Ink set of water-based overprint varnish and water-based ink, and method for producing laminate

The ink set with a water-based overprint varnish and ink, containing specific resin emulsions and solvents, addresses the lack of resistance and leveling issues in existing water-based inks, providing superior printing quality on polyolefin substrates.

JP2024166047APending Publication Date: 2024-11-28TOYO INK MFG CO LTD

Patent Information

Application Number
JP2023208261
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-16
Filing Date
2023-12-11
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Existing water-based inks and overprint varnishes lack excellent leveling properties, abrasion resistance, water abrasion resistance, and alcohol resistance, which are essential for high-quality printing on packaging materials.

Method used

An ink set comprising a water-based overprint varnish containing an aqueous acrylic resin emulsion, a high boiling point solvent, and a phosphate ester compound, along with a water-based ink that may include an aqueous acrylic resin emulsion or urethane resin, to enhance film toughness and adhesion, thereby improving leveling properties and resistance to abrasion and alcohol.

Benefits of technology

The ink set achieves excellent leveling properties, abrasion resistance, and alcohol resistance, making it suitable for high-quality printing on polyolefin substrates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024166047000001
    Figure 2024166047000001
  • Figure 2024166047000002
    Figure 2024166047000002
  • Figure 2024166047000003
    Figure 2024166047000003
Patent Text Reader

Abstract

To provide an ink set of a water-based ink and a water-based overprint varnish with superior surface leveling, rub resistance, water friction resistance, and alcohol resistance.SOLUTION: The present invention provides an ink set of a water-based overprint varnish and a water-based ink, where the water-based overprint varnish contains a water-based acryl resin emulsion (A), a high-boiling solvent with a boiling point of 105°C or higher, and a phosphoester compound, and where the water-based ink contains a water-based acryl resin emulsion (C) and / or a water-based urethane resin.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an ink set of an aqueous overprint varnish and an aqueous ink, and a method for producing a laminate. [Background technology]

[0002] In recent years, it has become common for product packages and other wrapping materials to be printed for decoration and surface protection. In addition, the quality of the print, such as the design, beauty, and luxury of the printed matter, can stimulate consumer purchasing motivation, and is of great industrial value.

[0003] On the other hand, from the viewpoints of environmental problems such as air pollution caused by organic solvents, safety and health issues in the work environment, and disaster prevention, the use of organic solvent-free, water-based materials has long been considered in the fields of printing inks and paints. In order to improve various resistances such as abrasion resistance, the binder components of water-based inks and water-based overprint varnishes in practical use are almost always acrylic resin emulsions or mixtures of one or two types of alkali-soluble acrylic resins.

[0004] As for water-based inks and water-based overprint varnishes, Patent Documents 1 and 2 describe water-based inks containing water-based acrylic resin emulsions. Patent Document 3 describes oil-based inks containing urethane resins, and water-based overprint varnishes containing water-based acrylic resin emulsions and phosphate ester compounds. Patent Document 4 describes water-based inks containing water-based acrylic resin emulsions, and water-based overprint varnishes containing water-based acrylic resin emulsions and high-boiling point solvents. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent Publication No. 2022-096161 [Patent Document 2] JP 2016-155965 A [Patent Document 3] JP 2023-5160 A [Patent Document 4] Patent Publication No. 2021-38022 Summary of the Invention [Problem to be solved by the invention]

[0006] An object of the present invention is to provide an ink set of a water-based ink and a water-based overprint varnish that has excellent leveling properties, abrasion resistance, water-abrasion resistance and alcohol resistance. [Means for solving the problem]

[0007] As a result of extensive research into the above problems, the present inventors have found that the above problems can be solved by using the packaging material described below, and have thus completed the present invention.

[0008] That is, the present invention provides: An ink set of a water-based overprint varnish and a water-based ink, the aqueous overprint varnish comprises an aqueous acrylic resin emulsion (A), a high-boiling point solvent having a boiling point of 105° C. or more, and a phosphoric acid ester compound; The present invention relates to an ink set, wherein the water-based ink comprises a water-based acrylic resin emulsion (C) and / or a water-based urethane resin.

[0009] The present invention also relates to the above ink set, wherein a mass ratio of the high boiling point solvent to the phosphate ester compound is 5:5 to 9.9:0.1.

[0010] The present invention also relates to the above ink set, wherein the water-based overprint varnish further contains a hydrocarbon wax (B).

[0011] The present invention also relates to the above ink set, wherein the hydrocarbon wax (B) contains a hydrocarbon wax (B1) having an average particle size of 1.5 μm or more, and a hydrocarbon wax (B2) having an average particle size of less than 1.5 μm.

[0012] The present invention also relates to the above ink set, wherein the aqueous acrylic resin emulsion (A) has an acid value of 100 mgKOH / g or less.

[0013] The present invention also relates to the above ink set, wherein the aqueous acrylic resin emulsion (A) comprises an aqueous acrylic resin emulsion (A1) having a glass transition temperature of 60°C or higher, and an aqueous acrylic resin emulsion (A2) having a glass transition temperature of lower than 60°C.

[0014] The present invention also relates to the above ink set, wherein the water-based ink further comprises a water-soluble acrylic resin (D), and the acid value of the water-soluble acrylic resin (D) is 200 mgKOH / g or less.

[0015] The present invention also relates to the above ink set, wherein the water-based overprint varnish and / or the water-based ink further comprises a surfactant.

[0016] The present invention also relates to the above ink set, wherein the surfactant is an acetylene glycol-based surfactant.

[0017] The present invention also relates to the above ink set, which is for gravure printing or flexographic printing.

[0018] The present invention also relates to the above ink set, which is for use on a polyolefin substrate.

[0019] The present invention also provides a method for producing a laminate having a substrate, a printed layer, and a surface protective layer, the method comprising the steps of: printing an aqueous ink containing an aqueous acrylic resin emulsion (C) and / or an aqueous urethane resin on a substrate to form a printed layer; and printing an aqueous overprint varnish containing an aqueous acrylic resin emulsion (A), a high-boiling point solvent having a boiling point of 105°C or higher, and a phosphate ester compound onto the printed layer to form a surface protective layer. Effect of the Invention

[0020] The present invention makes it possible to provide an ink set of a water-based ink and a water-based overprint varnish that has excellent leveling properties, abrasion resistance, water-abrasion resistance and alcohol resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] The following describes the embodiments of the present invention in detail. However, the following description of the embodiments or requirements is merely an example of how the present invention can be implemented, and the present invention is not limited to these details as long as it does not deviate from the gist of the present invention.

[0022] <Ink set> In the ink set of an aqueous overprint varnish and an aqueous ink, the aqueous overprint varnish contains an aqueous acrylic resin emulsion (A), a high-boiling point solvent having a boiling point of 105°C or higher, and a phosphate ester compound, and the aqueous ink contains an aqueous acrylic resin emulsion (C) and / or an aqueous urethane resin. As an example of a preferred embodiment, there is a laminate in which a printed layer is formed by printing an aqueous ink on a substrate, and a surface protective layer is formed by printing an aqueous overprint varnish on the printed layer. (1) The aqueous ink contains an aqueous acrylic resin emulsion (A) and / or an aqueous urethane resin, thereby improving the toughness of the coating film and the adhesion to the surface protective layer; (2) The aqueous acrylic resin emulsion and the phosphoric acid group of the phosphoric acid ester compound contained in the aqueous overprint varnish interact with each other, thereby improving the toughness of the coating film; and (3) The aqueous overprint varnish further contains a high boiling point solvent, thereby improving the solubility of the aqueous acrylic resin emulsion (A) and the phosphoric acid ester compound, and also improving the film-forming properties of the coating film. It is presumed that the effects of (1) to (3) above have enabled the realization of excellent leveling properties, abrasion resistance, water abrasion resistance, and alcohol resistance. The above presumption does not limit the invention in any way.

[0023] <Water-based overprint varnish> The water-based overprint varnish of the present invention contains an aqueous acrylic resin emulsion (A), a high-boiling point solvent having a boiling point of 105° C. or higher, and a phosphate ester compound.

[0024] <Water-based acrylic resin emulsion (A)> The aqueous acrylic resin emulsion (A) is a polymer or copolymer obtained by polymerizing a monomer component mainly composed of (meth)acrylic acid and / or (meth)acrylate, and may be referred to as an aqueous (meth)acrylic resin hereinafter. It is preferably a styrene-acrylic copolymer resin. Here, "(meth)acrylic acid" refers to both "acrylic acid" and "methacrylic acid". "(meth)acrylate" refers to both "acrylate" and "methacrylate".

[0025] The weight average molecular weight of the aqueous acrylic resin emulsion (A) is preferably 10,000 to 600,000, more preferably 50,000 to 500,000, further preferably 100,000 to 400,000, and particularly preferably 200,000 to 300,000. When it is within the above range, the friction resistance and water friction resistance are improved. The acid value of the aqueous acrylic resin emulsion (A) is preferably 30 to 150 mgKOH / g, more preferably 40 to 100 mgKOH / g, and further preferably 50 to 70 mgKOH / g. When it is within the above range, the water friction resistance is improved.

[0026] The average particle size of the aqueous acrylic resin emulsion (A) is preferably from 10 to 300 nm, and more preferably from 60 to 100 nm. When it is within the above range, the leveling property, abrasion resistance, and water abrasion resistance are improved.

[0027] The aqueous acrylic resin emulsion (A) preferably contains an aqueous acrylic resin emulsion (A1) having a glass transition temperature of 60°C or higher, and an aqueous acrylic resin emulsion (A2) having a glass transition temperature of less than 60°C.

[0028] <Water-based acrylic resin emulsion (A1)> The water-based acrylic resin emulsion (A1) has a glass transition temperature of 60° C. or higher, preferably in the range of 60° C. to 110° C., and more preferably 70° C. to 90° C. When it is in the above range, the leveling property, abrasion resistance, and water abrasion resistance are improved.

[0029] <Water-based acrylic resin emulsion (A2)> The water-based acrylic resin emulsion (A2) has a glass transition temperature of less than 60° C., preferably from 0° C. to 55° C., and more preferably from 40° C. to 50° C. When it is within the above range, the leveling property, abrasion resistance, and water abrasion resistance are improved.

[0030] The aqueous acrylic resin emulsion (A) is preferably contained in an amount of 80% by mass or more, more preferably 90 to 99.5% by mass, and even more preferably 95 to 99% by mass, based on 100% by mass of the solid content of the aqueous overprint varnish. When it is in the above range, the abrasion resistance and water abrasion resistance are improved. In addition, the solid content ratio of the aqueous acrylic resin emulsion (A1) to the aqueous acrylic resin emulsion (A2) is preferably 5:5 to 9:1, and more preferably 7:3 to 8:2. When it is in the above range, the leveling property, abrasion resistance, and water abrasion resistance are improved.

[0031] The aqueous overprint varnish may contain a resin other than the aqueous acrylic resin emulsion (A), such as an aqueous styrene-maleic acid resin, an aqueous urethane resin, an aqueous polylactic acid resin, polyvinylpyrrolidone, starch, methyl cellulose, carboxymethyl cellulose, or modified resins thereof. The aqueous overprint varnish may contain one or more of the above resins. The aqueous acrylic resin emulsion (A) is preferably contained in an amount of 40% by mass or more, more preferably 60% by mass, and even more preferably 80 to 100% by mass, based on the total resin solid content in the aqueous overprint varnish. When the amount is within the above range, the leveling property, abrasion resistance, water abrasion resistance, and alcohol resistance are improved.

[0032] Examples of the (meth)acrylate include alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, cyclohexyl (meth)acrylate, stearyl (meth)acrylate, lauryl (meth)acrylate, behenyl acrylate, trimethylcyclohexyl (meth)acrylate, and isobornyl (meth)acrylate; and aromatic (meth)acrylates such as phenyl (meth)acrylate, benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, and phenoxydiethylene glycol (meth)acrylate. Heterocyclic (meth)acrylates such as tetrahydrofurfuryl (meth)acrylate and oxetane (meth)acrylate; alkoxypolyalkylene glycol (meth)acrylates such as methoxypolypropylene glycol (meth)acrylate and ethoxypolyethylene glycol (meth)acrylate; Examples of the methacrylic acid include N-substituted (meth)acrylamides such as (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N-isopropyl(meth)acrylamide, diacetone(meth)acrylamide, and acryloylmorpholine; amino group-containing (meth)acrylates such as N,N-dimethylaminoethyl(meth)acrylate and N,N-diethylaminoethyl(meth)acrylate; and nitriles such as (meth)acrylonitrile.

[0033] In one embodiment, the monomer components constituting the aqueous (meth)acrylic resin may further contain, in addition to (meth)acrylic acid and / or (meth)acrylate, an ethylenically unsaturated monomer other than these monomers. Examples of the ethylenically unsaturated monomer include styrene-based monomers such as styrene and α-methylstyrene, vinyl-based monomers such as vinyl acetate and vinyl chloride, and carboxyl-containing ethylenically unsaturated monomers such as itaconic acid, maleic acid, fumaric acid, and crotonic acid. Among these, it is preferable to use styrene-based monomers, which make it easier to obtain excellent gloss.

[0034] In one embodiment, the aqueous (meth)acrylic resin may be a copolymer of (meth)acrylic acid and / or (meth)acrylate with a styrene-based monomer. More specifically, the aqueous (meth)acrylic resin may be a copolymer obtained by copolymerization of (meth)acrylic acid, (meth)acrylate, and styrene.

[0035] Although not particularly limited, specific examples of combinations of monomers constituting the aqueous (meth)acrylic resin include acrylic acid / styrene / n-butyl methacrylate / 2-ethylhexyl acrylate, acrylic acid / methyl methacrylate / 1,4-cyclohexanedimethanol monoacrylate / n-butyl methacrylate / 2-ethylhexyl acrylate, acrylic acid / styrene / n-butyl methacrylate, methacrylic acid / methyl methacrylate / styrene, acrylic acid / styrene / n-butyl methacrylate / 2-ethylhexyl acrylate, and the like.

[0036] The emulsion resin can be prepared according to a method known in the art. For example, the emulsion resin can be prepared by carrying out emulsion polymerization under conditions in which the monomer components are emulsified in micelles and dispersed in water. For example, the emulsion polymerization can be carried out in the presence of ammonium persulfate and sodium metabisulfite. After the emulsion polymerization, a basic compound such as aqueous ammonia can be added to adjust the acid value of the resin, if necessary.

[0037] In one embodiment, the aqueous (meth)acrylic resin may be neutralized to improve its solubility or dispersibility in aqueous solvents. For example, after introducing acid groups such as carboxyl groups during the synthesis of the resin, some or all of the acid groups can be neutralized to increase hydrophilicity. The neutralization of the carboxyl groups can be carried out using amines such as triethylamine or other basic compounds.

[0038] The aqueous acrylic resin emulsion (A1) may be a commercially available product, such as Joncryl PDX-7538, Joncryl PDX-7667, Joncryl PDX-7700, etc., manufactured by BASF. The aqueous acrylic resin emulsion (A2) may also be a commercially available product, such as Joncryl 537E, Joncryl PDX-7775, Joncryl PDX-7789, etc., manufactured by BASF.

[0039] <High boiling point solvents with a boiling point of 105°C or higher> In the present invention, the aqueous overprint varnish contains a high-boiling point solvent. The surface protective layer can be formed by applying the overprint varnish and drying it, and a part of the high-boiling point solvent remains in the surface protective layer upon drying, improving the film-forming properties of the surface protective layer. The boiling point of the high boiling point solvent is 105° C. or higher, preferably 140 to 260° C., more preferably 180 to 250° C., and even more preferably 220 to 240° C. When it is within the above range, the film-forming properties of the surface protective layer are good, and the leveling properties, abrasion resistance, and water abrasion resistance of the aqueous overprint varnish are good.

[0040] High boiling point solvents include ethylene glycol (boiling point 197°C), ethylene glycol monomethyl ether (boiling point 124°C), ethylene glycol monoethyl ether (boiling point 135°C), ethylene glycol monopropyl ether (boiling point 150°C), butyl cellosolve (ethylene glycol monobutyl ether (boiling point 168°C)), diethylene glycol monomethyl ether (boiling point 193°C), diethylene glycol monoethyl ether (boiling point 202°C), diethylene glycol monobutyl ether (boiling point 231°C), triethylene glycol (boiling point 177°C), and propylene glycol (boiling point 188°C). It is preferable that the glycerol-based copolymer contains at least one selected from the group consisting of propylene glycol monomethyl ether (boiling point 120° C.), propylene glycol monoethyl ether (boiling point 132° C.), propylene glycol monopropyl ether (boiling point 149° C.), propylene glycol monobutyl ether (boiling point 170° C.), dipropylene glycol (boiling point 230° C.), dipropylene glycol monomethyl ether (boiling point 189° C.), dipropylene glycol monopropyl ether (boiling point 210° C.), dipropylene glycol monobutyl ether (boiling point 230° C.), diethylene glycol (boiling point 245° C.), etc. These may be used alone or in combination of two or more.

[0041] The content of the high boiling point solvent in the aqueous overprint varnish is preferably 0.01 to 15% by mass, more preferably 0.1 to 10% by mass, even more preferably 1 to 5% by mass, and particularly preferably 1.5 to 3.5% by mass, based on 100% by mass of the aqueous overprint varnish. When the content is within the above range, the film-forming property of the surface protective layer is good, and the leveling property, abrasion resistance, and water abrasion resistance are good. In addition, the ratio of the solid content of the aqueous acrylic resin emulsion (A) to the high boiling point solvent in the aqueous overprint varnish is preferably 8:2 to 9.9:0.1, and more preferably 9:1 to 9.9:0.1. When the content is within the above range, the leveling property, abrasion resistance, and water abrasion resistance are improved.

[0042] <Phosphate ester compounds> The aqueous overprint varnish contains a phosphate ester compound. As the phosphate ester compound, a monoester, a diester, and a small amount of a triester, etc., represented by the following structural formula can be used. Among them, polyoxyethylene alkyl ether phosphate ester is preferable.

[0043] [ka]

[0044] In the above structural formula, n may be an integer of 1 or more, preferably 1 to 10. The above mixtures that can be used as phosphate ester compounds are also available as commercial products. Examples include Phosphanol RA-600, Phosphanol RD-720, and Phosphanol ML-220 manufactured by Toho Chemical Industry Co., Ltd.

[0045] In the aqueous overprint varnish of the above embodiment, the content of the phosphate ester compound is preferably 0.05 to 5 mass%, more preferably 0.1 to 3 mass%, and even more preferably 0.2 to 2 mass%, based on 100 mass% of the solid content of the aqueous overprint varnish. When it is in the above range, the leveling property and water friction resistance are good. Furthermore, the ratio of the solid content of the aqueous acrylic resin emulsion (A) to the solid content of the phosphate ester compound is preferably 9:1 to 9.9:0.1, and more preferably 9.5:0.5 to 9.9:0.1. When it is in the above range, the friction resistance and water friction resistance are improved. Furthermore, the ratio of the high boiling point solvent to the solid content of the phosphate ester compound is preferably 5:5 to 9.9:0.1, and more preferably 7:3 to 9:1. When it is in the above range, the leveling property and water friction resistance are improved.

[0046] <Additives contained in water-based overprint varnish> The aqueous overprint varnish of the above embodiment may further contain various additives that have been conventionally known. For example, in the production of the overcoat agent, additives such as a wetting agent, an adhesion promoter, a leveling agent, an antifoaming agent, an antistatic agent, a viscosity modifier, a chelating crosslinking agent, a trapping agent, and an antiblocking agent, waxes other than those mentioned above, and a silane coupling agent may be used as necessary.

[0047] <Wax> The aqueous overprint varnish preferably contains a wax. Examples of the wax include amide wax and hydrocarbon wax (B), and among them, it is more preferable to contain a hydrocarbon wax (B). In addition, the hydrocarbon wax (B) is preferably a polyethylene wax. The hydrocarbon wax (B) preferably contains a hydrocarbon wax (B1) having an average particle size of 1.5 μm or more and / or a hydrocarbon wax (B2) having an average particle size of less than 1.5 μm, as measured by the Coulter counter method, and more preferably contains a hydrocarbon wax (B1) having an average particle size of 1.5 μm or more and a hydrocarbon wax (B2) having an average particle size of less than 1.5 μm. The average particle size of the hydrocarbon wax (B1) is preferably 1.5 to 10 μm, more preferably 2 to 5 μm. When it is within the above range, the friction resistance and water friction resistance are improved. Moreover, the average particle size of the hydrocarbon wax (B2) is preferably 0.5 to 1.4 μm, more preferably 0.8 to 1.2 μm. When it is within the above range, the friction resistance and water friction resistance are improved. The hardness (penetration) of the hydrocarbon wax (B) at 25°C as specified in JIS K2207 is preferably 1 or more, more preferably 5 to 14, and even more preferably 8 to 12. When it is within the above range, the friction resistance and water friction resistance are improved. The density of the hydrocarbon wax (B) at 23°C as specified in JIS K7112 (Method B) is 880 to 990 kg / m 3 is preferably 900 to 940 kg / m 3It is more preferable that the melting point is within the above range. When it is within the above range, the friction resistance and water friction resistance are improved. The melting point of the hydrocarbon wax (B) in DSC measurement is preferably 90 to 150°C, more preferably 100 to 125°C. When it is within the above range, the blocking resistance is good. The melting point of the hydrocarbon wax (B) refers to the melting point of the peak top (minimum value) of the endothermic peak in the DSC temperature rise curve.

[0048] In the aqueous overprint varnish of the above embodiment, the content of the hydrocarbon wax (B) may be preferably 0.05 to 10 mass% based on the total solid content of the aqueous overprint varnish. The content may be more preferably 0.1 to 7 mass%, and further preferably 0.2 to 5 mass%. When it is within the above range, the abrasion resistance and water abrasion resistance are improved.

[0049] <Low boiling point solvents with boiling points below 105°C> The aqueous overprint varnish preferably contains a low-boiling point solvent having a boiling point of less than 105°C. The main component of the low-boiling point solvent is preferably water, but a hydrophilic organic solvent can be used in addition to water. Specifically, an alcohol-based organic solvent or the like can be added depending on the printing conditions (speed, plate depth, design, drying temperature). The content of the low-boiling point solvent is preferably 30 mass% or less based on the total amount of the aqueous overprint varnish. In the present invention, the main component being water means that the water content is the largest in the low boiling point solvent, and the hydrophilic organic solvent means a solvent that is liquid at 25°C and has a solubility in water at 25°C of 1% by mass or more.

[0050] Examples of the alcohol-based organic solvent include methanol, ethanol, propanol, isopropanol, isobutanol, normal butanol, tert-butanol, hexanol, octanol, and decanol. In one embodiment, the weight ratio of water to the hydrophilic organic solvent is preferably 90:10 to 60:40.

[0051] <Surfactant> From the viewpoint of improving leveling properties and alcohol resistance, the aqueous overprint varnish preferably contains a surfactant. Examples of the surfactant include acetylene-based surfactants, silicon-based surfactants, acrylic-based surfactants, fluorine-based surfactants, and alcohol alkoxylate-based surfactants, and among these, acetylene-based surfactants are preferred.

[0052] <Acetylene-based surfactant> The acetylene surfactant is a nonionic compound having an acetylene group. The acetylene surfactant is more preferably an ethylene oxide adduct. Commercially available acetylene glycol compounds include Olfin E1010 and Olfin E1020 manufactured by Nissin Chemical Industry Co., Ltd., Surfynol 104, Surfynol 420, Surfynol 440, Surfynol 465, and Surfynol 485 manufactured by Air Products and Chemicals Co., Ltd.

[0053] The acetylene surfactant preferably has an HLB value in the range of 1 to 17, more preferably in the range of 3 to 10, and even more preferably in the range of 4 to 8. When it is in the above range, the leveling property and alcohol resistance are improved.

[0054] The content of the surfactant in the aqueous overprint varnish is preferably 0.1 to 5 mass %, and more preferably 0.3 to 3 mass %, based on 100 mass % of the aqueous overprint varnish. When the content is within the above range, the leveling property and alcohol resistance are improved. In the aqueous overprint varnish, the ratio of the solid content of the aqueous acrylic resin emulsion (A) to the solid content of the surfactant is preferably 7.2:1 to 72:1, and more preferably 12:1 to 36:1. When it is within the above range, the leveling property and alcohol resistance are improved.

[0055] <Method of manufacturing water-based overprint varnish> The aqueous overprint varnish can be obtained by mixing and stirring a resin solution in which a resin is dissolved or dispersed in a solvent, a solvent, and additives in a stirrer equipped with a stirring blade, rotor, etc. There is no particular restriction on the stirring speed, and stirring can be performed at 50 to 2000 rpm. In order to improve the handling and coating properties of the overprint varnish, an aqueous medium can also be appropriately added. <Formation of surface protection layer> The surface protective layer can be formed, for example, by printing on a polyolefin substrate or on a printing layer described later using an aqueous overprint varnish, and then removing the solvent. As the printing method, known printing methods such as gravure printing and flexographic printing can be used, and gravure printing is preferred. For example, the aqueous overprint varnish is diluted with a diluting solvent to a viscosity suitable for gravure printing or flexographic printing, and is supplied to each printing unit alone or in a mixture and applied. Thereafter, the aqueous medium is removed by drying in an oven or the like to form a surface protective layer.

[0056] (gravure printing) << Gravure version >> In gravure printing, the gravure plate is a cylindrical metal plate on which recesses of each color are formed by engraving, etching, or laser. There are no restrictions on the use of engraving and laser, and they can be set arbitrarily according to the pattern. Lines per page are appropriately set to 80 to 250 lines, and the higher the line count, the finer the printing. The thickness of the printing layer is preferably 0.1 μm to 100 μm.

[0057] Gravure printing machine In the gravure printing press, one printing unit is equipped with the gravure plate and doctor blade. There are many printing units, and printing units corresponding to organic solvent-based printing inks and picture inks can be set, and each unit has an oven drying unit. Printing is performed by rotary printing, and a roll-to-roll printing method is used. The type of plate and the type of doctor blade are appropriately selected according to the specifications.

[0058] <Water-based ink> The water-based ink of the present invention contains a water-based acrylic resin emulsion (C) and / or a water-based urethane resin. When the water-based acrylic resin emulsion (C) is contained, it is preferable that the water-based ink further contains a water-soluble acrylic resin (D).

[0059] <Water-based acrylic resin emulsion (C)> The acid value of the aqueous acrylic resin emulsion (C) is preferably 5 to 80 mgKOH / g, and more preferably 20 to 60 mgKOH / g. When it is in the above range, the water-based friction resistance is improved. The glass transition temperature of the aqueous acrylic resin emulsion is preferably -20 to 60°C, and more preferably 0 to 40°C. When it is in the above range, the friction resistance and water-based friction resistance are improved. The weight average molecular weight of the aqueous acrylic resin emulsion (C) is preferably 10,000 to 600,000, more preferably 50,000 to 500,000, further preferably 100,000 to 400,000, and particularly preferably 200,000 to 300,000. When it is within the above range, the abrasion resistance and water abrasion resistance are improved. The emulsion particle size of the aqueous acrylic resin emulsion (C) is preferably 10 to 300 nm, more preferably 60 to 100 nm. When it is within the above range, the leveling property, abrasion resistance, and water abrasion resistance are improved.

[0060] The monomers constituting the aqueous acrylic resin emulsion (C) may be the same as those of the aqueous acrylic resin emulsion (A) described in the aqueous overprint varnish.

[0061] The aqueous acrylic resin emulsion (C) may be a commercially available product, for example, HE-1335, X-436, QE-1042, etc. manufactured by Seiko PMC Corporation.

[0062] <Water-soluble acrylic resin (D)> The acid value of the water-soluble acrylic resin (D) is preferably 200 mgKOH / g or less, more preferably 20 to 150 mgKOH / g, and even more preferably 40 to 100 mgKOH / g. When it is within the above range, the water-friction resistance is improved. The glass transition temperature of the water-soluble acrylic resin (D) is preferably 40 to 130°C, and more preferably 60 to 120°C. When it is within the above range, the abrasion resistance and the water-friction resistance are improved. The neutralizing agent for the water-soluble acrylic resin (D) is preferably ammonia, an organic amine, an alkali metal hydroxide, or the like, and more preferably ammonia. When the above neutralizing agent is used, the leveling property and the water-friction resistance are improved. The weight-average molecular weight of the water-soluble acrylic resin (D) is preferably 1500 to 50,000, more preferably 1500 to 30,000, and even more preferably 1500 to 8,000. When it is within the above range, the abrasion resistance and the water-friction resistance are improved.

[0063] The monomers constituting the water-soluble acrylic resin (D) can be the same as those in the <water-based acrylic resin emulsion (A)> described in the water-based overprint varnish.

[0064] The water-soluble acrylic resin (D) used in the present invention may be a commercially available product, for example, "Joncryl 67, Joncryl 678, Joncryl 680, Joncryl 819" manufactured by BASF.

[0065] The solid content ratio of the aqueous acrylic resin emulsion (C) to the water-soluble acrylic resin (D) is preferably 95:5 to 60:40, and more preferably 90:10 to 80:20. When it is within the above range, water friction resistance is improved.

[0066] <Water-based urethane resin> The aqueous urethane resin used in the present invention is obtained by reacting a urethane prepolymer having an isocyanate group at its terminal, which is obtained by reacting a polyisocyanate (a), a polymer polyol (b), and a compound (c) having a carboxyl group and at least two active hydrogen-containing groups in the molecule, with an organic diamine (d).

[0067] As the polyisocyanate (a) used in the aqueous urethane resin of the present invention, various known aromatic, aliphatic or alicyclic diisocyanates can be used. For example, 1,5-naphthylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 4,4'-diphenyldimethylmethane diisocyanate, 4,4'-dibenzyl isocyanate, dialkyldiphenylmethane diisocyanate, tetraalkyldiphenylmethane diisocyanate, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, tolylene diisocyanate, butane-1,4-diisocyanate, hexamethylene diisocyanate, isopropylene diisocyanate, methylene diisocyanate, 2,2,4-trimethylsilyl diisocyanate, 1,3,4-trimethylsilyl diisocyanate, 1,4,5 ...4,5-trimethylsilyl di Representative examples include methylhexamethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, cyclohexane-1,4-diisocyanate, xylylene diisocyanate, isophorone diisocyanate, lysine diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, 1,3-bis(isocyanatemethyl)cyclohexane, methylcyclohexane diisocyanate, m-tetramethylxylylene diisocyanate, and dimer diisocyanate in which the carboxyl group of a dimer acid is converted to an isocyanate group. These can be used alone or in a mixture of two or more. In terms of reactivity, isophorone diisocyanate is preferred.

[0068] The number average molecular weight of the polymer polyol (b) used in the aqueous urethane resin of the present invention is 3000 or less, that is, each number average molecular weight used as the polymer polyol (b) is 3000 or less. When it is within the above range, water resistance and adhesion to polyolefin substrates are improved. The number average molecular weight is calculated from the hydroxyl value, which is a value calculated by esterifying or acetylating the hydroxyl groups in the resin, back titrating the remaining acid with an alkali, converting the amount of hydroxyl groups in 1 g of resin into mg of potassium hydroxide, according to JIS K0070.

[0069] Examples of the polymer polyol (b) include polyester polyols, polyether polyols, polycaprolactone diols, polycarbonate polyols, polyolefin polyols, castor oil polyols, hydrogenated castor oil polyols, dimer diols, and hydrogenated dimer diols. Of these, polyester polyols, polycarbonate polyols, and polyether polyols are preferred.

[0070] The polymer polyol (b) is more preferably a polyester polyol. When the polymer polyol (b) is a polyester polyol, the leveling property and alcohol resistance are improved.

[0071] (Polyester polyol) The polyester polyol is a dehydration condensate or polymer of at least one selected from the group consisting of 1,2-propanediol, 1,3-butanediol, 2-methyl-1,3-propanediol, neopentyl glycol, 1,4-pentanediol, 3-methyl-1,5-pentanediol, 2,5-hexanediol, 2-methyl-1,4-pentanediol, 2,4-diethyl-1,5-pentanediol, 2-butyl-2-ethyl-1,3-propanediol, 2-methyl-1,8-octanediol, 2,2,4-trimethyl-1,3-pentanediol, and 2,2,4-trimethyl-1,6-hexanediol, and a polycarboxylic acid or a polycarboxylic acid anhydride. For example, 1,2-propanediol, 1,3-butanediol, 2-methyl-1,3-propanediol, Examples of the polyols include low molecular weight polyols having a branched structure such as ethanol, neopentyl glycol, 1,4-pentanediol, 3-methyl-1,5-pentanediol, 2,5-hexanediol, 2-methyl-1,4-pentanediol, 2,4-diethyl-1,5-pentanediol, 2-butyl-2-ethyl-1,3-propanediol, 2-methyl-1,8-octanediol, 2,2,4-trimethyl-1,3-pentanediol, and 2,2,4-trimethyl-1,6-hexanediol, and polycarboxylic acids such as adipic acid, phthalic acid, isophthalic acid, terephthalic acid, maleic acid, fumaric acid, succinic acid, oxalic acid, malonic acid, glutaric acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, trimellitic acid, and pyromellitic acid, or dehydration condensates or polymers of these anhydrides. These can be used alone or in combination of two or more. The polyester polyol preferably has a branched structure, and by using the low molecular weight polyols having the above-mentioned branched structure, a branched structure can be introduced into the polyester polyol.

[0072] When the polymer polyol (b) contains a polyester polyol, the content of the polyester polyol is preferably 30 to 99 mass%, more preferably 50 to 97 mass%, and even more preferably 80 to 95 mass%, based on 100 mass% of the polymer polyol. When the content is within the above range, the adhesion to polyolefin substrates and the abrasion resistance are improved.

[0073] (Polycarbonate polyol) The polycarbonate polyol is not limited by the production method or the diol species constituting the polycarbonate polyol, but a polycondensate obtained by an ester exchange reaction between a diol made of an alkylene glycol and a carbonate compound is preferably used. The polycarbonate polyol is preferably an alicyclic and / or aliphatic polycarbonate diol.

[0074] As the diol, for example, ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 2-methyl-1,3-propanediol, neopentyl glycol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, 1,9-nonanediol, 2-methyl-1,8-octanediol, 1,10-decanediol, 2-butyl-2-ethyl-1,3-propanediol, 1,4-butynediol, 2,2,4-trimethyl-1,3-pentanediol, 1,4-cyclohexanedimethanol, diethylene glycol, polypropylene glycol, dipropylene glycol, etc. are suitable, and these can be used alone or in combination of two or more. 3-methyl-1,5-pentanediol and other polycarbonate polyols having a diol structure with a branched structure are preferred. The carbonate compound is not particularly limited, but may be a dialkyl carbonate, a diaryl carbonate, or an alkylene carbonate. Specific examples of the carbonate compound include dialkyl carbonates such as dimethyl carbonate, diethyl carbonate, and dibutyl carbonate, diaryl carbonates such as diphenyl carbonate, and alkylene carbonates such as ethylene carbonate.

[0075] When the polymer polyol (b) contains a polycarbonate polyol, the content of the polycarbonate polyol is preferably 30 to 99 mass%, more preferably 50 to 97 mass%, and even more preferably 80 to 95 mass%, based on 100 mass% of the polymer polyol. When the content is within the above range, the adhesion to polyolefin substrates and the abrasion resistance are improved.

[0076] The active hydrogen-containing group in the aqueous urethane resin of the present invention refers to a group having an active hydrogen, such as a hydroxyl group or an amino group, which reacts with an isocyanate group.

[0077] Examples of the compound (c) having a carboxyl group and at least two active hydrogen-containing groups in the molecule, which is used in the aqueous urethane resin of the present invention, include dimethylolalkanoic acids such as 2,2-dimethylolpropionic acid, 2,2-dimethylolbutyric acid, and 2,2-dimethylolvaleric acid, and diamine-type amino acids such as glutamine, asparagine, lysine, diaminopropionic acid, ornithine, diaminobenzoic acid, and diaminobenzenesulfonic acid. These can be used alone or in combination of two or more kinds.

[0078] The organic diamine (d) used in the aqueous urethane resin of the present invention is an organic diamine having a hydroxyl group in an amount of 50% by weight to 100% by weight. If the organic diamine having a hydroxyl group is less than 50% by weight, the re-solubility in water-alcohol is poor.

[0079] Examples of organic diamines having a hydroxyl group used in the aqueous urethane resin of the present invention include 2-hydroxyethylethylenediamine, 2-hydroxyethylpropylenediamine, di-2-hydroxyethylethylenediamine, di-2-hydroxyethylpropylenediamine, 2-hydroxypropylethylenediamine, and di-2-hydroxypropylethylenediamine. These can be used alone or in combination of two or more.

[0080] Examples of organic diamines that do not have a hydroxyl group and are used in the aqueous urethane resin of the present invention include ethylenediamine, propylenediamine, hexamethylenediamine, isophoronediamine, dicyclohexylmethane-4,4'-diamine, and dimer acid. Dimer diamine in which a carboxyl group is converted to an amino group, etc. These may be used alone or in combination of two or more kinds.

[0081] The acid value of the aqueous urethane resin used in the present invention is preferably 25 to 65 mgKOH / g, and more preferably 25 to 45 mgKOH / g. When it is within the above range, water resistance and adhesion to polyolefin substrates are improved. The weight average molecular weight of the aqueous urethane resin is preferably 5,000 to 100,000, and more preferably 10,000 to 70,000, and even more preferably 20,000 to 40,000. When it is within the above range, friction properties and water friction resistance are improved.

[0082] The aqueous urethane resin used in the present invention can be obtained by the acetone method using an organic solvent that is inactive and hydrophilic to isocyanate, a solventless synthesis method that does not use any solvent at all, etc. In the present invention, the acetone method was used, which uses an organic solvent to reduce the viscosity and allows the synthesis reaction to be carried out uniformly and smoothly.

[0083] To obtain a urethane prepolymer having an isocyanate group at its end by reacting a polyisocyanate (a), a polymer polyol (b), and a compound (c) having a carboxyl group and at least two active hydrogen-containing groups in the molecule (hereinafter referred to as a prepolymer reaction), it is preferable to carry out the reaction at 50 to 100° C. for 10 minutes to 10 hours. The end point of the reaction is determined by viscosity measurement, NCO peak by IR measurement, NCO% measurement by titration, etc.

[0084] A catalyst can also be used in the prepolymer reaction. Known metal catalysts and amine catalysts can be used as catalysts. Metal catalysts include dibutyltin dilaurate, tin octoate, dibutyltin di(2-ethylhexoate), lead 2-ethylhexoate, 2-ethylhexyl titanate, iron 2-ethylhexoate, cobalt 2-ethylhexoate, zinc naphthenate, cobalt naphthenate, and tetra-n-butyltin. Amine catalysts include tertiary amines such as tetramethylbutanediamine. These catalysts are used in the range of 0.001 to 1 mol% based on the polymer polyol.

[0085] The reaction of the urethane prepolymer with the organic diamine (hereinafter, chain extension reaction) is preferably carried out for 10 minutes to 10 hours at 30 to 80° C. The end point of the reaction is determined by viscosity measurement, NCO peak by IR measurement, amine value measurement by titration, etc.

[0086] A reaction terminator may be used in the chain extension reaction. Examples of the reaction terminator include dialkylamines such as di-n-butylamine, as well as amines having a hydroxyl group such as monoethanolamine, diethanolamine, 2-amino-2-methyl-1-propanol, tri(hydroxymethyl)aminomethane, and 2-amino-2-ethyl-1,3-propanediol. Further examples include monoamine-type amino acids such as glycine, alanine, glutamic acid, taurine, aspartic acid, aminobutyric acid, valine, aminocaproic acid, aminobenzoic acid, aminoisophthalic acid, and sulfamic acid.

[0087] Examples of basic compounds that neutralize the carboxyl groups incorporated in the aqueous urethane resin used in the present invention include organic amines such as ammonia, monoethylamine, diethylamine, trimethylamine, triethylamine, triisopropylamine, tributylamine, triethanolamine, methyldiethanolamine, monoethanolamine, dimethylethanolamine, diethylethanolamine, morpholine, N-methylmorpholine, 2-amino-2-methyl-1-propanol, and the like; and inorganic alkalis such as sodium hydroxide and potassium hydroxide, and these may be used alone or in combination of two or more kinds. From the viewpoints of water resistance of printed matter, residual odor, and the like, preferred are compounds that are water-soluble and highly volatile so as to dissociate easily when heated, and ammonia is particularly preferred.

[0088] Examples of organic solvents that are inactive and hydrophilic to isocyanates include ethers such as tetrahydrofuran and dioxane, esters such as ethyl acetate, ketones such as acetone, methyl ethyl ketone, and cyclohexanone, and amides such as dimethylformamide and N-methylpyrrolidone. Since polyurethane is usually made aqueous by distillation under reduced pressure (solvent removal), and even if it is used without solvent removal, it is preferable to use a solvent with a lower boiling point than water in order to increase the drying speed. When solvent removal is performed, for example, water and a basic compound as a neutralizing agent are added to the reaction solution, and then the temperature is increased and the required amount of solvent is distilled off under normal pressure or reduced pressure. The aqueous urethane resin may be in the form of either an emulsion resin or a water-soluble resin.

[0089] <Coloring agent> The printed layer contains a colorant. The content of the colorant is preferably 1 to 60% by mass, and more preferably 30 to 50% by mass, based on the total mass of the printed layer. The colorant is preferably a pigment, and either an organic pigment or an inorganic pigment can be used.

[0090] (Organic pigments) Specific examples of organic pigments are shown by their Colour Index International (CI) numbers. Preferably, CI Pigment Red 57:1, CI Pigment Red 48:1, CI Pigment Red 48:2, CI Pigment Red 48:3, CI Pigment Red 146, CI Pigment Red 242, CI Pigment Yellow 83, CI Pigment Yellow 14, CI Pigment Orange 64, CI Pigment Orange 38, CI Pigment Orange 34, CI Pigment Orange 13, CI Pigment Yellow 180, CI Pigment Yellow 139, CI Pigment Red 185, CI Pigment Red 122, CI Pigment Red 178, CI Pigment Red 149, CI Pigment Red 144, CI Pigment Red 166, CI Pigment Violet 23, CI Pigment Violet 37, CI Pigment Blue 15, CI Pigment Blue 15:1, CI Pigment Blue 15:2, CI Pigment Blue 15:3, CI Pigment Blue 15:4, CI Pigment Blue 15:6, CI Pigment Green 7, and CI Pigment Black 7. These may be used alone or in combination of two or more.

[0091] (Inorganic pigments) Examples of inorganic pigments include titanium oxide, zinc oxide, zinc sulfide, barium sulfate, calcium carbonate, chromium oxide, aluminum hydroxide, silica, kaolin, clay, talc, aluminum particles, mica, bronze powder, chrome vermilion, yellow lead, cadmium yellow, cadmium red, ultramarine, Prussian blue, red iron oxide, yellow iron oxide, iron black, titanium oxide, and zinc oxide. Aluminum can be either leafing or non-leafing type, with the non-leafing type being preferred.

[0092] <Additives contained in water-based inks> The printing layer of the present invention may contain various additives as necessary, such as dispersants, waxes, extender pigments, leveling agents, antifoaming agents, and film-forming assistants. Specifically, various additives can be added, such as a dispersion of wax resin microparticles such as polyethylene wax to improve water friction resistance, inorganic microparticles and adhesive resins to impart anti-slip properties, vinyl acetate resins, leveling agents to improve leveling properties, antifoaming agents to impart antifoaming properties, basic compounds such as sodium hydroxide and potassium hydroxide to impart re-solubility, and film-forming assistants such as glycol compounds.

[0093] <Surfactant> From the viewpoint of improving leveling properties and alcohol resistance, the water-based ink preferably contains a surfactant. As the surfactant, the aspects of the <surfactant> described in the above <water-based overprint varnish> can be used.

[0094] The content of the surfactant in the aqueous ink is preferably 0.1 to 5% by mass, and more preferably 0.3 to 3% by mass, based on 100% by mass of the aqueous ink. When it is within the above range, the leveling property and alcohol resistance are improved. In addition, in the aqueous ink, the ratio of the total amount of the aqueous acrylic resin and the aqueous urethane resin in the aqueous ink to the solid content of the surfactant is preferably 2.5:1 to 65:1, more preferably 3.5:1 to 35:1, and even more preferably 7.5:1 to 20:1.

[0095] <Solvents contained in water-based inks> The solvent contained in the water-based ink has a boiling point of 105℃, as explained in the water-based overprint varnish. The above-mentioned high boiling point solvents and low boiling point solvents having a boiling point of less than 105°C can be used. Of these, it is preferable to use water, and the ratio of water in the solvent contained in the water-based ink is preferably 60 to 100 mass %, and more preferably 90 to 100 mass %.

[0096] <Method of manufacturing water-based ink> For example, printing ink can be manufactured by dispersing a pigment in an aqueous medium with a resin or the like using a disperser, and mixing the obtained pigment dispersion with a resin, various additives, an organic solvent, and the like. As the disperser, a commonly used one, for example, a roller mill, a ball mill, a pebble mill, an attritor, or a sand mill, can be used. The particle size distribution of the pigment in the pigment dispersion can be adjusted by appropriately adjusting the size of the grinding media of the disperser, the filling rate of the grinding media, the dispersion treatment time, the discharge speed of the pigment dispersion, the viscosity of the pigment dispersion, and the like. The viscosity of the printing ink at 25°C is preferably in the range of 50 mPa·s or more from the viewpoint of preventing the pigment from settling and dispersing appropriately, and 300 mPa·s or less from the viewpoint of workability and efficiency during ink manufacturing and printing.

[0097] <Method of forming the printing layer> The printing layer can be formed, for example, by printing on a polyolefin substrate using an aqueous ink and then removing the solvent. The aqueous ink can be appropriately diluted with a diluting solvent consisting of water or a water-soluble organic solvent when printing, and printed on various substrates. In addition, the diluting solvent that can be used is preferably a mixed solvent of water and an alcohol-based solvent, and the weight ratio is preferably 50:50 to 90:10 from the viewpoint of storage stability and drying of the ink. As the printing method, gravure printing, flexographic printing, screen printing and other printing methods can be used, with gravure printing being preferred.

[0098] <Laminate> The laminate of the above embodiment is constructed by printing an aqueous ink and an aqueous overprint varnish in this order on a polyolefin substrate. As the printing method, a gravure printing method, a flexographic printing method, a screen printing method, or other printing methods can be applied. The laminate is suitable for use as a packaging material.

[0099] <Printing base material> Examples of the printing substrate include polyolefin substrates such as polyethylene and polypropylene, paper substrates such as medium-quality paper, fine paper, cardboard, and impregnated paper, polyester substrates such as polyethylene terephthalate, polycarbonate, and polylactic acid, polystyrene-based substrates such as polystyrene, AS resin, and ABS resin, film substrates such as nylon substrates, polyamide substrates, polyvinyl chloride substrates, polyvinylidene chloride substrates, and cellophane substrates, and film substrates made of composite materials thereof. The plastic substrate may be vapor-deposited with metals or metal oxides such as silica, alumina, and aluminum, and the vapor-deposited surface may be further coated with a paint such as polyvinyl alcohol. Generally, the surface of the substrate to be printed is often subjected to surface treatment such as corona treatment. Furthermore, the substrate may be a film that has been previously processed with a plastic film, such as coating or kneading with an anti-fogging agent, or surface coating or kneading with a matting agent. The substrate may be a single layer, or may be a laminate (substrate layer) in which two or more substrates are laminated. The substrates constituting the substrate layer may be the same or different. Among these, a polyolefin substrate or a paper substrate is preferred, a polyolefin substrate is more preferred, polyethylene or polypropylene is even more preferred, and polyethylene is particularly preferred. The polyolefin substrate is preferably corona discharge treated. EXAMPLES

[0100] The present invention will be described in detail below with reference to the following examples. However, the present invention is not limited to these examples, and various modifications are possible. In the present invention, the terms "parts" and "%" refer to parts by mass and % by mass unless otherwise noted.

[0101] <Hydroxyl value> The hydroxyl value is the number of milligrams of potassium hydroxide required to neutralize acetic acid bonded to hydroxyl groups when 1 g of a sample is acetylated, and was measured by the method described in JIS K 0070. <Acid value> The acid value is the number of milligrams of potassium hydroxide required to neutralize the free fatty acids, resin acids, etc. contained in 1 g of a sample, and was measured by the method described in JIS K 0070.

[0102] <Amine value> The amine value is the amount of potassium hydroxide in mg equivalent to the amount of hydrochloric acid required to neutralize the amino groups contained in 1 g of sample, and was measured in accordance with JIS K 0070. 0.5 to 2 g of sample was precisely weighed out (sample solid content: Sg), and 50 mL of a mixed solution of methanol / methyl ethyl ketone = 60 / 40 (mass ratio) was added to the precisely weighed sample to dissolve it. Bromophenol blue was added as an indicator to the resulting solution, and the resulting solution was titrated with a 0.2 mol / L ethanolic hydrochloric acid solution (titer: f). The point at which the color of the solution changed from green to yellow was set as the end point, and the titration amount (AmL) at this time was used to calculate the amine value according to the following (Equation 1). (Formula 1) Amine value = (A x f x 0.2 x 56.108) / S [mgKOH / g]

[0103] <Mass average molecular weight> The weight average molecular weight was determined by measuring the molecular weight distribution using a gel permeation chromatography (GPC) device (HLC-8220 manufactured by Tosoh Corporation) and calculating the molecular weight converted using polystyrene as a standard substance. The measurement conditions are shown below. Columns: The following columns were used in series connection: Tosoh Corporation TSKgel Super AW2500 Tosoh Corporation TSKgel Super AW3000 Tosoh Corporation TSKgel Super AW4000 Tosoh Corporation's TSK gelguard column Super AWH Detector: RI (differential refractometer) Measurement conditions: Column temperature 40℃ Eluent: Tetrahydrofuran Flow rate: 1.0mL / min

[0104] <Glass transition temperature (Tg)> The glass transition temperature was determined by differential scanning calorimetry (DSC). The measurement was performed using a Rigaku DSC8231 with a measurement temperature range of -70 to 250°C and a heating rate of 10°C / min. The midpoint (inflection point) of the baseline shift due to the glass transition in the DSC curve was taken as the glass transition temperature.

[0105] <Measurement of coating amount for each layer> <Print layer> Five 10 cm square pieces were cut out from the substrate / printed layer component of the laminate, and five 10 cm square pieces were cut out from the substrate. The mass of each sample was measured, and the mass per unit area of ​​the anchor coat layer was calculated using the following formula (2). A polyethylene film with a thickness of 30 μm was used as the substrate. (Formula 2) Mass per unit area of ​​the printed layer (g / m 2 ) = (average mass of 5 samples of substrate / printed layer) - (average mass of 5 samples of substrate)

[0106] <Surface protective layer> Five 10 cm square pieces were cut out from the substrate / printed layer / surface protective layer component of the laminate, and five 10 cm square pieces were cut out from the substrate / printed layer component. The mass of each sample was measured, and the mass per unit area of ​​the surface protective layer was calculated using the following formula 3. A polyethylene film with a thickness of 30 μm was used as the substrate. (Formula 3) Mass per unit area of ​​surface protection layer (g / m 2 ) = (average mass of five samples of substrate / printed layer / surface protective layer) - (average mass of five samples of substrate / printed layer)

[0107] <Synthesis Example 1> Synthesis of water-based urethane resin PU1 In a reactor equipped with a thermometer, a stirrer, a reflux condenser and a nitrogen gas inlet tube, 178.2 parts of poly(3-methyl-1,5-pentane adipate)diol having a number average molecular weight of 2000, 18.2 parts of polyethylene glycol having a number average molecular weight of 2000, 33.4 parts of dimethylol butanoic acid and 116.5 parts of isophorone diisocyanate were reacted at the boiling point in 200 parts of methyl ethyl ketone for 6 hours while introducing nitrogen gas to obtain a terminal isocyanate prepolymer, and then cooled to 40°C and 100 parts of acetone were added to obtain a solvent solution of the terminal isocyanate prepolymer. Next, 646.3 parts of the obtained terminal isocyanate prepolymer solution was gradually added at room temperature to a mixture of 16.3 parts of 2-hydroxyethylethylenediamine and 400 parts of acetone, and the mixture was reacted at 50°C for 3 hours to obtain a solvent-based urethane resin solution. Next, 9.76 parts of 28% aqueous ammonia and 500 parts of deionized water were gradually added to the above solvent-based polyurethane resin solution to neutralize and make it water-soluble. Further, all of the methyl ethyl ketone and acetone were distilled off under azeotropic conditions, and then water was added to adjust the viscosity. As a result, an aqueous urethane resin PU1 with an acid value of 30 mgKOH / g, a solids content of 40% and a weight average molecular weight of 22,000 was obtained.

[0108] <Synthesis Example 2> Synthesis of water-based urethane resin PU2 In a reactor equipped with a thermometer, a stirrer, a reflux condenser and a nitrogen gas inlet tube, 235.6 parts of polycarbonate diol having a number average molecular weight of 2000 consisting of 1,6-hexanediol-derived units, 10.7 parts of polyethylene glycol having a number average molecular weight of 2000, 30.0 parts of 2,2-dimethylolpropanoic acid and 250 parts of methyl ethyl ketone were mixed and stirred while dropping 91.5 parts of isophorone diisocyanate over 1 hour, reacted at 80°C for 4 hours to obtain a terminal isocyanate prepolymer, then cooled to 30°C and 100 parts of isopropanol were added to obtain a solvent solution of the terminal isocyanate prepolymer. A mixture of 2.7 parts of 2-aminoethylethanolamine and 150 parts of isopropanol was gradually added to the obtained terminal isocyanate prepolymer at room temperature and reacted at 40°C for 2 hours to obtain a solvent-based urethane resin solution. Next, 13.6 parts of 28% aqueous ammonia and 851 parts of ion-exchanged water were gradually added to the above solvent-based urethane resin solution to neutralize and make it water-soluble, and then the methyl ethyl ketone and isopropanol were distilled off under reduced pressure, and water was added to adjust the solids content, thereby obtaining an aqueous urethane resin solution PU2 with a solids content of 40% and an acid value of 35 mg KOH / g, a hydroxyl value of 4 mg KOH / g, and a weight average molecular weight of 35,000.

[0109] <Production Example 1> Production of Water-Based Overprint Varnish V1 Water 14.49 parts, acrylic emulsion 1 (acid value 62 mg KOH / g, glass transition temperature: 75 ° C., solid content 45%) 60 parts, acrylic emulsion 4 (acid value 52 mg KOH / g, glass transition temperature: 50 ° C., solid content 45%) 20 parts, diethylene glycol monobutyl ether 2 parts, polyethylene wax 1 (particle size (Coulter counter method): 1 μm, hardness (penetration): 10, solid content 40%) 1.5 parts, polyethylene wax 2 (particle size (Coulter counter method): 3 μm, hardness (penetration): 10, solid content 40%) 1.5 parts, phosphate ester compound (Toho Chemical Industry Co., Ltd. Phosphanol RA-600, polyoxyethylene alkyl ether phosphate ester, solid content 100%) 0.5 parts, defoamer (EVONIC Co., Ltd. TEGO (registered trademark) 0.01 parts of Foamex 1488 (solid content 100%) was added and mixed with stirring to obtain water-based overprint varnish V1.

[0110] <Production Examples 2 to 16, Comparative Production Examples 1 to 4> Production of Water-Based Overprint Varnishes V2 to 19 Water-based overprint varnishes V2 to 20 were obtained in the same manner as in Production Example 1, except that the raw materials and blending ratios shown in Table 1 were used. The properties of the raw materials used are as follows. Acrylic emulsion 2 (acid value 100mgKOH / g, glass transition temperature: 110℃, solid content 45%) Acrylic emulsion 3 (acid value 165 mgKOH / g, glass transition temperature: 137°C, solid content 45%) Acrylic emulsion 5 (acid value 55 mgKOH / g, glass transition temperature: 40°C, solid content 45%) Acrylic emulsion 6 (acid value 51 mgKOH / g, glass transition temperature: 30°C, solid content 45%) Urethane emulsion 1 (Taisei Fine Chemical Co., Ltd. WBR-016U, solid content 45%) Water-soluble acrylic resin 1 (Seiko PMC YL-1098, acid value 240mgKOH / g, glass transition temperature: 126℃, solid content 45%) BDG: Diethylene glycol monobutyl ether (boiling point 231°C) · PGM: Propylene glycol monomethyl ether (boiling point 120℃) ·DEG: Diethylene glycol (boiling point 245℃) IPA: Isopropyl alcohol (boiling point 82.5°C)

[0111] [Table 1]

[0112] <Production Examples 26-30> Production of Overprint Varnish V21-25 Water-based overprint varnishes V21 to 25 were obtained in the same manner as in Production Example 1, except that the raw materials and blending ratios shown in Table 1-2 were used. The properties of the raw materials used are as follows. Acetylene-based surfactant (100% solids, HLB value = 6) Alcohol alkoxylate surfactant (100% solids, HLB value = 8) Silicone surfactant (100% solids, HLB value = 14)

[0113] [Table 1-2]

[0114] <Production Example 17> Production of Water-Based Ink W1 10 parts of a phthalocyanine blue pigment (Lionol Blue FG-7400G (CI Pigment Blue 15:4, solids content 100%) manufactured by Toyo Color Co., Ltd.), 14.5 parts of water, 50 parts of an aqueous acrylic resin emulsion 7 (acid value 35 mgKOH / g, glass transition temperature: 25°C, solids content 40%), 10 parts of a water-soluble acrylic resin 1 (acid value: 50 mgKOH / g, glass transition temperature: 110°C, solids content 40%), 15 parts of isopropyl alcohol, 0.5 parts of polyethylene wax 2 (particle size (Coulter counter method): 3 µm, hardness (penetration): 10, solids content 40%), and 0.01 parts of a silicone antifoaming agent (solids content 100%) were mixed and dispersed for 15 minutes using a bead mill to obtain a printing ink W1.

[0115] <Production Examples 18 to 25, Comparative Production Examples 5 and 6> Production of Water-Based Inks W2 to W11 Water-based inks W2 to 11 were obtained in the same manner as in Production Example 17, except that the raw materials and blending ratios shown in Table 2 were used. The properties of the raw materials used are as follows. Water-soluble acrylic resin 2 (acid value 80 mgKOH / g, glass transition temperature: 100°C, solid content 40%) Water-soluble acrylic resin 3 (acid value 215 mgKOH / g, glass transition temperature: 85°C, solid content 40%) Water-soluble acrylic resin 4 (acid value 41 mgKOH / g, glass transition temperature: 90°C, solid content 40%) Water-based styrene-maleic acid resin (Seiko PMC, PL-1231)

[0116] [Table 2]

[0117] <Production Examples 31 to 36> Production of Water-Based Inks W12 to W17 Water-based inks W12 to W17 were obtained in the same manner as in Production Example 17, except that the raw materials and blending ratios shown in Table 2-2 were used.

[0118] [Table 2-2]

[0119] (Manufacture of laminates) Example 1: Production of laminate P1 The water-based ink W1 was diluted with a dilution solvent (water / isopropyl alcohol = 30 / 70) to a Zahn cup #3 (manufactured by Rigo Co., Ltd.) of 15 seconds (25°C), and the water-based overprint varnish V1 was diluted with a dilution solvent (water / isopropyl alcohol = 30 / 70) to a Zahn cup #3 (manufactured by Rigo Co., Ltd.) of 15 seconds (25°C). Thereafter, a diluted water-based ink W1 was printed on the entire surface of the corona-treated surface of a 30 μm-thick polyethylene film (PE) at a printing speed of 40 m / min and an in-line oven temperature of 90°C using a gravure printing machine equipped with a gravure plate with 175 lines / inch heliograving to form a printed layer, and a diluted overprint varnish V1 was printed on the printed layer at a printing speed of 40 m / min and an in-line oven temperature of 90°C using a gravure printing machine equipped with a gravure plate with 175 lines / inch heliograving having a non-image area on one half of the plate to form a surface protective layer, thereby obtaining a laminate P1 having a structure of substrate / printed layer / surface protective layer. The coating amount of the printed layer of the laminate P1 was 1 g / m 2 , the coating amount of the surface protective layer was 0.5 g / m 2 It was.

[0120] <Examples 2 to 28 and Comparative Examples 1 to 6> Production of Laminates P1 to 34 Except for changing the raw materials and printing method as shown in Tables 3 and 4, laminates P2 to P34 were obtained in the same manner as in Example 1.

[0121] <Examples 29 to 40> Production of Laminates P35 to P48 Except for changing the raw materials and printing method as shown in Table 5, the same method as in Example 1 was used to obtain laminates P35 to P48.

[0122] <Characteristics evaluation> The laminates obtained in the above Examples and Comparative Examples were evaluated as described below. The evaluation results are shown in Tables 3 and 4, respectively.

[0123] <Leveling ability> The laminates produced in the above Examples and Comparative Examples were visually evaluated for the degree of bleeding and coating unevenness of the surface protective layer. The practical level was AA to C. (Evaluation Criteria) AA: No uneven coating or flow is observed, and the coating has a glossy appearance. A: No swimming or uneven coating is observed, or very little swimming or uneven coating is observed B: Slightly smeared and uneven application C: Slightly loose and uneven application. D: Significant unevenness in application and smearing

[0124] <Abrasion resistance> The laminates produced in the above examples and comparative examples were evaluated using a Gakushin type friction fastness tester manufactured by Tester Sangyo Co., Ltd. The test conditions were as follows: test piece width: 20 mm, test piece length: 300 mm, load: 500 g, number of reciprocations: 100, and high-quality paper was used. The practical levels were A to C. (Evaluation Criteria) A: No ink or very little ink adheres to the rubbed fine paper. B: A small amount of ink adheres to rubbed fine paper. C: Some ink has adhered to rubbed fine paper. D: Ink adheres to the entire surface of rubbed high-quality paper.

[0125] <Water friction resistance> The laminates produced in the above examples and comparative examples were evaluated for water friction resistance using a Gakushin-type friction fastness tester manufactured by Tester Sangyo Co., Ltd. The test conditions were as follows: test piece width: 20 mm, test piece length: 300 mm, load: 200 g, number of reciprocations: 100 times, and five drops of water were dropped onto cotton cloth as the test paper. The practical level was A to C. When the present invention is used as a packaging material for low-temperature foods such as ice cream, it is expected that water droplets will form on the printed surface due to condensation and that the printed surface will come into contact with other packaging materials during transportation, etc. With water droplets formed, the more contact there is, the more likely the printed surface will become worn, so high water friction resistance is required. For this reason, the water friction resistance test in the present invention was carried out with an unprecedented number of reciprocating strokes. (Evaluation Criteria) A: No ink or very little ink adheres to the cotton cloth. B: A small amount of ink adheres to the rubbed cotton cloth. C: Some ink adheres to the cotton cloth. D: Ink adheres to the entire surface of the rubbed cotton cloth.

[0126] <Alcohol resistance> The alcohol resistance of the laminates produced in the above examples and comparative examples was evaluated. The test conditions were to rub the laminate from the surface protective layer side with a cotton swab soaked in a 40 wt% ethanol aqueous solution, and to measure the number of times the laminate was rubbed before the ink began to be removed. One back and forth rub was counted as one rub. The practical level was AA to C. (Evaluation Criteria) AA: 50 or more times A: 30 to 49 times B: 20 ​​to 29 times C: 10 to 19 times D: Less than 10 times

[0127] [Table 3]

[0128] [Table 4]

[0129] [Table 5]

[0130] From the above results, in Comparative Example 1, the aqueous overprint varnish did not contain the aqueous acrylic resin emulsion (B) but contained a water-soluble acrylic resin, so the water-resistant friction and alcohol resistance were poor. In Comparative Example 2, the aqueous overprint varnish did not contain the aqueous acrylic resin emulsion (A) but contained an aqueous urethane resin emulsion, so the friction resistance was poor. In Comparative Example 3, the aqueous overprint varnish did not contain a phosphoric acid ester compound, so the leveling property was poor. In Comparative Example 4, the aqueous overprint varnish did not contain a high-boiling point solvent, so the leveling property and friction resistance were poor. In Comparative Example 5, the aqueous ink did not contain either the aqueous acrylic resin emulsion (A) or the aqueous urethane resin, so the friction resistance was poor. In Comparative Example 6, the aqueous acrylic resin did not contain the aqueous acrylic resin emulsion (A) but contained a water-soluble acrylic resin, so the leveling property, water-resistant friction and alcohol resistance were poor. On the other hand, in the Examples, the water-based overprint varnish contained the water-based acrylic resin emulsion (B), a high boiling point solvent, and a phosphate ester compound, and therefore the leveling properties, abrasion resistance, water abrasion resistance, and alcohol resistance were good.

Claims

1. An ink set of a water-based overprint varnish and a water-based ink, the aqueous overprint varnish comprises an aqueous acrylic resin emulsion (A), a high-boiling point solvent having a boiling point of 105° C. or higher, and a phosphoric acid ester compound; The ink set, wherein the water-based ink comprises an aqueous acrylic resin emulsion (C) and / or an aqueous urethane resin.

2. 2. The ink set according to claim 1, wherein a mass ratio of the high boiling point solvent to the phosphate ester compound is 5:5 to 9.9:0.

1.

3. The ink set according to claim 1 or 2, wherein the water-based overprint varnish further comprises a hydrocarbon wax (B).

4. The ink set according to claim 3 , wherein the hydrocarbon wax (B) comprises a hydrocarbon wax (B1) having an average particle size of 1.5 μm or more, and a hydrocarbon wax (B2) having an average particle size of less than 1.5 μm.

5. 3. The ink set according to claim 1, wherein the aqueous acrylic resin emulsion (A) has an acid value of 100 mgKOH / g or less.

6. 3. The ink set according to claim 1 or 2, wherein the aqueous acrylic resin emulsion (A) comprises an aqueous acrylic resin emulsion (A1) having a glass transition temperature of 60° C. or higher, and an aqueous acrylic resin emulsion (A2) having a glass transition temperature of lower than 60° C.

7. 3. The ink set according to claim 1, wherein the water-based ink further comprises a water-soluble acrylic resin (D), and the acid value of the water-soluble acrylic resin (D) is 200 mg KOH / g or less.

8. 3. The ink set according to claim 1, wherein the aqueous overprint varnish and / or the aqueous ink further comprises a surfactant.

9. The ink set according to claim 8, wherein the surfactant is an acetylene glycol surfactant.

10. 3. The ink set according to claim 1 or 2, which is for gravure printing or flexographic printing.

11. 3. The ink set according to claim 1 or 2, which is for use on a polyolefin substrate.

12. A method for producing a laminate having a substrate, a printing layer, and a surface protective layer, comprising the steps of: A step of printing an aqueous ink containing an aqueous acrylic resin emulsion (C) and / or an aqueous urethane resin on a substrate to form a printed layer; and printing an aqueous overprint varnish containing an aqueous acrylic resin emulsion (A), a high-boiling point solvent having a boiling point of 105°C or higher, and a phosphate ester compound onto the printed layer to form a surface protective layer.

Citation Information

Patent Citations

  • Aqueous printing ink composition for paper container

    JP2016155965A

  • Food packaging paper and food packaging method using the same

    JP2021038022A

  • Aqueous solution ink, printed material having been printed with the aqueous solution ink, and oilproof paper

    JP2022096161A

  • Aqueous overcoat agent, laminate for packaging material, and packaging material

    JP2023005160A

Cited By

  • Heat-resistant coating agent, coated article, laminate, and packaging material

    WO2026133759A1