Sheet for liquid development, and method for manufacturing sheet for liquid development

The liquid spreading sheet with a specific surfactant distribution profile on a polyester resin base film addresses bonding and spreading issues, achieving enhanced adhesion and test speed.

JP2024166099APending Publication Date: 2024-11-28TORAY INDUSTRIES INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024072235
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-17
Filing Date
2024-04-26
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Conventional liquid spreading sheets face challenges in achieving both excellent liquid spreading properties and strong bonding with test chip members, with issues such as uneven surfactant distribution and insufficient adhesive strength at the bonding interface.

Method used

A liquid spreading sheet configuration featuring a liquid receiving layer with a specific composition and depth profile of quaternary ammonium salt surfactant and acetylene glycol surfactant, measured by TOF-SIMS, on a polyester resin base film, ensuring optimal distribution and adhesion.

Benefits of technology

The sheet provides excellent bonding with test chip members, enhancing test speed and durability, with improved adhesion and liquid spreading properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024166099000001_ABST
    Figure 2024166099000001_ABST
Patent Text Reader

Abstract

To provide a sheet for liquid development which is excellent in joint to an inspection chip member, liquid developability, and durability.SOLUTION: A sheet for liquid development has a liquid receiving layer containing a polyester-based resin, a quaternary ammonium salt-based surface active agent, and an acetylene glycol-based surface active agent, on at least one surface of a base material film, wherein in a depth profile measured by time-of-flight type secondary ion mass spectrometer (TOF-SIMS), when C20H44 NO+fragment ions at a place where a depth from the surface on a side opposite to the base material film of the liquid receiving layer is 10% point of film thickness of the liquid receiving layer are represented by A, and C7H4O+fragment ions at the place are represented by B, B / A is 1 or more and 10 or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a sheet for spreading a liquid and a method for producing the sheet for spreading a liquid. [Background technology]

[0002] In recent years, point-of-care testing (POCT) in clinical medical settings has expanded to a wide range of test items. There is a strong demand for these POCT testing devices to quickly obtain test results. In particular, the hydrophilicity of the test sheet plays an important role in dominantly influencing the test speed, and thus various attempts have been made to date. For example, Patent Document 1 discloses a technique of using a binder and a surfactant in the liquid-receiving layer as a method for controlling the test speed.

[0003] Furthermore, since such test sheets are bonded to an electrode sheet or the like to be used as test chips for POCT testing equipment, various attempts have been made regarding the bonding methods. For example, Patent Document 2 discloses a technology for laminating a test sheet, a spacer, and an electrode sheet using an acrylic adhesive. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2001-349860 A [Patent Document 2] JP 2005-233917 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, although the technology described in the above-mentioned Patent Document 1 has excellent liquid spreading properties, the surfactant is unevenly distributed on the surface of the liquid receiving layer, and therefore, when the technology described in the above-mentioned Patent Document 2 is used, there is a problem in that the bonding with the test chip member is reduced, that is, the adhesive strength at the bond between the test sheet and the test chip member (spacer, electrode sheet, etc.) is insufficient. In other words, there is a problem in that conventional liquid spreading sheets are unable to achieve both excellent liquid spreading properties and excellent bonding with the test chip member.

[0006] SUMMARY OF THE PRESENT DISCLOSURE In order to solve the above problems, an object of the present invention is to provide a liquid spreading sheet which is excellent in bonding to a test chip member and in liquid spreading properties. [Means for solving the problem]

[0007] As a result of extensive research aimed at solving the above problems, the inventors have found that the problems can be solved as follows, and have arrived at the present invention. That is, a preferred embodiment of the liquid spreading sheet of the present invention has the following configuration. (1) A liquid-receiving layer containing a polyester resin, a quaternary ammonium salt surfactant, and an acetylene glycol surfactant on at least one surface of a base film, and in a depth profile measured by a time-of-flight secondary ion mass spectrometer (TOF-SIMS), the depth of the liquid-receiving layer from the surface on the opposite side of the base film is C at a point that is 10% of the thickness of the liquid-receiving layer. 20 H 44 A liquid spreading sheet in which, when NO+ fragment ions are A and C7H4O+ fragment ions are B, the B / A ratio is 1 or more and 10 or less. (2) In a depth profile measured by a time-of-flight secondary ion mass spectrometer (TOF-SIMS), the depth of the liquid-receiving layer from the surface opposite to the base film is 90% of the thickness of the liquid-receiving layer. 20 H 44 2. The liquid spreading sheet according to claim 1, wherein C / A is 0.1 or more and 10.0 or less, where C is an NO+ fragment ion. (3) In a depth profile measured by a time-of-flight secondary ion mass spectrometer (TOF-SIMS), 20 H 44 C on the surface of the liquid receiving layer opposite the substrate film with respect to NO fragment ions 20 H 44 The liquid spreading sheet according to (2), wherein the NO+ fragment ion content is 1% or more and 10% or less. (4) The liquid spreading sheet according to (3), wherein the thickness of the liquid receiving layer is from 0.5 μm to 5.0 μm. (5) The liquid spreading sheet according to (4), wherein the protective substrate and the substrate film are both polyethylene terephthalate films. (6) The liquid spreading sheet according to any one of (1) to (5), which is used as a biological fluid spreading sheet. Effect of the Invention

[0008] The present invention can provide a liquid spreading sheet that has excellent bonding to the test chip member and liquid spreading properties. As a result, a test chip using the liquid spreading sheet of the present invention has excellent testing speed and durability. In other words, a test chip using the liquid spreading sheet of the present invention enables inexpensive and rapid testing. Here, "excellent bonding of the liquid spreading sheet to the test chip member" means that the adhesive strength at the joint between the liquid spreading sheet and the test chip member is sufficiently high. Furthermore, if the adhesive strength at the joint between the liquid spreading sheet and the test chip member is sufficiently high, the durability of the test chip including the liquid spreading sheet and the test chip member will be excellent. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a schematic cross-sectional view of a liquid spreading sheet according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The liquid spreading sheet of the present invention has a liquid receiving layer containing a polyester resin, a quaternary ammonium salt surfactant, and an acetylene glycol surfactant on at least one side of a base film, and in a depth profile measured by a time-of-flight secondary ion mass spectrometer (TOF-SIMS), the depth of the liquid receiving layer from the surface opposite to the base film is C at a point that is 10% of the thickness of the liquid receiving layer. 20 H 44 When NO+ fragment ion is A and C7H4O+ fragment ion is B, B / A is 1 or more and 10 or less. By adopting such an embodiment, the liquid spreading sheet of the present invention is excellent in bonding with the test chip member, liquid spreading property, and durability. And the test chip using the liquid spreading sheet of the present invention is excellent in test speed and durability. Hereinafter, the liquid spreading sheet of the present invention will be specifically described.

[0011] In addition, since the liquid-spreading sheet has excellent adhesion between the liquid-receiving layer and the base film, and further has excellent hardness of the liquid-receiving layer in the temperature range used as the liquid-spreading sheet, the durability of the test chip using this liquid-spreading sheet is also excellent. Furthermore, since the liquid-spreading sheet has excellent liquid spreading properties, the test chip using this liquid-spreading sheet has excellent testing speed.

[0012] 1 is a schematic cross-sectional view of a liquid spreading sheet according to one embodiment of the present invention. This liquid spreading sheet 3 has a liquid receiving layer 1 and a base film 2 in this order.

[0013] (Liquid Receptive Layer) The liquid-receiving layer of the liquid-spreading sheet of the present invention contains a polyester resin, a quaternary ammonium salt surfactant, and an acetylene glycol surfactant, and in a depth profile measured by a time-of-flight secondary ion mass spectrometer (TOF-SIMS), the depth from the surface of the liquid-receiving layer opposite to the base film is C at a point that is 10% of the thickness of the liquid-receiving layer. 20 H 44When the NO+ fragment ion is A and the C7H4O+ fragment ion is B, the B / A is 1 to 10. Here, the above A is C 20 H 44 The larger the amount of NO+ fragment ions detected, that is, the larger the content of the quaternary ammonium salt surfactant at the 10% point, the larger the B. On the other hand, the larger the amount of C7H4O+ fragment ions detected, that is, the larger the content of the polyester resin at the 10% point, the larger the B. In other words, the value of B / A being 1 to 10 means that at the 10% point, that is, near the surface of the surface composed of the liquid receiving layer of the liquid developing sheet of the present invention, the content of the quaternary ammonium salt surfactant and the content of the polyester resin are the same, or the content of the polyester resin is greater than the content of the quaternary ammonium salt surfactant within a specific range. By adopting such a form, the liquid developing sheet has excellent bonding to the test chip member, liquid developing property, and durability.

[0014] The polyester resin is a polyester resin obtained by copolymerizing a glycol component and a dibasic acid component. By adopting such a form, the adhesion between the liquid receiving layer and the base film is improved. By improving the adhesion between the liquid receiving layer and the base film, the liquid receiving layer is prevented from peeling off from the base film, and the liquid spreading sheet has excellent durability. In addition, the adhesion with the adhesive for bonding between the test chip members is improved, and the liquid spreading sheet has excellent bonding with the test chip members.

[0015] Adhesives for bonding test chip components include polyester resins, polyolefin resins, acrylic resins, polyamide resins, polyurethane resins, polyphenylene oxide-polystyrene resins, polycarbonate resins, styrene copolymer resins, polystyrene resins, chlorinated polyolefin resins, chlorinated ethylene-vinyl acetate copolymer resins, cyclized rubber, coumarone-indene resins, polyurethane resins, polyvinyl ether resins, and polyvinyl acetate resins.

[0016] Examples of glycol components of polyester resins include propylene glycol, 1,3-propanediol, 2-methyl-1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, neopentyl glycol, diethylene glycol, dipropylene glycol, 2,2,4-trimethyl-1,3-pentanediol, neopentyl hydroxypivalic acid ester, 1,4-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,2-cyclohexanedimethanol, tricyclodecane dimethanol, and hydrogen. Examples of such bisphenol A include added bisphenol A, hydrogenated bisphenol S, ethylene oxide adducts and propylene oxide adducts of bisphenol A, ethylene oxide adducts and propylene oxide adducts of hydrogenated bisphenol A, ethylene oxide adducts and propylene oxide adducts of bisphenol S, ethylene oxide adducts and propylene oxide adducts of hydrogenated bisphenol S, 1,9-nonanediol, 2-methyloctanediol, 1,10-decanediol, 2-butyl-2-ethyl-1,3-propanediol, and tricyclodecane dimethanol.

[0017] Examples of the dibasic acid component of the polyester resin include aromatic dibasic acids such as orthophthalic acid, 1,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 4,4'-diphenyldicarboxylic acid, 2,2'-diphenyldicarboxylic acid, and 4,4'-diphenyletherdicarboxylic acid, and aliphatic or alicyclic dibasic acids such as adipic acid, 1,3-cyclohexanedicarboxylic acid, 1,2-cyclohexanedicarboxylic acid, and 4-methyl-1,2-cyclohexanedicarboxylic acid.

[0018] The glass transition temperature of the polyester resin is preferably 40°C or higher and 100°C or lower from the viewpoint of improving the bonding to the test chip member and durability as a liquid spreading sheet. By having a glass transition temperature of 100°C or lower, the adhesion between the liquid receiving layer and the base film is sufficient, so that the liquid spreading sheet has excellent durability. In addition, the adhesion to the adhesive for bonding the test chip members is improved, so that the liquid spreading sheet has excellent bonding to the test chip member. From the same viewpoint, it is more preferable to set the glass transition temperature to 90°C or lower.

[0019] In addition, by making the glass transition temperature of the polyester resin 40° C. or higher, the hardness of the liquid receiving layer is improved in the temperature range in which the liquid spreading sheet is used, and the liquid spreading sheet has excellent durability. From the same viewpoint, it is more preferable that the glass transition temperature of the polyester resin is 60° C. or higher. From the above viewpoint, it is more preferable that the glass transition temperature is 60° C. or higher and 100° C. or lower.

[0020] The polyester resin is preferably solvent-soluble from the viewpoint of processability of the liquid receiving layer to the base film. The term "solvent-soluble" as used herein means that the polyester resin is soluble in at least one of toluene, methyl ethyl ketone, cyclohexanone, tetrahydrofuran, and ethyl acetate alone or in a mixed solvent of any two or more of these solvents in any mixing ratio at 25°C in an amount of 3% by mass or more.

[0021] The content of the polyester resin is preferably 80.0% by mass or more in 100.0% by mass of the liquid receiving layer. By containing 80.0% by mass or more of the polyester resin, the adhesion between the liquid receiving layer and the base film and the adhesion with the adhesive for bonding between the test chip members is improved, and the surface hardness of the liquid receiving layer is improved, so that the liquid spreading sheet has excellent bonding with the test chip members and durability. From the same viewpoint, it is more preferable to contain 83.0% by mass or more, and even more preferable to contain 86.5% by mass or more.

[0022] The polyester resin content is preferably 98.9% by mass or less. By containing 98.9% by mass or less of the polyester resin, the content ratio of the quaternary ammonium salt surfactant and the acetylene glycol surfactant in the liquid receiving layer can be increased, so that the liquid spreading sheet has excellent liquid spreading properties. From the same viewpoint, the content is more preferably 96.7% by mass or less, and even more preferably 92.3% by mass or less.

[0023] From the above viewpoints, the polyester resin is preferably contained in an amount of 80.0% by mass or more and 98.9% by mass or less, more preferably 83.0% by mass or more and 96.7% by mass or less, and even more preferably 86.5% by mass or more and 92.3% by mass or less, based on 100.0% by mass of the liquid receiving layer.

[0024] The liquid receiving layer contains a quaternary ammonium salt surfactant, which reduces the surface resistance of the liquid receiving layer and improves the wettability of the liquid receiving layer, resulting in excellent liquid spreading properties as a liquid spreading sheet. In addition, the quaternary ammonium salt surfactant interacts with the polyester resin and the acetylene glycol surfactant, which can control the precipitation of the liquid receiving layer on the surface opposite to the substrate film, resulting in excellent bonding to the test chip member as a liquid spreading sheet. From the same viewpoint as above, polyoxyethylene trialkylammonium nitrate is more preferable as the quaternary ammonium salt surfactant.

[0025] Examples of the quaternary ammonium salt surfactant include alkyl dimethyl ammonium salt surfactant, alkyl trimethyl ammonium salt surfactant, hexadecyl trimethyl ammonium salt surfactant, dialkyl dimethyl ammonium salt surfactant, benzalkonium chloride surfactant, etc. These quaternary ammonium salt surfactants may be used alone or in combination.

[0026] By adopting such an embodiment, in a depth profile measured by a time-of-flight secondary ion mass spectrometer (TOF-SIMS), the depth of the liquid-receiving layer from the surface opposite to the base film is C at a point that is 10% of the thickness of the liquid-receiving layer. 20 H 44 When the NO+ fragment ion is A and the C7H4O+ fragment ion is B, the B / A is 1.0 or more and 10.0 or less.

[0027] By making B / A 1.0 or more, excessive precipitation of the quaternary ammonium salt surfactant on the surface of the liquid receiving layer opposite the substrate film is suppressed, and the liquid spreading sheet has excellent bonding to the test chip member. From the same viewpoint, it is more preferable that B / A is 3.0 or more.

[0028] Furthermore, by setting B / A to 10.0 or less, the quaternary ammonium salt surfactant is sufficiently precipitated on the surface of the liquid receiving layer opposite the substrate film, improving the wettability of the liquid receiving layer and the adhesion between the substrate film and the liquid receiving layer, resulting in a liquid spreading sheet with excellent liquid spreading properties and durability. From the same viewpoint, it is more preferable that B / A is 8.0 or less.

[0029] From the same viewpoint as above, in a depth profile of the liquid-receiving layer measured by a time-of-flight secondary ion mass spectrometer (TOF-SIMS), the depth of the liquid-receiving layer from the surface opposite to the base film is C at a point where the thickness of the liquid-receiving layer is 90%. 20 H 44 When the NO+ fragment ion is C, it is preferable that C / A is 0.10 or more and 10.00 or less.

[0030] By making the C / A ratio 0.10 or more, excessive precipitation of the quaternary ammonium salt surfactant on the surface of the liquid receiving layer opposite the base film is suppressed, resulting in a liquid spreading sheet with excellent bonding to the test chip component.

[0031] Furthermore, by setting the C / A to 10.00 or less, the quaternary ammonium salt surfactant is sufficiently precipitated on the surface of the liquid receiving layer opposite the base film, thereby improving the wettability of the liquid receiving layer and improving the adhesion between the base film and the liquid receiving layer, resulting in a liquid spreading sheet with excellent liquid spreading properties and durability.

[0032] Further, in the same respect as above, in a depth profile measured by a time-of-flight secondary ion mass spectrometer (TOF-SIMS), 20 H 44 C on the opposite surface of the substrate film to NO fragment ions 20 H 44 It is preferable that NO+ fragment ions account for 1% or more and 10% or less.

[0033] C of the entire liquid-receiving layer 20 H 44 C on the surface of the liquid receiving layer opposite the substrate film for NO fragment ions 20 H 44 By making the NO+ fragment ion content 1% or more, the quaternary ammonium salt surfactant is sufficiently precipitated on the surface of the liquid receiving layer opposite the base film, improving the wettability of the liquid receiving layer, resulting in a liquid spreading sheet with excellent liquid spreading properties.

[0034] In addition, C of the entire liquid receiving layer 20 H 44 C on the surface of the liquid receiving layer opposite the substrate film for NO fragment ions 20 H 44 By keeping the NO+ fragment ion content at 10% or less, excessive precipitation of the quaternary ammonium salt surfactant on the surface opposite the base film of the liquid receiving layer is suppressed, resulting in a liquid spreading sheet with excellent bonding to the test chip component.

[0035] The depth profile measured by a time-of-flight secondary ion mass spectrometer (TOF-SIMS) can be measured using a time-of-flight secondary ion mass spectrometer TOF.SIMS 5 (manufactured by ION-TOF) under the following conditions: primary ions are Bi3++, secondary ion polarity is positive, and edging ions are Ar gas cluster ion beam.

[0036] By setting the content of the quaternary ammonium salt surfactant to 1.0% by mass or more in 100.0% by mass of the liquid receiving layer, the surface resistance value of the liquid receiving layer can be reduced, the wettability of the liquid receiving layer can be improved, and the liquid spreading sheet can have excellent liquid spreading properties. From the same viewpoint, it is more preferable that the content is 3.0% by mass or more, and even more preferable that the content is 7.0% by mass or more.

[0037] In addition, by setting the content of the quaternary ammonium salt surfactant to 17.0 mass% or less in 100.0 mass% of the liquid receiving layer, excessive precipitation of the quaternary ammonium salt surfactant on the surface of the liquid receiving layer opposite the substrate film is suppressed, resulting in excellent bonding to the test chip member. From the same viewpoint, it is more preferable to contain 15.0 mass% or less, and even more preferable to contain 12.0 mass% or less. The weight average molecular weight of the quaternary ammonium salt surfactant is preferably 5000 or more.

[0038] From the above viewpoint, the quaternary ammonium salt surfactant in the present invention is preferably contained in an amount of 1.0 mass% or more and 17.0 mass% or less, more preferably 3.0 mass% or more and 15.0 mass% or less, and even more preferably 7.0 mass% or more and 12.0 mass% or less, based on 100.0 mass% of the liquid receiving layer.

[0039] The acetylene glycol surfactant used in the present invention is a substance that, when it is added alone to pure water at 5 mass %, can reduce the surface tension of the pure water by 30% or more. The liquid-receiving layer has excellent liquid spreading properties as a liquid-spreading sheet because the wettability of the liquid-receiving layer is improved by containing the acetylene glycol surfactant. In addition, the acetylene glycol surfactant interacts with the polyester resin and the quaternary ammonium salt surfactant, and the precipitation of the quaternary ammonium salt surfactant on the surface of the liquid-receiving layer opposite the substrate film can be controlled, so that the liquid-spreading sheet has excellent bonding to the test chip member. From the same viewpoint as above, polyoxyethylene acetylenic glycol ether is more preferable as the acetylene glycol surfactant.

[0040] By making the content of the acetylene glycol surfactant 0.1% by mass or more in 100.0% by mass of the liquid receiving layer, the wettability of the liquid receiving layer and the adhesion between the base film and the liquid receiving layer are improved, so that the liquid spreading sheet has excellent liquid spreading properties and durability. From the same viewpoint, it is more preferable to contain 0.3% by mass or more, and even more preferable to contain 0.7% by mass or more.

[0041] In addition, by making the content of the acetylene glycol surfactant 3.0% by mass or less in 100.0% by mass of the liquid receiving layer, it is possible to suppress the precipitation of the quaternary ammonium salt surfactant and the acetylene glycol surfactant on the surface of the liquid receiving layer opposite the base film, and therefore the liquid spreading sheet has excellent bonding to the test chip member. From the same viewpoint, it is more preferable to contain 2.0% by mass or less, and even more preferable to contain 1.5% by mass or less.

[0042] From the above viewpoints, the acetylene glycol-based surfactant in the present invention is preferably contained in an amount of 0.1% by mass or more and 3.0% by mass or less, more preferably 0.3% by mass or more and 2.0% by mass or less, and even more preferably 0.7% by mass or more and 1.5% by mass or less, based on 100.0% by mass of the liquid receiving layer.

[0043] The thickness of the liquid receiving layer of the present invention is preferably 0.5 μm or more and 5.0 μm or less from the viewpoint of providing excellent liquid spreading properties and durability as a liquid spreading sheet. By making the thickness of the liquid receiving layer 0.5 μm or more, it is possible to prevent the liquid receiving layer from slipping off due to scratches during processing of the liquid spreading sheet and the occurrence of pinholes, and further, the adhesion between the liquid receiving layer and the base film is improved, resulting in a liquid spreading sheet with excellent durability. From the same viewpoint, it is more preferable to make the thickness 0.7 μm or more.

[0044] Furthermore, by making the thickness of the liquid receiving layer 5.0 μm or less, the liquid receiving layer is stably heated in the process of coating the liquid receiving layer on the base film, so that the acetylene glycol surfactant interacts with the polyester resin and the quaternary ammonium salt surfactant, and the precipitation of the quaternary ammonium salt surfactant on the surface of the liquid receiving layer opposite the base film can be controlled, resulting in a liquid spreading sheet that is excellent in bonding to the test chip member. From the same viewpoint, it is more preferable to make the thickness 3.0 μm or less.

[0045] When the composition of the polyester resin, quaternary ammonium salt surfactant, and acetylene glycol surfactant in the liquid receiving layer of the present invention cannot be determined from the blending of the raw materials, the following LC / MS / MS (liquid chromatography mass spectrometry) and pyrolysis GC / MS can be preferably used as qualitative and quantitative analysis methods.

[0046] <Separation / Extraction> Weigh 0.04 g of the layer into a 25 mL measuring flask. Next, add 1 mL of HFIP (1,1,1,1,3,3,3-hexafluoro-2-propanol) / chloroform (volume ratio 1 / 1) to the measuring flask to dissolve the layer, add 2 mL of chloroform, and then gradually add acetonitrile to insolubilize the polyester resin component.

[0047] Add acetonitrile and adjust the volume to 25 mL. Dilute the adjusted solution 100-fold with acetonitrile, filter it through a PTFE disk filter (0.45 μm), and use the filtrate as the measurement solution.

[0048] <Qualitative analysis> The measurement solution is subjected to LC / MS / MS, and the retention time and peak area at which the peaks derived from the quaternary ammonium salt surfactant and the acetylene glycol surfactant are detected from the chromatogram are confirmed. Then, the peaks derived from the quaternary ammonium salt surfactant and the acetylene glycol surfactant are qualitatively analyzed by mass spectrometry. The acetylene glycol surfactant is qualitatively identified by confirming the formula weights of the positive and negative ions derived therefrom.

[0049] The insolubilized polyester resin is subjected to pyrolysis GC / MS, and a peak derived from the polyester resin is subjected to mass spectrometry for qualitative analysis.

[0050] <Adjusting standard solutions and creating calibration curves> Weigh out 0.01 g of the qualified quaternary ammonium salt surfactant and acetylene glycol surfactant samples into a 10 mL measuring flask, dissolve in methanol and adjust the volume to 10 mL to make a standard solution. Aliquot the standard solution and dilute each with methanol to obtain a total of four standard solutions of arbitrary concentrations, which are then subjected to LC / MS / MS to confirm the peak area of ​​the chromatogram for each concentration. A calibration curve is obtained by linearly approximating the relationship between the solution concentration and the peak area.

[0051] <Quantitative analysis> The peak areas at which the peaks derived from the quaternary ammonium salt-based surfactant and the acetylene glycol-based surfactant are detected from the chromatogram confirmed by the qualitative analysis are substituted into the equation for the calibration curve, and the concentrations of the quaternary ammonium salt-based surfactant and the acetylene glycol-based surfactant contained in the layer are calculated to obtain the contents of the polyester resin, the quaternary ammonium salt-based surfactant and the acetylene glycol-based surfactant.

[0052] The above LC / MS / MS analysis can be performed using LC20-A (LC system, manufactured by Shimadzu Corporation), API4000 (MS system, manufactured by AB SCIEX Corporation), and ODS-3 (manufactured by GL Sciences Inc., column, "Intersil" (registered trademark)) under the following conditions: APCI (atmospheric pressure chemical ionization) ionization method, positive ion detection and negative ion detection, SRM (selected reAction monitoring) measurement mode, column temperature of 50°C, flow rate of 0.25 mL / min, and injection volume of 1 μL.

[0053] In addition, pyrolysis GC / MS can be performed using a PY3030D (Frontier Labs, Inc.) and a GCMS-QP2010 (Shimadzu Corporation) at a heating temperature of 500°C and a heating rate of 50°C / min.

[0054] (Base film) From the viewpoint of dimensional stability and durability, the base film in the liquid spreading sheet of the present invention is preferably a film made of polyester, such as polyethylene terephthalate, polyethylene 2,6-naphthalate, polyethylene α,β-bis(2-chlorophenoxy)ethane 4,4'-dicarboxylate, polybutylene terephthalate, etc. These may be copolymers. Among these, from the viewpoint of excellent handling properties and durability of the liquid spreading sheet, it is particularly preferable that the base film is a film made of polyethylene terephthalate, i.e., a polyethylene terephthalate film, and from the same viewpoint, a biaxially oriented polyethylene terephthalate film is most preferable.

[0055] The thickness of the base film is preferably 10 μm or more from the viewpoint of excellent dimensional stability and durability. From the same viewpoint, it is more preferable to set it to 20 μm or more, and even more preferable to set it to 30 μm or more. Moreover, the thickness of the base film is preferably 500 μm or less from the viewpoint of excellent handleability as an inspection sheet. From the same viewpoint, it is more preferable to set it to 300 μm or less, and even more preferable to set it to 200 μm or less.

[0056] From the above viewpoints, the thickness of the base film is preferably from 10 μm to 500 μm, more preferably from 20 μm to 300 μm, and even more preferably from 30 μm to 200 μm.

[0057] (Liquid spreading sheet) The liquid spreading sheet of the present invention has at least a liquid receiving layer and a base film in this order, and when this liquid spreading sheet is used in a test chip, it is excellent in test speed and durability. As a result, it can be suitably used as a liquid spreading sheet for testing and quantifying specific components contained in biological samples such as blood and urine, raw materials and products in the food industry, samples such as fruit juice, etc.

[0058] The method for producing the liquid spreading sheet of the present invention can include, for example, the following exemplary materials, amounts used, treatment contents, treatment procedures, etc.

[0059] The liquid spreading sheet of the present invention can be produced, for example, by applying a coating composition containing a polyester resin, a quaternary ammonium salt surfactant, and an acetylene glycol surfactant to one side of a substrate film, and then subjecting the coated film to a heat treatment. The heating temperature for the heat treatment is preferably 100°C or higher and 150°C or lower. By setting the heating temperature to 100°C or higher, the quaternary ammonium salt surfactant and the acetylene glycol surfactant can be precipitated on the opposite side of the substrate film of the liquid receiving layer, resulting in a liquid spreading sheet having excellent liquid spreading properties and durability. In addition, by setting the heating temperature to 150°C or lower, the dimensional stability of the substrate film is ensured, resulting in a liquid spreading sheet having excellent handleability.

[0060] In obtaining a coating composition containing a polyester resin, a quaternary ammonium salt surfactant, and an acetylene glycol surfactant for obtaining a liquid receiving layer, there is no particular limitation on the method of mixing and dispersing each component, and known mixing and dispersing methods such as a magnetic stirrer, a homodisper, ultrasonic irradiation, vibration dispersion, and manual mixing and dispersion can be used. In addition, the coating composition preferably contains an organic solvent from the viewpoint of improving the coatability to the substrate film. Examples of organic solvents include ethyl methyl ketone, methyl isobutyl ketone, butyl acetate, ethyl acetate, methanol, isopropanol, cyclohexanone, toluene, and xylene. In addition, inorganic particles, organic particles, leveling agents, etc. can be blended into the coating composition from the viewpoint of preventing blocking when wound up on a film roll and improving the coatability to the substrate film, as long as the effect of the present invention is not impaired.

[0061] Preferred methods for laminating the liquid receiving layer onto the base film include, for example, the comma coating method, the applicator method, the dip coating method, the roller coating method, the wire bar coating method, the reverse coating method, the kiss coating method, the gravure coating method, and the die coating method (see U.S. Pat. No. 2,681,294), and from the viewpoint of processability, the wire bar coating method, the reverse coating method, and the gravure coating method are more preferred.

[0062] The liquid spreading sheet of the present invention can be suitably used as a biological fluid spreading sheet, where biological fluid means blood, urine, etc. EXAMPLES

[0063] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0064] [Measurement and evaluation methods] (1) Thickness of the liquid-receiving layer The thickness (μm) of the liquid receiving layer was determined by cutting the liquid spreading sheet in a direction perpendicular to the thickness using a manual rotary microtome (Leica Microsystems, "HistoCore BIOCUT" (registered trademark)) to obtain a cross-section of the liquid spreading sheet, and observing the cross-section of the conductive layer using a scanning electron microscope (FEI, XL30 SFEG) at an accelerating voltage of 20 kV and an observation magnification of 100,000 times, and measuring any five points on the cross-sectional photograph to calculate the average value obtained.

[0065] (2) Depth profile measured by time-of-flight secondary ion mass spectrometry (TOF-SIMS) The liquid spreading sheet wound in a roll was cut into 100 mm x 100 mm squares at three randomly selected locations, and a time-of-flight secondary ion mass spectrometer TOF.SIMS 5 (manufactured by ION-TOF) and measurement software SURFACE LAB 6 (manufactured by ION-TOF) were used to measure the primary ions in the depth direction from the opposite surface of the base film of the liquid receiving layer of the liquid spreading sheet under conditions of Bi3++ primary ions, positive secondary ion polarity, and Ar gas cluster ion beam edging ions. The C at a point where the depth from the opposite surface of the base film of the liquid receiving layer to the 10% thickness of the liquid receiving layer was measured. 20 H 44 NO+ fragment ions are A, C7H4O+ fragment ions are B, and the depth is C at a point that is 90% of the thickness of the liquid-receiving layer. 20 H 44 The NO+ fragment ion was defined as C, and B / A and C / A were calculated using the average values ​​of three points.

[0066] In addition, C of the entire liquid receiving layer 20 H 44 C on the surface of the liquid receiving layer opposite the substrate film for NO fragment ions 20 H 44 For NO+ fragment ions, the C from the surface of the liquid-receiving layer to the substrate film interface 20 H 44 The total number of NO fragment ions is D, and the surface of the liquid receiving layer opposite the substrate film is C20 H 44 The NO+ fragment ion was taken as E, and E / D was calculated using the average value of the three locations, and the obtained value was multiplied by 100 to calculate E / D×100. The unit of E / D×100 is %.

[0067] (3) Composition analysis of the liquid-receiving layer The liquid spreading sheet wound up in a roll is cut into a 100mm x 100mm square at a randomly selected location, the liquid receiving layer is peeled off from the liquid spreading sheet, and dissolved in HFIP (1,1,1,1,3,3,3-hexafluoro-2-propanol) / chloroform (volume ratio 1 / 1), 2mL of chloroform is added, and then acetonitrile is gradually added to insolubilize the resin component. Next, acetonitrile is added and the volume is adjusted to 25mL, and the adjusted solution is diluted 100 times with acetonitrile, and the filtrate obtained by filtering with a PTFE disk filter (0.45μm) is used as the measurement solution. The obtained measurement solution was subjected to LC / MS / MS using LC20-A (LC system, manufactured by Shimadzu Corporation), API4000 (MS system, manufactured by AB SCIEX Corporation), and ODS-3 (manufactured by GL Sciences Inc., column, "Intersil" (registered trademark)) under the conditions of APCI (atmospheric pressure chemical ionization) ionization method, positive ion detection and negative ion detection, SRM (selected reAction monitoring) measurement mode, column temperature of 50°C, flow rate of 0.25 mL / min, and injection volume of 1 μL, and mass analysis was performed on the peak of the obtained substance to analyze the composition other than the resin component.

[0068] The insolubilized resin was subjected to pyrolysis GC / MS at a heating temperature of 500°C and a heating rate of 50°C / min using a PY3030D (Frontier Labs, Inc.) and a GCMS-QP2010 (Shimadzu Corporation). The resin component composition was analyzed by mass spectrometry of the peaks derived from the resin.

[0069] (4) Composition analysis of the base film Using the method described in (3), the substrate film from which the liquid-receiving layer had been peeled off was subjected to pyrolysis GC / MS at a heating temperature of 500°C and a heating rate of 50°C / min using a PY3030D (Frontier Labs, Inc.) and a GCMS-QP2010 (Shimadzu Corporation). Mass spectrometry was then performed on the peaks derived from the substrate film to analyze the composition of the substrate film components.

[0070] (3) Adhesion between the liquid-receiving layer and the base film The liquid spreading sheet wound into a roll was cut into 100 mm x 100 mm squares at three randomly selected locations, and the adhesion between the liquid receiving layer and the base film was evaluated using a cross-cut guide CCJ-1 (manufactured by Cortex Co., Ltd.) based on JIS K5600-5-6 (1999) and the following criteria, with a score of C or above being considered a pass. A: Classification 0 B: Classification 1 C: Classification 2 D: Classification 3, Classification 4, Classification 5 (4) Liquid spreading property of the liquid receiving layer The liquid spreading sheet wound into a roll was cut into 100mm x 100mm squares at three points, 10%, 50%, and 90% of the total length of the film, to prepare measurement samples. 5μl of glucose injection solution (Otsuka Sugar Solution 50% manufactured by Otsuka Pharmaceutical Co., Ltd.) was dropped onto the surface of the liquid receiving layer of the measurement sample, and the spread of the glucose injection solution was measured 30 seconds after dropping. The spread was measured by measuring the diameter of the liquid, and if the liquid was elliptical, the short diameter was considered to be the diameter. The average value of the three points was calculated, and if the spread of the glucose injection solution was 5mm or more, it was considered to have passed. However, if the spread was 5mm or more but the glucose injection solution flowed to the back side of the liquid receiving layer, it was marked as N and failed.

[0071] (5) Adhesion to test chip components The liquid spreading sheet wound into a roll was cut into three rectangles measuring 10 mm x 150 mm at 10%, 50%, and 90% of the total length of the film. The polyester resin surface of a polyester resin laminate film made by laminating polyester resin (Aronmelt (registered trademark) PES310S30, manufactured by Toagosei Co., Ltd.) to a biaxially oriented polyethylene terephthalate film (Lumirror (registered trademark) S10, manufactured by Toray Industries, Inc.) was overlapped with the liquid receiving layer surface. The two were then thermally bonded using a laminator (MLP-600W laminator, manufactured by MCK Corporation) at a laminator temperature of 120°C, a line speed of 2 m / min, and a linear pressure of 2 kgf cm to prepare samples for adhesion measurement. The polyester resin surface and the liquid receiving layer surface of this adhesion measurement sample were forcibly peeled off, and a 180° peel test was performed using a tensile tester (Orientec Tensilon UCT-100) with an initial tensile chuck distance of 100 mm and a tensile speed of 100 mm / min. Measurements were continued until the peel length reached 130 mm (chuck distance 230 mm), and the average load value from a peel length of 25 mm to 125 mm was used to evaluate the bondability with the test chip member, and evaluation was performed according to the following criteria, with a grade of C or higher being considered a pass. A:6.0N / cm or more B: 4.0N / cm or more and less than 6.0N / cm C: 2.0N / cm or more and less than 4.0N / cm D: Less than 2.0N / cm [material] (polyester resin) Polyester resin (Takamatsu Oil Co., Ltd. "Pesresin" (registered trademark) S140) (Surfactant A) Polyoxyethylene trialkylammonium nitrate ("Anstex" (registered trademark) C-200X, manufactured by Toho Chemical Industry Co., Ltd.) (Surfactant B) Polyoxyethylene acetylene glycol ether ("Olfine" (registered trademark) E1004, manufactured by Nissin Chemical Industry Co., Ltd.) (Surfactant C) Alkyltrimethylammonium salt surfactant ("Katinal" (registered trademark) LTC-35A, manufactured by Toho Chemical Industry Co., Ltd.) (Base film A) Polyethylene terephthalate film (Toray Industries, Inc.'s "Lumirror" (registered trademark) S10, thickness 75 μm) (Base film B) Polybutylene terephthalate film (ESRM manufactured by Okura Kogyo Co., Ltd., thickness 75 μm) [Example 1] The raw materials for obtaining the liquid receiving layer were made to have the composition shown in Table 1, and each was dissolved in ethyl methyl ketone, and the raw materials were mixed and dispersed using Homodisper (manufactured by Primix Corporation) to obtain a 10 mass% adjusted solution. Next, the adjusted solution for obtaining the liquid receiving layer was applied by gravure coating to one side of a 75 μm thick base film (biaxially oriented polyethylene terephthalate film "Lumirror" (registered trademark) S10 manufactured by Toray Industries, Inc.), and dried at 120° C., after which a 1.0 μm thick liquid receiving layer was laminated to obtain a liquid spreading sheet, which was then wound into a roll.

[0072] [Examples 2 to 10, Comparative Examples 1 to 3] A liquid spreading sheet was produced with the composition of each layer excluding the solvent, the base film, the drying temperature after coating of the liquid receiving layer, and the thickness of the liquid receiving layer as shown in Tables 1 to 3. The evaluation results are shown in Tables 1 to 3.

[0073] All of the liquid spreading sheets of Examples 1 to 10 were excellent in bonding of the liquid receiving layer to the test chip member, liquid spreading property, and durability.

[0074] On the other hand, the liquid spreading sheet of Comparative Example 1 was inferior to the liquid spreading sheets of the Examples in terms of adhesion between the liquid receiving layer and the base film, and in terms of liquid spreading properties.

[0075] Furthermore, the liquid spreading sheets of Comparative Examples 2 and 3 were inferior in bonding to the test chip member compared to the liquid spreading sheet of the Examples.

[0076] [Table 1]

[0077] [Table 2]

[0078] [Table 3] [Explanation of symbols]

[0079] 1: Liquid receiving layer 2: Base film 3: Liquid spreading sheet [Industrial Applicability]

[0080] The liquid spreading sheet of the present invention is preferably used when testing and quantifying liquids, for example, biological fluid components such as blood and urine, and can be suitably used as a biological fluid spreading sheet.

Claims

1. A liquid-receiving layer containing a polyester resin, a quaternary ammonium salt surfactant, and an acetylene glycol surfactant on at least one surface of a substrate film, wherein in a depth profile measured by a time-of-flight secondary ion mass spectrometer (TOF-SIMS), the depth of the liquid-receiving layer from the surface on the opposite side of the substrate film is C at a point that is 10% of the thickness of the liquid-receiving layer. 20 H 44 NO+ fragment ions are A and C 7 H 4 A liquid spreading sheet in which B / A is 1 or more and 10 or less, when B is an O+ fragment ion.

2. In a depth profile measured by a time-of-flight secondary ion mass spectrometer (TOF-SIMS), the depth of the liquid-receiving layer from the surface opposite to the substrate film is C at a point where the thickness of the liquid-receiving layer is 90%. 20 H 44 2. The liquid spreading sheet according to claim 1, wherein, when the NO+ fragment ion is C, the ratio C / A is 0.1 or more and 10.0 or less.

3. In a depth profile measured by a time-of-flight secondary ion mass spectrometer (TOF-SIMS), 20 H 44 C on the surface of the liquid receiving layer opposite the substrate film to NO fragment ions 20 H 44 3. The liquid spreading sheet according to claim 2, wherein the NO+ fragment ion content is from 1% to 10%.

4. 4. The liquid spreading sheet according to claim 3, wherein the thickness of the liquid receiving layer is from 0.5 to 5.0 μm.

5. 5. The liquid spreading sheet according to claim 4, wherein each of said base films is a polyethylene terephthalate film.

6. 6. The liquid spreading sheet according to claim 1, which is used as a biological fluid spreading sheet.

Citation Information

Patent Citations

  • Sheet for developing liquid

    JP2001349860A

  • Biosensor and method for manufacturing the same

    JP2005233917A