Photocurable organopolysiloxane, photocurable organopolysiloxane composition and cured product
A photocurable organopolysiloxane with specific T unit, functional group, and alkoxysilyl group proportions addresses durability and reworkability issues, enabling effective recyclability and pattern reshaping.
Patent Information
- Application Number
- JP2023082207
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-18
- Publication Date
- 2024-11-28
AI Technical Summary
Existing photocurable polysiloxanes lack sufficient durability and reworkability, making them unsuitable for applications requiring recyclability and pattern reshaping in processes like solar panel recycling and lithography.
A photocurable organopolysiloxane with specific proportions of T units, polymerizable functional groups, and alkoxysilyl groups, within defined ranges, ensuring excellent durability and reworkability.
The solution provides a photocurable organopolysiloxane with enhanced durability and reworkability, allowing easy cleaning and reshaping of cured products.
Smart Images

Figure 2024165738000001 
Figure 2024165738000002 
Figure 2024165738000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a photocurable organopolysiloxane, a photocurable organopolysiloxane composition, and a cured product. [Background technology]
[0002] Photocurable polysiloxanes are used in a wide range of applications, including as coating materials, adhesive materials, packaging materials, and electronic materials, because the compositions containing the photocurable polysiloxanes themselves have excellent coatability (fluidity), and the resulting cured products also have excellent durability.
[0003] Specific applications of photocurable polysiloxanes include protective coating agents for light-emitting diodes (LEDs) and solar panels (eg, Patent Document 1), and base polymers for photoresists (eg, Patent Documents 2 and 3). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Special Publication No. 2015-516478 [Patent Document 2] Special Publication No. 2011-23698 [Patent Document 3] WO2016 / 072202 issue Summary of the Invention [Problem to be solved by the invention]
[0005] "Reworkability," which allows polysiloxane resin to be easily washed once it has been cured, is becoming an important required performance. In the above-mentioned applications, in the case of solar panels, the protective coating agent needs to be removed when recycling panels that have deteriorated over time, and in the case of lithography processes, if the pattern shape of the formed resist film is not the desired shape, the resist film is peeled off and a new resist film is formed. None of the polysiloxane resins disclosed in Patent Documents 1 to 3 can be said to have sufficient durability and reworkability, and there has been a demand for polysiloxane resins with excellent reworkability.
[0006] An object of the present invention is to provide a photocurable organopolysiloxane which gives a cured product with excellent durability and reworkability. Another problem to be solved by the present invention is to provide a cured product of a composition containing a photocurable organopolysiloxane that has excellent durability and reworkability. [Means for solving the problem]
[0007] As a result of extensive investigations aimed at solving the above problems, the present inventors have found that an organopolysiloxane in which the proportion of T units and the amounts of polymerizable functional groups and alkoxysilyl groups fall within specific ranges will give a cured product with excellent durability and reworkability, and have completed the present invention.
[0008] That is, the present invention relates to a photocurable organopolysiloxane. 1. A photocurable organopolysiloxane having a polymerizable functional group and an alkoxysilyl group, represented by the following general formula (1): The ratio of T units to all siloxy units is 70 mol % or more, A photocurable organopolysiloxane containing 40 mass % or more of the polymerizable functional group represented by the general formula (1) and containing the alkoxysilyl group in the range of 0.1 to 10 mass %. [ka] (In the general formula (1), R 11 is a single bond or an alkylene group having 1 to 12 carbon atoms, Y is a group containing a carbon-carbon unsaturated bond, * indicates the bonding position to the silicon atom of the organopolysiloxane.) 2. The photocurable organopolysiloxane according to 1, wherein the polymerizable functional group represented by the general formula (1) is a polymerizable functional group represented by the following general formula (1-2): [ka] (In the general formula (1-2), R 11 is a single bond or an alkylene group having 1 to 12 carbon atoms, R 12 is a hydrogen atom or an alkyl group having 1 to 12 carbon atoms, * indicates the bonding position to the silicon atom of the organopolysiloxane.) 3. The photocurable organopolysiloxane according to 1 or 2, wherein the content of the polysiloxane structure is 35% by mass or more. 4. The photocurable organopolysiloxane according to any one of 1 to 3, having a viscosity at 25° C. of 150 mPas or less. 5. A photocurable organopolysiloxane composition comprising the photocurable organopolysiloxane according to any one of 1 to 4 and a photopolymerization initiator. 6. The photocurable organopolysiloxane composition according to 5, which is a resist composition. 7. A cured product of the photocurable organopolysiloxane composition according to 5 or 6. Effect of the Invention
[0009] The present invention provides a photocurable organopolysiloxane that has excellent coatability, and gives a cured product that has excellent durability and reworkability. The present invention can provide a cured product of a composition containing a photocurable organopolysiloxane that has excellent durability and reworkability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] An embodiment of the present invention will be described below. The present invention is not limited to the following embodiment, and can be implemented by making appropriate modifications within the scope that does not impair the effects of the present invention. The compounds in the present specification may be derived from fossil resources or biological resources.
[0011] [Photocurable organopolysiloxane] The photocurable organopolysiloxane of the present invention has a polymerizable functional group represented by the following general formula (1) and an alkoxysilyl group, and contains 40 mass % or more of the polymerizable functional group represented by the general formula (1) and contains the alkoxysilyl group in the range of 0.1 to 10 mass %.
[0012] [ka] (In the general formula (1), R 11 is a single bond or an alkylene group having 1 to 12 carbon atoms, Y is a group containing a carbon-carbon unsaturated bond, * indicates the bonding position to the silicon atom of the organopolysiloxane.)
[0013] In the present invention, the amount of alkoxysilyl groups in the organopolysiloxane is within a specific range, the amount of specific polymerizable functional groups is at least a certain level, and the proportion of T units in all siloxy units in the organopolysiloxane is at least a certain level, thereby making it possible to improve the coatability of the composition itself and the durability and reworkability of the resulting cured product.
[0014] The polymerizable functional group represented by the general formula (1) has a decomposable bond. It is presumed that when the organopolysiloxane is treated with an acid or alkali, the bond of the polymerizable functional group decomposes, causing the crosslinked structure of the organopolysiloxane to collapse, making it possible to clean. Therefore, by having a certain amount of the polymerizable functional group represented by the general formula (1), reworkability can be ensured.
[0015] In the general formula (1), examples of the group containing a carbon-carbon unsaturated bond for Y include a (meth)acryloyl group, a (meth)acryloyloxy group, a (meth)acryloylamino group, a vinyl ether group, an allyl group, a styryl group, and a maleimide group.
[0016] R 11 Examples of the alkylene group having 1 to 12 carbon atoms include a methylene group, an ethylene group, an n-propylene group, an n-butylene group, an n-pentylene group, an n-hexylene group, an n-heptylene group, an n-octylene group, an n-nonylene group, an n-decylene group, an n-dodecylene group, an isopropylene group, a 2-methylpropylene group, a 2-methylhexylene group, and a tetramethylethylene group.
[0017] R 11 The alkylene group having 1 to 12 carbon atoms is preferably an alkylene group having 1 to 5 carbon atoms, and more preferably a methylene group, an ethylene group, an n-propylene group or an isopropylene group.
[0018] R 11 In the alkylene group having 1 to 12 carbon atoms, some of the -CH2- may be replaced by a carbonyl group (-C(=O)-), an ether bond (-O-), a phenylene group, an amide bond or a urethane bond, and a hydroxyl group or the like may further be substituted on the carbon atom.
[0019] The upper limit of the amount of the polymerizable functional groups in the photocurable organopolysiloxane of the present invention is not particularly limited, and is, for example, 80% by mass or less, 60% by mass or less, or 50% by mass or less.
[0020] The alkoxysilyl group is hydrolyzed by treatment with an acid or alkali to become a silanol group, which can improve the cleaning properties of the organopolysiloxane. Therefore, by having a certain amount of alkoxysilyl groups, reworkability can be ensured.
[0021] The content of alkoxysilyl groups in the photocurable organopolysiloxane of the present invention is in the range of 0.1 to 10 mass %, preferably in the range of 0.1 to 8.0 mass %, and more preferably in the range of 0.1 to 6.0 mass %.
[0022] The alkoxysilyl group contained in the photocurable organopolysiloxane of the present invention is preferably an alkoxysilyl group represented by the following general formula (2).
[0023] [ka] (In the general formula (2), R 21 is an alkyl group having 1 to 12 carbon atoms, * indicates the bonding position to the silicon atom of the organopolysiloxane.)
[0024] R 21 The alkyl group having 1 to 12 carbon atoms is preferably an alkyl group having 1 to 6 carbon atoms, and more preferably an alkyl group having 1 to 3 carbon atoms. R 21 The alkyl group of R does not contain a carbon-carbon unsaturated bond. 21 The alkyl group may further have a substituent such as a halogen atom, a hydroxyl group, a cyano group or an amino group.
[0025] The amount of polymerizable functional groups and alkoxysilyl groups in the photocurable organopolysiloxane of the present invention is confirmed by the method described in the Examples.
[0026] The siloxy unit is RSiO 1 / 2 Unit (M unit), SiO 4 / 2 Units (Q units), R2SiO 2 / 2 Units (D units) and RSiO 3 / 2 The photocurable organopolysiloxane of the present invention has a ratio of T units to all siloxy units of 70 mol % or more. By having a ratio of T units of 70 mol % or more, it is possible to obtain a photocurable organopolysiloxane that can achieve both the coatability of the composition and the durability and reworkability of the obtained cured product. The proportion of each siloxy unit in the photocurable organopolysiloxane is confirmed by the method described in the Examples.
[0027] There is no particular upper limit to the proportion of T units in the photocurable organopolysiloxane of the present invention, and it may be, for example, 100 mol % or less.
[0028] The aliphatic hydrocarbon group of R in the siloxy unit is, for example, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a phenyl group, or a phenoxy group.
[0029] The number average molecular weight of the photocurable organopolysiloxane of the present invention is preferably in the range of 500 to 5,000. The number average molecular weight of the photocurable organopolysiloxane can be confirmed by GPC measurement.
[0030] The content of the polysiloxane structure in the photocurable organopolysiloxane of the present invention is preferably 35% by mass or more, and more preferably 50% by mass or more, from the viewpoint of improving the durability and weather resistance of the cured product. The term "polysiloxane structure" refers to a repeating structure represented by "Si-O-Si." The upper limit of the content of the polysiloxane structure is not particularly limited, but is, for example, 60% by mass or less or 70% by mass or less. The content of the polysiloxane structure in the photocurable organopolysiloxane is confirmed by the method described in the examples.
[0031] When a composition containing a photocurable polysiloxane is used as a coating material for electronic devices, the coating property of the composition containing the photocurable polysiloxane is an important performance. When a composition whose viscosity has been reduced by diluting with a solvent is used for coating electronic devices, the volatile components of the solvent may cause corrosion or deterioration of electric and electronic components and the circuit boards on which they are mounted. Therefore, it is required that the photocurable polysiloxane alone has a viscosity suitable for coating to a degree that allows it to follow the fine uneven surfaces of electronic components and heat sinks. The photocurable organopolysiloxane of the present invention exhibits coatability sufficient to enable the resin alone to conform to the finely irregular surfaces of electronic components and heat sinks. The viscosity of the photocurable organopolysiloxane of the present invention is preferably 150 mPas or less, more preferably 100 mPas or less. There is no particular lower limit to the viscosity, but it is, for example, 10 mPas or more. The viscosity of the photocurable organopolysiloxane can be confirmed by the method described in the examples.
[0032] The photocurable organopolysiloxane of the present invention is preferably a compound in which a group Y containing a carbon-carbon unsaturated bond and a silicon atom are linked by a bond represented by Si-ORY, and the silicon atom is a part of a silicone oligomer. Similarly, the photocurable organopolysiloxane of the present invention is preferably a compound in which the silicon atom of the alkoxysilyl group is part of a silicone oligomer.
[0033] The synthesis of the photocurable organopolysiloxane of the present invention is not particularly limited, and any known and commonly used method can be used. For example, there is a method of synthesizing a compound having a polymerizable unsaturated group and a hydroxyl group as a raw material with a chlorosilane compound by dehydrochlorination reaction, a method of synthesizing with an alkoxysilane compound by ester exchange, and a method of reacting with a silane hydride compound using a Lewis acid catalyst such as a boron compound.
[0034] The photocurable organopolysiloxane of the present invention is preferably a compound having as reaction components a silicone oligomer having an alkoxysilyl group and a compound having a hydroxyl group and a group containing a carbon-carbon unsaturated bond. Here, the term "reactive component" refers to a component that constitutes the structure of the photocurable organopolysiloxane, and does not include solvents, catalysts, and the like that do not constitute the structure.
[0035] The silicone oligomer having an alkoxysilyl group can be prepared by a known polycondensation reaction using a hydrolyzable alkoxysilane compound as a reactant. The hydrolyzable alkoxysilane compound used may be one type alone or two or more types. By adjusting the type and amount of the hydrolyzable alkoxysilane compound, the ratio of T units in the obtained photocurable organopolysiloxane, the content of the polysiloxane structure, the amount of alkoxysilyl groups, etc. can be adjusted.
[0036] The silicone oligomer having an alkoxysilyl group used in the production of the photocurable organopolysiloxane can be a commercially available product.
[0037] The compound having a hydroxyl group and a group containing a carbon-carbon unsaturated bond is preferably a (meth)acrylate compound having a hydroxyl group. In this case, the polymerizable functional group in the organopolysiloxane is, for example, a functional group represented by the following general formula (1-2).
[0038] [ka] (In the general formula (1-2), R 11 is a single bond or an alkylene group having 1 to 12 carbon atoms, R 12 is a hydrogen atom or an alkyl group having 1 to 12 carbon atoms, * indicates the bonding position to the silicon atom of the organopolysiloxane.)
[0039] In the general formulas (1) and (1-2), R 11 The alkylene group having 1 to 12 carbon atoms is preferably an alkylene group having 1 to 5 carbon atoms, and R 12 is preferably a hydrogen atom or a methyl group.
[0040] The (meth)acrylate compound having a hydroxyl group is preferably a compound in which the "*" portion of the functional group represented by the general formula (1-2) is a hydrogen atom.
[0041] Specific examples of the (meth)acrylate compound having a hydroxyl group include 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, 4-hydroxybutyl acrylate, 4-hydroxybutyl methacrylate, tricyclodecane dimethanol acrylate, adamantanediol acrylate, β-carboxyethyl acrylate, and pentaerythritol triacrylate.
[0042] The (meth)acrylate compound having a hydroxyl group may be used alone or in combination of two or more kinds.
[0043] The method for producing the photocurable organopolysiloxane is not particularly limited, and the photocurable organopolysiloxane can be produced by the methods described above. However, as a particularly convenient production method, the reaction between a silicone oligomer having an alkoxysilyl group and a compound having a hydroxyl group and a group containing a carbon-carbon unsaturated bond can be carried out by heating in the presence of an acid catalyst (e.g., sulfuric acid). By adjusting the alkoxysilyl group equivalent of the silicone oligomer to an amount in excess of the hydroxyl group equivalent of the compound having a hydroxyl group and a polymerizable group, the photocurable organopolysiloxane of the present invention can be produced.
[0044] [Photocurable organopolysiloxane composition] The photocurable organopolysiloxane of the present invention can be suitably used as a base polymer for the photocurable organopolysiloxane composition of the present invention (hereinafter sometimes simply referred to as the "composition of the present invention"). The photocurable organopolysiloxane composition has excellent coatability, and the obtained cured product has excellent durability and reworkability.
[0045] The content of the photocurable organopolysiloxane of the present invention in the composition of the present invention is, for example, 80 mass % or more, and preferably 90 mass % or more, of the solid content in the composition. The term "solid content" as used herein means the sum of the components excluding the solvent, which will be described later, from the total amount of the composition.
[0046] The composition of the present invention contains the photocurable organopolysiloxane of the present invention and a photopolymerization initiator. The photopolymerization initiator may be appropriately selected from those that have absorption in the light source used for photocuring. For example, 2,2-dimethoxy-1,2-diphenylethan-1-one, 1-hydroxy-cyclohexyl-phenyl-ketone, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-1-butanone, bis(2,4, 6-trimethylbenzoyl)-phenylphosphine oxide, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]-phenyl}-2-methyl-propane, 1,2-octanedione, 1-[4-(phenylthio)-, 2-(O-benzoyloxime)], 2-hydroxy-2-methyl-1-phenyl-propan-1-one, phenylglyoxylic acid methyl ester, 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, and the like can be used.
[0047] The photopolymerization initiator may be a commercially available product, for example, OMNIRAD1000, OMNIRAD248, OMNIRAD481, OMNIRAD4817, OMNIRAD4MBZ-flakes, OMNIRAD500, OMNIRAD659, OMNIRAD73, OMNIRAD784, OMNIRAD81, OMNIRADBDK, OMNIRADMBS, OMNIRADBP-flakes, OMNIRADDETX, OMNIRADEDB, OMNIRADEHA, OMNIRADEMK, OMNIRADITX, OMNIRADMBF, OMNIRADTPO, OMNIRAD410, OMNIRADBL72. 3, BL724, BL750, BL751, 1173, 127, 184, 184FF, 2022, 2100, 2959, 369, 369E, 379, 379EG, 4265, 754, 819, 819DW, 907, 907FF, BP, 127D, ESACURE1001M, ONE, A198, KIP 160, KIP 150, KIP100F, KIP-LT, KIP-IT, KTO-46, DP-250, TZT, KT-55 (manufactured by IMG), etc.
[0048] The content of the photopolymerization initiator in the composition of the present invention is, for example, in the range of 0.01 to 10 parts by mass, and preferably in the range of 0.1 to 5 parts by mass, per 100 parts by mass of the photocurable organopolysiloxane.
[0049] The composition of the present invention may contain a polymerization inhibitor. As the polymerization inhibitor, known ones can be used, such as hydroquinone, p-methoxyphenol, di-tert-butyl-p-cresol, pyrogallol, tert-butylcatechol, benzoquinone, 4,4'-thiobis(3-methyl-6-tert-butylphenol), 2,2'-methylenebis(4-methyl-6-t-butylphenol), N-nitrosophenylhydroxyamine salts (e.g., ammonium salts, cerous salts), and the like.
[0050] The content of the photopolymerization initiator in the composition of the present invention is, for example, in the range of 0.001 part by mass or more and 1 part by mass or less, and preferably in the range of 0.01 part by mass or more and 0.5 part by mass or less, relative to 100 parts by mass of the photocurable organopolysiloxane of the present invention.
[0051] The composition of the present invention may contain a solvent. By adding a solvent, the viscosity of the composition and the coating film thickness can be adjusted. Examples of the solvent that can be used include aliphatic or alicyclic hydrocarbons such as n-hexane, n-heptane, n-octane, cyclohexane, and cyclopentane; aromatic hydrocarbons such as toluene, xylene, ethylbenzene, and anisole; alcohols such as methanol, ethanol, n-butanol, ethylene glycol monomethyl ether, propylene glycol monomethyl ether, and propylene glycol monoethyl ether; esters such as ethyl acetate, n-butyl acetate, isobutyl acetate, ethylene glycol monomethyl ether acetate, and propylene glycol monomethyl ether acetate; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; alkyl ethers; ethers such as 1,2-dimethoxyethane, tetrahydrofuran, and dioxane; N-methylpyrrolidone, dimethylformamide, and dimethylacetamide.
[0052] The content of the solvent in the composition of the present invention is not particularly limited, and may be appropriately set according to the intended viscosity and coating film thickness.
[0053] The composition of the present invention may contain a surfactant. The surfactant may be any of a nonionic surfactant, an anionic surfactant, a cationic surfactant and an amphoteric surfactant, with a nonionic surfactant being preferred.
[0054] Examples of nonionic surfactants include polyoxyalkylene alkyl ether surfactants, polyoxyalkylene fatty acid ester surfactants, sorbitan fatty acid ester surfactants, polyoxyalkylene alkylamine surfactants, Pluronic (registered trademark) type (triblock copolymer of polyethylene oxide and polypropylene oxide) surfactants, fluorine-based surfactants, silicone-based surfactants, and acrylic polymerization surfactants.
[0055] Examples of the anionic surfactant include alkylbenzene sulfonate surfactants, alkyl alcohol sulfate surfactants, polyoxyalkylene alkyl ether sulfate surfactants, alkyl alcohol phosphate surfactants, polyoxyalkylene alkyl ether phosphate surfactants, polyoxyalkylene alkyl ether acetate surfactants, and fluorine-based surfactants. Either an acid type or a neutral type may be used.
[0056] Examples of the cationic surfactant include tetraalkylammonium halide surfactants, alkylpyridinium halide surfactants, and alkylimidazoline halide surfactants.
[0057] Examples of the amphoteric surfactant include alkyl betaine surfactants, alkyl imidazolinium betaine surfactants, and lecithin surfactants.
[0058] The content of the surfactant in the composition of the present invention is, for example, in the range of 0.001 part by mass or more and 10 parts by mass or less, preferably in the range of 0.01 part by mass or more and 8 parts by mass or less, and more preferably in the range of 0.1 part by mass or more and 5 parts by mass or less, relative to 100 parts by mass of the photocurable organopolysiloxane of the present invention.
[0059] The composition of the present invention may contain other ingredients as long as the effects of the present invention are not impaired. Examples of other ingredients include organic pigments, inorganic pigments, extender pigments, organic fillers, inorganic fillers, photosensitizers, ultraviolet absorbers, antioxidants, adhesion aids, etc.
[0060] The composition of the present invention is capable of exhibiting sufficient coatability using the resin alone by controlling the terminal functional groups and molecular weight of the photocurable organopolysiloxane. In JP 2011-23698 A, the coatability of the silicone polymer is improved by adding an alkoxysilane compound, but in the present invention, the flowability of the photocurable organopolysiloxane itself is good, so there is no need to add a low molecular weight alkoxysilane compound.
[0061] The components in the photocurable organopolysiloxane composition of the present invention have been explained above. Each component may be used alone or in combination of two or more kinds.
[0062] The photocurable organopolysiloxane composition of the present invention is a photocurable composition that can be cured by irradiation with light. For example, the photocurable organopolysiloxane composition of the present invention can be applied to a substrate to form a coating film, and the coating film can be irradiated with light to form a cured layer on the substrate.
[0063] The substrate may be appropriately selected depending on the purpose, and examples thereof include quartz, sapphire, glass, plastic, ceramic materials, vapor deposition films (CVD, PVD, sputtering), magnetic films, reflective films, metal substrates such as Ni, Cu, Cr, Fe, and stainless steel, paper, polymer substrates such as SOG (spin on glass), SOC (spin on carbon), polyester films, polycarbonate films, and polyimide films, TFT array substrates, electrode plates for PDPs, conductive substrates such as ITO and metals, insulating substrates, and semiconductor fabrication substrates such as silicon, silicon nitride, polysilicon, silicon oxide, and amorphous silicon. The shape of the substrate is not particularly limited, and may be any shape according to the purpose, such as a flat plate, a sheet, or a three-dimensional shape having a curvature entirely or partially, etc. Furthermore, there is no limitation on the hardness, thickness, etc. of the substrate.
[0064] As a method for coating the photocurable organopolysiloxane composition of the present invention, various methods can be used, such as spraying, spin coating, dipping, roll coating, blade coating, doctor roll method, doctor blade method, curtain coating, slit coating, screen printing, and ink jet method. The spin coating method is preferred because it can provide a coating film with good in-plane uniformity in thickness.
[0065] Examples of light sources for irradiation include low pressure mercury lamps, high pressure mercury lamps, ultra-high pressure mercury lamps, metal halide lamps, xenon lamps, carbon arcs, mercury xenon lamps, excimer lasers (XeCl, KrF, ArF, etc.), ultraviolet or visible light lasers, and ultraviolet or visible light LEDs. The amount of light irradiation may be appropriately set, for example, from 10 to 10,000 mJ / cm 2 The range is.
[0066] A baking step may be provided in which the substrate is heated after coating with the photocurable organopolysiloxane composition and before irradiation with light. As the baking method, various methods such as a proximity method, an adsorption method, a conveyor method, induction heating using microwaves, etc. can be used, and these methods can also be combined. The baking conditions are not particularly limited, but for example, the baking temperature is in the range of 70 to 180° C., and the baking time is in the range of 0.3 to 10 minutes.
[0067] When the photocurable organopolysiloxane composition of the present invention is used for photoimprinting, a mold on which a pattern has been formed in advance is pressed against the coating film of the photocurable organopolysiloxane composition formed on the above-mentioned substrate, and the coating film is cured by irradiating it with light while the mold is in contact, thereby obtaining a film of a cured product on which a pattern has been formed. The baking step may be performed before the mold is brought into contact with the substrate, or after the mold is pressed against the substrate.
[0068] Examples of the material for the optical imprinting mold include light-transmitting materials such as quartz, ultraviolet-transmitting glass, sapphire, diamond, silicone materials such as polydimethylsiloxane, fluororesins, cycloolefin resins, and other light-transmitting resin materials. If the substrate used is a light-transmitting material, the imprinting mold may be made of a material that does not transmit light. Examples of light-transmitting materials include metal, SiC, and mica. Among these, a quartz mold is particularly preferred because it transmits ultraviolet light well, has high hardness, and has high surface smoothness. The mold for photoimprinting may be of any shape, such as a flat shape, a belt shape, a roll shape, or a roll belt shape.
[0069] The mold for photoimprinting may be subjected to a release treatment to improve releasability between the photocurable composition and the mold surface. Examples of the release treatment include treatment with a silicone-based or fluorine-based silane coupling agent.
[0070] Regarding the method of irradiating light, when the mold is made of a material that transmits light, a method of irradiating light from the mold side can be used, and when the base material is made of a material that transmits light, a method of irradiating light from the base material side can be used.
[0071] When there is a concern about the conformability of the pattern to be formed, the composition may be heated to a temperature at which sufficient fluidity is obtained upon irradiation with light. The temperature when heating is preferably 0 to 300° C., more preferably 0 to 200° C., further preferably 0 to 150° C., and particularly preferably 25 to 80° C. Within the above temperature range, the shape of the pattern formed from the photocurable composition is maintained with good accuracy.
[0072] After curing, the mold is released to obtain a cured film having a concave-convex pattern formed by transferring the concave-convex pattern of the mold. In order to prevent deformation such as warping of the substrate and to increase the accuracy of the concave-convex pattern, the peeling step is preferably performed after the temperature of the cured film has decreased to around room temperature (25°C).
[0073] If any residue of the cured product is found on the mold after it is released, it is advisable to clean it with a cleaning solution. Since the mold is used repeatedly, any residue of the cured product on the mold may adversely affect pattern formation. The photocurable organopolysiloxane contained in the photocurable organopolysiloxane composition of the present invention is a Si-OR 11 -Y, and the polymerizable functional group Si-OR 11 Since the moiety is highly decomposable in cleaning fluids, the photocurable organopolysiloxane composition of the present invention has excellent reworkability.
[0074] The cleaning liquid used for cleaning the mold may be appropriately selected depending on the material of the mold, and either an acid cleaning liquid or an alkaline cleaning liquid can be used. Examples of acid cleaning solutions include sulfuric acid, hydrochloric acid, nitric acid, carbonic acid, acetic acid, phosphoric acid, aqua regia, dilute hydrofluoric acid, sulfuric acid / hydrogen peroxide, and hydrochloric acid / hydrogen peroxide. Examples of alkaline cleaning solutions include caustic alkalis such as caustic soda and caustic potash, inorganic alkalis such as various silicates, phosphates, and carbonates, as well as organic alkalis such as tetramethylammonium hydroxide, ammonia water, ammonia hydrogen water, and ammonia hydrogen peroxide.
[0075] Since the alkaline cleaning solution may dissolve SiO2, when the mold is made of glass or quartz, an acid cleaning solution is preferred, and sulfuric acid / hydrogen peroxide is particularly preferred. In particular, when cleaning a quartz mold having a fine pattern of 100 nm or less, the rectangular shape of the mold may be damaged by the alkaline cleaning solution's dissolving action on SiO2, so by using an acid cleaning solution, the mold can be cleaned without damaging the fine pattern and can be used repeatedly.
[0076] The cleaning method is not particularly limited, but examples thereof include spraying, showering, immersion, heated immersion, ultrasonic immersion, spinning, bubbling, rocking, brushing, steaming, polishing, and the like. In order to prevent redeposition of cleaned contaminants, the spinning method is particularly preferred.
[0077] The laminate produced using the photocurable organopolysiloxane composition of the present invention may be prepared by applying a resist material onto a substrate and curing it in situ to form a resist film, or by peeling off the resist film formed on the temporary substrate and attaching it to a substrate to form a laminate. If the resist film is patterned, the laminate can be dry-etched to obtain a patterned product in which the pattern is transferred to the substrate by dry etching.
[0078] The gas used for dry etching may be any known gas, for example, oxygen atom-containing gas such as oxygen, carbon monoxide, carbon dioxide, etc., inert gas such as helium, nitrogen, argon, etc., chlorine-based gas such as chlorine, boron trichloride, etc., fluorine gas, fluorocarbon-based gas, hydrogen gas, ammonia gas, etc., and these gases may be used alone or in appropriate mixture. By etching with these etching gases, a desired pattern can be formed on a substrate. EXAMPLES
[0079] The present invention will be specifically described below with reference to examples and comparative examples. However, the present invention is not limited to the following examples.
[0080] The following silicone oligomer having an alkoxysilyl group was used to produce the photocurable organopolysiloxane described below. Alkoxysilane compound (a-1): "KR-500" manufactured by Shin-Etsu Chemical Co., Ltd., trifunctional monomer base, viscosity: 25 mPas, methoxy group content: 28% by mass Alkoxysilane compound (a-2): "X-40-9225" manufactured by Shin-Etsu Chemical Co., Ltd., trifunctional monomer base, viscosity: 100 mPas, methoxy group content: 24% by mass Alkoxysilane compound (a-3): "DOWSIL AY42-163" manufactured by Dow Toray Co., Ltd., trifunctional monomer base, viscosity: 30 mPas, methoxy group content: 25% by mass Alkoxysilane compound (a-4): "DOWSIL SR2402" manufactured by Dow Toray Co., Ltd., trifunctional monomer base, viscosity: 26 mPas, methoxy group content: 31% by mass Alkoxysilane compound (a-5): "X-40-9250" manufactured by Shin-Etsu Chemical Co., Ltd., based on bifunctional and trifunctional monomers, viscosity: 80 mPas, methoxy group content: 25% by mass Alkoxysilane compound (a-6): "KC-89S" manufactured by Shin-Etsu Chemical Co., Ltd., trifunctional monomer base, viscosity: 5 mPas, methoxy group content: 45% by mass Alkoxysilane compound (a-7): "X-40-9246" manufactured by Shin-Etsu Chemical Co., Ltd., based on bifunctional and trifunctional monomers, viscosity: 80 mPas, methoxy group content: 12% by mass Alkoxysilane compound (a-8): "Methyl Silicate 51" manufactured by Colcoat Co., Ltd., tetrafunctional monomer base, viscosity: 5 mPas, methoxy group content: 66% by mass
[0081] [Example 1: Preparation and evaluation of photocurable organopolysiloxane] A reaction vessel was charged with 200 parts by mass of alkoxysilane compound (a-1), 128 parts by mass of 2-hydroxyethyl acrylate, and sulfuric acid (50 ppm by mass). The mixture was stirred and reacted for 8 hours under heating at 70°C while distilling off the produced methanol, to obtain 294 g of photocurable organopolysiloxane (A-1).
[0082] The resulting photocurable organopolysiloxane (A-1) was subjected to the following evaluations, and the results are shown in Table 1.
[0083] (Polymerizable Functional Group Content) Regarding the obtained photocurable organopolysiloxane 1 H-NMR measurement was carried out, and the content of polymerizable functional groups was calculated from the detected spectrum intensity. Specifically, in Example 1, 2-hydroxyethyl acrylate was used to prepare the photocurable organopolysiloxane, and the content of polymerizable functional groups bonded to the polysiloxane resin was calculated from the ratio of the intensity of the peak (δ=3.97, CH2-O-Si) in the spectrum generated by bonding 2-hydroxyethyl acrylate and the silicone oligomer via a Si-O-C bond to the peak derived from a standard substance added in advance to the measurement sample.
[0084] In addition, the above 1 H-NMR was carried out under the following conditions. Measurement equipment: "AVANCE NEO 400" manufactured by Bruker Japan Co., Ltd. Magnetic field strength: 400MHz Number of times: 16 Solvent: Deuterated chloroform (CDCl3) Sample concentration: 30mg / 0.6ml
[0085] (Residual alkoxysilyl group amount) The photocurable organopolysiloxane obtained was subjected to the same measurement of the content of polymerizable functional groups under the same conditions. 1 H-NMR measurement was carried out, and the content of alkoxysilyl groups was calculated from the detected spectrum intensity. Specifically, in Example 1, a silicone oligomer having a methoxy group was used to prepare a photocurable organopolysiloxane, and the amount of remaining alkoxysilyl groups (methoxysilyl groups) was calculated from the ratio of the intensity of the peak of the methoxy group of the silicone oligomer in the spectrum (δ=3.52, Si-OCH3) to the peak derived from a standard substance that was added in advance to the measurement sample.
[0086] (Polysiloxane Structure Content) The content of the polysiloxane structure in the photocurable organopolysiloxane was evaluated by measuring the ash content. Specifically, about 1.0 g of the obtained photocurable organopolysiloxane was weighed out and placed in a crucible, and dried in a dryer at 130°C for 30 minutes. The crucible was then moved to an electric furnace and fired at 850°C for 3 hours. After cooling, it was taken out and the ash content derived from the polysiloxane structure was calculated from the weight loss, and evaluated according to the following criteria. The higher the content of polysiloxane structure, the greater the durability and weather resistance of the cured product. (A): 45% by mass or more (B): 35% by mass or more and less than 45% by mass (C): Less than 35% by mass
[0087] (Applicability evaluation) Approximately 1.0 g of the obtained photocurable organopolysiloxane was weighed out and the viscosity was measured using an E-type viscometer (manufactured by Toki Sangyo, product name: TV-22) with the stage temperature set to 25°C, at a rotation speed of 100 rpm and rotor No. 1, and evaluated according to the following criteria: The lower the viscosity, the better the coatability. (A): 100mPas or less (B): More than 100mPas and less than 150mPas (C):More than 150mPas
[0088] (Storage modulus evaluation) A photocurable composition was prepared by mixing 100 parts by mass of the obtained photocurable organopolysiloxane, 2 parts by mass of 1-hydroxycyclohexyl-phenyl ketone ("OMNIRAD184" manufactured by IGM) as a photopolymerization initiator, and 0.02 parts by mass of p-methoxyphenol as a polymerization inhibitor, and diluting the mixture with propylene glycol monomethyl ether acetate as a solvent to a solids concentration of 50% by mass.
[0089] The photocurable composition thus obtained was spin-coated onto a 6-inch silicon wafer at 1500 rpm for 30 seconds, and then baked on a hot plate at 80°C for 60 seconds to form a coating film. At this time, the film thickness was approximately 2.0 μm. Next, using a UV irradiation device (manufactured by Minaga Electric Manufacturing Co., Ltd.), the coating film was irradiated with 100 mJ / cm2 under a nitrogen atmosphere. 2 A UV-cured film was obtained by irradiation. The storage modulus E' of the obtained cured film was measured at an indentation depth of 200 nm using a nanoindenter ("ENT2100" manufactured by Elionix) and evaluated according to the following criteria. The storage modulus E' is an index of the durability of the cured film, and the higher the better. (A):1,500MPa or more (B): 1,000 MPa or more and less than 1,500 MPa (C): Less than 1,000 MPa
[0090] (Reworkability evaluation) The cured film prepared for the storage modulus evaluation was immersed in sulfuric acid / hydrogen peroxide solution (sulfuric acid:hydrogen peroxide solution = 4:1 (volume ratio)) for 5 minutes, and then rinsed with ion-exchanged water for 30 seconds. The state of the cured film during this process was visually observed, and the reworkability of the cured film was evaluated according to the following criteria. (A): The cured film dissolves in sulfuric acid / hydrogen peroxide and does not remain on the silicon wafer. (B): The cured film peeled off from the silicon wafer, and no film remained on the silicon wafer. (C): No change was observed in the cured film.
[0091] [Examples 2-6 and Comparative Examples 1-2: Preparation and Evaluation of Photocurable Organopolysiloxanes] Photocurable organopolysiloxanes were produced in the same manner as in Example 1, except that the alkoxysilane compounds and 2-hydroxyethyl acrylate were used in the amounts shown in Table 1, and the same evaluations were carried out as in Example 1. The results are shown in Tables 1 and 2.
[0092] [Table 1]
[0093] [Table 2]
[0094] In Comparative Example 6, a photocurable silicone monomer represented by the following formula was used in place of the photocurable organopolysiloxane.
[0095] [ka]
[0096] The results in Tables 1 and 2 show that by using an organopolysiloxane in which the proportion of T units and the amount of polymerizable functional groups and alkoxysilyl groups are within specific ranges, a cured product with excellent durability and reworkability can be obtained.
Claims
1. A photocurable organopolysiloxane having a polymerizable functional group and an alkoxysilyl group, represented by the following general formula (1): The ratio of T units to all siloxy units is 70 mol % or more, A photocurable organopolysiloxane containing 40% by mass or more of the polymerizable functional group represented by the general formula (1) and containing the alkoxysilyl group in the range of 0.1 to 10% by mass. [Formula 1] (In the general formula (1), R 11 is a single bond or an alkylene group having 1 to 12 carbon atoms, Y is a group containing a carbon-carbon unsaturated bond, * indicates the bonding position with the silicon atom of the organopolysiloxane.)
2. 2. The photocurable organopolysiloxane according to claim 1, wherein the polymerizable functional group represented by the general formula (1) is a polymerizable functional group represented by the following general formula (1-2): [Case 2] (In the general formula (1-2), R 11 is a single bond or an alkylene group having 1 to 12 carbon atoms, R 12 is a hydrogen atom or an alkyl group having 1 to 12 carbon atoms, * indicates the bonding position with the silicon atom of the organopolysiloxane.)
3. 3. The photocurable organopolysiloxane according to claim 1, wherein the content of the polysiloxane structure is 35% by mass or more.
4. 3. The photocurable organopolysiloxane according to claim 1, which has a viscosity at 25° C. of 150 mPas or less.
5. A photocurable organopolysiloxane composition comprising the photocurable organopolysiloxane according to claim 1 or 2 and a photopolymerization initiator.
6. 6. The photocurable organopolysiloxane composition according to claim 5, which is a resist composition.
7. A cured product of the photocurable organopolysiloxane composition according to claim 5.
Citation Information
Patent Citations
Composition for nanoimprint, and method of forming pattern
JP2011023698A
Composition comprising resin-linear organosiloxane block copolymer and organopolysiloxane
JP2015516478A
Curable composition, resist material and resist film
WO2016072202A1