Coating composition for rubber sealing member
A coating composition of HNBR and perfluorofluororesin with a specific blending ratio and silane coupling agent addresses the issue of non-adhesion to metal, ensuring durable and effective sealing performance for rubber seal members.
Patent Information
- Application Number
- JP2023082365
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-18
- Publication Date
- 2024-11-28
AI Technical Summary
Existing coating compositions for rubber seal members fail to maintain non-adhesion to metal surfaces over a long period, compromising sealing performance and durability.
A coating composition comprising hydrogenated acrylonitrile butadiene rubber (HNBR) and perfluorofluororesin, specifically a tetrafluoroethylene/hexafluoropropylene copolymer, with a blending ratio of 25:75 to 55:45, along with a silane coupling agent, forms a coating film that exhibits excellent non-tackiness and durability on rubber seal members.
The composition provides long-lasting non-adhesion to metal, maintains sealing performance, and enhances abrasion resistance, while being environmentally friendly and cost-effective due to its water-based formulation.
Smart Images

Figure 2024165833000001 
Figure 2024165833000002 
Figure 2024165833000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a fluororesin coating composition suitable for use in rubber sealing members, and more particularly to a fluororesin coating composition capable of imparting excellent non-adhesive properties to metals to rubber sealing members that come into contact with metals. [Background technology]
[0002] Rubber sealing members such as seal rings, gaskets, valve seals, check valves, etc. are widely used in the fields of automobiles, industrial machinery, etc. In rubber sealing members, a film made of a coating agent containing a rubber component and fluororesin particles may be formed on the surface of the rubber sealing member for the purpose of preventing adhesion to the mating material, instantaneous opening and closing of the seal, etc. As such a coating agent, for example, the following Patent Document 1 describes a coating agent for oil seals, which is prepared as an organic solvent solution containing 100 parts by weight of isocyanate group-containing 1,2-polybutadiene, 10 to 90 parts by weight in total of fluororesin particles having a particle size of 2 μm or less and filler particles other than the fluororesin particles having a particle size of 0.5 to 30 μm, and 10 to 40 parts by weight of wax having a melting point of 40 to 160° C., and in which the fluororesin particles are used in a proportion of 20 to 80% by weight of the total filler amount.
[0003] The present inventors have also proposed a coating composition capable of forming a coating film that exhibits excellent releasability over a long period of time on substrates with poor heat resistance, such as rubber or plastic substrates (see Patent Document 2 below). This coating composition also has high coating film adhesion to substrates, and so its use on rubber seal members as mentioned above is also being considered. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2021 / 014901 [Patent Document 2] JP 2022-136748 A Summary of the Invention [Problem to be solved by the invention]
[0005] Rubber sealing members that are used in contact with metals are required to be non-sticky so as not to adhere to metal members even when lightly touching them, so as not to impair their sealing performance (sealing rings and gaskets do not stick to metal members, and valve seals and valves are capable of instantaneous opening and closing). However, it was found that the coating film made of the paint composition described in Patent Document 2 is excellent in terms of imparting releasability to bladders, etc., but is unable to control the non-stickiness (non-tacking properties) required for metals.
[0006] Therefore, an object of the present invention is to provide a coating composition capable of forming a coating film having excellent durability and exhibiting excellent adhesion to a rubber substrate and non-stickiness (non-tacking properties) to the mating metal member for a long period of time in a rubber sealing member used in contact with metal. Another object of the present invention is to provide a rubber sealing member, such as a seal ring, a gasket, a valve seal, or a check valve, which has a coating film that has excellent non-adhesive (non-tacking) properties with respect to metal members. [Means for solving the problem]
[0007] According to the present invention, there is provided a coating composition for rubber sealing members, which contains hydrogenated acrylonitrile butadiene rubber (hereinafter sometimes referred to as "HNBR") and perfluoro fluororesin (hereinafter sometimes simply referred to as "fluororesin"), and is characterized in that the blending ratio (solid content mass ratio) of the hydrogenated acrylonitrile butadiene rubber to the perfluoro fluororesin is 25:75 to 55:45.
[0008] In the coating composition for rubber seal members of the present invention, (1) The perfluororesin is a heat-meltable perfluororesin; (2) The heat-meltable perfluororesin is a tetrafluoroethylene-hexafluoropropylene copolymer; (3) Contains a silane coupling agent; (4) The hydrogenated acrylonitrile butadiene rubber and the perfluororesin are in the form of an aqueous dispersion, and the composition is an aqueous coating composition; (5) the compounding ratio (solid content mass ratio) of the hydrogenated acrylonitrile butadiene rubber to the perfluoro fluorine resin is 35:65 to 50:50; is preferred.
[0009] The present invention also provides a rubber sealing member characterized in that the surface thereof is coated with a coating film containing hydrogenated acrylonitrile butadiene rubber and perfluororesin in a blending ratio (mass ratio of solid contents) of 25:75 to 55:45.
[0010] In the rubber seal member of the present invention, (1) The perfluororesin is a heat-meltable perfluororesin; (2) The heat-meltable perfluororesin is a tetrafluoroethylene-hexafluoropropylene copolymer; (3) A φ5 mm probe (made of SUS304) is pressed against the coating at room temperature with a load of 100 gf at a speed of 5 mm / min. The probe is held at this load for 3 seconds, and then the probe is pulled away at a speed of 10 mm / min. The adhesive force (peak value) received by the probe is 20 gf or less. (4) A seal ring, gasket, valve seal, or check valve; is preferred. Effect of the Invention
[0011] The coating composition for rubber sealing members of the present invention can impart non-stickiness (non-tacking properties) to rubber sealing members so that they do not adhere at all even when lightly contacted with the mating metal material, allowing the rubber sealing members to optimally exhibit the sealing performance they should have.The coating composition also has excellent abrasion resistance and can maintain such excellent non-stickiness for a long period of time. In addition, the coating composition for rubber sealing members of the present invention has elasticity and can form a coating film with excellent conformability at low temperatures even on rubber sealing members that do not have high heat resistance, and also has excellent durability. Furthermore, the coating composition for rubber sealing members of the present invention can be made into an aqueous coating composition in which HNBR and a fluororesin are dispersed in water, and therefore is also excellent in terms of the environment and cost. Furthermore, rubber sealing members such as seal rings and check valves having a coating film made of the coating composition of the present invention have excellent non-stick properties that prevent them from sticking even when they come into contact with metal, and the sealing performance of the rubber sealing members is maintained without being impaired. Furthermore, it is possible to form a coating film at low temperatures on the surface of rubber seal members, which have poor heat resistance, and this also provides excellent productivity. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] (Paint composition) The coating composition for rubber seal members of the present invention is characterized in that the blending ratio (solid mass ratio) of the HNBR to the fluororesin is 25:75 to 55:45 in the coating composition containing hydrogenated acrylonitrile butadiene rubber and perfluororesin, and it is particularly preferable that the blending ratio is 35:65 to 50:50. When the blending amount of HNBR is less than the above range, it is difficult to form a continuous coating film compared to when it is within the above range, and there is a risk of coating defects such as cracks occurring, and there is a risk of the adhesion between the rubber seal member and the coating film decreasing. On the other hand, when the blending amount of HNBR is more than the above range, it is difficult to impart the desired non-stickiness to the coating film compared to when it is within the above range.
[0013] [Hydrogenated acrylonitrile butadiene rubber (HNBR)] In the coating composition of the present invention, the HNBR, which serves as the base resin, has heat resistance, durability after vulcanization, adhesion to rubber sealing members, and non-stick properties, and also has the property of being able to maintain an elongation of 50% or more even after the formation of a coating film. HNBR is used in an unvulcanized state and is vulcanized when the coating film is formed. Since the vulcanization temperature can be kept below 200°C (preferably below 180°C), the coating composition of the present invention can be used without problem on rubber sealing members that can be used at temperatures above that temperature. The HNBR preferably has a hydrogenation rate of 80 to 99%, an acrylonitrile content of 18 to 50 mass%, and a Mooney viscosity at 100° C. ML(1+4) (in accordance with JIS K6300) of 30 to 150. When the coating composition of the present invention is a water-based coating composition, an aqueous dispersion (latex) of HNBR prepared by a conventional method is suitably used.
[0014] [Perfluororesin] In the coating composition of the present invention, the perfluororesin is contained, so that the surface energy of the coating film is reduced, the slipperiness is improved, and the non-adhesiveness of the coating film can be controlled. In addition, the abrasion resistance is improved by reducing the friction coefficient, so that the non-adhesiveness is maintained for a long period of time, and the durability is also improved. Furthermore, as described below, by baking the coating at a temperature of around 180°C, the fluororesin particles do not melt in the coating, but instead form a sea-island structure in which the fluororesin particles are islands in a matrix (sea) made of HNBR, so the elasticity of the HNBR coating is not impaired.
[0015] Examples of such perfluororesins include, but are not limited to, polytetrafluoroethylene (PTFE), low molecular weight polytetrafluoroethylene (low molecular weight PTFE), tetrafluoroethylene-perfluoro(alkyl vinyl ether) copolymer (PFA), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), tetrafluoroethylene-hexafluoropropylene-perfluoro(alkyl vinyl ether) copolymer, and other heat-meltable perfluororesins. Among these, heat-meltable perfluororesins, particularly FEP, can be preferably used. As described later, it is difficult to form a coating film on a rubber seal member by high-temperature treatment, so by using FEP, which has a low melting point among the above fluororesins, a good coating film can be formed on the rubber seal member. In addition, as is clear from the results of the examples described later, the adhesion to the rubber seal member is also superior to other fluororesins. FEP may be a copolymer consisting of only tetrafluoroethylene (TFE) and hexafluoropropylene (HFP), or may be a copolymer consisting of TFE, HFP, and polymerization units based on a monomer copolymerizable with TFE and HFP. Examples of the polymerization units based on a monomer copolymerizable with TFE and HFP include perfluoro(alkyl vinyl ether). The amount of tetrafluoroethylene (TFE) in the FEP is preferably in the range of 75 to 97% by mass.
[0016] The melt flow rate (MFR) of the melt processable fluororesin is preferably 1 to 100 g / 10 min, more preferably 1 to 80 g / 10 min, and further preferably 1 to 50 g / 10 min. The MFR is measured at a temperature of 372° C. and a load of 5 kg using a melt indexer in accordance with ASTM D1238.
[0017] The fluororesin can be used as fluororesin powder particles, but since excellent non-stickiness can be obtained by finely dispersing the fluororesin particles in the coating film, it is preferable to mix the dispersion obtained by emulsion polymerization and use it as a raw material for the paint. The average particle size of the fluororesin particles is preferably 0.5 μm or less, and particularly 0.3 μm or less. In the present invention, the average particle size means the particle size at 50% of the cumulative value in the particle size distribution determined by the laser diffraction / scattering method.
[0018] [Silane coupling agents] The coating composition of the present invention preferably contains a silane coupling agent in order to improve adhesion between the coating film and the rubber sealing member. Silane coupling agents that can be used in the coating composition of the present invention may be conventionally known, and are not limited thereto. Examples of such agents include amino group-containing silane coupling agents such as γ-(2-aminoethyl)aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, N-β(aminoethyl)γ-aminopropyltrimethoxysilane, and N-β(aminoethyl)γ-aminopropylmethyldimethoxysilane; glycidyl group-containing silane coupling agents such as γ-glycidoxypropyltrimethoxysilane and γ-glycidoxypropylmethyldimethoxysilane; and γ-mercaptopropyltrimethoxysilane. Examples of the silane coupling agents include mercapto group-containing silane coupling agents such as vinyltriethoxysilane, vinyltrimethoxysilane, vinyltris(methoxyethoxy)silane, etc.; vinyl group-containing silane coupling agents such as vinyltriethoxysilane, vinyltris(methoxyethoxy)silane, etc.; (meth)acryloyl group-containing silane coupling agents such as γ-(meth)acryloyloxypropyltrimethoxysilane, γ-(meth)acryloyloxypropyltriethoxysilane, γ-(meth)acryloyloxypropyldimethoxymethylsilane, etc.; and isocyanate group-containing silane coupling agents such as γ-isocyanatepropyltriethoxysilane, γ-isocyanatepropyltrimethoxysilane, etc.
[0019] The silane coupling agent is preferably blended in an amount of 0.5 to 3.0 mass %, particularly 0.8 to 2.5 mass %, based on the total solid content of the resin (total of HNBR and fluororesin) in the coating composition. If the amount of the silane coupling agent is less than the above range, the above-mentioned effects obtained by blending the silane coupling agent are not sufficiently obtained, while if the amount of the silane coupling agent is more than the above range, the non-adhesiveness of the coating film may be impaired compared to when it is within the above range.
[0020] [Preparation of coating composition] The coating composition of the present invention may be in the form of a water-based or solvent-based coating composition, or a powder coating composition, but is preferably a water-based coating composition in consideration of environmental aspects. The coating composition may be prepared, but is not limited to, by the following preparation method. When the coating composition of the present invention is prepared as a water-based coating composition, it can be prepared by mixing an aqueous dispersion (latex) of HNBR or a solution of a precursor of HNBR prepared by a conventional method with an aqueous dispersion of fluororesin particles or a mixture thereof (for example, an existing water-based fluororesin coating material) so that the blending ratio (mass ratio of solid contents) of HNBR to fluororesin is 25:75 to 55:45, and further adding a silane coupling agent or other additives described later, if necessary, and mixing.
[0021] The aqueous dispersion of HNBR can be prepared by a conventionally known method, including but not limited to emulsion polymerization, suspension polymerization, a method using an emulsifying device such as a high-speed homogenizer, an inversion emulsification method, a phase inversion temperature emulsification method, an emulsification method using a surfactant, or the like. In the aqueous dispersion of HNBR, it is preferable that HNBR particles having an average particle size of 0.01 to 0.5 μm are dispersed in the aqueous dispersion at 10 to 70 mass %. The aqueous dispersion of fluororesin particles can be prepared by uniformly and stably dispersing the fluororesin particles in an aqueous medium using a surfactant or the like, or by subjecting the fluororesin to aqueous emulsion polymerization using a surfactant and an initiator, and if necessary, a chain transfer agent, etc. A commercially available aqueous dispersion of fluororesin prepared from an aqueous dispersion obtained by aqueous emulsion polymerization can also be used. In the fluororesin aqueous dispersion, it is preferable that fluororesin particles having an average particle size of 0.01 to 180 μm are dispersed in the aqueous dispersion at 10 to 70 mass %. In particular, an aqueous dispersion of fluororesin particles having an average particle size of 0.1 to 0.3 μm is preferably used.
[0022] In the coating composition of the present invention, the above-mentioned aqueous dispersion of HNBR and aqueous dispersion of fluororesin can be used as is, but fillers and various additives used in ordinary coatings can also be added depending on the desired properties, such as dispersibility, electrical conductivity, foaming prevention, and improved abrasion resistance. For example, surfactants (e.g., Leocol (registered trademark) manufactured by Lion Corporation, Polyoxyethylene alkyl ethers, polyoxyethylene alkyl phenyl ether-based nonionic surfactants such as TRITON (registered trademark), TERGITOL (registered trademark) series, and Kao Corporation's Emulgen (registered trademark); sulfosuccinates, alkyl ether sulfonates, mono-long-chain alkyl sulfate-based anionic surfactants such as Lion Corporation's Repearl (registered trademark), Kao Corporation's Emal (registered trademark), and Pelex (registered trademark); polycarboxylates, acrylate-based polymer surfactants, such as Lion Corporation's Leoar (registered trademark) and Dow Chemical Company's OROTAN (registered trademark); film-forming agents (for example, polymer-based film-forming agents such as polyamide, polyamideimide, acrylic, and acetate, higher alcohols, ethers, and polymer surfactants having a film-forming effect), thickeners (water-soluble celluloses, solvent dispersion thickeners, sodium alginate, casein, sodium caseinate, xanthan gum, polyacrylic acid, and acrylic acid esters) can also be added.
[0023] <Water-based paint composition> The water-based coating composition of the present invention can be prepared by mixing and stirring the aqueous dispersion of HNBR prepared by the above-mentioned method, the aqueous dispersion of the fluororesin, or an aqueous composition thereof (such as a solution or a ready-made coating material). In an aqueous coating composition, it is preferable to use water as the main medium from the standpoint of environmental and cost considerations, but a polar solvent that is compatible with water can also be added from the standpoint of adjusting the rheological properties such as the viscosity of the coating composition, improving the dispersibility of the filler, or improving the volatility of the solvent during drying after coating to form a uniform coating film.
[0024] Examples of such polar solvents include, but are not limited to, methanol, ethanol, 1-propanol, 2-propanol, ethylene glycol, diethylene glycol, diethylene glycol monomethyl ether, triethylene glycol monomethyl ether, diethylene glycol monoethyl ether, triethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monobutyl ether, triethylene glycol monobutyl ether, ethylene glycol hexyl ether, diethylene glycol hexyl ether, ethylene glycol monobutyl ether acetate, diethylene glycol monobutyl ether acetate, ethylene glycol phenyl ether, propylene glycol, propylene glycol monomethyl ether, dipropylene glycol monomethyl ether, tripropylene glycol monomethyl ether, Examples of the alkyl ether include ethyl ether, propylene glycol monopropyl ether, dipropylene glycol monopropyl ether, propylene glycol monobutyl ether, dipropylene glycol monobutyl ether, tripropylene glycol monobutyl ether, propylene glycol methyl ether acetate, dipropylene glycol methyl ether acetate, propylene glycol diacetate, propylene glycol phenyl ether, polyethylene glycol, polypropylene glycol, 3-methoxy-N,N-dimethylpropanamide, 3-butoxy-N,N-dimethylpropanamide, N-methyl-2-pyrrolidone (NMP), N-ethylmorpholine, N-formylmorpholine, N-acetylmorpholine, N,N'-dimethylethyleneurea, N,N-dimethylacetamide or N,N-dimethylformamide, and γ-butyrolactone.
[0025] <Solvent-based coating composition> When preparing a solvent-based coating composition, liquid HNBR, an HNBR solvent dispersion, a fluororesin solution, or a fluororesin solvent dispersion is prepared, and these are stirred and mixed to prepare the composition, and various additives exemplified for the water-based coating composition can be used.
[0026] <Powder coating composition> When used as a powder coating composition, the aqueous dispersion of HNBR and the aqueous dispersion of fluororesin prepared by the above method can be stirred to coagulate HNBR and fluororesin. Specifically, by stirring at a stirring speed of 100 to 500 rpm for 1 to 60 minutes, the aggregated granules having an average particle size of 1 to 200 μm are granulated, and then separated, washed, and dried to prepare a composite powder consisting of primary particles of HNBR and fluororesin. If necessary, large coarse particles having a particle size of 200 μm or more generated during the aggregation and granulation process can be crushed to make them finer. In order to chemically aggregate the primary rubber / fluororesin particles, it is preferable to mix in an electrolyte such as HCl, H2SO4, HNO3, H3PO4, Na2SO4, MgCl2, CaCl2, HCOONa, CH3COOK, (NH4)2CO3, etc. Furthermore, if necessary, it is preferable to add an organic solvent that is incompatible with water (preferably a fluorine-based solvent) to uniformly granulate the aggregated particles.
[0027] <Other> Various organic and inorganic fillers can be added to the coating composition of the present invention depending on the desired properties. Examples of organic fillers include engineering plastics such as polyarylene sulfide, polyether ether ketone, polyamide, and polyimide. Examples of inorganic fillers include metal powder, metal oxides (aluminum oxide, zinc oxide, tin oxide, titanium oxide, etc.), glass, ceramics, silicon carbide, silicon oxide, calcium fluoride, carbon black, graphite, mica, and barium sulfate. Fillers of various shapes such as particulate, fibrous, and flake shapes can be used, but in order to obtain the extensibility of the coating film required for the coating composition of the present invention, it is preferable to use particulate fillers with small anisotropy, and it is more preferable to use spherical fillers. In addition to the above, pigments and various additives that have traditionally been used in paints can be blended depending on the desired characteristics, such as electrical conductivity, foam prevention, improved abrasion resistance, improved corrosion resistance, coloring, etc. The use of these fillers can impart various properties to the coating.
[0028] The amount of filler to be blended depends on the type of filler used and cannot be generally determined, but is preferably in the range of 0.1 to 10 mass% based on the paint solids content of the paint composition (the total amount of HNBR, fluororesin, and filler). If the amount of filler to be blended is less than the above range, the improvement in properties due to the blending of the filler is poor, while if the amount is more than the above range, there is a risk that the non-stickiness will decrease and the stretchability will deteriorate compared to when the amount is within the above range. When the coating composition is a liquid coating such as a water-based coating, the filler is preferably used by dispersing it in a liquid medium such as water.
[0029] (Coating method) The coating composition of the present invention can be applied to the surface of a rubber sealant by a conventional coating method such as spray coating or dip coating. After coating, the coated coating composition is heated to the crosslinking temperature of HNBR to form a coating film. As described above, in the coating composition of the present invention, since the crosslinking temperature of HNBR is as low as 120 to 200°C, even if the coating composition is directly coated on a rubber seal member and then heat-treated, a uniform coating film can be formed without damaging the rubber seal member. The heating conditions (baking conditions) of the coating composition of the present invention vary depending on the composition and form of the coating composition, the coating amount, the desired crosslinking temperature, etc., and cannot be generally specified, but it is preferable to heat at a temperature equal to or higher than the crosslinking temperature of HNBR for 5 to 120 minutes. In addition, by carrying out the heat treatment multiple times, it is possible to promote crosslinking and improve abrasion resistance. Furthermore, since the coating composition of the present invention has excellent adhesion to rubber sealing members, it can be directly applied to the surface of a substrate without the need for a primer layer or surface treatment of the substrate.
[0030] (Rubber seal material) As described above, the coating composition of the present invention can form a coating film at low temperatures, and can exhibit excellent non-adhesiveness (non-tacking properties) that does not adhere to metal even when it lightly touches it, and has excellent adhesion to rubber substrates and elasticity that can follow the expansion and contraction of the rubber substrate. Therefore, it can be suitably used as a surface coating film for rubber seal members that come into contact with metal as a mating material, such as seal rings such as O-rings and oil seals, gaskets, valve seals, and umbrella-type check valves.
[0031] The rubber sealing member can be molded from various rubbers or thermoplastic elastomers (which may be collectively referred to as "rubber materials") depending on the type and application. Examples of rubber include, but are not limited to, saturated polyolefin-based rubbers such as ethylene-propylene copolymer, ethylene-α-olefin copolymer, propylene-α-olefin copolymer, chlorinated polyethylene, and chlorosulfonated polyethylene; α-olefin-diene copolymer-based rubbers such as ethylene-propylene-diene copolymer, α-olefin-diene copolymer, ethylene-diene copolymer, propylene-diene copolymer, and halogenated and hydrogenated versions of these; diene polymer-based rubbers such as isoprene rubber, butadiene rubber, and halogenated and hydrogenated versions of these; silicone-based rubbers such as methyl silicone rubber, vinyl-methyl silicone rubber, and phenyl-methyl silicone rubber; fluorinated silicone rubber; Examples of such rubbers include fluororubbers such as polyvinylidene fluoride rubber, tetrafluoroethylene-propylene rubber, and tetrafluoroethylene-perfluoromethylvinyl ether rubber; styrene-diene copolymer rubbers such as styrene-butadiene copolymer and styrene-isoprene copolymer; butyl rubber, its halides, hydrogenated products and other butyl-based rubbers; chloroprene, its halides, hydrogenated products and other chloroprene-based rubbers; epichlorohydrin rubber, epichlorohydrin-ethylene oxide rubber and other epichlorohydrin-based rubbers; polyether urethane rubber, polyester urethane rubber and other urethane-based rubbers; acrylonitrile-butadiene rubber, its halides, hydrogenated products and other acrylonitrile-butadiene-based rubbers; and natural rubber.
[0032] Examples of thermoplastic elastomers include styrene-butadiene-styrene block copolymers, styrene-isoprene-styrene block copolymers, styrene-ethylene-butadiene-styrene block copolymers, styrene-isoprene-butadiene-styrene block copolymers, styrene-ethylene-propylene-styrene block copolymers, halogenated and hydrogenated polystyrene-based thermoplastic elastomers, blends of olefin resins and olefin rubber, blends of olefin resins and olefin-diene copolymers, halogenated and hydrogenated polyolefin-based thermoplastic elastomers, polyurethane-based thermoplastic elastomers, and polyester-based thermoplastic elastomers.
[0033] The coating composition of the present invention is capable of imparting the desired non-stick properties to metals while maintaining excellent adhesion to sealing members made of the above-mentioned rubber materials, particularly fluororubber, butyl rubber, and ethylene-propylene rubber (EPM, EPDM). In addition, depending on the material used, a crosslinking agent, a polymerization initiator, a filler, a pigment, an ultraviolet absorber, an anti-aging agent, a foaming agent, an antifoaming agent, an antioxidant, etc. may be added to the above-mentioned rubber material constituting the rubber sealing member in a conventionally known manner. The coating film formed by the coating composition of the present invention has excellent durability and can maintain non-adhesive (non-tacking) properties for a long period of time, making it suitable for use as a coating material to be applied to the surfaces of automotive seal rings, etc.
[0034] (Paint film) The thickness of the surface coating of the rubber sealing member can be appropriately selected depending on the type and use of the sealing member, but when used to impart non-adhesiveness to the above-mentioned seal ring or check valve, it is preferable to apply so that the film thickness after heat treatment is 5 μm or more, particularly 5 to 300 μm. If the film thickness is thinner than the above range, a continuous coating cannot be formed compared to when it is within the above range, and there is a risk of coating defects occurring, and there is a risk of early loss of coating performance (non-adhesiveness (non-tacking property), slipperiness) due to wear. On the other hand, even if the film thickness is thicker than the above range, further improvement in coating performance such as non-adhesiveness cannot be expected, and it becomes less economical.
[0035] The coating film formed on the surface of the rubber seal member has excellent non-adhesive properties that prevent it from adhering to metals, which allows the seal member having such a coating film formed on its surface to exhibit excellent sealing performance as a seal member. Furthermore, the coating film formed on the surface of the rubber seal member has a contact angle with pure water of 90 degrees or more, preferably 95 degrees or more, which also proves that the coating film has high non-stickiness. Furthermore, the coating film formed on the surface of the rubber seal member has excellent adhesive strength (adhesion) to the rubber seal member. This allows the rubber seal member having such a coating film formed on its surface to stably maintain the excellent non-stickiness, abrasion resistance, stretchability, etc. that the coating film has for a long period of time. The method for measuring the peel strength to the rubber seal member will be described later. EXAMPLES
[0036] (Creating test pieces) The following three types of test pieces were used to evaluate the performance of rubber sealing members. Vinylidene fluoride rubber (FKM) (size: 100mm x 50mm x 2mmt, manufactured by Paltec Co., Ltd.) Ethylene propylene diene rubber (EPDM) (size: 100mm x 50mm x 2mmt, manufactured by Paltec Co., Ltd.) -Butyl rubber (IIR) sheet (size: 100mm x 50mm x 2mmt, manufactured by Paltec Co., Ltd.)
[0037] Each of the above substrates was sprayed with air using an air spray gun (ANEST IWATA Corp. W-88-10E2 φ1mm nozzle (manual gun)) at an air pressure of 2.5-3.0kgf / cm. 2 Then, coating was carried out by spraying the coating compositions of the examples and comparative examples described below. Coating was carried out so that the mass of the coated liquid was about 0.65 g (0.60 to 0.70 g) per substrate, and test pieces were prepared. The baking conditions are as follows: After drying by heating at 60°C for 10 minutes, it was transferred to another oven and heated at 120°C for 10 minutes, then transferred to another oven and heated for crosslinking at 180°C for 10 minutes, and then transferred to another oven. The secondary crosslinking treatment was carried out by heating at 120°C for 60 minutes.
[0038] (Evaluation method) [Coating film formation condition (visual inspection)] The resulting coating film was visually inspected for defects such as cracks. Coatings that did not have any defects such as cracks were deemed to pass. The results are shown in Table 2.
[0039] [Non-adhesiveness evaluation (tacking test)] Using a tacking tester TAC1000 manufactured by Rhesca Co., Ltd., a φ5mm probe (material: SUS304) was pressed against the sample at room temperature at a speed of 5mm / min with a load of 100gf, and the probe was held at this load for 3 seconds, after which it was pulled away at a speed of 10mm / min to measure the adhesive force (peak value) (gf) received by the probe. The results are shown in Table 2.
[0040] [Releasability evaluation (pure water contact angle (°))] Using the test pieces obtained by the above method, the contact angle (°) of pure water (droplet size: about 2 μL) was measured in a measurement environment of 25°C and 60% RH using a fully automatic contact angle meter (Kyowa Interface Science Co., Ltd. DM-701). The results are shown in Table 2.
[0041] [Adhesion evaluation (cross-cut test)] The coating surface of the test piece obtained by the above method was subjected to the following cross-cut test in accordance with JIS K 5600.5.6. (1) Using a cutter knife, make 11 cuts reaching down to the base material on the test surface to create 100 grids. A cutter guide was used, and the cuts were spaced 1 mm apart. (2) Firmly press Scotch tape (registered trademark) onto the grid area, then quickly peel off one end of the tape at a 45° angle and evaluate the condition of the grid. The evaluation results were expressed as the number of peeled squares (per 100), and are shown in Table 2.
[0042] [Evaluation of coating film stretchability] A dumbbell-shaped test piece (based on ASTM D-2116) was cut out from a test piece prepared by coating a butyl rubber (IIR) sheet with the coating compositions of Examples 2 to 5 described below, and a stretching test was carried out using a constant extension repeated fatigue tester (MYSS Tester, H9537 / H9606, manufactured by Mize Testing Instruments Co., Ltd.) under the following conditions: measurement temperature: 100°C, deviation stroke: 11 mm (50% stretched), stretching speed and return speed: 11 mm / min, and number of stretches: 100 times. After the test, the condition of the coating film was confirmed. None of the coating films made of the coating compositions of Examples 2 to 5 showed cracks or peeling.
[0043] [Paint film abrasion resistance test] The surface of an aluminum substrate (JIS A5052 compliant, 100mm x 50mm x 1mmt) was degreased with isopropyl alcohol, and the surface was roughened by shot blasting with #60 alumina (Showa Denko K.K., Showa Blaster) using a sandblaster (Fuji Manufacturing Co., Ltd., Pneumatic Blaster SGF-4(A)S-E566). Air pressure 2.5~3.0kgf / cm 2 Then, coating was carried out by spraying the coating compositions of the examples and comparative examples described below. Coating was carried out so that the mass of the coated liquid was about 0.65 g (0.60 to 0.70 g) per substrate, and test pieces were prepared. The baking conditions are as follows: After drying by heating at 60°C for 10 minutes, it was transferred to another oven and heated at 120°C for 10 minutes, then transferred to another oven and heated for crosslinking treatment at 180°C for 10 minutes, and then transferred to another oven and heated at 120°C for 60 minutes to perform a secondary crosslinking treatment.
[0044] The obtained test pieces were subjected to an abrasion resistance test in accordance with JIS K5600-5-10 (reciprocating test piece method) using a Suga abrasion tester NUS-ISO3 manufactured by Suga Test Instruments Co., Ltd. The test conditions were as follows. Load: 1N Number of reciprocations: 100 (stroke 30 mm) Abrasive paper used: Silicon carbide paper P-400 grade (width 12 mm) Wear Resistance (WR) was calculated from the change in mass before and after the measurement using the following formula. Measurements were performed three times, and the average values obtained are shown in Table 2.
[0045]
number
[0046] Example 1 2.08g of pure water and 203.3g of FEP aqueous dispersion as fluororesin (Teflon (registered trademark) FEP 120-JR, FEP resin solid content 54.5% by mass, manufactured by Mitsui-Chemours Fluoro Products Co., Ltd.) were placed in a 1-liter stainless steel beaker and stirred for 3 minutes at 200 rpm using a downflow type propeller-type 4-blade stirrer, and then 268.27g of hydrogenated acrylonitrile butadiene rubber aqueous dispersion (latex) (HNBR R2230LX, manufactured by Zeon Corporation, HNBR resin solid content 41.3% by mass) was added and further stirred for 5 minutes at 150 rpm. 7.79g of carbon black aqueous dispersion adjusted to a concentration of 25% by mass was added to the above mixture and stirred for 5 minutes at 250 rpm. To this were added 16.10 g of a 6% aqueous methylcellulose solution and 2.46 g of a silane coupling agent (KBM-603, manufactured by Shin-Etsu Chemical Co., Ltd.), and the mixture was stirred at 250 rpm for 15 minutes to obtain 500 g of a coating composition.
[0047] (Example 2, Example 3, Comparative Example 1, Comparative Example 2) The composition ratio of the fluororesin (FEP) and HNBR in the paint was adjusted to the ratio shown in Table 1, and the paint composition was prepared in the same manner as in Example 1 so that the concentration was also the same as in Example 1.
[0048] [Table 1]
[0049] Example 4 A coating composition was prepared by adjusting the composition ratio to be the same as in Example 3 using an aqueous PFA dispersion (Teflon (registered trademark) PFA 334-JR, manufactured by Mitsui-Chemours Fluoroproducts Co., Ltd., PFA resin solid content 60.0 mass%) as the fluororesin.
[0050] Example 5 A coating composition was prepared by adjusting the composition ratio to be the same as in Example 3 using an aqueous PTFE dispersion (Teflon (registered trademark) PTFE 31-JR, manufactured by Mitsui-Chemours Fluoroproducts Co., Ltd., PTFE resin solid content 59.4 mass%) as the fluororesin.
[0051] Comparative Example 3 A coating composition was prepared in the same manner as in Example 1, using only HNBR without using any fluororesin, and adjusting the resin solids concentration (total of fluororesin and HNBR) to the same concentration as in the coating composition of Example 1.
[0052] [Table 2] [Industrial Applicability]
[0053] The coating composition for rubber sealing members of the present invention is capable of forming a coating film that can impart excellent non-adhesive properties to metals for a long period of time, and can be suitably used as a coating for rubber sealing members such as seal rings, gaskets, valve seals, and check valves.
Claims
1. A coating composition for rubber seal members, comprising hydrogenated acrylonitrile butadiene rubber and a perfluoro fluorine resin, wherein the blending ratio (mass ratio of solid contents) of the hydrogenated acrylonitrile butadiene rubber to the perfluoro fluorine resin is 25:75 to 55:
45.
2. 2. A coating composition for rubber seal members according to claim 1, wherein said perfluororesin is a heat-meltable perfluororesin.
3. 3. A coating composition for rubber seal members according to claim 2, wherein said heat-meltable perfluororesin is a tetrafluoroethylene-hexafluoropropylene copolymer.
4. 3. The coating composition for rubber seal members according to claim 1 or 2, which further contains a silane coupling agent.
5. 3. A coating composition for rubber seal members according to claim 1, wherein said hydrogenated acrylonitrile butadiene rubber and said perfluororesin are in the form of an aqueous dispersion, and said coating composition is an aqueous coating composition.
6. 3. The coating composition for rubber seal members according to claim 1, wherein a compounding ratio (mass ratio of solid contents) of said hydrogenated acrylonitrile butadiene rubber and said perfluoro fluorine resin is 35:65 to 50:
50.
7. A rubber seal member characterized in that it has on its surface a coating film containing hydrogenated acrylonitrile butadiene rubber and perfluoro fluorine resin in a compounding ratio (mass ratio of solid contents) of 25:75 to 55:
45.
8. 8. The rubber sealing member according to claim 7, wherein the perfluororesin is a heat-meltable perfluororesin.
9. 9. The rubber seal member according to claim 8, wherein said heat-meltable perfluororesin is a tetrafluoroethylene-hexafluoropropylene copolymer.
10. 9. The rubber sealing member according to claim 7 or 8, wherein a φ5 mm probe (material: SUS304) is pressed against the coating film at room temperature at a speed of 5 mm / min with a load of 100 gf, and the probe is held at the 100 gf load for 3 seconds, and then pulled away at a speed of 10 mm / min. The adhesive force (peak value) received by the probe is 20 gf or less.
11. 9. The rubber sealing member according to claim 7 or 8, which is a seal ring, a gasket, a valve seal or a check valve.
Citation Information
Patent Citations
Paint composition
JP2022136748A
Coating agent for oil seal
WO2021014901A1