parts by mass of the rubber component.

[0037] In one embodiment, the filler may be predominantly carbon black, i.e., the amount of carbon black relative to the total weight of the filler may be greater than 50%, greater than 70%, or even 100% by weight.

[0038] In one embodiment, the filler may be predominantly silica, i.e., the amount of silica based on the total weight of the filler may be greater than 50%, 60% or more, 70% or more, or even 100% by weight.

[0039] When silica is blended as a filler, the rubber composition preferably further contains a silane coupling agent. Examples of the silane coupling agent include sulfide silane coupling agents such as bis(3-triethoxysilylpropyl)tetrasulfide, bis(3-triethoxysilylpropyl)disulfide, bis(2-triethoxysilylethyl)tetrasulfide, bis(4-triethoxysilylbutyl)disulfide, bis(3-trimethoxysilylpropyl)tetrasulfide, and bis(2-trimethoxysilylethyl)disulfide, and mercaptosilane coupling agents such as 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropyldimethylmethoxysilane, and mercaptoethyltriethoxysilane. These can be used alone or in combination of two or more. The amount of the silane coupling agent is preferably 5 to 20 parts by mass, and more preferably 5 to 15 parts by mass, based on 100 parts by mass of silica.

[0040] In addition to the above components, the rubber composition according to this embodiment may contain various additives that are generally used in rubber compositions, such as zinc oxide, stearic acid, an antioxidant, wax, oil, a vulcanizing agent, and a vulcanization accelerator.

[0041] The content of zinc oxide is not particularly limited, and may be, for example, 0 to 10 parts by mass, 0.5 to 5 parts by mass, or 1 to 4 parts by mass relative to 100 parts by mass of the rubber component.

[0042] The content of stearic acid is not particularly limited, and may be, for example, 0 to 10 parts by mass, 0.5 to 5 parts by mass, or 1 to 4 parts by mass relative to 100 parts by mass of the rubber component.

[0043] As the vulcanizing agent, sulfur is preferably used. The content of the vulcanizing agent is not particularly limited, but may be 0.1 to 10 parts by mass, 0.5 to 5 parts by mass, or 1 to 3 parts by mass, based on 100 parts by mass of the rubber component.

[0044] Examples of the vulcanization accelerator include various vulcanization accelerators such as sulfenamide-based, guanidine-based, dithiocarbamate-based, thiuram-based, and thiazole-based, and any one of them can be used alone or in combination of two or more. The content of the vulcanization accelerator is not particularly limited, but is preferably 0.1 to 7 parts by mass, more preferably 0.5 to 5 parts by mass, and may be 1 to 3 parts by mass, relative to 100 parts by mass of the rubber component.

[0045] The rubber composition according to the present embodiment can be prepared by kneading in a conventional manner using a commonly used mixer such as a Banbury mixer, kneader, or roll. That is, for example, in the first mixing stage (non-pro kneading process), additives other than the vulcanizing agent and vulcanization accelerator are added and mixed with the rubber component together with the nucleating agent and filler. Next, in the final mixing stage (pro kneading process), the vulcanizing agent and vulcanization accelerator are added and mixed to the obtained mixture. This allows the preparation of an unvulcanized rubber composition.

[0046] The rubber composition according to the present embodiment can be used for various rubber members such as tires, anti-vibration rubber, conveyor belts, etc. It is preferably for tires, and can be applied to various parts of tires such as treads, sidewalls, and beads of pneumatic tires of various sizes for various purposes such as tires for passenger cars and large tires for trucks and buses.

[0047] In one embodiment, a tire including a rubber portion (e.g., tread rubber, sidewall rubber, etc.) made of the rubber composition is manufactured as follows. The rubber composition is molded into a predetermined shape by a conventional method, for example, extrusion processing. The obtained molded product is combined with other parts to produce a green tire. The green tire is vulcanized and molded at, for example, 140 to 180°C to produce a pneumatic tire.

[0048] The rubber composition according to the present embodiment can improve the strength (tensile product) by elongation crystallization, and therefore can improve the abrasion resistance. Therefore, in one embodiment, it is preferably used as a rubber composition constituting a tire tread. That is, the tire according to one embodiment is a tire having a tread made by using the above rubber composition. EXAMPLES

[0049] Examples will be shown below, but the present invention is not limited to these examples.

[0050] The components used in the examples and comparative examples are as follows. Hydrogenated NBR-1: Zeon Corporation's "Zetpol 2010L" (bound acrylonitrile content: 36.2% by mass, hydrogenation rate of butadiene part: 98% by mole) Hydrogenated NBR-2: Zeon Corporation's "Zetpol 2020L" (bound acrylonitrile content: 36.2% by mass, hydrogenation rate of butadiene part: 92% by mole) Hydrogenated NBR-3: Zetpol 2030L manufactured by Zeon Corporation (bound acrylonitrile content: 36.2% by mass, hydrogenation rate of butadiene part: 80% by mole)

[0051] Hydrogenated SBR: Hydrogenated styrene butadiene rubber prepared according to Synthesis Example 1 below (Mw: 350,000, bound styrene content: 20% by mass, hydrogenation rate of butadiene part: 90 mol%) [Synthesis Example 1] In a nitrogen-substituted heat-resistant reaction vessel, 2.5 L of cyclohexane, 50 g of tetrahydrofuran (THF), 0.12 g of n-butyl lithium, 100 g of styrene, and 400 g of 1,3-butadiene were placed and polymerization was carried out at a reaction temperature of 50°C. After the polymerization was completed, 1.7 g of N,N-bis(trimethylsilyl)aminopropylmethyldiethoxylane was added and reacted for 1 hour, and then hydrogen gas was supplied at a pressure of 0.4 MPa-gauge and stirred for 20 minutes. Next, the hydrogen gas supply pressure was set to 0.7 MPa-gauge and the reaction temperature was set to 90°C, and the reaction was carried out using a catalyst mainly composed of titanocene dichloride until the desired hydrogenation rate was reached, and the solvent was removed to obtain hydrogenated SBR.

[0052] SBR: Styrene butadiene rubber, "HPR350" manufactured by ENEOS Materials Co., Ltd. Carbon black: "Seat KH (N339)" manufactured by Tokai Carbon Co., Ltd. Silica: "Nipsil AQ" manufactured by Tosoh Silica Corporation Silane coupling agent: "Si75" manufactured by Evonik Japan Co., Ltd.

[0053] Nucleating agent A: ADEKA Corporation's "ADEKA STAB NA-21" (main component: hydroxyaluminum bis[2,2'-methylenebis(4,6-di-tert-butylphenyl)phosphate] (R 1 ~R 4 =t-Bu, R 5 = H, M = Al-OH, n = 2)

[0054] Nucleating agent B: ADEKA Corporation's "ADEKA STAB NA-27" (aromatic phosphate ester metal salt compound)

[0055] Nucleating agent C: ADEKA Corporation's "ADEKA STAB NA-11" (sodium 2,2'-methylenebis(4,6-di-tert-butylphenyl) phosphate (R 1 ~R 4 =t-Bu, R 5 =H, M=Na, n=1)

[0056] Nucleating agent D: ADEKA Corporation's "ADEKA STAB NA-71" (lithium-2,2'-methylenebis(4,6-di-tert-butylphenyl)phosphate (R 1 ~R 4 =t-Bu, R 5 = H, M = Li, n = 1) and a mixture of fatty acid alkali metal salts)

[0057] Zinc oxide: "Zinc oxide No. 3" manufactured by Mitsui Mining & Smelting Co., Ltd. Stearic acid: Kao Corporation's "Lunac S-20" Sulfur: "Powdered sulfur" manufactured by Tsurumi Chemical Industry Co., Ltd. Vulcanization accelerator 1: "Soxinol CZ" manufactured by Sumitomo Chemical Co., Ltd. Vulcanization accelerator 2: "Noccera-D" manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Vulcanization accelerator 3: Sancerer ZBE manufactured by Sanshin Chemical Industry Co., Ltd.

[0058] The methods for measuring the bound acrylonitrile amount, bound styrene amount, hydrogenation rate and Mw of the hydrogenated diene rubber are as follows.

[0059] [Bound acrylonitrile content] A 1% by mass solution was prepared using deuterated chloroform as the solvent, and a 400 MHz 1 The ratio of the spectral intensity of protons based on acrylonitrile units to that of protons based on butadiene-derived structural units (including hydrogenated portions) was calculated from the spectrum obtained by measuring H-NMR.

[0060] [Bound styrene content] A 1% by mass solution was prepared using deuterated chloroform as the solvent, and a 400 MHz 1 The ratio was calculated by determining the spectral intensity ratio of the protons based on the styrene unit and the protons based on the butadiene-derived structural unit (including the hydrogenated portion) from the spectrum obtained by measuring H-NMR.

[0061] [Hydrogenation rate] A 1% by mass solution was prepared using deuterated chloroform as the solvent, and a 400 MHz 1 From the spectrum obtained by measuring H-NMR, the hydrogenation rate (mol %) was calculated from the ratio of all butadiene-derived structural units to the hydrogenated structural units among the butadiene-derived structural units.

[0062] [Mw] The weight average molecular weight Mw was determined in terms of polystyrene by gel permeation chromatography (GPC). In detail, the measurement was performed using Shimadzu Corporation's "LC-10A" as a measuring device, Polymer Laboratories' "PLgel-MIXED-C" as a column, a refractive index detector (RI) as a detector, tetrahydrofuran (THF) as a solvent, a measurement temperature of 40°C, a flow rate of 1.0 mL / min, a concentration of 1.0 g / L, and an injection amount of 40 μL, and the weight average molecular weight Mw was calculated in terms of polystyrene using commercially available standard polystyrene.

[0063] In the following experimental examples, the tensile product and the crystallinity were measured as follows. [Tensile product] A dumbbell-shaped test piece No. 3 was prepared from the vulcanized sample. The test piece was subjected to a tensile test according to JIS K6251:2017 using an autograph manufactured by Shimadzu Corporation to measure the tensile strength. The tensile strength at break Tb (MPa) and the elongation at break Eb (%) were calculated, and the tensile product (Tb x Eb ÷ 100) was obtained. The results were expressed as an index with the tensile product of Comparative Example 1 in the first experimental example, the tensile product of Comparative Example 2 in the second experimental example, the tensile product of Comparative Example 3 in the third experimental example, the tensile product of Comparative Example 4 in the fourth experimental example, and the tensile product of Comparative Example 5 in the fifth experimental example taken as 100. The larger the index, the higher the strength and the better the wear resistance.

[0064] [Crystallization degree] The vulcanized sample was stretched 100%, and a diffraction image was obtained using a BRUKER X-ray diffraction device "D8 DISCOVER", and the crystallization index was calculated from the ratio [I25 / I19] of the intensity value at 2θ=25 degrees [I25] to the intensity value at 2θ=19 degrees [I19]. The results were expressed as an index with the crystallization index of Comparative Example 1 in the first experimental example, the crystallization index of Comparative Example 2 in the second experimental example, the crystallization index of Comparative Example 3 in the third experimental example, the crystallization index of Comparative Example 4 in the fourth experimental example, and the crystallization index of Comparative Example 5 in the fifth experimental example set to 100. A larger index indicates a higher degree of elongation crystallinity.

[0065] [First Experimental Example] Using a Daihan lab mixer (300cc), the rubber components were masticated for 30 seconds according to the composition (parts by mass) shown in Table 1 below, and then the compounding ingredients except for sulfur and vulcanization accelerator were added, kneaded for 240 seconds, and then discharged. Next, the discharged rubber composition was added to the lab mixer, kneaded for 180 seconds, and then discharged. Furthermore, the discharged rubber composition, sulfur, and vulcanization accelerator were added to the lab mixer, kneaded for 60 seconds, and then discharged. Using two rolls, sheeting was performed so that the thickness of the obtained unvulcanized rubber composition was 2 mm, and then vulcanization pressing was performed at 160 ° C for 20 minutes to obtain vulcanized samples (thickness 2 mm) of Comparative Example 1 and Examples 1 to 5. The tensile product and crystallinity of the obtained vulcanized samples were measured. The results are shown in Table 1.

[0066] [Table 1]

[0067] [Second Experimental Example] According to the composition (parts by mass) shown in Table 2 below, vulcanized samples of Comparative Example 2 and Example 6 were obtained in the same manner as in Experimental Example 1. The tensile product and crystallinity of the obtained vulcanized samples were measured. The results are shown in Table 2.

[0068] [Table 2]

[0069] [Third Experimental Example] According to the formulation (parts by mass) shown in Table 3 below, and otherwise in the same manner as in Experimental Example 1, vulcanized samples of Comparative Example 3 and Examples 7 to 14 were obtained. The tensile product and crystallinity of the obtained vulcanized samples were measured. The results are shown in Table 3.

[0070] [Table 3]

[0071] [Fourth Experimental Example] According to the composition (parts by mass) shown in Table 4 below, the vulcanized samples of Comparative Example 4 and Example 15 were obtained in the same manner as in the first experimental example. The tensile product and crystallinity of the obtained vulcanized samples were measured. The results are shown in Table 4.

[0072] [Table 4]

[0073] [Fifth Experimental Example] According to the formulation (parts by mass) shown in Table 5 below, and otherwise in the same manner as in Experimental Example 1, vulcanized samples of Comparative Examples 5 and 6 were obtained. The tensile product and crystallinity of the obtained vulcanized samples were measured. The results are shown in Table 5.

[0074] [Table 5]

[0075] As shown in Table 1, the rubber compositions of Examples 1 to 5, in which aromatic phosphate metal salt was blended as a nucleating agent with hydrogenated NBR, had improved tensile products compared to the rubber composition of Comparative Example 1, in which no nucleating agent was added. In addition, crystallization of these rubber compositions was promoted during elongation, and the greater the blending amount of nucleating agent, the higher the degree of elongation crystallization and the greater the effect of improving the tensile product. From this, it is believed that the blending of aromatic phosphate metal salt promoted the elongation crystallization of hydrogenated NBR, improving its strength.

[0076] As shown in Table 2, even when carbon black was added as a filler, adding an aromatic phosphate metal salt as a nucleating agent to hydrogenated NBR promoted elongational crystallization and improved the tensile product.

[0077] As shown in Table 3, even when hydrogenated SBR was used as the hydrogenated diene rubber, Examples 7 to 14, which contained an aromatic phosphate metal salt as a nucleating agent, had improved tensile product compared to Comparative Example 3, which did not contain the nucleating agent. Furthermore, crystallization of these rubber compositions was promoted during elongation, and the greater the amount of nucleating agent, the higher the degree of crystal elongation and the greater the effect of improving the tensile product. As shown in Table 4, even when silica was compounded as a filler, the addition of an aromatic phosphate metal salt to the hydrogenated SBR promoted elongation crystallization and improved the tensile product.

[0078] On the other hand, as shown in Table 5, in Comparative Example 6, in which an aromatic phosphate metal salt was blended with non-hydrogenated SBR, the elongation-induced crystallization was not promoted and no improvement in the tensile product was observed compared to the control Comparative Example 5.

[0079] Hydrogenated NBR and hydrogenated SBR have a polyolefin structure (polyethylene structure) due to the hydrogenation of the conjugated diene portion. By blending aromatic phosphate metal salts, which have traditionally been used as nucleating agents only in olefin resins, with hydrogenated diene rubber, it is believed that the stretch crystallization resulting from the polyolefin structure contained in the hydrogenated diene rubber is promoted, improving the strength (tensile product).

[0080] There have been no previous reports that the reason why hydrogenated SBR has high strength is due to elongation crystallization, and this is the first time that elongation crystallization has been found to be one of the factors that increases the strength of hydrogenated SBR.

[0081] In addition, the various numerical ranges described in the specification can be arbitrarily combined with their upper and lower limits, and all such combinations are considered to be preferred numerical ranges described in the specification. In addition, a numerical range described as "X to Y" means from X to Y.

[0082] Although several embodiments of the present invention have been described above, these embodiments are presented as examples and are not intended to limit the scope of the invention. These embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the gist of the invention. These embodiments and their omissions, substitutions, modifications, etc. are included in the scope and gist of the invention as well as the invention and its equivalents described in the claims.

Claims

1. A rubber composition comprising: a rubber component containing a hydrogenated diene rubber; and a nucleating agent containing an aromatic phosphate metal salt, wherein the amount of the nucleating agent per 100 parts by mass of the hydrogenated diene rubber is 0.05 to 10 parts by mass.

2. The rubber composition according to claim 1, wherein the hydrogenated diene rubber is a hydrogenated styrene butadiene rubber and / or a hydrogenated acrylonitrile butadiene rubber.

3. The rubber composition according to claim 1, wherein the hydrogenated diene rubber has a hydrogenation rate of 70 to 99 mol %.

4. The rubber composition according to claim 1, further comprising a filler, the amount of the filler being 10 to 200 parts by mass per 100 parts by mass of the rubber component.

5. A tire produced using the rubber composition according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Diene-based rubber composition

    JP1997031248A

  • Improved Rubber Composition and Its Use

    JP2017537176A

  • High strength hydrogenated polymer and rubber composition incorporating the same

    JP2021138967A

  • Nucleating agent composition, olefin-based resin composition, molded article thereof, and method for producing olefin-based resin composition

    WO2020153343A1