Pattern formation method
The described method addresses resist residue and indentation issues by applying a metal-containing resist composition and edge bead removal process, enhancing the quality and reducing defects in fine pattern formation.
Patent Information
- Application Number
- JP2024069232
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-17
- Filing Date
- 2024-04-22
- Publication Date
- 2024-11-28
- Estimated Expiration
- 2044-04-22
AI Technical Summary
The formation of fine patterns in semiconductor manufacturing is hindered by resist residue and indentation at the edges and back surface of the silicon substrate, leading to defects in subsequent processes such as etching and ion implantation.
A pattern forming method involving the application of a metal-containing resist composition, followed by an edge bead removal process using a specific edge bead removal composition, a heat treatment, and subsequent exposure and development to control the maximum height of the hump on the resist layer to 300 nm or less.
This method reduces the defect rate in fine pattern formation by effectively removing edge beads and controlling hump height, thereby improving the integrity and quality of the resist pattern.
Smart Images

Figure 2024166091000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a pattern forming method including a step of applying an edge bead removing composition and performing an edge bead removal treatment. [Background technology]
[0002] In recent years, the semiconductor industry has experienced a continuous decline in critical dimensions, which has created a demand for new types of high performance resist materials and patterning methods to meet the demands of fabricating and patterning smaller and smaller features.
[0003] In addition, with the recent rapid development of the semiconductor industry, there is a demand for semiconductor devices with higher operating speeds and larger memory capacities, and technologies to improve the integration, reliability, and response speed of semiconductor devices are also being developed to meet these demands. In particular, it is important to precisely control / inject impurities into the active regions of a silicon substrate, and to interconnect these regions to form elements and ultra-high density direct circuits, which is made possible by the photolithography process. That is, it is becoming important to consider integration in the photolithography process, which includes coating a resist on a substrate, selectively exposing it to ultraviolet light (including extreme ultraviolet light), electron beams, or X-rays, and then developing it.
[0004] In particular, in the process of forming the resist layer, the resist is applied to the substrate while the substrate is rotated, and in this process, the resist is also applied to the edge and back surface of the substrate. This may cause indenter induction and pattern defects in subsequent semiconductor processes such as etching and ion implantation. Therefore, a process of stripping and removing the resist applied to the edge and back surface of the silicon substrate using a thinner composition, i.e., an EBR (EDGE BEAD REMOVAL) process, is performed.
[0005] The EBR process uses a composition that exhibits excellent solubility in resist, effectively removes beads and resist remaining on the substrate, and does not leave any resist residue. Summary of the Invention [Problem to be solved by the invention]
[0006] An object of the present invention is to provide a pattern forming method which reduces the defect rate when forming a fine pattern. [Means for solving the problem]
[0007] A pattern forming method according to one aspect of the present invention includes the steps of: 1. A step of applying a metal-containing resist composition onto a substrate to form a resist layer; a removing step of applying an edge bead removing composition to the resist layer along the outer periphery of the substrate to remove the edge bead; a first heat treatment step of drying and heating the resist layer that has been subjected to the removal treatment in the removal step; and a resist pattern forming step of performing an exposure process and a development process on the resist layer that has been subjected to the drying process and the heating process in the first heat treatment step to form a resist pattern; After the first heat treatment step and before the resist pattern forming step, the maximum height of a hump in the resist layer in a region extending from the outer circumferential edge of the substrate toward the center thereof to a distance of 1 mm to 30 mm is 300 nm or less.
[0008] 2. In the pattern formation method described in 1 above, the maximum height of the hump may be 10 nm or more and 300 nm or less.
[0009] 3. In the pattern formation method described in 1. or 2. above, the difference between the surface energy of the resist layer and the surface tension of the edge bead removal composition may be 2 mN / m or more and 15 mN / m or less.
[0010] 4. In the pattern formation method according to any one of the above 1. to 3., the surface tension of the edge bead removing composition may be 25.0 mN / m or more and 40.0 mN / m or less.
[0011] 5. In the pattern formation method according to any one of the above 1. to 4., the surface tension of the edge bead removal composition may be 27.0 mN / m or more and 36.0 mN / m or less.
[0012] 6. In the pattern formation method according to any one of 1. to 5. above, the viscosity of the edge bead removing composition may be 1 cPs or more and 10 cPs or less.
[0013] 7. In the pattern formation method according to any one of 1. to 6. above, the removal treatment in the removing step may be carried out while rotating the substrate at a speed of 500 rpm or more and 4,500 rpm or less.
[0014] 8. In the pattern formation method according to any one of 1. to 7. above, the metal compound contained in the metal-containing resist composition may include at least one selected from the group consisting of organic oxy group-containing tin compounds and organic carbonyloxy group-containing tin compounds.
[0015] 9. In the pattern formation method according to any one of the above items 1. to 8., the metal-containing resist composition may contain a metal compound represented by the following chemical formula 1 or a condensate thereof.
[0016] [ka]
[0017] In the above Chemical Formula 1, R 1is a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, a substituted or unsubstituted arylalkyl group having 6 to 30 carbon atoms, or -L a -OR a (Here, L a is a single bond or a substituted or unsubstituted alkylene group having 1 to 20 carbon atoms, R a is a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms; R 2 ~R 4 each independently represents a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, a substituted or unsubstituted arylalkyl group having 6 to 30 carbon atoms, -OR b and -OC(=O)R c and R 2 ~R 4 At least one of the is -OR b and OC(=O)R c is selected from among In this case, R b is a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, or a combination thereof; R c is a hydrogen atom, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, or a combination thereof. Effect of the Invention
[0018] According to the present invention, it is possible to provide a pattern formation method that reduces the defect rate when forming a fine pattern. [Brief description of the drawings]
[0019] [Figure 1] FIG. 2 is a schematic diagram showing a resist coating apparatus. [Diagram 2] FIG. 2 is a schematic diagram for explaining a hump. [Diagram 3] 1 is an image taken by an electron microscope of a resist layer according to an embodiment after spraying an edge bead removal composition onto the resist layer on a substrate, as measured by a profiler device. [Figure 4] 1 is an image taken by an electron microscope of a resist layer according to a comparative example after an edge bead removal composition is sprayed onto the resist layer on a substrate, as measured by a profiler device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] Hereinafter, an embodiment of the present invention will be described in detail with reference to the accompanying drawings. However, in describing the present invention, a description of functions or configurations that are already known will be omitted in order to clarify the gist of the description.
[0021] In order to clearly explain the present description, parts unnecessary for the description will be omitted, and the same or similar components will be labeled with the same reference numerals throughout the specification. Furthermore, the size and thickness of each component shown in the drawings are arbitrarily shown for the convenience of explanation, and the present invention is not necessarily limited to those shown in the drawings.
[0022] In the drawings, the thicknesses of various layers and regions are exaggerated to clearly show the layers and regions. Also, in the drawings, the thicknesses of some layers and regions are exaggerated for ease of explanation. When a part such as a layer, film, region, plate, etc. is "on" or "on" another part, this includes not only the case where it is "directly on" the other part, but also the case where there is another part therebetween.
[0023] In this description, "substituted" means that a hydrogen atom is substituted with a deuterium atom, a halogen atom, a hydroxyl group, an amino group, a substituted or unsubstituted amine group having 1 to 30 carbon atoms, a nitro group, a substituted or unsubstituted silyl group having 1 to 40 carbon atoms, an alkyl group having 1 to 30 carbon atoms, a haloalkyl group having 1 to 10 carbon atoms, an alkylsilyl group having 1 to 10 carbon atoms, a cycloalkyl group having 3 to 30 carbon atoms, an aryl group having 6 to 30 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, or a cyano group. "Unsubstituted" means that a hydrogen atom is not substituted with another substituent and remains as a hydrogen atom.
[0024] In this description, unless otherwise specified, an "alkyl group" refers to a straight-chain or branched-chain aliphatic hydrocarbon group. The alkyl group may be a "saturated alkyl group" that does not contain any double or triple bonds.
[0025] The alkyl group may be an alkyl group having 1 to 20 carbon atoms. More specifically, the alkyl group may be an alkyl group having 1 to 10 carbon atoms or an alkyl group having 1 to 6 carbon atoms. For example, an alkyl group having 1 to 5 carbon atoms means that the alkyl chain contains 1 to 5 carbon atoms and indicates that the alkyl group is selected from the group consisting of methyl, ethyl, propyl, iso-propyl, n-butyl, iso-butyl, sec-butyl, t-butyl, n-pentyl, isopentyl, tert-pentyl, and neopentyl.
[0026] Specific examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a t-butyl group, a pentyl group, and a hexyl group.
[0027] In this specification, unless otherwise defined, the term "cycloalkyl group" refers to a monovalent cyclic aliphatic hydrocarbon group. The cycloalkyl group refers to a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, etc.
[0028] As used herein, unless otherwise defined, an "alkenyl group" refers to a straight-chain or branched-chain aliphatic hydrocarbon group that is an aliphatic unsaturated alkenyl group containing one or more double bonds.
[0029] As used herein, unless otherwise defined, an "alkynyl group" refers to a straight-chain or branched-chain aliphatic hydrocarbon group that is an aliphatic unsaturated alkynyl group containing one or more triple bonds.
[0030] As used herein, an "aryl group" refers to a substituent in which all of the elements of a cyclic substituent have p-orbitals and these p-orbitals form conjugation, and includes monocyclic or fused-ring polycyclic (i.e., rings which share adjacent pairs of carbon atoms) functional groups.
[0031] More specifically, the substituted or unsubstituted aryl group having 6 to 30 carbon atoms may be, but is not limited to, a substituted or unsubstituted phenyl group, a substituted or unsubstituted naphthyl group, a substituted or unsubstituted anthracenyl group, a substituted or unsubstituted phenanthrenyl group, a substituted or unsubstituted naphthacenyl group, a substituted or unsubstituted pyrenyl group, a substituted or unsubstituted biphenyl group, a substituted or unsubstituted p-terphenyl group, a substituted or unsubstituted m-terphenyl group, a substituted or unsubstituted o-terphenyl group, a substituted or unsubstituted chrysenyl group, a substituted or unsubstituted benzophenanthrenyl group, a substituted or unsubstituted triphenylene group, a substituted or unsubstituted perylenyl group, a substituted or unsubstituted fluorenyl group, a substituted or unsubstituted indenyl group, or a combination thereof.
[0032] 1 is a schematic diagram showing a photoresist coating apparatus. In this specification, photoresist is also simply referred to as resist.
[0033] 1, the resist coating apparatus includes a substrate support 1 on which a substrate (W) is placed. The substrate support 1 includes a spin chuck or a spin coater.
[0034] The substrate support 1 rotates in a first direction at a predetermined rotation speed to provide centrifugal force to the substrate (W). A spray nozzle 2 is located above the substrate support 1. The spray nozzle 2 is located in an area away from the top of the substrate (W) and can move above the substrate in the process of supplying the solution to spray the resist solution 10. As a result, the resist solution 10 is applied to the substrate surface by centrifugal force. At this time, the resist solution 10 supplied to the center of the substrate (W) is applied while spreading to the edge of the substrate (W) by centrifugal force, and part of it moves to the side of the substrate and the underside of the edge of the substrate.
[0035] That is, in the process of forming a resist layer on a substrate, the resist solution 10 is mainly applied onto the substrate by a spin coating method. In the spin coating method, a predetermined amount of viscous resist solution 10 is supplied to the center of the substrate (W), and the resist solution 10 gradually spreads toward the edge of the substrate by centrifugal force.
[0036] Therefore, the resist is formed to a constant thickness by the rotation of the substrate support 1.
[0037] However, as the solvent evaporates, the viscosity of the resist solution 10 increases, and a relatively large amount of resist accumulates at the edge of the substrate due to the action of surface tension. Even more serious, resist accumulates on the underside of the edge of the substrate, which is called an edge bead 12.
[0038] A pattern forming method according to one embodiment of the present invention will be described below. Note that, hereinafter, the resist solution 10 is also referred to as a metal-containing resist composition.
[0039] In this specification, a hump refers to a raised portion of a resist layer that occurs at the boundary between a flat area extending from the center of the resist layer toward the edge thereof and the removed area after the edge bead is removed, as shown in the schematic diagram of FIG.
[0040] A pattern forming method according to one embodiment of the present invention includes the steps of: applying a metal-containing resist composition onto a substrate to form a resist layer; applying an edge bead removal composition to the resist layer along the outer periphery of the substrate to remove the edge bead; a first heat treatment step of drying and heating the resist layer that has been subjected to the removal step; and a resist pattern forming step of exposing and developing the resist layer that has been dried and heated in the first heat treatment step to form a resist pattern. After the first heat treatment step and before the resist pattern forming step, the maximum height of a hump in the resist layer in a region extending from the outer circumferential edge of the substrate toward the center of the substrate is 300 nm or less.
[0041] Here, the maximum height of the hump means the step (ΔThickness) between the flat part of the resist layer other than the hump and the most elevated part of the hump, as shown in Fig. 2b. The maximum height of the hump can be measured, for example, using a Tencor Profiler P17OF device.
[0042] The maximum value of the maximum height of the hump in the region from the outer peripheral edge of the substrate toward the center of 1 mm to 30 mm is 300 nm or less, but may be 250 nm or less, 200 nm or less, 150 nm or less, or 100 nm or less. Or, the minimum value of the maximum height of the hump may be 10 nm or more, or 20 nm or more. That is, the maximum height of the hump may be 10 nm or more to 300 nm, 20 nm or more to 300 nm, 10 nm or more to 250 nm, 20 nm or more to 250 nm, 10 nm or more to 200 nm, 20 nm or more to 200 nm, 10 nm or more to 150 nm, 20 nm or more to 150 nm, 10 nm or more to 100 nm, or 20 nm or more to 100 nm.
[0043] (Step of forming a resist layer) More specifically, the process of forming a resist layer by applying a metal-containing resist composition onto a substrate may include a process of applying the metal-containing resist composition onto a substrate by spin coating, slit coating, inkjet printing, or the like, and a process of drying the applied metal-containing resist composition to form a resist layer.
[0044] Metal-Containing Resist Composition The metal compound contained in the metal-containing resist composition may be, for example, a tin compound, and the tin compound may include, for example, at least one selected from the group consisting of organic oxy group-containing tin compounds and organic carbonyloxy group-containing tin compounds.
[0045] An example of the metal compound contained in the metal-containing resist is a compound represented by the following Chemical Formula 1 or a condensation product thereof.
[0046] [ka]
[0047] In chemical formula 1, R 1is a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, a substituted or unsubstituted arylalkyl group having 6 to 30 carbon atoms, or -L a -OR a (Here, L a is a single bond or a substituted or unsubstituted alkylene group having 1 to 20 carbon atoms, R a is a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms; R 2 ~R 4 each independently represents a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, a substituted or unsubstituted arylalkyl group having 6 to 30 carbon atoms, -OR b and -OC(=O)R c and R 2 ~R 4 At least one of the is -OR b and -OC(=O)R c is selected from among In this case, R b is a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, or a combination thereof; R c is a hydrogen atom, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, or a combination thereof.
[0048] The metal compound contained in the metal-containing resist composition according to an embodiment may be a compound represented by the following chemical formula C or D.
[0049] [ka]
[0050] [ka]
[0051] The metal-containing resist composition according to an embodiment may include a solvent. The solvent is not particularly limited, and may be any solvent that is applicable to resist compositions in the art, such as, but not limited to, aromatic compounds (e.g., xylene, toluene), alcohols (e.g., 4-methyl-2-pentanol, 4-methyl-2-propanol, 1-butanol, methanol, isopropyl alcohol, 1-propanol), ethers (e.g., anisole, tetrahydrofuran), esters (n-butyl acetate, propylene glycol monomethyl ether acetate, ethyl acetate, ethyl lactate), ketones (e.g., methyl ethyl ketone, 2-heptanone), and mixtures thereof.
[0052] In addition, the metal-containing resist composition according to an embodiment may include at least one selected from the group consisting of a surfactant, a dispersant, a moisture absorbent, and a coupling agent.
[0053] The surfactant may play a role in improving the coating uniformity of the resist composition and improving the wetting. In one embodiment, the surfactant may be, but is not limited to, a sulfate salt, a sulfonate salt, a phosphate salt, a soap, an amine salt, a quaternary ammonium salt, a polyethylene glycol, an alkylphenol ethylene oxide adduct, a polyhydric alcohol, a nitrogen-containing vinyl polymer, or a combination thereof. For example, the surfactant may include an alkylbenzene sulfonate salt, an alkylpyridinium salt, a polyethylene glycol, or a quaternary ammonium salt. When the resist composition includes a surfactant, the surfactant is included in an amount of about 0.001% by weight to about 3% by weight based on the total weight of the resist composition.
[0054] The dispersant can serve to uniformly disperse each component of the resist composition in the resist composition. In one embodiment, the dispersant is an epoxy resin, polyvinyl alcohol, polyvinyl butyral, polyvinylpyrrolidone, glucose, sodium dodecyl sulfate, sodium citrate, oleic acid, linoleic acid, or a combination thereof, but is not limited thereto. When the resist composition includes a dispersant, the dispersant is included in an amount of about 0.001 wt % to about 5 wt % based on the total weight of the resist composition.
[0055] The moisture absorbent can prevent adverse effects of moisture on the resist composition. For example, the moisture absorbent can prevent metals contained in the resist composition from being oxidized by moisture. In one embodiment, the moisture absorbent is polyoxyethylenenonylphenolether, polyethylene glycol, polypropylene glycol, polyacrylamide, or a combination thereof, but is not limited thereto. When the resist composition includes the moisture absorbent, the moisture absorbent is included in an amount of about 0.001 wt % to about 10 wt % based on the total weight of the resist composition.
[0056] The coupling agent can improve the adhesion of the resist composition to the lower film when the resist composition is coated on the lower film. In one embodiment, the coupling agent can include a silane coupling agent. The silane coupling agent can be vinyltrimethoxysilane, vinyltriethoxysilane, vinyltrichlorosilane, vinyltris(β-methoxyethoxy)silane, 3-methacryloxypropyltrimethoxysilane, 3-acryloxypropyltrimethoxysilane, p-styryltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, or trimethoxy[3-(phenylamino)propyl]silane, but is not limited thereto. When the resist composition includes a coupling agent, the coupling agent is included in an amount of about 0.001% by weight to about 5% by weight based on the total weight of the resist composition.
[0057] (Removal process) Next, in the pattern formation method according to one embodiment of the present invention, a removing step is carried out in which an edge bead removing composition is applied to the resist layer along the outer periphery of the substrate to remove the edge bead.
[0058] In this process, after the edge bead is removed by applying the edge bead removal composition, a hump is generated at the boundary between the flat area extending from the center of the resist layer toward the edge and the removed area.
[0059] The hump can cause cracks or film peeling during firing of the layer, which can lead to mask contamination and non-uniformity in subsequent processes. Therefore, there is a need for an edge bead removal composition that can provide a resist layer (resist film) with a better edge cut shape after application of the edge bead removal composition.
[0060] In the process of applying the edge bead removal composition according to one embodiment of the present invention, the hump height that is unlikely to cause problems in the subsequent process was examined by adjusting the main physical properties of the resist and the edge bead removal composition, particularly the viscosity and surface energy difference, and the process conditions of the edge bead removal process, and an optimized method for achieving the hump height was also examined. Here, the surface energy difference means the difference between the surface energy of the resist layer and the surface tension of the edge bead removal composition.
[0061] The difference between the surface energy of the resist layer and the surface tension of the edge bead removal composition may be 2 mN / m or more and 15 mN / m or less. When the difference between the surface energy of the resist layer and the surface tension of the edge bead removal composition is 15 mN / m or less, the problem that the wetting property is low and it is difficult for the edge bead removal composition to dissolve the resist, resulting in a low cleaning power, can be solved. In addition, when the affinity at the interface is low, mutual repulsion acts, the hump becomes larger, and the dissolved resist is not removed and remains in a solid form near the interface, can be solved. In addition, when the difference between the surface energy of the resist layer and the surface tension of the edge bead removal composition is 2 mN / m or more, the problem that the penetration of the edge bead removal composition into the resist becomes fast, resulting in damage to the resist layer and expansion development, can be solved. In the pattern formation method according to an embodiment of the present invention, the difference between the surface energy of the resist layer and the surface tension of the edge bead removal composition is appropriate, and the effect on the resist layer is minimized while metal substrate contamination is reduced, thereby meeting the requirements for processing and patterning of smaller features. In addition, the difference between the surface energy of the resist layer and the surface tension of the edge bead removal composition may be 3 mN / m to 15 mN / m, 3 mN / m to 10 mN / m, 4 mN / m to 15 mN / m, or 4 mN / m to 10 mN / m.
[0062] The difference in surface energy between the resist layer and the edge bead removal composition can be measured by the method described in the examples.
[0063] The surface energy of the resist layer may be 25.0 mN / m or more and 50.0 mN / m or less, or 30.0 mN / m or more and 45.0 mN / m or less. When the surface energy of the resist layer is in the above range, the edge bead can be removed more effectively, and the maximum height of the hump can be effectively suppressed. The surface energy of the resist layer can be measured by the method described in the examples.
[0064] The surface tension of the edge bead removal composition may be 25.0 mN / m or more and 40.0 mN / m or less, 27.0 mN / m or more and 40.0 mN / m or less, 27.0 mN / m or more and 36.0 mN / m or less, or 27.0 mN / m or more and 33.0 mN / m or less. When the surface tension of the edge bead removal composition is in the above range, the edge bead can be removed more effectively, and the maximum height of the hump can also be effectively suppressed.
[0065] The surface tension of the edge bead removing composition can be measured using a surface tension system K11-MK1 (manufactured by KRUSS Co., Ltd.) More specifically, the surface tension of the edge bead removing composition can be measured by the method described in the Examples.
[0066] The viscosity of the edge bead removing composition may be 1 cPs or more and 10 cPs or less. The viscosity of the edge bead removing composition may be 1 cPs or more and 9 cPs or less, 1 cPs or more and 8 cPs or less, 1 cPs or more and 7 cPs or less, 1 cPs or more and 6 cPs or less, 1 cPs or more and 5 cPs or less, 1 cPs or more and 4 cPs or less, or 1 cPs or more and 3 cPs or less. By having the viscosity of the edge bead removing composition in the above range, the edge bead can be more effectively removed, and the maximum height of the hump can also be effectively suppressed, so that the pattern defect rate is further reduced.
[0067] For example, when the resist layer contains a metal compound represented by chemical formula C, the viscosity of the edge bead removal composition may be 1 cPs or more and 10 cPs or less, 1 cPs or more and 9 cPs or less, 1 cPs or more and 8 cPs or less, 1 cPs or more and 7 cPs or less, 1 cPs or more and 6 cPs or less, 1 cPs or more and 5 cPs or less, 1 cPs or more and 4 cPs or less, or 1 cPs or more and 3 cPs or less. When the resist layer contains a metal compound represented by chemical formula C, the viscosity of the edge bead removal composition in the above range can more fully remove the edge bead, and the maximum height of the hump can also be more effectively suppressed.
[0068] The viscosity of the edge bead removing composition can be measured using LVDV-III-UCP (manufactured by BROOKFIELD Corp.) More specifically, the viscosity of the edge bead removing composition can be measured by the method described in the Examples.
[0069] The edge bead removal composition according to an embodiment of the present invention may include an additive and a solvent. The additive and the solvent are materials that can be applied to edge bead removal compositions in the art and may be selected within a range that satisfies the above-mentioned conditions. When the viscosity of the edge bead removal composition is within the above-mentioned range, the edge bead can be effectively removed and the maximum height of the hump can be suppressed.
[0070] The additive contained in the edge bead removal composition according to one embodiment may be at least one of acid compounds such as carboxylic acid, phosphoric acid, phosphorous acid, phosphonic acid, sulfuric acid, and sulfonic acid, alcohol compounds, and ketone compounds. In particular, from the viewpoint of more efficiently removing the edge bead, the additive may be one or more selected from the group consisting of ethanesulfonic acid, methanesulfonic acid, butylphosphonic acid, methylphosphonic acid, trifluoroacetic acid, propionic acid, glycolic acid, difluoroacetic acid, vinylphosphonic acid, stearic acid, oleic acid, 4-nitrocatechol, tropolone, and acetylacetone.
[0071] The solvent contained in the edge bead removal composition according to one embodiment is not particularly limited, but may include at least one selected from the group consisting of ethers, alcohols, glycol ethers, aromatic hydrocarbon compounds, ketones, esters, amides, sulfoxides, and nitriles, and may include at least one selected from the group consisting of ethers, glycol ethers, esters, and alcohols. Examples of the solvent include propylene glycol methyl ether (PGME), propylene glycol methyl ether acetate (PGMEA), propylene glycol butyl ether (PGBE), ethylene glycol methyl ether, diethylene glycol ethyl methyl ether, dipropylene glycol dimethyl ether, ethanol, 2-butoxyethanol, n-propanol, isopropanol, n-butanol, isobutyl alcohol, hexanol, ethylene glycol, propylene glycol, heptanone, propylene carbonate, butylene carbonate, diethyl ether, dibutyl ether, ethyl acetate, n-butyl acetate (nBA), methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, diisopentyl ether, xylene, acetone, methyl ethyl ketone, methyl isobutyl ketone, tetrahydrofuran, dimethyl sulfoxide, dimethylformamide, acetonitrile, diacetone alcohol, 3,3-Dimethyl-2-butanone, N-methyl-2-pyrrolidone, dimethylacetamide, cyclohexanone methyl-2-hydroxy-2-methylpropionate (HBM), gamma-butyrolactone (GBL), 1-butanol (n-Butanol), ethyl lactate (EL), diethyl butyl ether (DBE), diisopropyl ether (DIAE), acetylacetone, butyl lactate (n-Butylactate), 4-methyl-2-pentanol (or methyl isobutyl carbinol (MIBC), 1-methoxy-2-propanol, 1-ethoxy-2-propanol, toluene, cyclopentanone, cyclohexanone, ethyl 2-hydroxypropionate, ethyl 2-hydroxy-2-methylpropionate, ethyl ethoxyacetate, ethyl hydroxyacetate, methyl 2-hydroxy-3-methylbutanoate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, ethyl 3-ethoxypropionate, methyl 3-ethoxypropionate, methyl pyruvate, ethyl pyruvate, butyl acetate, methyl 2-hydroxyisobutyrate, methoxybenzene, n-butyl acetate, 1-methoxy-2-propyl acetate, methoxyethoxypropionate, ethoxyethoxypropionate, or mixtures thereof. Among these, from the viewpoint of more efficient removal of the edge bead, the solvent is preferably one or more selected from the group consisting of propylene glycol methyl ether (PGME), propylene glycol methyl ether acetate (PGMEA), gamma butyrolactone (GBL), ethyl lactate (EL), and 4-methyl-2-pentanol (MIBC).
[0072] In addition, the combination of the above-mentioned solvent and additive is not particularly limited, but when the solvent is an ether, the additive to be combined may be an acid compound (particularly, a carboxylic acid). For example, when the solvent is propylene glycol methyl ether (PGME), the additive to be combined may be one or more selected from the group consisting of propionic acid and difluoroacetic acid.
[0073] In addition, when the solvent is a glycol ether, the additive to be combined may be one selected from the group consisting of an alcohol compound and an acid compound. For example, when the solvent is propylene glycol methyl ether acetate (PGMEA), the additive may be one or more selected from the group consisting of 4-nitrocatechol, butylphosphonic acid, methylphosphonic acid, tropolone, vinylphosphonic acid, and oleic acid.
[0074] Also, when the solvent is an ester, the additive to be combined may be one or more selected from an acid compound and a ketone compound, or the ester solvent may be used alone without any additive. For example, when the solvent is ethyl lactate (EL), the additive may be one or more selected from the group consisting of ethanesulfonic acid, glycolic acid, acetylacetone, and stearic acid, or ethyl lactate (EL) may be used alone without any additive. Also, when the solvent is gamma butyrolactone (GBL), the additive may be one or more selected from the group consisting of trifluoroacetic acid and propionic acid.
[0075] In addition, when the solvent is an alcohol, the additive to be combined may be an acid compound. For example, when the solvent is 4-methyl-2-pentanol (MIBC), the additive may be methanesulfonic acid.
[0076] In one embodiment, the edge bead removal composition may include from 0.01% to 50% by weight of the additives described above, and from 50% to 99.99% by weight of a solvent.
[0077] The edge bead removal composition may further contain at least one selected from the group consisting of a surfactant, a dispersant, a moisture absorbent, and a coupling agent. When these are contained, the solvent is contained in the amount remaining excluding the contained components. As the surfactant, dispersant, moisture absorbent, and coupling agent contained in the edge bead removal composition, those described in the section on the metal-containing resist composition can be appropriately adopted.
[0078] The step of applying the edge bead removing composition according to one embodiment and performing the edge bead removal process can be performed while spinning the substrate at a speed of, for example, 800 rpm to 4,500 rpm. The speed at which the substrate is rotated may be 1000 rpm to 4500 rpm, 1500 rpm to 4500 rpm, 2000 rpm to 4500 rpm, 2500 rpm to 4500 rpm, 1000 to 4000 rpm, 1500 rpm to 4000 rpm, 2000 rpm to 4000 rpm, or 2500 rpm to 4000 rpm. By rotating the substrate at a speed within the above range, the maximum height of the bump can be made lower. In one embodiment, the time for rotating the substrate at the above speed is preferably 10 seconds to 100 seconds, and more preferably 20 seconds to 60 seconds.
[0079] In one embodiment, the process of applying the edge bead removal composition may be repeated several times to reduce metal base contamination applied to the edge and backside of the substrate and to reduce resist to the desired level.
[0080] Furthermore, the area to which the edge bead removal composition of one embodiment is applied is not particularly limited as long as it is along the outer periphery of the substrate so that the edge bead can be removed; for example, the composition may be applied to a position within 30 mm from the outer periphery of the substrate toward the center, within 25 mm, within 20 mm, within 15 mm, within 10 mm, within 5 mm, within 4 mm, within 3 mm, within 2 mm, or within 1 mm.
[0081] Patterning methods that include applying an edge bead removal composition according to the present invention and removing the edge bead are particularly effective in removing metal-containing resists, and more specifically, undesirable metal residues, such as tin-based metal residues.
[0082] (First heat treatment process) Next, a first heat treatment step is performed to dry and heat the substrate on which the resist layer is formed. The first heat treatment step is not particularly limited, but may be performed at a temperature of 70°C to 170°C, or 80°C to 160°C. The heating time at the temperature is not particularly limited, but may be 30 seconds to 120 seconds, or 40 seconds to 80 seconds. In this process, the solvent is released in an increased amount, and the resist layer is more firmly attached to the substrate.
[0083] (Resist pattern formation process) Subsequently, the resist layer that has been subjected to the drying treatment and the heating treatment in the first heat treatment step is subjected to an exposure treatment and a development treatment to form a resist pattern in a resist pattern formation step.
[0084] In the exposure process, the resist layer can be selectively exposed.
[0085] For example, examples of light that can be used in the exposure process include light with short wavelengths such as activation irradiation conductor i-line (wavelength 365 nm), KrF excimer laser (wavelength 248 nm), and ArF excimer laser (wavelength 193 nm), as well as light with high energy wavelengths such as EUV (Extreme Ultra Violet; wavelength 13.5 nm) and E-Beam (electron beam).
[0086] More specifically, the exposure light according to one embodiment may be short-wavelength light having a wavelength range of 5 nm to 150 nm, or may be light having a high-energy wavelength such as EUV (Extreme Ultra Violet; wavelength 13.5 nm) or E-Beam (electron beam).
[0087] In the resist pattern forming step, a negative pattern can be formed.
[0088] The exposed areas of the resist layer form polymers through cross-linking reactions such as condensation between metal compounds, and thus have a different solubility from the unexposed areas of the resist layer.
[0089] Subsequently, in the resist pattern forming step of one embodiment, the substrate may be subjected to a second heat treatment step. The second heat treatment step may be performed at a temperature of 90°C to 200°C. The heating time is not particularly limited, but may be 30 seconds or more and 120 seconds or less, or 40 seconds or more and 80 seconds or less. By performing the second heat treatment step, the exposed area of the resist layer becomes difficult to dissolve in a developer.
[0090] Subsequently, in the development process, development can be carried out using a developer composition.
[0091] Specifically, the resist layer in the unexposed area is dissolved using a developer composition and then removed, completing a resist pattern corresponding to a negative tone image.
[0092] The developer composition used in the development process may be, for example, an organic solvent, for example, ketones such as methyl ethyl ketone, acetone, cyclohexanone, and 2-hubtanone; alcohols such as 4-methyl-2-propanol, 1-butanol, isopropanol, 1-propanol, methanol, propylene glycol methyl ether (PGME), and methyl isobutyl carbinol (MIBC); esters such as propylene glycol methyl ether acetate, ethyl acetate, ethyl lactate, n-butyl acetate, methyl-2-hydroxyisobutyrate, and butyrolactone; aromatic compounds such as benzene, xylene, and toluene, or combinations thereof.
[0093] As described above, the resist pattern formed by exposure to light having a wavelength such as i-line (wavelength 365 nm), KrF excimer laser (wavelength 248 nm), ArF excimer laser (wavelength 193 nm), and high-energy light such as EUV (Extreme Ultra Violet; wavelength 13.5 nm) and E-Beam (electron beam) can have a thickness width of 5 nm to 100 nm. For example, the resist pattern can be formed with a thickness width of 5 nm to 90 nm, 5 nm to 80 nm, 5 nm to 70 nm, 5 nm to 60 nm, 5 nm to 50 nm, 5 nm to 40 nm, 5 nm to 30 nm, or 5 nm to 20 nm.
[0094] On the other hand, the resist pattern can have a half-pitch of about 50 nm or less, such as 40 nm or less, such as 30 nm or less, such as 20 nm or less, such as 15 nm or less, and a line width roughness of about 10 nm or less, about 5 nm or less, about 3 nm or less, about 2 nm or less.
[0095] Although the embodiment of the present invention has been described in detail above, it is clear that the embodiment is merely illustrative and exemplary, and is not limiting, and the scope of the present invention should be interpreted according to the appended claims. For example, the pattern formation method according to one embodiment of the present invention also includes the following embodiments. (i) applying a metal-containing resist composition onto a substrate to form a resist layer; applying an edge bead removal composition along an edge of the substrate; a heat treatment step of drying and heating; and A step of forming a resist pattern by exposure and development. Including, The method for forming a pattern, wherein after applying the edge bead removing composition, the maximum hump height of the resist layer is 300 nm or less in a region of 1 mm to 30 mm from the edge of the substrate toward the center of the substrate. (ii) The pattern formation method according to (i), wherein the maximum hump height is 10 nm to 300 nm. (iii) The pattern forming method described in (i) or (ii), wherein the difference between the surface energy of the resist layer and the surface tension of the edge bead removing composition is 2 mN / m to 15 mN / m. (iv) The pattern formation method according to any one of (i) to (iii), wherein the surface tension of the edge bead removing composition is 25.0 mN / m to 40.0 mN / m. (v) The pattern formation method according to any one of (i) to (iv), wherein the surface tension of the edge bead removing composition is 27.0 mN / m to 36.0 mN / m. (vi) The method of forming a pattern according to any one of (i) to (v), wherein the viscosity of the composition for removing edge beads is 1 to 10 cPs. (vii) The pattern forming method according to any one of (i) to (vi), wherein the step of applying the edge bead removing composition is performed while rotating the substrate at a speed of 1,000 to 4,000 rpm. (viii) The pattern formation method according to any one of (i) to (vii), wherein the metal compound contained in the metal-containing resist includes at least one of an organic oxy group-containing tin compound and an organic carbonyloxy group-containing tin compound. (ix) The method for forming a pattern according to any one of (i) to (viii), wherein the metal compound contained in the metal-containing resist is represented by the following chemical formula 1:
[0096] [ka]
[0097] In the above Chemical Formula 1, R 1 is a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C2 to C20 alkynyl group, a substituted or unsubstituted C6 to C30 aryl group, a substituted or unsubstituted C6 to C30 arylalkyl group, and -L a -OR a (Here, L a is a single bond or a substituted or unsubstituted C1 to C20 alkylene group, R a is a substituted or unsubstituted C1 to C20 alkyl group; R 2 ~R 4 each independently represents a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C2 to C20 alkynyl group, a substituted or unsubstituted C6 to C30 aryl group, a substituted or unsubstituted C6 to C30 arylalkyl group, -OR b and -OC(=O)R c and R 2 ~R 4 At least one of the is -OR b and OC(=O)R c is selected from among In this case, R b is a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C2 to C20 alkynyl group, a substituted or unsubstituted C6 to C30 aryl group, or a combination thereof; R cis a hydrogen atom, a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C2 to C20 alkynyl group, a substituted or unsubstituted C6 to C30 aryl group, or a combination thereof. EXAMPLES
[0098] Hereinafter, the present invention will be described in more detail with reference to examples of the above-mentioned pattern forming method, but the technical features of the present invention are not limited to the following examples.
[0099] (Preparation of Metal-Containing Resist Composition) <Manufacturing example A> A metal compound having the structure of the following chemical formula C was dissolved in 4-methyl-2-pentanol at a concentration of 1 wt % and filtered through a 0.1 μm PTFE syringe filter to prepare a resist composition.
[0100] [ka]
[0101] <Manufacturing example B> A resist composition was prepared in the same manner as in Preparation Example A, except that a metal compound having the structure of the following chemical formula D was used.
[0102] [ka]
[0103] (Production of edge bead removal composition) Manufacturing Example 1 to Manufacturing Example 22 The additives and the solvent were mixed according to the compositions shown in Table 1 below, and then the mixture was shaken at room temperature (25°C) to completely dissolve. The mixture was then passed through a PTFE filter with a pore size of 1 μm to obtain a final edge bead removal composition. In the table, PGMEA stands for propylene glycol methyl ether acetate, EL stands for ethyl lactate, GBL stands for gamma butyrolactone, MIBC stands for 4-methyl-2-pentanol, PGME stands for propylene glycol methyl ether, and nBA stands for n-butyl acetate.
[0104] [Table 1]
[0105] (Manufacture of developing solution) <Manufacturing example C> A developer was prepared by dissolving 1.0 wt % of acetic acid in PGMEA.
[0106] (Creating a resist layer) 2.0 mL of the metal-containing resist compositions of Preparation Examples A and B were poured onto an 8-inch silicon wafer, left to stand for 20 seconds, and then spin-coated at a speed of 1500 rpm for 30 seconds. In Table 2, the metal-containing resist composition using Preparation Example A is represented as PR(A), and the metal-containing resist composition using Preparation Example B is represented as PR(B). Next, 10 mL of the edge bead removal composition according to the Preparation Examples shown in Table 2 below was poured onto the wafer 1 mm above the outer periphery, rotated at the rotation speed (rpm) shown in Table 2 for 30 seconds, and then dried at 160°C for 60 seconds.
[0107] [Evaluation 1: Measurement of surface energy (surface tension) (mN / m) of the resist layer] 2.0 mL of the metal compound-containing resist composition according to the manufacturing example was poured onto an 8-inch silicon wafer, left to stand for 20 seconds, then spin-coated at a speed of 1500 rpm for 30 seconds, and then heat-treated at 100°C for 60 seconds to form a resist layer.
[0108] After cleaning the surface of the resist layer, DSA100 (KRUSS) was placed on the surface to measure the contact angle of deionized water (DIW), the contact angle of diiodomethane, and the surface energy (surface tension) calculated by the geometric mean method (OWRK Method). The same measurement was repeated five times, and the average of the three measurements excluding the upper and lower limits was calculated and is shown in Table 2.
[0109] [Evaluation 2: Measurement of surface tension (mN / m) of edge bead removal composition] Using a K11-MK1 (KRUSS) surface tension tester, the surface tension of the edge bead removal compositions of Preparation Examples 1 to 22 at 25°C was measured five times, and the average value of three measured values excluding the upper and lower limits was measured and shown in Table 2.
[0110] The difference in surface energy (mN / m) was calculated by subtracting the surface energy value of the resist layer obtained in Evaluation 1 from the surface tension value of the edge bead removal composition obtained in Evaluation 2. The results are shown in Table 2.
[0111] [Evaluation 3: Viscosity measurement of edge bead removal composition] The absolute viscosity of the edge bead removal compositions of Preparation Examples 1 to 22 was measured five times using an LVDV-III-UCP (manufactured by BROOKFIELD Corporation) at 25°C and a Torque% of 45%, and the average value of three measured values excluding the upper and lower limits was measured. The results are shown in Table 2.
[0112] [Rating 4: Hump rating] Fig. 2 is a schematic diagram of a hump. Referring to Fig. 2, a hump refers to a convexly raised portion at the end of a metal compound-containing resist thin film (resist layer) that is generated when an edge bead is removed by spraying an edge bead removal composition.
[0113] Here, the maximum height of the hump was measured. The maximum height of the hump means the step (ΔThickness) between the flat part of the resist layer other than the hump and the most elevated part of the hump, as shown in Figure 2b. The maximum height of the hump was measured using a Profiler P17OF device manufactured by Tencor. The measured values are shown in Table 2 below.
[0114] The maximum height of the measured hump was evaluated according to the following criteria, and the results were also recorded.
[0115] A: Maximum height of hump ≦100 nm B: 100nm<max hump height≦300nm C: 300nm<max hump height≦1,000nm D: 1,000 nm < maximum hump height [Evaluation 5: Evaluation of edge pattern defect rate] The wafers of each example, from which the edge bead had been removed, were exposed to light with a dose of 40 mJ using an ArFscanner (XT1250D manufactured by ASML) in a square pattern measuring 1 cm x 1 cm, and then cured for 60 seconds at 170°C. Subsequently, a development process was carried out using a developer composition (Preparation Example C) at a spin rate of 1500 rpm for 30 seconds, and then cured for 60 seconds at 240°C.
[0116] After the curing process, the pattern wafer with the Line / Space CD pattern was transferred to the CD-SEM measurement equipment to measure the critical dimension (CD). The critical dimension was determined as the average value after measuring 12 points with the CD-SEM image, and the target critical dimension was set to 80 nm. The points that deviated from the error range (±10%) from the target critical dimension or where bridges or scombs occurred were considered to be defective shots, and the failure rate was calculated using the following formula 1. If the failure rate was 1.5% or less, it was evaluated as good, and if it was over 1.5%, it was evaluated as bad, and the results are shown in Table 2.
[0117]
number
[0118] [Table 2]
[0119] Referring to Table 2, it can be seen that the maximum hump heights of the patterned wafers formed in Examples 1 to 18 were measured to be lower than those of Comparative Examples 1 to 11, and therefore the pattern defect rates were lower.
[0120] As described above, the specific embodiment of the present invention has been described and illustrated, but the present invention is not limited to the described embodiment, and it is obvious to those skilled in the art that various modifications and variations are possible without departing from the spirit and scope of the present invention. Therefore, such modifications or variations should not be understood separately from the technical spirit or viewpoint of the present invention, and the modified embodiments should be considered to belong to the scope of the claims of the present invention. [Explanation of symbols]
[0121] 1 Substrate support 2. Injection nozzle 10. Resist solution 12 Edge Bead a Resist layer b Maximum height of hump c and W substrates
Claims
1. A step of applying a metal-containing resist composition onto a substrate to form a resist layer; a removing step of applying an edge bead removing composition to the resist layer along the outer periphery of the substrate to remove the edge bead; a first heat treatment step of drying and heating the resist layer that has been subjected to the removal treatment in the removal step; and a resist pattern forming step of performing an exposure process and a development process on the resist layer that has been subjected to the drying process and the heating process in the first heat treatment step to form a resist pattern; the maximum height of a hump of the resist layer in a region extending from an outer peripheral edge of the substrate toward the center thereof being 1 mm or more and 30 mm or less after the first heat treatment step and before the resist pattern forming step is 300 nm or less.
2. The pattern formation method according to claim 1 , wherein the maximum height of the hump is 10 nm or more and 300 nm or less.
3. 2. The pattern forming method according to claim 1, wherein a difference between a surface energy of the resist layer and a surface tension of the edge bead removal composition is 2 mN / m or more and 15 mN / m or less.
4. 2. The pattern formation method according to claim 1, wherein the edge bead removal composition has a surface tension of 25.0 mN / m or more and 40.0 mN / m or less.
5. 2. The pattern formation method according to claim 1, wherein the edge bead removal composition has a surface tension of 27.0 mN / m or more and 36.0 mN / m or less.
6. 2. The pattern forming method according to claim 1, wherein the viscosity of the edge bead removing composition is from 1 cPs to 10 cPs.
7. 2. The pattern formation method according to claim 1, wherein the removing process in the removing step is performed while rotating the substrate at a speed of 800 rpm or more and 4,500 rpm or less.
8. 2. The pattern formation method according to claim 1, wherein the metal compound contained in the metal-containing resist composition comprises at least one selected from the group consisting of organic oxy group-containing tin compounds and organic carbonyloxy group-containing tin compounds.
9. 2. The method of claim 1, wherein the metal-containing resist composition comprises a metal compound represented by the following Chemical Formula 1 or a condensate thereof: 【Chemistry 1】 In the above Chemical Formula 1, R 1 is a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, a substituted or unsubstituted arylalkyl group having 6 to 30 carbon atoms, or -L a -O-R a (Here, L a is a single bond or a substituted or unsubstituted alkylene group having 1 to 20 carbon atoms; R a is a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms; R 2 ~R 4 each independently represents a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, a substituted or unsubstituted arylalkyl group having 6 to 30 carbon atoms, -OR b and -OC(=O)R c and R 2 ~R 4 At least one of the groups is -OR b and OC(=O)R c is selected from among At this time, R b is a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, or a combination thereof; R c is a hydrogen atom, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, or a combination thereof.
Citation Information
Patent Citations
Diluent composition for metal-containing resist
CN114624967A
Method of coating, method of manufacturing semiconductor device
JP2006253207A
Wafer for oil immersion lithography and its manufacturing method
JP2008235542A
Point of Use Solvent Mixing for Film Removal
US20220334485A1
Method of forming patterns
WO2023003215A1