Rubber composition and tire
By adding an aromatic phosphate ester metal salt as a nucleating agent to synthetic diene homopolymers, the strength and wear resistance of rubber compositions are enhanced through promoted elongation crystallization, addressing the limitations of existing synthetic diene rubbers.
Patent Information
- Application Number
- JP2023082201
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-18
- Publication Date
- 2024-11-28
AI Technical Summary
Existing rubber compositions, particularly those based on synthetic diene rubbers, lack sufficient strength and wear resistance, necessitating improved nucleating agents to enhance elongation crystallization.
Incorporating an aromatic phosphate ester metal salt as a nucleating agent into synthetic diene homopolymers, such as isoprene rubber and polybutadiene rubber, promotes elongation crystallization, thereby increasing the strength and wear resistance of the rubber composition.
The addition of the aromatic phosphate metal salt enhances the tensile strength and promotes elongation crystallization, leading to improved wear resistance and durability of the rubber composition.
Smart Images

Figure 2024165735000001 
Figure 2024165735000002 
Figure 2024165735000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a rubber composition and a tire using the same. [Background technology]
[0002] Recently, there has been a demand for longer life for rubber products such as tires from the perspective of sustainability, etc. To extend the life of tires, improved abrasion resistance is required, which in turn requires a rubber composition with high strength, i.e., high tensile product.
[0003] It is known that natural rubber exhibits high strength properties through strain-induced crystallization. In contrast, synthetic diene rubbers such as synthetic isoprene rubber and polybutadiene rubber do not exhibit strain-induced crystallization to the same extent as natural rubber. Therefore, it has been proposed to incorporate a nucleating agent into synthetic diene rubber to promote crystallization and increase its strength.
[0004] For example, Patent Document 1 discloses blending paraffins or higher saturated fatty acids as a crystal nucleating agent and low molecular weight diene polymers or fatty acid esters as a plasticizer into diene rubber. Patent Document 2 discloses blending dimetal tetracarboxylates as a nucleating agent into diene rubber to promote strain-induced crystallization. Nucleating agents that promote strain-induced crystallization have been reported in this way, but the number is small, and there is a lot of room for improvement with superior nucleating agents.
[0005] On the other hand, it is known to add a nucleating agent to a resin material. In the case of a resin material, after processing in a molten state, it is necessary to cool it when demolding, and adding a nucleating agent can increase the demolding temperature and improve productivity. In this way, the nucleating agent in a resin material is useful for generating uniform and fine crystals by promoting nucleation in the polymer crystallization process, and its purpose is significantly different from that of a rubber material. For example, Patent Document 3 discloses that a nucleating agent containing an aromatic phosphate metal salt is added to an olefin resin, thereby increasing the crystallization speed of the olefin resin and improving its properties. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 9-31248 [Patent Document 2] Special Publication No. 2017-537176 [Patent Document 3] International Publication No. 2020 / 153343 Summary of the Invention [Problem to be solved by the invention]
[0007] The present inventors hypothesized that by applying a nucleating agent, which has conventionally been used in olefin-based resins, to diene-based rubber, it might be possible to increase strength through strain-induced crystallization.
[0008] In view of the above, an object of an embodiment of the present invention is to provide a rubber composition having high strength. [Means for solving the problem]
[0009] The present inventors have discovered that by adding an aromatic phosphate metal salt as a nucleating agent to a synthetic diene-based homopolymer, the strain-induced crystallization of the synthetic diene-based homopolymer is promoted, and a high-strength rubber composition can be obtained.
[0010] The present invention includes the embodiments set forth below. [1] A rubber composition comprising: a rubber component containing a synthetic diene homopolymer; and a nucleating agent containing an aromatic phosphate metal salt, wherein the amount of the nucleating agent is 0.05 to 10 parts by mass per 100 parts by mass of the synthetic diene homopolymer. [2] The rubber composition according to [1], wherein the synthetic diene-based homopolymer is a synthetic isoprene rubber and / or a polybutadiene rubber. [3] The rubber composition according to [1] or [2], further comprising a filler, the amount of the filler being 10 to 200 parts by mass per 100 parts by mass of the rubber component. [4] A tire produced using the rubber composition according to any one of [1] to [3]. Effect of the Invention
[0011] According to an embodiment of the present invention, the strength of a rubber composition containing a synthetic diene-based homopolymer can be increased by adding a nucleating agent containing an aromatic phosphate metal salt. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The rubber composition according to the embodiment includes a rubber component including a synthetic diene-based homopolymer and a nucleating agent including an aromatic phosphate metal salt.
[0013] The synthetic diene homopolymer is a homopolymer rubber chemically synthesized using a diene monomer having a conjugated double bond as a monomer. Examples of the synthetic diene homopolymer include synthetic isoprene rubber (IR) and polybutadiene rubber (BR), and either one of them may be used or they may be used in combination.
[0014] The weight average molecular weight (Mw) of the synthetic diene homopolymer is not particularly limited, and may be, for example, 200,000 to 2,000,000, or 300,000 to 1,000,000. Here, the weight average molecular weight Mw is a value calculated in terms of polystyrene by gel permeation chromatography (GPC). For example, the weight average molecular weight Mw can be calculated in terms of polystyrene using a commercially available standard polystyrene at a measurement temperature of 40°C, a flow rate of 1.0 mL / min, a concentration of 1.0 g / L, and an injection amount of 40 μL, using Shimadzu Corporation's "LC-10A" as a measuring device, Polymer Laboratories' "PLgel-MIXED-C" as a column, a refractive index detector (RI) as a detector, and tetrahydrofuran (THF) as a solvent.
[0015] The rubber component contains the synthetic diene homopolymer, and may contain only the synthetic diene homopolymer or may contain other diene rubbers together with the synthetic diene homopolymer. The content of the synthetic diene homopolymer in the rubber component is preferably 50 to 100 mass%, more preferably 70 to 100 mass%, further preferably 80 to 100 mass%, and may be 100 mass%.
[0016] Examples of other diene rubbers that may be used in combination with the synthetic diene homopolymer include natural rubber (NR), styrene butadiene rubber (SBR), acrylonitrile butadiene rubber (NBR), etc. These other diene rubbers may be used alone or in combination of two or more.
[0017] In this embodiment, an aromatic phosphate metal salt is used as a nucleating agent to be added to the synthetic diene homopolymer. As described above, the aromatic phosphate metal salt is known as a nucleating agent that improves the crystallization rate of olefin resins, but in this embodiment, it is used to promote the strain-induced crystallization of the synthetic diene homopolymer. In this embodiment, the nucleating agent is a drug that promotes the strain-induced crystallization of the synthetic diene homopolymer, and is also called a crystal nucleating agent. Strain-induced crystallization refers to a phase change in an amorphous material that is stretched and deformed to approach a crystalline state.
[0018] The aromatic phosphate metal salt is preferably a compound represented by the following general formula (1). [ka] In formula (1), R 1 ~R 4 each independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms; R 5 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, n represents 1 or 2, when n is 1, M represents an alkali metal atom or dihydroxyaluminum, and when n is 2, M represents an alkaline earth metal atom or hydroxyaluminum.
[0019] R1 ~R 4 Examples of the alkyl group having 1 to 6 carbon atoms represented by the formula (I) include methyl, ethyl, propyl, isopropyl, butyl, sec-butyl, tert-butyl, isobutyl, amyl, isoamyl, tert-amyl, hexyl, 2-hexyl, and 3-hexyl. 1 ~R 4 is preferably tert-butyl or isopropyl.
[0020] R 5 Examples of the alkyl group having 1 to 3 carbon atoms represented by the formula (I) include methyl, ethyl, propyl, and isopropyl. 5 is preferably a hydrogen atom or methyl.
[0021] Examples of the alkali metal atom represented by M include lithium, sodium, and potassium. Examples of the alkaline earth metal atom include magnesium and calcium. M is preferably an alkali metal atom or hydroxyaluminum, and more preferably lithium, sodium, or hydroxyaluminum.
[0022] Specific examples of the aromatic phosphate metal salt represented by the general formula (1) include sodium-2,2'-methylenebis(4,6-di-tert-butylphenyl)phosphate, sodium-2,2'-ethylidenebis(4,6-di-tert-butylphenyl)phosphate, sodium-2,2'-methylenebis(4,6-diisopropylphenyl)phosphate, lithium-2,2'-methylenebis(4,6-di-tert-butylphenyl)phosphate, and lithium-2,2'-ethylidenebis(4,6-di-tert-butylphenyl)phosphate. , lithium-2,2'-methylenebis(4,6-diisopropylphenyl)phosphate, lithium-2,2'-methylenebis(4-methyl-6-tert-butylphenyl)phosphate, hydroxyaluminum bis[2,2'-methylenebis(4,6-di-tert-butylphenyl)phosphate], hydroxyaluminum bis[2,2'-methylenebis(4,6-diisopropylphenyl)phosphate], hydroxyaluminum bis[2,2'-ethylidenebis(4,6-di-tert-butylphenyl)phosphate]. These may be used alone or in combination of two or more.
[0023] The nucleating agent may be an aromatic phosphate metal salt alone, or may contain, together with the aromatic phosphate metal salt, other compounds such as, for example, fatty acid alkali metal salts. The content of the aromatic phosphate metal salt in the nucleating agent is not particularly limited, but is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 95% by mass or more, and may be 100% by mass.
[0024] The amount of the nucleating agent in the rubber composition is preferably 0.05 to 10 parts by mass relative to 100 parts by mass of the synthetic diene homopolymer. By using an amount of the nucleating agent of 0.05 parts by mass or more, the elongation crystallization of the synthetic diene homopolymer is promoted, and the strength of the rubber composition can be increased. The amount of the nucleating agent is preferably 0.1 to 8 parts by mass, more preferably 0.5 to 5 parts by mass, and even more preferably 1 to 5 parts by mass.
[0025] The rubber composition according to the present embodiment may contain a filler. As the filler, carbon black and / or silica are preferable.
[0026] The carbon black is not particularly limited, and various known types can be used.Specific examples include SAF grade (N100 series), ISAF grade (N200 series), HAF grade (N300 series), FEF grade (N500 series), GPF grade (N600 series) (all ASTM grades), etc.These grades of carbon black can be used alone or in combination of two or more types.
[0027] The silica is not particularly limited, and examples thereof include wet silica, dry silica, etc. It is preferable to use wet silica such as wet precipitation silica and wet gelation silica.
[0028] The amount of the filler is preferably 10 to 200 parts by mass per 100 parts by mass of the rubber component, and can be appropriately set depending on the application, etc. The amount of the filler is more preferably 40 to 150 parts by mass per 100 parts by mass of the rubber component.
[0029] In one embodiment, the filler may be predominantly carbon black, i.e., the amount of carbon black relative to the total weight of the filler may be greater than 50%, greater than 70%, or even 100% by weight.
[0030] In one embodiment, the filler may be predominantly silica, i.e., the amount of silica based on the total weight of the filler may be greater than 50%, 60% or more, 70% or more, or even 100% by weight.
[0031] When silica is blended as a filler, the rubber composition preferably further contains a silane coupling agent. Examples of the silane coupling agent include sulfide silane coupling agents such as bis(3-triethoxysilylpropyl)tetrasulfide, bis(3-triethoxysilylpropyl)disulfide, bis(2-triethoxysilylethyl)tetrasulfide, bis(4-triethoxysilylbutyl)disulfide, bis(3-trimethoxysilylpropyl)tetrasulfide, and bis(2-trimethoxysilylethyl)disulfide, and mercaptosilane coupling agents such as 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropyldimethylmethoxysilane, and mercaptoethyltriethoxysilane. These can be used alone or in combination of two or more. The amount of the silane coupling agent is preferably 5 to 20 parts by mass, and more preferably 5 to 15 parts by mass, based on 100 parts by mass of silica.
[0032] In addition to the above components, the rubber composition according to this embodiment may contain various additives that are generally used in rubber compositions, such as zinc oxide, stearic acid, an antioxidant, wax, oil, a vulcanizing agent, and a vulcanization accelerator.
[0033] The content of zinc oxide is not particularly limited, and may be, for example, 0 to 10 parts by mass, 0.5 to 5 parts by mass, or 1 to 4 parts by mass relative to 100 parts by mass of the rubber component.
[0034] The content of stearic acid is not particularly limited, and may be, for example, 0 to 10 parts by mass, 0.5 to 5 parts by mass, or 1 to 4 parts by mass relative to 100 parts by mass of the rubber component.
[0035] As the vulcanizing agent, sulfur is preferably used. The content of the vulcanizing agent is not particularly limited, but may be 0.1 to 10 parts by mass, 0.5 to 5 parts by mass, or 1 to 3 parts by mass, based on 100 parts by mass of the rubber component.
[0036] Examples of the vulcanization accelerator include various vulcanization accelerators such as sulfenamide-based, guanidine-based, dithiocarbamate-based, thiuram-based, and thiazole-based, and any one of them can be used alone or in combination of two or more. The content of the vulcanization accelerator is not particularly limited, but is preferably 0.1 to 7 parts by mass, more preferably 0.5 to 5 parts by mass, and may be 1 to 3 parts by mass, relative to 100 parts by mass of the rubber component.
[0037] The rubber composition according to the present embodiment can be prepared by kneading in a conventional manner using a commonly used mixer such as a Banbury mixer, kneader, or roll. That is, for example, in the first mixing stage (non-pro kneading process), additives other than the vulcanizing agent and vulcanization accelerator are added and mixed with the rubber component together with the nucleating agent and filler. Next, in the final mixing stage (pro kneading process), the vulcanizing agent and vulcanization accelerator are added and mixed to the obtained mixture. This allows the preparation of an unvulcanized rubber composition.
[0038] The rubber composition according to the present embodiment can be used for various rubber members such as tires, anti-vibration rubber, conveyor belts, etc. It is preferably for tires, and can be applied to various parts of tires such as treads, sidewalls, and beads of pneumatic tires of various sizes for various purposes such as tires for passenger cars and large tires for trucks and buses.
[0039] In one embodiment, a tire including a rubber portion (e.g., tread rubber, sidewall rubber, etc.) made of the rubber composition is manufactured as follows. The rubber composition is molded into a predetermined shape by a conventional method, for example, extrusion processing. The obtained molded product is combined with other parts to produce a green tire. The green tire is vulcanized and molded at, for example, 140 to 180°C to produce a pneumatic tire.
[0040] The rubber composition according to the present embodiment can improve the strength (tensile product) by elongation crystallization, and therefore can improve the abrasion resistance. Therefore, in one embodiment, it is preferably used as a rubber composition constituting a tire tread. That is, the tire according to one embodiment is a tire having a tread made by using the above rubber composition. EXAMPLES
[0041] Examples will be shown below, but the present invention is not limited to these examples.
[0042] The components used in the examples and comparative examples are as follows. SBR: Styrene butadiene rubber, "HPR350" manufactured by ENEOS Materials Co., Ltd. NR: Natural rubber, RSS#3 BR: Polybutadiene rubber, "UBEPOL BR 150B" manufactured by UBE Elastomers Co., Ltd. IR: Synthetic isoprene rubber, "IR2200" manufactured by ENEOS Materials Co., Ltd.
[0043] Nucleating agent A: ADEKA Corporation's "ADEKA STAB NA-21" (main component: hydroxyaluminum bis[2,2'-methylenebis(4,6-di-tert-butylphenyl)phosphate] (R 1 ~R 4 =t-Bu, R 5 = H, M = Al-OH, n = 2)
[0044] Nucleating agent B: ADEKA STAB NA-11 (sodium 2,2'-methylenebis(4,6-di-tert-butylphenyl)phosphate (R 1 ~R 4 =t-Bu, R 5 =H, M=Na, n=1)
[0045] Carbon black: "Seat KH (N339)" manufactured by Tokai Carbon Co., Ltd. Zinc oxide: "Zinc oxide No. 3" manufactured by Mitsui Mining & Smelting Co., Ltd. Stearic acid: Kao Corporation's "Lunac S-20" Sulfur: "Powdered sulfur" manufactured by Tsurumi Chemical Industry Co., Ltd. Vulcanization accelerator 1: "Soxinol CZ" manufactured by Sumitomo Chemical Co., Ltd. Vulcanization accelerator 2: "Noccelaer D" manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Vulcanization accelerator 3: "Noccela NS-P" manufactured by Ouchi Shinko Chemical Industry Co., Ltd.
[0046] In the following experimental examples, the tensile product and the crystallinity were measured as follows. [Tensile product] A dumbbell-shaped test piece No. 3 was prepared from the vulcanized sample. The test piece was subjected to a tensile test according to JIS K6251:2017 using an autograph manufactured by Shimadzu Corporation to measure the tensile strength. The tensile strength at break Tb (MPa) and the elongation at break Eb (%) were calculated, and the tensile product (Tb x Eb ÷ 100) was obtained. The results were expressed as an index with the tensile product of Comparative Example 1 in the first experimental example, the tensile product of Comparative Example 3 in the second experimental example, the tensile product of Comparative Example 4 in the third experimental example, the tensile product of Comparative Example 6 in the fourth experimental example, and the tensile product of Comparative Example 7 in the fifth experimental example taken as 100. The larger the index, the higher the strength and the better the wear resistance.
[0047] [Crystallization degree] With the vulcanized sample stretched 100%, a diffraction image was obtained using a BRUKER X-ray diffraction device "D8 DISCOVER" and the crystallization index was calculated from the ratio [I25 / I19] of the intensity value at 2θ=25 degrees [I25] to the intensity value at 2θ=19 degrees [I19]. The results were expressed as an index with the crystallization index of Comparative Example 1 in the first experimental example, the crystallization index of Comparative Example 3 in the second experimental example, the crystallization index of Comparative Example 4 in the third experimental example, the crystallization index of Comparative Example 6 in the fourth experimental example, and the crystallization index of Comparative Example 7 in the fifth experimental example each set to 100. A larger index indicates a higher degree of elongation crystallinity.
[0048] [First Experimental Example] Using a Daihan lab mixer (300cc), the rubber components were masticated for 30 seconds according to the composition (parts by mass) shown in Table 1 below, and then the compounding ingredients except for sulfur and vulcanization accelerator were added, kneaded for 150 seconds, and then discharged. Furthermore, the discharged rubber composition, sulfur, and vulcanization accelerator were added to the lab mixer, kneaded for 60 seconds, and then discharged. Using two rolls, sheeting was performed so that the thickness of the obtained unvulcanized rubber composition was 2 mm, and then vulcanization pressing was performed at 160 ° C for 20 minutes to obtain vulcanized samples (thickness 2 mm) of Comparative Examples 1 to 2. The tensile product and crystallinity of the obtained vulcanized samples were measured. The results are shown in Table 1.
[0049] [Table 1]
[0050] [Second Experimental Example] According to the composition (parts by mass) shown in Table 2 below, vulcanized samples of Comparative Example 3 and Example 1 were obtained in the same manner as in Experimental Example 1. The tensile product and crystallinity of the obtained vulcanized samples were measured. The results are shown in Table 2.
[0051] [Table 2]
[0052] [Third Experimental Example] According to the formulation (parts by mass) shown in Table 3 below, and otherwise in the same manner as in Experimental Example 1, vulcanized samples of Comparative Examples 4 and 5 were obtained. The tensile product and crystallinity of the obtained vulcanized samples were measured. The results are shown in Table 3.
[0053] [Table 3]
[0054] [Fourth Experimental Example] According to the formulation (parts by mass) shown in Table 4 below, and otherwise in the same manner as in Experimental Example 1, vulcanized samples of Comparative Example 6 and Examples 2 to 6 were obtained. The tensile product and crystallinity of the obtained vulcanized samples were measured. The results are shown in Table 4.
[0055] [Table 4]
[0056] [Fifth Experimental Example] According to the composition (parts by mass) shown in Table 5 below, vulcanized samples of Comparative Example 7 and Example 7 were obtained in the same manner as in Experimental Example 1. The tensile product and crystallinity of the obtained vulcanized samples were measured. The results are shown in Table 5.
[0057] [Table 5]
[0058] As shown in Table 2, the rubber composition of Example 1, in which an aromatic phosphate metal salt was blended as a nucleating agent into a rubber composition containing BR, had an improved tensile product compared to the rubber composition of Comparative Example 3, in which no nucleating agent was added. As shown in Table 4, the rubber compositions of Examples 2 to 6, in which an aromatic phosphate metal salt was blended into a rubber composition containing IR, had an improved tensile product compared to the rubber composition of Comparative Example 6, in which no nucleating agent was added. In addition, crystallization was promoted during elongation in these rubber compositions, and the greater the blending amount of the nucleating agent, the higher the degree of elongation crystallization and the greater the effect of improving the tensile product. From this, it is believed that the blending of the aromatic phosphate metal salt promoted the elongation crystallization of BR and IR, thereby improving their strength.
[0059] As shown in Table 5, even when carbon black was added as a filler, the addition of an aromatic phosphate metal salt as a nucleating agent to IR promoted elongational crystallization and improved the tensile product.
[0060] In contrast, when SBR was used as the rubber component, strain-induced crystallization did not occur and strength did not increase even when aromatic phosphate metal salt was added, as shown in Table 1. Furthermore, when NR was used as the rubber component, strain-induced crystallization occurred even without adding aromatic phosphate metal salt as a nucleating agent, so the effect of adding a nucleating agent was not obtained, as shown in Table 3.
[0061] In addition, the various numerical ranges described in the specification can be arbitrarily combined with their upper and lower limits, and all such combinations are considered to be preferred numerical ranges described in the specification. In addition, a numerical range described as "X to Y" means from X to Y.
[0062] Although several embodiments of the present invention have been described above, these embodiments are presented as examples and are not intended to limit the scope of the invention. These embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the gist of the invention. These embodiments and their omissions, substitutions, modifications, etc. are included in the scope and gist of the invention as well as the invention and its equivalents described in the claims.
Claims
1. A rubber composition comprising a rubber component containing a synthetic diene homopolymer and a nucleating agent containing an aromatic phosphate metal salt, the amount of the nucleating agent being 0.05 to 10 parts by mass per 100 parts by mass of the synthetic diene homopolymer.
2. 2. The rubber composition according to claim 1, wherein the synthetic diene-based homopolymer is a synthetic isoprene rubber and / or a polybutadiene rubber.
3. The rubber composition according to claim 1, further comprising a filler, the amount of the filler being 10 to 200 parts by mass per 100 parts by mass of the rubber component.
4. A tire produced using the rubber composition according to any one of claims 1 to 3.
Citation Information
Patent Citations
Diene-based rubber composition
JP1997031248A
Improved Rubber Composition and Its Use
JP2017537176A
Nucleating agent composition, olefin-based resin composition, molded article thereof, and method for producing olefin-based resin composition