Film for lid material

A polyethylene-based lidding film with a tailored ethylene/α-olefin copolymer and tackifier composition addresses recyclability and adhesion issues, offering excellent adhesion to various plastic containers and improving recyclability.

JP2024166100APending Publication Date: 2024-11-28TOSOH CORP

Patent Information

Application Number
JP2024072410
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-17
Filing Date
2024-04-26
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Existing packaging materials, particularly lidding films for plastic containers, face challenges in recyclability and adhesion, limiting their application to specific types of plastic containers and hindering effective recycling.

Method used

A film for lidding material comprising a polyethylene-based base material and a sealant layer with specific ethylene/α-olefin copolymer and tackifier composition, optimized for recyclability and adhesion to various plastic containers.

Benefits of technology

The film provides excellent adhesiveness to plastic containers while being highly recyclable, suitable for a wide range of plastic materials including polyethylene terephthalate, polystyrene, polypropylene, and polyvinyl chloride, enhancing recyclability and application versatility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024166100000001
    Figure 2024166100000001
  • Figure 2024166100000002
    Figure 2024166100000002
Patent Text Reader

Abstract

To provide a film for a lid material, having high recyclability and excellent adhesiveness to a plastic container.SOLUTION: The film for a lid material is used which is a laminate including a substrate and a sealant layer. The substrate is a stretched film composed of polyethylene. The sealant layer is composed of a resin composition containing (A) 80-97 pts.wt. of an ethylene / α-olefin copolymer having a density of 880-910 kg / m3 and (B) 3-20 pts.wt. of a tackifier.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a film for covering material. [Background technology]

[0002] 2. Description of the Related Art Conventionally, plastic containers made of polypropylene, polystyrene, polyethylene terephthalate, polyvinyl chloride, etc., and paper containers mainly made of paper have been used for packaging foods, beverages, pharmaceuticals, industrial parts, etc., and the lids used for these containers are films that have stable adhesive properties to protect the contents and have easy-peel properties that allow them to be opened with appropriate strength when peeled off.

[0003] Such films for covering materials usually have a substrate and a sealant layer, and the substrate generally uses a resin film such as a polyester film, a polyamide film, or a polypropylene film, which has excellent strength and heat resistance. On the other hand, the sealant layer mainly uses a resin composition consisting of an ethylene-vinyl acetate copolymer, an ethylene-α-olefin copolymer, or the like, and a tackifier, and different types of resin films are used for the substrate and the sealant layer in ordinary packaging materials (see, for example, Patent Documents 1 to 4).

[0004] In recent years, social issues such as waste plastics have been attracting attention, and along with the increasing demand for building a recycling-oriented society, there is a demand for improving the recyclability of packaging materials. The packaging materials that combine different types of resin films as described above have the problem that they are difficult to recycle, such as by material recycling or chemical recycling, and in response to this, packaging materials made of the same type of resin materials have been proposed (see, for example, Patent Documents 5 and 6).

[0005] However, the above-mentioned packaging materials are limited to applications such as standing pouches in which sealant layers of the same film are heat-sealed together, and the adhesiveness is insufficient when used as a film for covering plastic containers made of polypropylene, polystyrene, polyethylene terephthalate, polyvinyl chloride, etc. Therefore, a film for covering that can be suitably used for these applications has been desired. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2020-158763 A (see, for example, the claims.) [Patent Document 2] Japanese Patent Application Laid-Open No. 11-228757 (see, for example, the claims) [Patent Document 3] Japanese Patent Application Laid-Open No. 10-147672 (see, for example, the claims) [Patent Document 4] JP-A-11-269320 (see, for example, the claims) [Patent Document 5] JP 2022-165191 A (see, for example, the claims.) [Patent Document 6] WO 2021 / 054349 (see, for example, the claims). Summary of the Invention [Problem to be solved by the invention]

[0007] The present invention has been made to solve the above problems, and has an object to provide a film for a covering material that is highly recyclable and has excellent adhesion to plastic containers. [Means for solving the problem]

[0008] As a result of intensive research aimed at solving the above problems, the inventors have discovered that a film for covering material comprising a substrate having specific properties and a sealant layer exhibits excellent recyclability and adhesiveness, and have thus completed the present invention.

[0009] That is, the respective aspects of the present invention are as follows [1] to

[11] . [1] A laminate comprising a substrate and a sealant layer, the substrate being a stretched film made of polyethylene, and the sealant layer having a density of 880 to 910 kg / m 3 The film for covering material is composed of a resin composition containing 80 to 97 parts by weight of an ethylene / α-olefin copolymer (A) and 3 to 20 parts by weight of a tackifier (B) (the total of the ethylene / α-olefin copolymer (A) and the tackifier (B) is 100 parts by weight). [2] The film for covering materials according to [1] above, wherein the ethylene-α-olefin copolymer (A) has an α-olefin carbon number of 3 to 20 and has a melt mass flow rate, measured in accordance with JIS K7210-1 at 190°C under a load of 2.16 kg, in the range of 0.1 to 25 g / 10 min. [3] The film for covering materials according to [1] or [2], wherein the tackifier (B) is an alicyclic saturated hydrocarbon resin having a softening temperature of 105 to 150°C as determined by a ring and ball method and a hydrogenation rate of aromatic nuclei of 80% or more. [4] The polyethylene constituting the substrate has a weight average molecular weight (Mw) measured by gel permeation chromatography of 70,000 to 250,000, and the proportion of molecular weights of 10,000 or less is 8% by weight or less, and a density measured by JIS K6922-1 of 945 to 980 kg / m 3 The film for covering material according to any one of the above [1] to [3], [5] The film for covering materials according to any one of [1] to [4] above, wherein the resin composition constituting the sealant layer contains 3 to 20 parts by weight of a low-density polyethylene (C) satisfying the following requirements (a) and (b) per 100 parts by weight in total of the ethylene-α-olefin copolymer (A) and the tackifier (B): (a) The melt mass flow rate measured in accordance with JIS K7210-1 at 190°C under a load of 2.16 kg is in the range of 0.3 to 5.0 g / 10 min. (b) The swell ratio (SR) calculated by dividing the diameter (D) of the strand extruded at a temperature of 235°C and an extrusion rate of 3 g / min using a melt indexer used in JIS K7210-1 by the orifice diameter (D0) of the melt indexer is in the range of 1.7 to 3.0. [6] The film for covering material according to any one of [1] to [5] above, which comprises an intermediate layer between the substrate and the sealant layer, the intermediate layer being made of polyethylene or an ethylene copolymer. [7] The film for covering materials according to [6], wherein the thickness (Y) of the sealant layer relative to the sum (X) of the thickness of the substrate and the thickness of the intermediate layer satisfies the relationship (X) ≧ (Y). [8] The film for covering material according to any one of [1] to [7] above, wherein the content of the polyethylene resin in the entire film for covering material is 90% by weight or more. [9] An easy-peel lid material comprising the lid material film according to [1] above.

[10] A method for sealing a container, comprising adhering the lid material described in [9] above to an opening of a container made of at least one material selected from the group consisting of polyethylene terephthalate, polystyrene, polypropylene, polyvinyl chloride, and polylactic acid.

[11] A packaging container comprising a container having an opening and the lid material described in [9] above that seals the opening, wherein the container is made of at least one member selected from the group consisting of polyethylene terephthalate, polystyrene, polypropylene, polyvinyl chloride, and polylactic acid. Effect of the Invention

[0010] According to the present invention, it is possible to provide a film for a lid material which is excellent in adhesion to various kinds of plastic containers in addition to being easily recyclable. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present invention will be described in detail below.

[0012] The covering film according to one embodiment of the present invention is a laminate comprising a substrate and a sealant layer.

[0013] The substrate is a polyethylene that has been subjected to a stretching treatment. The stretching treatment can improve the strength and heat resistance of the substrate, and can satisfy the physical properties required for, for example, the outer layer of a packaging material. The stretching may be uniaxial or biaxial.

[0014] The polyethylene used for the substrate has a weight average molecular weight (Mw) measured by gel permeation chromatography of 70,000 to 250,000, preferably 100,000 to 200,000, and more preferably 100,000 to 150,000. When Mw is 70,000 or more, the strength of the substrate obtained is sufficient, which is preferable, and when Mw is 250,000 or less, the melt extrudability in material recycling is excellent and the performance of the obtained recycled resin is not deteriorated, which is preferable.

[0015] The polyethylene has a molecular weight of 10,000 or less as measured by gel permeation chromatography of 8% by weight or less, preferably 6% by weight or less, and more preferably 4% by weight or less. When this ratio is 8% by weight or less, the stretched film has excellent heat resistance and the heat seal appearance of the laminate film is not deteriorated, which is preferable. This is presumably because the molecular chains are relaxed by molecules with low molecular weight during the stretching process, resulting in insufficient orientation of the polyethylene crystals.

[0016] The polyethylene used in the above substrate has a density of 945 to 980 kg / m as measured according to JIS K6922-1 (1997). 3 It is preferable that the density is 945 kg / m 3 In the case of above, the heat resistance of the polyethylene stretched film is excellent, which is preferable, and the density is 980 kg / m 3 The following polyethylenes are easy to produce industrially:

[0017] Such polyethylene can be obtained by homopolymerizing ethylene or copolymerizing ethylene with a small amount of α-olefin of 5 mol% or less. For the polymerization, a Ziegler catalyst consisting of a solid catalyst component containing magnesium and titanium and an organoaluminum compound, a metallocene catalyst consisting of an organotransition metal compound containing a cyclopentadienyl derivative and a compound and / or an organometallic compound that reacts with the organotransition metal compound to form an ionic complex, a vanadium catalyst, etc. can be used, and metallocene catalysts and vanadium catalysts are preferred because they make it easy to control the proportion of molecular weights of 10,000 or less. The method for producing polyethylene is not particularly limited, and it can be produced by, for example, a slurry method, a solution method, a gas phase method, etc. The slurry method or solution method is preferred because it makes it easy to control the proportion of molecular weights of 10,000 or less.

[0018] Furthermore, the polyethylene may contain additives, such as antioxidants, lubricants, neutralizing agents, antiblocking agents, surfactants, slip agents, and the like, which are generally used in polyolefins, as required.

[0019] The sealant layer has a density of 880 to 910 kg / m 3 The resin composition comprises 80 to 97 parts by weight of an ethylene-α-olefin copolymer (A) and 3 to 20 parts by weight of a tackifier (B) (the total of the ethylene-α-olefin copolymer (A) and the tackifier (B) is 100 parts by weight).

[0020] As the ethylene-α-olefin copolymer (A), any one that belongs to the category generally referred to as an ethylene-α-olefin copolymer can be used. Although there is no particular limitation on the α-olefin, it is preferable that the number of carbon atoms is 3 to 20, and examples thereof include 1-butene, 1-pentene, 1-hexene, 1-octene, 1-heptene, 4-methyl-1-pentene, 4-methyl-1-hexene, 4,4-dimethyl-1-pentene, and octadecene. Among these α-olefins, it is preferable to use 1-hexene, 1-octene, 1-heptene, and 4-methyl-1-pentene, and particularly preferable is 1-hexene, which has high adhesive strength and stable strength. These ethylene-α-olefin copolymers (A) can be suitably produced by copolymerizing ethylene and α-olefins using a Ziegler catalyst, a chromium catalyst, or a metallocene catalyst. Examples of the polymerization method include a solution polymerization method, a high-pressure polymerization method, and a gas phase polymerization method.

[0021] The ethylene-α-olefin copolymer (A) has excellent low-temperature adhesion and is therefore suitable for use with a density of 880 to 910 kg / m as measured according to JIS K6922-1. 3 , preferably 900 to 910 kg / m 3 It is preferable that the density is in the range of 880 kg / m 3 If it is less than 910 kg / m, the heat resistance of the resin composition is poor and the density is 3 If it exceeds this value, the adhesiveness of the resulting covering film will be poor.

[0022] The ethylene / α-olefin copolymer (A) preferably has a melt mass flow rate (hereinafter sometimes referred to as MFR) in the range of 0.1 to 25 g / 10 min, measured at 190° C. under a load of 2.16 kg according to JIS K7210-1. Ethylene / α-olefin polymers having a melt mass flow rate in such a range are advantageous in that they have excellent formability when producing a film for a covering material.

[0023] Furthermore, since the ethylene-α-olefin copolymer has little low molecular weight components that impair adhesion, it is preferable that the ratio of weight average molecular weight (Mw) to number average molecular weight (Mn) (Mw / Mn) measured by gel permeation chromatography (GPC) is 3 or less.

[0024] The tackifier (B) may be any resin that falls within the category of tackifier resins, such as aliphatic hydrocarbon resins, aromatic hydrocarbon resins, aliphatic-aromatic copolymer hydrocarbon resins, alicyclic hydrocarbon resins obtained by hydrogenating aromatic hydrocarbon resins, synthetic terpene hydrocarbon resins having a structure containing aliphatic, alicyclic and aromatic groups, terpene hydrocarbon resins made from α,β-pinene in turpentine oil, coumaroindene hydrocarbon resins made from indene and styrenes in coal tar naphtha, low molecular weight styrene resins and rosin hydrocarbon resins. Among these tackifiers, aliphatic hydrocarbon resins and alicyclic hydrocarbon resins made by hydrogenating aromatic hydrocarbon resins are preferred because they have excellent dispersibility in the ethylene-α-olefin copolymer that is the main component, and the film for the lid material has excellent adhesion.

[0025] The tackifier (B) preferably has a softening temperature measured by the ring and ball method in the range of 105 to 150°C, more preferably 115 to 140°C. Furthermore, alicyclic hydrocarbons having a hydrogenation rate to aromatic nuclei of 80% or more, preferably 85% or more, are particularly preferred. When the softening temperature is 105°C or more, the resulting film for a lid material has excellent adhesiveness, while when the softening temperature is 150°C or less, the production is not restricted by the outside temperature and is excellent in terms of stable production. Furthermore, when the hydrogenation rate is 80% or more, the resulting film for a lid material is excellent in terms of hygiene and is suitable for use in food applications.

[0026] The tackifier (B) may be a commercially available product. Specifically, examples of alicyclic hydrocarbon resins include (trade names) Alcon P115, Alcon P125, Alcon P140, Alcon M115, and Alcon M135 (all manufactured by Arakawa Chemical Industries Co., Ltd.), Imave S110, Imave P125 (all manufactured by Idemitsu Kosan Co., Ltd.), T-REZ RC115, and T-REZ HA125 (all manufactured by JXTG Energy Corporation). Examples of rosin resins include Pine Crystal KE-311 (manufactured by Arakawa Chemical Industries Co., Ltd.). Examples of terpene resins include YS Resin PX1150 and YS Resin PX1150N (all manufactured by Yasuhara Chemical Co., Ltd.).

[0027] The blending ratio of the ethylene-α-olefin copolymer (A) and tackifier (B) constituting the above sealant layer is as follows: The total of (A) and (B) is 100 parts by weight.

[0028] The blending ratio of the ethylene-α-olefin copolymer (A) is within the range of 80 to 97 parts by weight, and preferably 90 to 97 parts by weight. If the blending ratio of (A) is less than 80 parts by weight, the resulting covering film will have poor formability, and if it exceeds 97 parts by weight, the adhesiveness will be poor, which is not preferred.

[0029] The blending ratio of the tackifier (B) is within the range of 3 to 20 parts by weight, and preferably 3 to 10 parts by weight. If the blending ratio of (B) is less than 3 parts by weight, the resulting film for covering material will have poor adhesiveness, and if it exceeds 20 parts by weight, the blocking property during molding will be poor, which is not preferable.

[0030] The resin composition constituting the sealant layer may contain a low-density polyethylene (C) in order to further improve moldability.

[0031] The low-density polyethylene (C) is a low-density polyethylene obtained by polymerizing only ethylene using a known high-pressure polymerization method, and has a density of 910 to 940 kg / m as measured according to JIS K6922-1. 3It is preferable that the range is 100%.

[0032] The low-density polyethylene (C) preferably has a melt mass flow rate in the range of 0.3 to 5.0 g / 10 min, more preferably 0.5 to 5.0 g / 10 min, and even more preferably 1.0 to 5.0 g / 10 min, as measured in accordance with JIS K7210-1 at 190° C. under a load of 2.16 kg. A melt mass flow rate of 0.3 g / 10 min or more reduces the extrusion load during processing into a film for a covering material, and a melt mass flow rate of 5.0 g / 10 min or less is preferred because it increases the effect of improving moldability.

[0033] Furthermore, the low-density polyethylene (C) preferably has a swell ratio (SR) in the range of 1.7 to 3.0, more preferably 1.7 to 2.5, and even more preferably 1.9 to 2.5. The inclusion of a low-density polyethylene having an SR in this range in the sealant layer is preferable because it improves molding processability. The SR can be measured by using a melt indexer used in JIS K7210-1, extruding the resin filled in the device from the orifice under conditions of a temperature of 235°C and an extrusion rate of 3g / min, collecting a strand-shaped extrudate in a measuring cylinder containing isopropanol placed directly below the orifice, and dividing the diameter (D) of the extruded strand by the orifice diameter (D0) of the melt indexer.

[0034] The blending ratio of the low-density polyethylene (C) is preferably within the range of 3 to 20 parts by weight, more preferably 3 to 13 parts by weight, and even more preferably 3 to 10 parts by weight, per 100 parts by weight of the total resin composition containing the ethylene-α-olefin copolymer (A) and the tackifier (B). When the blending ratio of (C) is 3 parts by weight or more, the effect of improving the formability of the covering film is excellent, and when it is 20 parts by weight or less, excellent adhesion is obtained, which is preferable.

[0035] The resin composition constituting the sealant layer may contain other thermoplastic resins or rubbers, as well as light stabilizers, ultraviolet absorbers, nucleating agents, lubricants, antioxidants, antiblocking agents, flow improvers, release agents, flame retardants, colorants, inorganic neutralizing agents, hydrochloric acid absorbers, filler conductive agents, and the like, within the scope of not impairing the effects of the present invention.

[0036] There is no particular restriction on the method for preparing the resin composition constituting the sealant layer. For example, the ethylene-α-olefin copolymer (A), the tackifier (B) and materials to be added thereto are pre-blended simultaneously in a mixer such as a Henschel mixer or a tumbler, and then melt-kneaded in a single-screw or twin-screw extruder.

[0037] The above-mentioned film for covering material is a film for covering material comprising a substrate and a sealant layer, and an intermediate layer may be provided between the substrate and the sealant layer to enhance the adhesion between the two layers. The intermediate layer is a polyethylene or ethylene copolymer. The ethylene copolymer is not limited as long as it is a copolymer of ethylene and a monomer copolymerizable therewith, and examples thereof include ethylene-α-olefin copolymer, propylene-ethylene copolymer, ethylene-acrylic acid copolymer, ethylene-methacrylic acid copolymer, and ethylene-methyl acrylate copolymer. Modified products thereof may also be used. The intermediate layer may contain various additives, such as antioxidants, lubricants, antistatic agents, conductive agents, antiblocking agents, light stabilizers, and ultraviolet absorbing agents, within the scope of not impairing the effects of the present invention.

[0038] The intermediate layer may be a single layer or a laminate, and may be a laminate selected from any polyethylene or ethylene copolymer, such as polyethylene / ethylene-α-olefin copolymer / polyethylene.

[0039] The thickness of the substrate is preferably 10 to 200 μm, more preferably 12 to 100 μm, and further preferably 14 to 50 μm. Within such a range, a laminate film having sufficient strength as a substrate for a film for a covering material can be obtained.

[0040] The thickness of the intermediate layer can be selected depending on the application as long as workability is not impaired, but is generally about 5 to 30 μm. The thickness of the sealant layer is preferably 3 to 50 μm, more preferably 5 to 40 μm, and even more preferably 5 to 25 μm. When the thickness is 5 μm or more, the resulting covering film has excellent adhesiveness, and when it is 25 μm or less, it shows sufficient adhesiveness and is economical.

[0041] Furthermore, the sum of the thicknesses of the substrate and intermediate layer (X) and the thickness of the sealant layer (Y) preferably satisfy the relationship (X) ≧ (Y). When the thicknesses satisfy the relationship (X) ≧ (Y), the substrate of the resulting lid material film can maintain sufficient strength, and the intermediate layer can sufficiently adhere the substrate and the sealant layer, so that the resulting lid material film exhibits good adhesive strength to various containers. Furthermore, the proportion of non-polyethylene resin contained in the sealant layer is reduced, so that the resulting lid material film has excellent recyclability.

[0042] The content of polyethylene resin in the entire film for covering material is preferably 90% by weight or more. Since such a film uses the same type of resin material, it can be classified as a mono-material material and has excellent recyclability. Here, polyethylene resin means the polyethylene of the substrate, the polyethylene or ethylene copolymer of the intermediate layer, the ethylene-α-olefin copolymer (A) of the sealant layer, and the low-density polyethylene (C).

[0043] The above-mentioned covering film can be suitably used as an easy-peel covering material for plastic containers made of resins mainly composed of polyethylene terephthalate, polystyrene, polypropylene, etc., and various other resins.

[0044] Specific examples of materials for the plastic container include polyolefin resins, acrylic resins, polyamide resins, polyester resins, polycarbonate resins, polystyrene resins, styrene-acrylonitrile copolymers, and polyvinyl chloride resins.

[0045] Examples of polyolefin resins include low-density polyethylene, high-density polyethylene, ethylene-α-olefin copolymer, ethylene-vinyl acetate copolymer, polypropylene, etc. Examples of acrylic resins include polyacrylic acid, polymethyl acrylate, polyethyl acrylate, polybutyl acrylate, polyoctyl acrylate, polymethacrylic acid, polymethyl methacrylate, polyethyl methacrylate, polybutyl methacrylate, polyoctyl methacrylate, etc. Examples of polyamide resins include nylon 6, nylon 6,6, nylon 11, nylon 12, etc. Examples of polyester resins include polyethylene terephthalate, polybutylene terephthalate, polylactic acid (including poly-L-lactic acid, poly-D-lactic acid, copolymers of L-lactic acid and D-lactic acid, and stereocomplexes of poly-L-lactic acid and poly-D-lactic acid), polybutylene succinate, poly(butylene succinate / adipate), polyethylene succinate, poly(butylene succinate / terephthalate), poly(butylene adipate / terephthalate), poly(hydroxybutyrate / hydroxyhexanoate), polyglycolic acid, poly 3-hydroxybutyrate, and polycaprolactone.

[0046] Furthermore, a barrier layer can be provided between the substrate and the intermediate layer. The barrier layer can be made of a gas barrier resin, such as an ethylene-vinyl alcohol copolymer, polyvinyl alcohol, polyamide resin, polyester resin, or polyurethane resin. Alternatively, a vapor-deposited barrier layer can be provided instead of the gas barrier resin, such as an aluminum vapor-deposited layer formed by vapor-depositing a metal such as aluminum. The presence of the barrier layer can improve the oxygen barrier property and water vapor barrier property.

[0047] In the present invention, an anchor coat layer of polyurethane or the like may be provided between the substrate and the sealant layer, or between the substrate and the intermediate layer, in order to enhance adhesion between the two layers.

[0048] The method for producing the above-mentioned covering material is not particularly limited, but examples thereof include a method of laminating a resin composition for the sealant layer with a substrate, and a method of co-extruding a sealant adhesive with an intermediate layer.

[0049] Examples of lamination methods include (1) an extrusion lamination method in which an anchor coating agent is applied to a substrate, and a sealant layer is melt-extruded; (2) an extrusion lamination method in which an anchor coating agent is applied to a substrate, and an intermediate layer is melt-extruded, and then a sealant layer is melt-extruded on top of the intermediate layer; (3) an extrusion lamination method in which an intermediate layer having excellent adhesion to the substrate, such as an ethylene-methacrylic acid copolymer or an ethylene-methyl methacrylate copolymer, is melt-extruded on the substrate, and then a sealant layer is melt-extruded on top of the intermediate layer; (4) a co-extrusion lamination method in which an anchor coating agent is applied to a substrate, and then an intermediate layer and a sealant layer are melt-extruded simultaneously; and (5) a co-extrusion lamination method in which an anchor coating agent is applied to a substrate, and then an intermediate layer and a sealant layer are melt-extruded simultaneously. 1) the co-extrusion lamination method, in which an intermediate layer having excellent adhesion to the substrate, such as an ethylene-methacrylic acid copolymer or an ethylene-methyl methacrylate copolymer, and a sealant layer are simultaneously melt-extruded onto the substrate; (6) the dry lamination method, in which a film containing at least one sealant layer is formed in advance by an inflation molding method or a cast molding method, and then laminated to a substrate coated with an anchor coating agent; and (7) the sandwich extrusion lamination method, in which an intermediate layer is melt-extruded using an extrusion lamination to laminate between a substrate coated with an anchor coating agent and a film containing at least one sealant layer.

[0050] The above-mentioned lid material can be adhered to the opening of a plastic container to seal the opening of the container. The main component of the plastic container may be a single component or a composition of multiple resins. The container may also be a multi-layered laminate of multiple materials. The above-mentioned lid material can be suitably used for containers made of polyethylene terephthalate, polystyrene, polypropylene, polyvinyl chloride, and polylactic acid.

[0051] Furthermore, a packaging container according to one embodiment of the present invention is a packaging container comprising a container having an opening and the above-mentioned lid material that seals the opening, wherein the container is made of at least one member selected from the group consisting of polyethylene terephthalate, polystyrene, polypropylene, polyvinyl chloride, and polylactic acid. EXAMPLES

[0052] The present invention will be described in more detail below based on examples, but the present invention is not limited to these examples. (molecular weight) The molecular weight was measured using a GPC device (Tosoh Corporation (product name) HLC-8121GPC / HT) and a column (Tosoh Corporation (product name) TSKgel GMHhr-H(20)HT) with the column temperature set at 140°C and 1,2,4-trichlorobenzene as the eluent. The measurement sample was prepared at a concentration of 1.0 mg / ml, and 0.3 ml was injected for measurement. The molecular weight calibration curve was calibrated using a polystyrene sample with a known molecular weight. The weight average molecular weight Mw and the proportion of components with a molecular weight of 10,000 or less were calculated from the chromatogram obtained as a result of the measurement. (density) Measurements were performed in accordance with JIS K6922-1. (Swell ratio SR) The SR of each material was measured using a melt indexer according to JIS K7210. The resin filled in the device was extruded from the orifice at a temperature of 235°C and an extrusion rate of 3g / min. A strand-like extrudate was collected in a measuring cylinder filled with isopropanol placed directly below the orifice, and the diameter (D) of the extruded strand was divided by the orifice diameter (D0) of the melt indexer. (Adhesive strength) The sealant layer of the lid material obtained in the embodiment was laminated with a 0.35 mm thick amorphous polyethylene terephthalate sheet (A-PET, manufactured by Toyobo Co., Ltd.), a 0.35 mm thick impact resistant polystyrene sheet (HIPS, manufactured by DIC Corporation), and a 0.30 mm thick polypropylene sheet (PP, manufactured by OJK Corporation), and was heat-pressed using a heat seal tester (manufactured by Tester Sangyo Co., Ltd., TP-701 model) at a temperature of 130°C, an air pressure of 0.2 MPa, and a time of 1 second. After cooling, the seal strength was measured at a peel angle of 180° and a peel speed of 300 mm / min. (Moldability) The formability during lamination processing when producing the covering material films described in the examples was evaluated. The case where the films could be formed without problems was marked with an ⊚, the case where the molten film was somewhat unstable but the film could be formed without problems was marked with an ◯, and the case where the film broke and the film could not be formed was marked with an ×. (Recyclability) The lid material obtained in the examples was crushed and melt-kneaded using a twin-screw extruder (manufactured by Technovel, product name ULTnano25TW) with a screw diameter of 25 mm at a resin temperature of 160°C and a screw rotation speed of 300 rpm to obtain strands. The smoothness of the obtained strands was evaluated, and smooth strands were deemed to have excellent recyclability. (Heat resistance) The sealant layer of the lid material obtained in the examples was placed on an A-PET cup (manufactured by Rispack Co., Ltd.) with a capacity of 210 ml and a diameter of 101 mm, and cut into a circle with a diameter of 101 mm. Next, using a cup sealer UF-500 (manufactured by Sunnypack Co., Ltd.), the cup was heated and pressed at a temperature of 130°C, an air pressure of 0.8 MPa, and a time of 1 second, and then allowed to cool, and the appearance of the laminate was evaluated. When the heat shrinkage of the lid material was large and it peeled off from the cup, it was marked with ×, and when the heat shrinkage was small and there was no peeling, it was marked with ◯.

[0053] [Example 1] [Preparation of organically modified clay] In a 1-liter flask, 300 ml of industrial alcohol (product name Ekinen F-3, manufactured by Japan Alcohol Sales Co., Ltd.) and 300 ml of distilled water were added, and 15.0 g of concentrated hydrochloric acid and dioleylmethylamine ((C 18 H 35)2(CH3)N, 63.7g (120mmol) of (Lipomin MO, manufactured by Lion Specialty Chemicals Co., Ltd.) was added and heated to 45℃, after which 100g of synthetic hectorite (Laponite RD, manufactured by BYK Co., Ltd.) was dispersed, and the temperature was raised to 60℃ and stirred for 1 hour while maintaining the temperature. After filtering the slurry, it was washed twice with 600ml of water at 60℃ and dried in a dryer at 85℃ for 12 hours to obtain 130g of organically modified clay. This organically modified clay was pulverized in a jet mill to a median diameter of 15μm.

[0054] [Preparation of polymerization catalyst] After replacing the air in a 300mL flask equipped with a thermometer and reflux condenser with nitrogen, 25.0g of the organically modified clay obtained in [Preparation of organically modified clay] and 108mL of hexane were added, followed by the addition of 0.392g (1mmol) of bis(indenyl)zirconium dichloride and 142mL of 20% triisobutylaluminum, and stirring for 3 hours at 60°C. After cooling to room temperature, the supernatant was removed and washed twice with 220mL of hexane, and then 220mL of hexane was added to obtain a catalyst suspension (solid weight content: 12.0wt%).

[0055] [Production of polyethylene powder] A 2L autoclave was charged with 1.2L of hexane, 1.0mL of 20% triisobutylaluminum, and 200mg (equivalent to 24mg of solids) of the catalyst suspension obtained in [Preparation of polymerization catalyst], and after heating to 85°C, ethylene / hydrogen mixed gas was continuously fed so that the partial pressure was 0.90MPa (hydrogen concentration in ethylene / hydrogen mixed gas: 450ppm). After 90 minutes, the pressure was released, and the slurry was filtered and dried to obtain polyethylene powder. The obtained polyethylene powder had a weight average molecular weight of 111,000, a proportion of components with molecular weights of 10,000 or less of 3.4%, and a density of 950kg / m 3 The obtained polyethylene powder was melt-kneaded using a twin-screw extruder (manufactured by Technobel, product name ULTnano25TW) with a screw diameter of 25 mm under conditions of a resin temperature of 160° C. and a screw rotation speed of 300 rpm to obtain polyethylene pellets.

[0056] [Production of oriented polyethylene film] The polyethylene pellets were then made into a film using an inflation molding machine having an extruder with a screw diameter of 50 mm. The extrusion temperature was 220°C, the die lip clearance (L) was 3 mm, and the thickness of the resulting polyethylene film was 100 μm. The resulting polyethylene film was uniaxially stretched at 120°C to a stretch ratio of 4 times using a tenter method stretching machine (manufactured by Toyo Seiki Seisakusho Co., Ltd., product name EX10-B) to obtain a polyethylene stretched film (I). The thickness of the resulting polyethylene stretched film (I) was 25 μm.

[0057] [Production of Resin Composition for Sealant Layer] Ethylene-α-olefin copolymer (A) with a density of 905 kg / m 3 90 parts by weight of ethylene-1-hexene copolymer (A1) (manufactured by Tosoh Corporation, product name Nipolon HM510R) with MFR of 12g / 10min, and 10 parts by weight of alicyclic hydrocarbon resin (B1) (manufactured by Arakawa Chemical Industries, product name Alcon P125; softening temperature 125°C, fully hydrogenated) as a tackifier (B) were pre-blended in a tumbler mixer, and then melt-kneaded at 160°C using a twin-screw extruder to obtain pellets of the resin composition. In consideration of thermal stability, 0.05 parts by weight of a phenolic antioxidant (manufactured by BASF, product name Irganox 1010) and 0.2 parts by weight of a slip agent (manufactured by Lion Akzo, product name Armowax E) were added to the resin composition per 100 parts by weight of the sealant adhesive.

[0058] [Production of lid materials] After applying an anchor coating agent (a mixture of Takelac A3210 and Takenate A3072, manufactured by Mitsui Chemicals) to the surface of the polyethylene stretched film substrate, the intermediate layer and the sealant layer were co-extrusion laminated at a processing temperature of 230°C using a co-extrusion laminator (manufactured by Sumiju Modern Industries, screw diameter 40 mm) in the order of substrate / intermediate layer / sealant layer to obtain a lid material. Low-density polyethylene (manufactured by Tosoh, product name Petrothene 203) was used as the intermediate layer, and the lid material had a structure of substrate 25 μm / intermediate layer 12 μm / sealant layer 20 μm. The evaluation results of the obtained lid material are shown in Table 1.

[0059] [Example 2] The resin composition for the sealant layer of Example 1 was used as an ethylene-α-olefin copolymer (A) having a density of 905 kg / m 3 A covering material was obtained in the same manner as in Example 1, except that the ethylene-1-hexene copolymer (A2) having an MFR of 4.0 g / 10 min was 90 parts by weight, and the tackifier (B1) was 10 parts by weight. The evaluation results of the resulting covering material are shown in Table 1.

[0060] [Example 3] The resin composition for the sealant layer of Example 1 was used as an ethylene-α-olefin copolymer (A) having a density of 885 kg / m 3 A covering material was obtained in the same manner as in Example 1, except that the amount of the ethylene-1-butene copolymer (A3) having a MFR of 3.5 g / 10 min was 90 parts by weight, and the amount of the tackifier (B1) was 10 parts by weight. The evaluation results of the resulting covering material are shown in Table 1.

[0061] [Example 4] The resin composition for the sealant layer of Example 1 was used as an ethylene-α-olefin copolymer (A) having a density of 900 kg / m 3 A covering material was obtained in the same manner as in Example 1, except that the amount of the ethylene-1-hexene copolymer (A4) having a MFR of 20 g / 10 min was 82 parts by weight, and the amount of the tackifier (B1) was 18 parts by weight. The evaluation results of the resulting covering material are shown in Table 1.

[0062] [Example 5] A covering material was obtained in the same manner as in Example 1, except that 90 parts by weight of ethylene-α-olefin copolymer (A1) and 10 parts by weight of alicyclic hydrocarbon resin (B2) (manufactured by Arakawa Chemical Industries, Ltd., product name Alcon P140; softening temperature 140° C., fully hydrogenated) were used as the tackifier (B) relative to the resin composition for the sealant layer in Example 1. The evaluation results of the resulting covering material are shown in Table 1.

[0063] [Example 6] The resin composition for the sealant layer of Example 1 was mixed with 90 parts by weight of an ethylene-α-olefin copolymer (A1), 10 parts by weight of a tackifier (B1), and a low-density polyethylene (C) having a density of 924 kg / m 3 A lid material was obtained in the same manner as in Example 1, except that 5 parts by weight of low-density polyethylene (C1) (manufactured by Tosoh Corporation, product name Petrothene 205) having a MFR of 3.0 g / 10 min and a SR of 2.02 was used. The evaluation results of the obtained lid material are shown in Table 1.

[0064] [Example 7] The resin composition for the sealant layer of Example 1 was mixed with 90 parts by weight of an ethylene-α-olefin copolymer (A1), 10 parts by weight of a tackifier (B1), and a low-density polyethylene (C) having a density of 922 kg / m 3 A lid material was obtained in the same manner as in Example 1, except that 14 parts by weight of low-density polyethylene (C2) (manufactured by Tosoh Corporation, product name Petrothene 175R) having a MFR of 0.6 g / 10 min and a SR of 1.81 was used. The evaluation results of the obtained lid material are shown in Table 1.

[0065] [Example 8] The resin composition for the sealant layer of Example 1 was mixed with 90 parts by weight of an ethylene-α-olefin copolymer (A1), 10 parts by weight of a tackifier (B1), and a low-density polyethylene (C) having a density of 924 kg / m 3 A lid material was obtained in the same manner as in Example 1, except that 5 parts by weight of low-density polyethylene (C3) (manufactured by Tosoh Corporation, product name Petrothene 183) having a MFR of 2.0 g / 10 min and a SR of 1.63 was used. The evaluation results of the obtained lid material are shown in Table 1.

[0066] [Example 9] A covering material was obtained in the same manner as in Example 1, except that 90 parts by weight of the ethylene-α-olefin copolymer (A1), 10 parts by weight of the tackifier (B1), and 2 parts by weight of the low-density polyethylene (C1) were used in place of the resin composition for the sealant layer in Example 1. The evaluation results of the resulting covering material are shown in Table 1.

[0067] [Example 10] Instead of the stretched polyethylene film (I) of Example 1, a film having a weight average molecular weight of 122,000, a proportion of components having a molecular weight of 10,000 or less of 10.2%, and a density of 954 kg / m 3 A covering material was obtained in the same manner as in Example 1, except that a 25 μm-thick stretched polyethylene film (II) made from polyethylene pellets (manufactured by Tosoh Corporation, product name Nipolonhard 5700) was used. The evaluation results of the resulting covering material are shown in Table 1.

[0068] [Example 11] A covering material was obtained in the same manner as in Example 1, except that 90 parts by weight of ethylene-α-olefin copolymer (A1) and 10 parts by weight of alicyclic hydrocarbon resin (B3) (manufactured by Arakawa Chemical Industries, Ltd., product name Alcon P100; softening temperature 100°C, fully hydrogenated) were used as the tackifier (B) relative to the resin composition for the sealant layer in Example 1. The evaluation results of the resulting covering material are shown in Table 1.

[0069] [Example 12] A covering material was obtained in the same manner as in Example 1, except that 90 parts by weight of ethylene-α-olefin copolymer (A1) and 10 parts by weight of polymerized rosin ester resin (B4) (manufactured by Arakawa Chemical Industries, Ltd., product name Pencel D125; softening temperature 125° C.) were used as the tackifier (B) relative to the resin composition for the sealant layer in Example 1. The evaluation results of the resulting covering material are shown in Table 1.

[0070] [Example 13] A lid material was obtained in the same manner as in Example 4, except that a 15 μm thick polyethylene stretched film (IV) was used instead of the 25 μm thick polyethylene stretched film (I) of Example 4, the thickness of the intermediate layer made of low-density polyethylene (manufactured by Tosoh Corporation, product name Petrothene 203) was set to 2 μm, and the thickness of the sealant layer was set to 30 μm. The polyethylene stretched film (IV) was produced by uniaxially stretching a 60 μm thick polyethylene film produced in the same manner as the polyethylene stretched film (I) at 120° C. to a stretch ratio of 4 times. The evaluation results of the obtained lid material are shown in Table 1.

[0071] [Table 1]

[0072] [Comparative Example 1] A lid material was obtained in the same manner as in Example 1, except that a biaxially oriented polyester film (III) having a thickness of 25 μm (manufactured by Toyobo Co., Ltd., product name E5100) was used instead of the stretched polyethylene film (I) in Example 1. The evaluation results of the obtained lid material are shown in Table 2. The obtained lid material had a poor strand appearance during melt-kneading and was poor in recyclability. Furthermore, even when the resin temperature during melt-kneading was increased to 250° C., the strand appearance was similarly poor and the recyclability was poor.

[0073] [Comparative Example 2] The resin composition for the sealant layer of Example 1 was used as an ethylene-α-olefin copolymer (A) having a density of 920 kg / m 3 A covering material was obtained in the same manner as in Example 1, except that the ethylene-1-hexene copolymer (A5) having an MFR of 2.0 g / 10 min was 90 parts by weight, and the tackifier (B1) was 10 parts by weight. The evaluation results of the resulting covering material are shown in Table 2. The resulting covering material had poor adhesion.

[0074] [Comparative Example 3] An attempt was made to prepare a lid in the same manner as in Example 1, except that 70 parts by weight of the ethylene-α-olefin copolymer (A1) and 30 parts by weight of the tackifier (B1) were used in place of the resin composition for the sealant layer in Example 1. However, breakage of the molten film and blocking to the forming roll occurred during molding, making it difficult to prepare a lid.

[0075] [Table 2]

Claims

1. A laminate comprising a substrate and a sealant layer, the substrate being a stretched film made of polyethylene, and the sealant layer having a density of 880 to 910 kg / m 3 The film for covering material is composed of a resin composition containing 80 to 97 parts by weight of an ethylene / α-olefin copolymer (A) and 3 to 20 parts by weight of a tackifier (B) (the total of the ethylene / α-olefin copolymer (A) and the tackifier (B) is 100 parts by weight).

2. The ethylene / α-olefin copolymer (A) has an α-olefin carbon number of 3 to 20, and has a melt mass flow rate measured in accordance with JIS K7210-1 at 190° C. under a load of 2.16 kg in the range of 0.1 to 25 g / 10 min. The film for covering materials according to claim 1.

3. The film for covering material according to claim 1, wherein the tackifier (B) is an alicyclic saturated hydrocarbon resin having a softening temperature of 105 to 150°C as measured by the ring and ball method and a hydrogenation rate of aromatic nuclei of 80% or more.

4. The polyethylene constituting the substrate has a weight average molecular weight (Mw) measured by gel permeation chromatography of 70,000 to 250,000, and the proportion of molecular weights of 10,000 or less is 8% by weight or less, and a density measured by JIS K6922-1 of 945 to 980 kg / m 3 The covering film according to claim 1 ,

5. The resin composition constituting the sealant layer contains 3 to 20 parts by weight of a low-density polyethylene (C) that satisfies the following requirements (a) and (b) per 100 parts by weight in total of the ethylene-α-olefin copolymer (A) and the tackifier (B). The film for covering materials according to claim 1. (a) The melt mass flow rate, measured in accordance with JIS K7210-1 at 190° C. under a load of 2.16 kg, is in the range of 0.3 to 5.0 g / 10 min. (b) The swell ratio (SR) calculated by dividing the diameter (D) of a strand extruded at a temperature of 235° C. and an extrusion rate of 3 g / min using a melt indexer used in JIS K7210-1 by the orifice diameter (D0) of the melt indexer is in the range of 1.7 to 3.

0.

6. The film for covering material according to claim 1, further comprising an intermediate layer between the substrate and the sealant layer, the intermediate layer being made of polyethylene or an ethylene copolymer.

7. 7. The covering film according to claim 6, wherein the thickness (Y) of the sealant layer relative to the sum (X) of the thickness of the substrate and the thickness of the intermediate layer satisfies the relationship (X) ≥ (Y).

8. 2. The film for covering material according to claim 1, wherein the content of the polyethylene resin in the entire film for covering material is 90% by weight or more.

9. An easy-peel covering material comprising the covering film according to claim 1.

10. A method for sealing a container, comprising adhering the lid material according to claim 9 to an opening of a container made of at least one material selected from the group consisting of polyethylene terephthalate, polystyrene, polypropylene, polyvinyl chloride, and polylactic acid.

11. A packaging container comprising a container having an opening and a lid material as described in claim 9 that seals the opening, wherein the container is made of at least one member selected from the group consisting of polyethylene terephthalate, polystyrene, polypropylene, polyvinyl chloride, and polylactic acid.

Citation Information

Patent Citations

  • Ethylene copolymer composition and easily unsealable seal material using the same

    JP1998147672A

  • Adhesive composition and film comprising the same

    JP1999228757A

  • Thermoplastic resin composition

    JP1999269320A

  • Resin composition and film for lid material

    JP2020158763A

  • Laminate and packaging material

    JP2022165191A

Cited By

  • Ethylene-α-olefin copolymer, film, and laminated film

    WO2026191770A1