Resin composition, method for producing resin composition, pellet, molded product, and laminate
The resin composition addresses agglomeration issues by using controlled particle diameter ratios and high shear kneading to enhance impact strength and electrical properties in molded articles.
Patent Information
- Application Number
- JP2024153263
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-02-22
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-28
AI Technical Summary
Existing resin compositions face challenges in achieving high impact strength due to agglomeration of fluorine-containing copolymers during molding, which compromises mechanical properties and electrical performance.
A resin composition comprising an amorphous resin and a fluorine-containing copolymer with controlled particle diameter ratios and high shear kneading to prevent agglomeration, ensuring a dispersed phase structure that maintains mechanical and electrical properties.
The composition produces molded articles with enhanced impact strength, flexibility, and improved electrical properties by suppressing particle agglomeration, resulting in superior mechanical and dielectric performance.
Smart Images

Figure 2024166254000001 
Figure 2024166254000002
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a resin composition, a method for producing a resin composition, pellets, a molded article, and a laminate. [Background technology]
[0002] Amorphous resins belonging to super engineering plastics (super engineering plastics) are used in various products due to their excellent properties such as strength and heat resistance. Fluorine-containing copolymers are also used in various products due to their excellent properties such as sliding properties, heat resistance, chemical resistance, solvent resistance, weather resistance, flexibility, and electrical properties.
[0003] Patent Document 1 describes that by using a fluororesin composition containing an amorphous polymer (amorphous resin) and a fluoropolymer (fluorine-containing copolymer), each of which has specific physical properties, it is possible to obtain an injection-molded article which has little surface peeling tendency, is highly uniform, and has high strength. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2001-72882 A Summary of the Invention [Problem to be solved by the invention]
[0005] The present disclosure provides a resin composition from which molded articles having excellent impact strength can be produced. [Means for solving the problem]
[0006] The present disclosure (1) is a resin composition comprising an amorphous resin (A) belonging to super engineering plastics and a fluorinated copolymer (B), in which the ratio r2 / r1 of an average dispersed particle size r1 of the amorphous resin (A) or the fluorinated copolymer (B) to an average dispersed particle size r2 of the amorphous resin (A) or the fluorinated copolymer (B) after a melt flow rate is measured in accordance with ASTM D1238 at 380°C or a temperature at which the resin composition melts, under a load of 5000 g, and with a preheating time of 5 minutes is less than 1.70. (However, r1 and r2 were measured for the same resin or the same copolymer.)
[0007] The present disclosure (2) is the resin composition according to the present disclosure (1), wherein the amorphous resin (A) has a glass transition temperature of 190°C to 290°C.
[0008] The present disclosure (3) is the resin composition according to the present disclosure (1) or (2), in which the amorphous resin (A) has a continuous use temperature of 140° C. or higher.
[0009] The present disclosure (4) is the resin composition according to any one of the present disclosures (1) to (3), in which the amorphous resin (A) has an imide structure.
[0010] The present disclosure (5) is the resin composition according to the present disclosure (4), wherein the amorphous resin (A) has an amide structure and an imide structure.
[0011] The present disclosure (6) is the resin composition according to the present disclosure (4) or (5), wherein the amorphous resin (A) is a thermoplastic polyimide.
[0012] The present disclosure (7) is the resin composition according to any one of the present disclosures (4) to (6), in which the amorphous resin (A) is polyetherimide.
[0013] The present disclosure (8) is the resin composition according to any one of the present disclosures (1) to (7), wherein the fluorine-containing copolymer (B) has a melting point of 200 to 323°C.
[0014] The present disclosure (9) is directed to a fluorine-containing copolymer (B) comprising tetrafluoroethylene and the following general formula (1): CF 2 =CF-Rf 1 (1) (In the formula, Rf 1 -CF 3 ORf 2 Represents Rf 2 represents a perfluoroalkyl group having 1 to 5 carbon atoms. The resin composition according to any one of the present disclosures (1) to (8), which is a copolymer of a perfluoroethylenically unsaturated compound represented by the formula:
[0015] The present disclosure (10) is the resin composition according to the present disclosure (9), wherein the perfluoroethylenically unsaturated compound is at least one selected from the group consisting of hexafluoropropylene and perfluoro(alkyl vinyl ether).
[0016] The present disclosure (11) is the resin composition according to the present disclosure (9) or (10), wherein the fluorine-containing copolymer (B) is at least one selected from the group consisting of a tetrafluoroethylene / hexafluoropropylene copolymer and a tetrafluoroethylene / perfluoro(alkyl vinyl ether) copolymer.
[0017] The present disclosure (12) relates to a method for manufacturing the amorphous resin (A) having a thickness of 2.0 μm or less, wherein r1 and r2 are measured for the amorphous resin (A), and r2 is 2.0 μm or less. In the resin composition according to any one of the present disclosures (1) to (11), when r1 and r2 are values measured for the fluorine-containing copolymer (B), r2 is 1.0 μm or less.
[0018] The present disclosure (13) is the resin composition according to any one of the present disclosures (1) to (12), wherein the mass ratio (A):(B) of the amorphous resin (A) to the fluorine-containing copolymer (B) is 99:1 to 10:90.
[0019] The present disclosure (14) is the resin composition according to the present disclosure (13), wherein the mass ratio (A):(B) is 80:20 to 20:80.
[0020] The present disclosure (15) is the resin composition according to any one of the present disclosures (1) to (14), which has a phase structure composed of a continuous phase and a dispersed phase, and a component of the continuous phase is present in the dispersed phase.
[0021] The present disclosure (16) is a resin composition having a phase structure in which one of the thermoplastic resin (X) and the fluorinated copolymer (B) is a continuous phase and the other is a dispersed phase, and components of the continuous phase are present in the dispersed phase.
[0022] The present disclosure (17) is a method for producing a resin composition according to any one of the present disclosures (1) to (15), comprising a step of melt-kneading an amorphous resin (A) and a fluorinated copolymer (B) at a shear rate calculated from the following formula 1 of 600 / sec or more: Equation 1: γ = πDr / C γ: Shear rate ( / sec) D: Screw outer diameter (mm) r: screw rotation speed (rpm) C: Tip clearance (mm)
[0023] The present disclosure (18) is the production method according to the present disclosure (17), in which the shear rate is 800 / sec or more and 3000 / sec or less, the melt-kneading time is 5 to 300 seconds, and the melt-kneading temperature is 260 to 400°C.
[0024] The present disclosure (19) is a pellet obtained by molding the resin composition according to any one of the present disclosures (1) to (16).
[0025] The present disclosure (20) is a molded article formed from the resin composition of any one of the present disclosures (1) to (16).
[0026] The present disclosure (21) has a Charpy impact strength of 5 kJ / m as measured by an impact tester in accordance with ASTM D6110-02. 2 The above is the molded product according to the present disclosure (20).
[0027] The present disclosure (22) is a molded article according to the present disclosure (20) or (21) used for materials requiring dielectric properties.
[0028] The present disclosure (23) is a molded article according to any one of the present disclosures (20) to (22), which is a material for a high-frequency circuit board.
[0029] The present disclosure (24) is a laminate including a metal foil and the molded article according to any one of the present disclosures (20) to (23).
[0030] The present disclosure (25) is the laminate according to the present disclosure (24), wherein the metal foil is copper. Effect of the Invention
[0031] According to the present disclosure, a molded article having excellent impact strength can be produced. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0032] The first resin composition of the present disclosure comprises an amorphous resin (A) belonging to super engineering plastics and a fluorine-containing copolymer (B), and the ratio r2 / r1 of the average dispersed particle size r1 of the amorphous resin (A) or the fluorine-containing copolymer (B) to the average dispersed particle size r2 of the amorphous resin (A) or the fluorine-containing copolymer (B) after measuring the melt flow rate (MFR) at 380°C or a temperature at which the resin composition melts, under a load of 5000g, and preheating for 5 minutes according to ASTM D1238 is less than 1.70 (wherein r1 and r2 are measured for the same resin or the same copolymer).
[0033] Since a fluorine-containing copolymer has low compatibility with other resins, a resin composition obtained by mixing a fluorine-containing copolymer and another resin tends to have a tendency for dispersed particles to aggregate during molding, resulting in deterioration of physical properties. As a result of intensive studies conducted by the present inventors to solve the above-mentioned problems, the present inventors have focused on the shear rate during kneading and found that a resin composition capable of suppressing aggregation of dispersed particles during molding can be produced by effectively applying shear during kneading. The first resin composition of the present disclosure has the above-mentioned constitution, and thus can suppress the aggregation of dispersed particles during molding, and as a result, can maintain good mechanical properties even after molding, and can produce molded products with excellent impact strength. In addition, flexibility and electrical properties can be improved compared to the case of the amorphous resin (A) alone.
[0034] In the first resin composition of the present disclosure, it is preferable that the fluorinated copolymer (B) is dispersed in the form of particles in the amorphous resin (A), or that the amorphous resin (A) is dispersed in the form of particles in the fluorinated copolymer (B). Usually, in a form in which the fluorine-containing copolymer (B) is dispersed in the form of particles in the amorphous resin (A), the amorphous resin (A) forms a continuous phase and the fluorine-containing copolymer (B) forms a dispersed phase, and in a form in which the amorphous resin (A) is dispersed in the form of particles in the fluorine-containing copolymer (B), the fluorine-containing copolymer (B) forms a continuous phase and the amorphous resin (A) forms a dispersed phase. In a case in which the content of the amorphous resin (A) is greater than the content of the fluorine-containing copolymer (B), the former form is generally observed, and in a case in which the content of the amorphous resin (A) is less than the content of the fluorine-containing copolymer (B), the latter form is generally observed.
[0035] As long as r1 and r2 are measured for the same resin or the same copolymer, they may be measured for the amorphous resin (A) or for the fluorine-containing copolymer (B). In addition, r1 and r2 are usually measured for the resin or copolymer forming the dispersed phase. Therefore, in a form in which the fluorine-containing copolymer (B) is dispersed in particulate form in the amorphous resin (A), r1 and r2 are measured for the fluorine-containing copolymer (B), and in a form in which the amorphous resin (A) is dispersed in particulate form in the fluorine-containing copolymer (B), r1 and r2 are measured for the amorphous resin (A).
[0036] In the first resin composition of the present disclosure, r2 / r1 is less than 1.70. When the amorphous resin (A) or the fluorine-containing copolymer (B) dispersed in particulate form aggregates due to MFR measurement, r2 / r1 becomes large. Therefore, r2 / r1 being less than 1.70 indicates that the particles of the amorphous resin (A) or the fluorine-containing copolymer (B) are less likely to aggregate after MFR measurement. The ratio r2 / r1 may be less than 1.70, but is preferably 1.50 or less, more preferably 1.40 or less, since a molded product having even better impact strength can be obtained. The lower limit is not particularly limited, but may be, for example, 1.0.
[0037] When r1 and r2 are measured for the amorphous resin (A), r2 is preferably 2.5 μm or less, more preferably 2.0 μm or less, and even more preferably 1.5 μm or less. If r2 is within the above range, a molded product having better impact strength can be obtained. The lower limit is not particularly limited, but may be, for example, 0.01 μm.
[0038] When r1 and r2 are measured for the fluorine-containing copolymer (B), r2 is preferably 2.0 μm or less, more preferably 1.5 μm or less, even more preferably 1.0 μm or less, and particularly preferably 0.5 μm or less. If r2 is within the above range, a molded product with even better impact strength can be obtained. The lower limit is not particularly limited, but may be, for example, 0.01 μm.
[0039] r1 and r2 are determined according to the following procedure. First, a piece cut from a strand or pellet of the resin composition is cut perpendicular to the extrusion direction, and the cross section is observed with a confocal laser microscope. The obtained microscopic image is analyzed using image analysis software (Image J). Then, the dispersed phase is selected, and the circle equivalent diameter is obtained. The circle equivalent diameters of 20 dispersed phase particles are calculated, and the average is taken as r1 (average dispersed particle diameter). r2 is determined by carrying out the same procedure on strands or pellets of the resin composition after MFR measurement.
[0040] The amorphous resin (A) is a resin belonging to super engineering plastics. For example, a resin having a glass transition temperature within a specific range or a resin having a continuous use temperature within a specific range can be used as such a resin. As the amorphous resin (A), one type or two or more types can be used.
[0041] The glass transition temperature of the amorphous resin (A) is preferably 190°C or higher, more preferably 200°C or higher, and even more preferably 210°C or higher, and is preferably 290°C or lower, more preferably 250°C or lower, and even more preferably 220°C or lower. In this specification, the glass transition temperature is measured in accordance with JIS K7121 using a differential scanning calorimetry (DSC) device under the condition of a temperature rise rate of 20° C. / min.
[0042] The continuous use temperature of the amorphous resin (A) is preferably 140° C. or higher, more preferably 160° C. or higher, and even more preferably 170° C. or higher. There is no particular upper limit, and the higher the temperature, the better. For example, it may be 260° C. In this specification, the continuous use temperature is the temperature at which a physical property value deteriorates by 50% from its initial value when left in the atmosphere at a constant temperature for 40,000 hours, and is measured in accordance with UL746B.
[0043] The amorphous resin (A) preferably has an imide structure. An example of the amorphous resin (A) having an imide structure is polyimide (PI). In this specification, the polyimide is a polycondensate having an imide structure in the main chain. In view of excellent moldability, the polyimide is preferably a thermoplastic polyimide (TPI), and more preferably a polyetherimide (PEI).
[0044] It is also preferable that the amorphous resin (A) has an amide structure and an imide structure. An example of the amorphous resin (A) having an amide structure and an imide structure is polyamideimide (PAI). In this specification, polyamideimide is a polycondensate having an amide structure and an imide structure in the main chain.
[0045] The amorphous resin (A) may be a resin other than the above-mentioned polyimide and polyamideimide, for example, polysulfone (PSU), polyethersulfone (PES), polyphenylsulfone (PPSU), and polyarylate (PAR).
[0046] The melt flow rate (MFR) of the amorphous resin (A) is preferably 1 to 150 g / 10 min, more preferably 5 to 130 g / 10 min, and even more preferably 10 to 100 g / 10 min, under the measurement conditions of 380° C. or the temperature at which the amorphous resin (A) melts and a load of 5000 g. By being in the above range, a molded product having even more excellent impact strength can be obtained. The MFR of the amorphous resin (A) is a value obtained by measuring the temperature of 380° C. or the temperature at which the amorphous resin (A) melts under a load of 5000 g in accordance with ASTM D1238 after a preheating time of 5 minutes. The temperature at which the amorphous resin (A) melts may be, for example, 400° C.
[0047] The fluorine-containing copolymer (B) is, for example, a polymer having a polymerization unit based on at least one fluorine-containing ethylenic monomer. The fluorine-containing copolymer (B) is preferably a melt-processable fluororesin. As the fluorine-containing copolymer (B), one type may be used, or two or more types may be used.
[0048] Examples of the fluorine-containing copolymer (B) include tetrafluoroethylene (TFE) / hexafluoropropylene (HFP) copolymer [FEP], TFE / HFP / perfluoro(alkyl vinyl ether) (PAVE) copolymer, TFE / PAVE copolymer [PFA], ethylene (Et) / TFE copolymer, Et / TFE / HFP copolymer, polychlorotrifluoroethylene [PCTFE], chlorotrifluoroethylene (CTFE) / TFE copolymer, CTFE / TFE / PAVE copolymer, Et / CTFE copolymer, TFE / vinylidene fluoride (VdF) copolymer, VdF / HFP / TFE copolymer, VdF / HFP copolymer, polyvinylidene fluoride (PVdF), and polyvinyl fluoride (PVF). In addition, if it is melt-processable, it is also possible to use low molecular weight polytetrafluoroethylene (PTFE). As the PAVE, those having an alkyl group having 1 to 6 carbon atoms are preferable, and examples thereof include perfluoro(methyl vinyl ether), perfluoro(ethyl vinyl ether), perfluoro(propyl vinyl ether), and perfluoro(butyl vinyl ether).
[0049] As the fluorine-containing copolymer (B), a copolymer containing tetrafluoroethylene (TFE) and a fluoropolymer represented by the following general formula (1): CF 2 =CF-Rf 1 (1) (In the formula, Rf 1 -CF 3 ORf 2 Represents Rf 2 Rf represents a perfluoroalkyl group having 1 to 5 carbon atoms. 1 Ga-ORf 2 If Rf 2 is preferably a perfluoroalkyl group having 1 to 3 carbon atoms.
[0050] As the perfluoroethylenically unsaturated compound represented by general formula (1), at least one selected from the group consisting of hexafluoropropylene (HFP) and perfluoro(alkyl vinyl ether) (PAVE) is preferable, since it is possible to obtain a molded article having even better impact strength, at least one selected from the group consisting of hexafluoropropylene (HFP), perfluoro(methyl vinyl ether) (PMVE), perfluoro(ethyl vinyl ether) (PEVE) and perfluoro(propyl vinyl ether) (PPVE) is more preferable, and at least one selected from the group consisting of hexafluoropropylene and perfluoro(propyl vinyl ether) is even more preferable.
[0051] The fluorocopolymer (B) is preferably at least one selected from the group consisting of FEP and PFA, since this allows the production of molded articles with even more excellent impact strength.
[0052] The fluorine-containing copolymer (B) is preferably composed of 98-75% by mass of polymerization units based on TFE (TFE units) and 2-25% by mass of a perfluoroethylenically unsaturated compound represented by general formula (1) based on all polymerization units. The lower limit of the content of TFE constituting the fluorine-containing copolymer (B) is more preferably 77% by mass, further preferably 80% by mass, particularly preferably 83% by mass, and particularly preferably 85% by mass. The upper limit of the content of TFE constituting the above fluorine-containing copolymer (B) is more preferably 97% by mass, further preferably 95% by mass, and particularly preferably 92% by mass. The lower limit of the content of the perfluoroethylenically unsaturated compound represented by general formula (1) constituting the fluorine-containing copolymer (B) is more preferably 3% by mass, further preferably 5% by mass. The upper limit of the content of the perfluoroethylenically unsaturated compound represented by general formula (1) constituting the fluorine-containing copolymer (B) is more preferably 23% by mass, further preferably 20% by mass, particularly preferably 17% by mass, and particularly preferably 15% by mass. The fluorine-containing copolymer (B) is preferably a copolymer consisting only of TFE and a perfluoroethylenic compound represented by the general formula (1).
[0053] The melt flow rate (MFR) of the fluorocopolymer (B) is preferably 0.1 to 100 g / 10 min, more preferably 0.5 to 80 g / 10 min, and even more preferably 0.5 to 70 g / 10 min. Within the above range, a molded product having even more excellent impact strength can be obtained. The MFR of the fluorine-containing copolymer (B) may be 7 g / 10 min or more. The MFR of the fluorocopolymer (B) is measured using a melt indexer under conditions of 380°C or the melting temperature of the fluorocopolymer (B) or higher and a load of 5000 g in accordance with ASTM D1238. The temperature higher than the melting temperature of the fluorocopolymer (B) may be, for example, 400°C.
[0054] The melting point of the fluorocopolymer (B) is preferably 200° C. or higher, more preferably 220° C. or higher, and even more preferably 240° C. or higher, since this can improve the heat resistance of the resulting molded article. Also, the melting point is preferably 323° C. or lower, more preferably 320° C. or lower, and even more preferably 315° C. or lower, since this can suppress thermal deterioration during kneading. The melting point of the fluororesin (II) was determined as the temperature corresponding to the maximum value in the heat of fusion curve when the temperature was increased at a rate of 10° C. / min using a differential scanning calorimeter (DSC).
[0055] The fluorine-containing copolymer (B) may be one which has been treated with fluorine gas or ammonia by a known method.
[0056] In the first resin composition of the present disclosure, a fluorine-containing copolymer containing a reactive functional group can be used from the viewpoint of suppressing aggregation and aggregation of the fluorine-containing copolymer phase (B) and facilitating control of the rate of change in the dispersed particle size within a desired range. The reactive functional group is not particularly limited, and specifically includes vinyl group, epoxy group, carboxy group, acid anhydride group, ester group, aldehyde group, carbonyldioxy group, haloformyl group, alkoxycarbonyl group, amino group, hydroxyl group, styryl group, methacryl group, acrylic group, ureido group, mercapto group, sulfide group, isocyanate group, hydrolyzable silyl group, etc., among which at least one selected from the group consisting of epoxy group, carboxy group, acid anhydride group, amino group and hydroxyl group is preferred, and at least one selected from the group consisting of carboxy group and acid anhydride group is more preferred. Two or more of these reactive functional groups may be contained. In addition, the reactive functional group may be introduced into either the main chain terminal or the side chain of the fluorine-containing copolymer.
[0057] The amount of the functional group in the fluorine-containing copolymer containing a reactive functional group is not particularly limited, but from the viewpoints of sufficiently proceeding with the reaction and preventing deterioration of fluidity, it is preferably in the range of 0.01 mol % to 15 mol %.
[0058] The fluorine-containing copolymer (B) may not have a reactive functional group in the structure. The fluorine-containing copolymer (B) not having a reactive functional group in the structure can be obtained, for example, by fluorinating the terminals.
[0059] In the first resin composition of the present disclosure, the mass ratio (A):(B) of the amorphous resin (A) to the fluorine-containing copolymer (B) is not particularly limited, but is preferably, for example, 99:1 to 10:90. In this mass ratio, the upper limit of the amorphous resin (A) is preferably 95, more preferably 80, and the lower limit is preferably 20, more preferably 35, and even more preferably 40. The upper limit of the fluorine-containing copolymer (B) is preferably 80, more preferably 65, and even more preferably 60, and the lower limit is preferably 5, more preferably 20.
[0060] The first resin composition of the present disclosure has a phase structure composed of a continuous phase and a dispersed phase, and it is preferable that the continuous phase component is present in the dispersed phase, thereby making it possible to obtain a molded product having even more excellent impact strength. The amorphous resin (A) may be the continuous phase and the fluorine-containing copolymer (B) may be the dispersed phase, or vice versa.
[0061] In the first resin composition of the present disclosure, the method for confirming the components in the dispersed phase is not particularly limited, but for example, infrared spectroscopy (IR) can be used. More specifically, when IR is performed on the dispersed phase isolated from the resin composition according to JIS K0117:2017, if not only the peaks of the components of the dispersed phase but also the peaks of the components of the continuous phase are detected, the components of the continuous phase are present in the dispersed phase. The amount of the continuous phase component present in the dispersed phase is not particularly limited.
[0062] The first resin composition of the present disclosure preferably has a melt flow rate (MFR) of 0.1 to 200 g / 10 min at 380° C. or the temperature at which the resin composition melts, and more preferably 1 to 150 g / 10 min. A resin composition having an MFR within the above range has better fluidity. If the MFR is smaller than the above range, the moldability may be poor. If the MFR is larger than the above range, the desired performance may not be achieved. The MFR of the first resin composition of the present disclosure is a value obtained by measuring in accordance with ASTM D1238 with a preheating time of 5 minutes, a temperature of 380°C or a temperature at which the resin composition melts, and a load of 5000 g. The temperature at which the resin composition melts may be, for example, 400°C.
[0063] The first resin composition of the present disclosure preferably has a relative dielectric constant of 3.0 or less, more preferably 2.9 or less, and even more preferably 2.7 or less. There is no particular lower limit to the relative dielectric constant, but it is preferably 2.1 or more. The relative dielectric constant is a value measured by a cavity resonator perturbation method.
[0064] The first resin composition of the present disclosure preferably has a dielectric loss tangent of 0.006 or less, more preferably 0.005 or less, and even more preferably 0.004 or less. The lower limit of the dielectric loss tangent is not particularly limited, but is preferably 0.0001 or more. The dielectric loss tangent is a value measured by a cavity resonator perturbation method.
[0065] The first resin composition of the present disclosure may contain components other than the amorphous resin (A) and the fluorine-containing copolymer (B) as necessary. The components other than the amorphous resin (A) and the fluorine-containing copolymer (B) are not particularly limited, but may include whiskers such as potassium titanate, glass fibers, asbestos fibers, carbon fibers, ceramic fibers, potassium titanate fibers, aramid fibers, and other high-strength fibers, as well as fibrous reinforcing materials; inorganic fillers such as talc, mica, clay, carbon powder, graphite, artificial graphite, natural graphite, and glass beads; colorants; flame retardants and other commonly used inorganic or organic fillers; lubricants such as silicone oil and molybdenum disulfide; pigments; conductive agents such as carbon black; impact resistance improvers such as rubber; lubricants such as magnesium stearate; ultraviolet absorbers such as benzotriazole compounds; foaming agents such as boron nitride; and other additives. These additives may be added to the raw material amorphous resin (A) or the raw material fluorocopolymer (B) within the range not impairing the effects of the present application. Furthermore, when the amorphous resin (A) and the fluorocopolymer (B) are kneaded, they may be added to the molten raw materials by a side feed method or the like within the range not impairing the effects of the present application.
[0066] Fibrous filler (C) The first resin composition of the present disclosure further preferably contains a fibrous filler. Examples of the fibrous filler used in the resin composition of the present disclosure include fibrous inorganic fillers such as glass fiber, carbon fiber, carbon milled fiber, metal fiber, asbestos, rock wool, ceramic fiber, slag fiber, potassium titanate whisker, boron whisker, aluminum borate whisker, calcium carbonate whisker, titanium oxide whisker, wollastonite, xonotlite, palygorskite (attapulgite), and sepiolite, fibrous heat-resistant organic fillers such as aramid fiber, polyimide fiber, and polybenzothiazole fiber, as well as fibrous fillers in which the surface of these fillers is coated with a different material such as a metal or metal oxide. Examples of fillers in which a different material is surface-coated include metal-coated glass fiber and metal-coated carbon fiber. The method for coating the surface of a different material is not particularly limited, and examples thereof include various known plating methods (e.g., electrolytic plating, electroless plating, hot-dip plating, etc.), vacuum deposition, ion plating, CVD (e.g., thermal CVD, MOCVD, plasma CVD, etc.), PVD, and sputtering. Among these fibrous fillers, at least one selected from the group consisting of glass fiber, carbon fiber, carbon milled fiber, and aramid fiber is preferred, and at least one selected from the group consisting of glass fiber and carbon fiber is more preferred. The fiber diameter of the fibrous filler is preferably in the range of 0.1 to 20 μm. The upper limit of the fiber diameter is more preferably 18 μm, and even more preferably 15 μm. Meanwhile, the lower limit of the fiber diameter is more preferably 1 μm, and even more preferably 6 μm. The fiber diameter here refers to the number average fiber diameter. The number average fiber diameter is a value calculated from an image obtained by observing, with a scanning electron microscope, the residue collected after dissolving the molded product in a solvent or decomposing the resin with a basic compound, and the ashing residue collected after ashing in a crucible. When the fibrous filler used in the resin composition of the present disclosure is a glass fiber, the glass composition of the glass fiber is not particularly limited and may be any of various glass compositions such as A-glass, C-glass, and E-glass. Such a glass filler may contain TiO 2 , S.O. 3 , and P 2 O 5The glass fibers may contain components such as fluorine, fluorine-based resin ... The flat cross-section glass fiber is a glass fiber having an average major axis of the fiber cross-section of preferably 10 to 50 μm, more preferably 15 to 40 μm, and even more preferably 20 to 35 μm, and an average major axis to minor axis ratio (major axis / minor axis) of preferably 1.5 to 8, more preferably 2 to 6, and even more preferably 2.5 to 5. When a flat cross-section glass fiber having an average major axis to minor axis ratio in this range is used, the anisotropy is greatly improved compared to when a noncircular cross-section fiber having a ratio of less than 1.5 is used. In addition, examples of the flat cross-section shape include noncircular cross-section shapes such as ellipse, eyebrow, and trilobe, or shapes similar thereto, in addition to flat. Among them, a flat shape is preferable from the viewpoint of improving mechanical strength and low anisotropy. The ratio of the average fiber length to the average fiber diameter (aspect ratio) of the flat cross section glass fiber is preferably 2 to 120, more preferably 2.5 to 70, and even more preferably 3 to 50. If the ratio of the fiber length to the average fiber diameter is less than 2, the effect of improving the mechanical strength may be small, and if the ratio of the fiber length to the average fiber diameter exceeds 120, the anisotropy may be large and the appearance of the molded product may be deteriorated. The average fiber diameter of the flat cross section glass fiber refers to the number average fiber diameter when the flat cross section shape is converted into a perfect circle of the same area. The average fiber length refers to the number average fiber length in the resin composition of the present disclosure.The number average fiber length is a value calculated by an image analyzer from an image obtained by observing under an optical microscope the residue of the filler collected after high-temperature incineration of the molded product, dissolution with a solvent, decomposition with a chemical, etc. The value is calculated by using the fiber diameter as a guide and excluding fibers having a length less than the diameter. The mass ratio of the fibrous filler (C) is preferably from 0 to 50 mass %, more preferably from 5 to 40 mass %, and even more preferably from 10 to 30 mass %, relative to the resin composition of the present disclosure.
[0067] (Other additives) In the first resin composition of the present disclosure, additives used for improving the design, etc. are advantageously used in the resin composition. These additives will be specifically described below.
[0068] Dyes and pigments (D) The first resin composition of the present disclosure further contains various dyes and pigments, and can provide molded articles that exhibit a variety of designs. Examples of dyes and pigments used in the resin composition of the present disclosure include perylene dyes, coumarin dyes, thioindigo dyes, anthraquinone dyes, thioxanthone dyes, ferrocyanides such as Prussian blue, perinone dyes, quinoline dyes, quinacridone dyes, dioxazine dyes, isoindolinone dyes, and phthalocyanine dyes. Furthermore, the resin composition of the present disclosure can be blended with a metallic pigment to obtain a better metallic color. Aluminum powder is suitable as the metallic pigment. In addition, by blending a fluorescent brightener or other fluorescent dye that emits light, a better design effect that makes use of the luminous color can be imparted.
[0069] Compounds with heat absorbing properties (E) The first resin composition of the present disclosure may contain a compound having heat absorbing ability. Suitable examples of such compounds include phthalocyanine-based near infrared absorbing agents, metal oxide-based near infrared absorbing agents such as ATO, ITO, iridium oxide, ruthenium oxide, immonium oxide, and titanium oxide, various metal compounds having excellent near infrared absorbing ability such as metal boride-based and tungsten oxide-based near infrared absorbing agents such as lanthanum boride, cerium boride, and tungsten boride, and carbon fillers. As such phthalocyanine-based near infrared absorbing agents, for example, MIR-362 manufactured by Mitsui Chemicals, Inc. is commercially available and easily available. Examples of carbon fillers include carbon black, graphite (both natural and artificial), and fullerene, and preferably carbon black and graphite. These can be used alone or in combination of two or more. The content of the phthalocyanine-based near infrared absorbing agent is preferably 0.0005 to 0.2 parts by mass, more preferably 0.0008 to 0.1 parts by mass, and even more preferably 0.001 to 0.07 parts by mass, relative to 100 parts by mass of the resin composition of the present disclosure. The contents of the metal oxide-based near infrared absorbing agent, the metal boride-based near infrared absorbing agent, and the carbon filler are preferably in the range of 0.1 to 200 ppm (mass ratio), and more preferably in the range of 0.5 to 100 ppm, in the resin composition of the present disclosure.
[0070] Highly light-reflective white pigment (F) The first resin composition of the present disclosure can be blended with a highly light-reflective white pigment to impart a light-reflecting effect. Titanium dioxide (particularly titanium dioxide treated with an organic surface treatment agent such as silicone) pigment is particularly preferred as such a white pigment. The content of such highly light-reflective white pigment is preferably 3 to 30 parts by mass, more preferably 8 to 25 parts by mass, per 100 parts by mass of the resin composition. Two or more types of highly light-reflective white pigments can be used in combination.
[0071] Ultraviolet absorber (G) The first resin composition of the present disclosure can be blended with an ultraviolet absorbing agent to impart weather resistance.Specific examples of such ultraviolet absorbing agents include benzophenone-based agents such as 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-octoxybenzophenone, 2-hydroxy-4-benzyloxybenzophenone, 2-hydroxy-4-methoxy-5-sulfoxybenzophenone, 2,2'-dihydroxy-4-methoxybenzophenone, 2,2',4,4'-tetrahydroxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxy-5-sodiumsulfoxybenzophenone, bis(5-benzoyl-4-hydroxy-2-methoxyphenyl)methane, 2-hydroxy-4-n-dodecyloxybenzophenone, and 2-hydroxy-4-methoxy-2'-carboxybenzophenone.Specific examples of the ultraviolet absorber include benzotriazole-based ultraviolet absorbers such as 2-(2-hydroxy-5-methylphenyl)benzotriazole, 2-(2-hydroxy-5-tert-octylphenyl)benzotriazole, 2-(2-hydroxy-3,5-dicumylphenyl)phenylbenzotriazole, 2-(2-hydroxy-3-tert-butyl-5-methylphenyl)-5-chlorobenzotriazole, 2,2'-methylenebis[4-(1,1,3,3-tetramethylbutyl)-6-(2H-benzotriazol-2-yl)phenol], 2-(2-hydroxy-3,5-di-tert-butylphenyl)benzotriazole, 2-(2-hydroxy-3,5-di-tert-butylphenyl)-5-chlorobenzotriazole, 2-(2-hydroxy-3,5-di-tert-amylphenyl)benzotriazole, 2-(2-hydroxy-5-tert-octylphenyl)benzotriazole, Examples of the copolymer include 2-hydroxyphenyl-2H-benzotriazole skeleton such as 2-(2-hydroxy-5-acryloxyethylphenyl)-2H-benzotriazole, 2-(2-hydroxy-5-tert-butylphenyl)-benzotriazole, 2-(2-hydroxy-4-octoxyphenyl)-benzotriazole, 2,2'-methylenebis(4-cumyl-6-benzotriazolephenyl), 2,2'-p-phenylenebis(1,3-benzoxazin-4-one), and 2-[2-hydroxy-3-(3,4,5,6-tetrahydrophthalimidomethyl)-5-methylphenyl]benzotriazole, as well as copolymers of 2-(2'-hydroxy-5-methacryloxyethylphenyl)-2H-benzotriazole and vinyl monomers copolymerizable with the monomer, and copolymers of 2-(2'-hydroxy-5-acryloxyethylphenyl)-2H-benzotriazole and vinyl monomers copolymerizable with the monomer.Specific examples of the ultraviolet absorber include, in the hydroxyphenyltriazine series, 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-hexyloxyphenol, 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-methyloxyphenol, 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-ethyloxyphenol, 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-propyloxyphenol, and 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-butyloxyphenol.Further examples include compounds in which the phenyl group of the above-mentioned compounds is a 2,4-dimethylphenyl group, such as 2-(4,6-bis(2,4-dimethylphenyl)-1,3,5-triazin-2-yl)-5-hexyloxyphenol. Specific examples of ultraviolet absorbents include cyclic iminoesters such as 2,2'-p-phenylenebis(3,1-benzoxazine-4-one), 2,2'-m-phenylenebis(3,1-benzoxazine-4-one), and 2,2'-p,p'-diphenylenebis(3,1-benzoxazine-4-one). Specific examples of ultraviolet absorbents include cyanoacrylates such as 1,3-bis-([(2'-cyano-3',3'-diphenylacryloyl)oxy]-2,2-bis-[(2-cyano-3,3-diphenylacryloyl)oxy]methyl)propane and 1,3-bis-[(2-cyano-3,3-diphenylacryloyl)oxy]benzene. Furthermore, the ultraviolet absorber may be a polymer type ultraviolet absorber obtained by copolymerizing such an ultraviolet absorbing monomer and / or a light stable monomer with a monomer such as an alkyl (meth)acrylate by adopting a structure of a radically polymerizable monomer compound. Suitable examples of the ultraviolet absorbing monomer include compounds containing a benzotriazole skeleton, a benzophenone skeleton, a triazine skeleton, a cyclic imino ester skeleton, and a cyanoacrylate skeleton in the ester substituent of a (meth)acrylic acid ester.Among the above, benzotriazole and hydroxyphenyltriazine are preferred in terms of ultraviolet absorbing ability, and cyclic iminoester and cyanoacrylate are preferred in terms of heat resistance and color. Specific examples include "Chemisorb 79" from Chemipro Chemical Co., Ltd. and "Tinuvin 234" from BASF Japan Ltd. The ultraviolet absorbing agents may be used alone or in a mixture of two or more kinds. The content of the ultraviolet absorber is preferably 0.01 to 3 parts by mass, more preferably 0.01 to 1 part by mass, still more preferably 0.05 to 1 part by mass, and particularly preferably 0.05 to 0.5 part by mass, relative to 100 parts by mass of the resin composition of the present disclosure.
[0072] Antistatic agent (H) The first resin composition of the present disclosure may require antistatic performance, and in such a case, it is preferable to include an antistatic agent. Examples of such antistatic agents include (1) organic sulfonate phosphonium salts such as arylsulfonate phosphonium salts, such as dodecylbenzenesulfonate phosphonium salts, and alkylsulfonate phosphonium salts, as well as borate phosphonium salts such as tetrafluoroborate phosphonium salts. The content of the phosphonium salt is appropriately 5 parts by mass or less, preferably 0.05 to 5 parts by mass, more preferably 1 to 3.5 parts by mass, and even more preferably 1.5 to 3 parts by mass, relative to 100 parts by mass of the resin composition of the present disclosure. Examples of antistatic agents include (2) organic sulfonate alkali (earth) metal salts such as lithium organic sulfonate, sodium organic sulfonate, potassium organic sulfonate, cesium organic sulfonate, rubidium organic sulfonate, calcium organic sulfonate, magnesium organic sulfonate, and barium organic sulfonate. As mentioned above, such metal salts are also used as flame retardants. More specifically, the metal salt may be, for example, a metal salt of dodecylbenzenesulfonic acid or a metal salt of perfluoroalkanesulfonic acid. The content of the alkali (earth) metal salt of organic sulfonate is suitably 0.5 parts by mass or less, preferably 0.001 to 0.3 parts by mass, and more preferably 0.005 to 0.2 parts by mass, relative to 100 parts by mass of the resin composition of the present disclosure. In particular, alkali metal salts such as potassium, cesium, and rubidium are suitable. The antistatic agent may be, for example, (3) an organic ammonium sulfonate such as an alkylsulfonate ammonium salt and an arylsulfonate ammonium salt. The amount of the ammonium salt is suitably 0.05 parts by mass or less per 100 parts by mass of the resin composition of the present disclosure. The antistatic agent may be, for example, (4) a polymer containing a poly(oxyalkylene) glycol component as a constituent component, such as polyether ester amide. The amount of the polymer is suitably 5 parts by mass or less per 100 parts by mass of the resin composition of the present disclosure.
[0073] Filler (I) The first resin composition of the present disclosure can be blended with various fillers known as reinforcing fillers other than fibrous fillers. Examples of such fillers include various plate-like fillers and granular fillers. Here, the plate-like filler is a filler whose shape is plate-like (including those with uneven surfaces and those with curved plates). The granular filler is a filler whose shape is other than these, including those with irregular shapes. Preferred examples of the plate-like filler include glass flakes, talc, mica, kaolin, metal flakes, carbon flakes, and graphite, as well as plate-like fillers obtained by surface-coating these fillers with different materials such as metals and metal oxides. The particle size is preferably in the range of 0.1 to 300 μm. The particle size refers to the value of the median diameter (D50) of the particle size distribution measured by the X-ray transmission method, which is one of the liquid phase precipitation methods, in the region up to about 10 μm, the value of the median diameter (D50) of the particle size distribution measured by the laser diffraction / scattering method in the region of 10 to 50 μm, and the value of the vibration sieving method in the region of 50 to 300 μm. The particle size is the particle size in the resin composition. The plate-like filler may be surface-treated with various coupling agents such as silane-, titanate-, aluminate-, and zirconate-based coupling agents, or may be in the form of granules that have been bundled or compressed with various resins such as olefin-, styrene-, acrylic-, polyester-, epoxy-, and urethane-based resins, or higher fatty acid esters.
[0074] Other resins and elastomers (J) In the first resin composition of the present disclosure, other resins or elastomers can be used in small proportions in the range where the effects of the present disclosure are exhibited, instead of a part of the resin components, as long as the effects of the present disclosure are not impaired. The amount of the other resins or elastomers is preferably 20 parts by mass or less, more preferably 10 parts by mass or less, even more preferably 5 parts by mass or less, and most preferably 3 parts by mass or less, relative to 100 parts by mass of the resin composition of the present disclosure. Examples of such other resins include polyester resins such as polyethylene terephthalate and polybutylene terephthalate, polyamide resins, polyimide resins, polyetherimide resins, polyurethane resins, silicone resins, polyphenylene ether resins, polyphenylene sulfide resins, polysulfone resins, polymethacrylate resins, phenolic resins, and epoxy resins. Examples of elastomers include isobutylene / isoprene rubber, styrene / butadiene rubber, ethylene / propylene rubber, acrylic elastomers, polyester elastomers, polyamide elastomers, core-shell elastomers such as MBS (methyl methacrylate / styrene / butadiene) rubber, MB (methyl methacrylate / butadiene) rubber, MAS (methyl methacrylate / acrylonitrile / styrene) rubber, fluororubber, and fluorine-containing elastomers.
[0075] Other Additives (K) The first resin composition of the present disclosure may contain other flow modifiers, antibacterial agents, dispersants such as liquid paraffin, photocatalytic antifouling agents, photochromic agents, and the like.
[0076] In the first resin composition of the present disclosure, the total content of the amorphous resin (A) and the fluorine-containing copolymer (B) is preferably 100% by mass to 50% by mass. If it is less than 50% by mass, sufficient impact strength and flexibility may not be obtained. In addition, in the first resin composition of the present disclosure, the total of the amorphous resin (A) and the fluorinated copolymer (B) may be 90 mass% or more, 95 mass% or more, 99 mass% or more, 99.5 mass% or more, or 99.9 mass% or more.
[0077] The second resin composition of the present disclosure has a phase structure in which one of the thermoplastic resin (X) and the fluorinated copolymer (B) is a continuous phase and the other is a dispersed phase, and components of the continuous phase are present in the dispersed phase.
[0078] The second resin composition of the present disclosure, like the first resin composition of the present disclosure, has the above-mentioned constitution, and thus can suppress the aggregation of dispersed particles during molding, and as a result, can maintain good mechanical properties even after molding, and can produce molded products with excellent impact strength. In addition, flexibility and electrical properties can be improved compared to the form of the thermoplastic resin (X) alone.
[0079] In the second resin composition of the present disclosure, the method for confirming the components in the dispersed phase is not particularly limited, but for example, they can be confirmed by the same method as in the first resin composition of the present disclosure. The amount of the continuous phase component present in the dispersed phase is not particularly limited.
[0080] In the second resin composition of the present disclosure, it is preferable that the fluorinated copolymer (B) is dispersed in the form of particles in the thermoplastic resin (X), or that the thermoplastic resin (X) is dispersed in the form of particles in the fluorinated copolymer (B). Usually, in a form in which the fluorine-containing copolymer (B) is dispersed in the form of particles in the thermoplastic resin (X), the thermoplastic resin (X) forms a continuous phase and the fluorine-containing copolymer (B) forms a dispersed phase, and in a form in which the thermoplastic resin (X) is dispersed in the form of particles in the fluorine-containing copolymer (B), the fluorine-containing copolymer (B) forms a continuous phase and the thermoplastic resin (X) forms a dispersed phase. In a case in which the content of the thermoplastic resin (X) is greater than the content of the fluorine-containing copolymer (B), the former form is generally observed, and in a case in which the content of the thermoplastic resin (X) is less than the content of the fluorine-containing copolymer (B), the latter form is generally observed.
[0081] In the second resin composition of the present disclosure, r2 / r1, where r1 is the average dispersed particle size of the thermoplastic resin (X) or the fluorine-containing copolymer (B) and r2 is the average dispersed particle size of the thermoplastic resin (X) or the fluorine-containing copolymer (B) after measuring the melt flow rate (MFR) at 380°C or the temperature at which the resin composition melts, under a load of 5000g, and preheating for 5 minutes according to ASTM D1238, is preferably less than 1.70, more preferably 1.50 or less, and even more preferably 1.40 or less. The lower limit is not particularly limited, but may be, for example, 1.0. In addition, r1 and r2 may be measured for the thermoplastic resin (X) or for the fluorocopolymer (B) as long as they are measured for the same resin or the same copolymer. The temperature equal to or higher than the melting point of the thermoplastic resin (X) may be, for example, 400°C.
[0082] When r1 and r2 are measured for the thermoplastic resin (X), r2 is preferably 2.5 μm or less, more preferably 2.0 μm or less, and even more preferably 1.5 μm or less. If r2 is within the above range, a molded product with even better impact strength can be obtained. The lower limit is not particularly limited, but may be, for example, 0.01 μm.
[0083] When r1 and r2 are measured for the fluorine-containing copolymer (B), r2 is preferably 2.0 μm or less, more preferably 1.5 μm or less, and even more preferably 1.0 μm or less. If r2 is within the above range, a molded product having even better impact strength can be obtained. The lower limit is not particularly limited, but may be, for example, 0.01 μm.
[0084] As the fluorine-containing copolymer (B), the same ones as in the first resin composition of the present disclosure can be used.
[0085] As the thermoplastic resin (X), the amorphous resin (A) explained in the first resin composition of the present disclosure can be suitably used.
[0086] As the thermoplastic resin (X), a resin other than the amorphous resin (A) may be used. Examples of the resin other than the amorphous resin (A) include crystalline resins belonging to super engineering plastics.
[0087] Examples of crystalline resins that belong to the super engineering plastics include aromatic polyether ketone resins, polyphenylene sulfide (PPS), liquid crystal polymers (LCP), and polyphthalamide (PPA).
[0088] In the second resin composition of the present disclosure, the mass ratio (X):(B) of the thermoplastic resin (X) to the fluorine-containing copolymer (B) is not particularly limited, but is preferably, for example, 99:1 to 10:90. In this mass ratio, the upper limit of the thermoplastic resin (X) is preferably 95, more preferably 80, and the lower limit is preferably 20, more preferably 35, and even more preferably 40. The upper limit of the fluorine-containing copolymer (B) is preferably 80, more preferably 65, and even more preferably 60, and the lower limit is preferably 5, more preferably 20.
[0089] In the second resin composition of the present disclosure, the preferred ranges of MFR, relative dielectric constant, and dielectric loss tangent are the same as those in the first resin composition of the present disclosure.
[0090] The second resin composition of the present disclosure may contain components other than the fluorine-containing copolymer (B) and the thermoplastic resin (X) as necessary. As the components other than the fluorine-containing copolymer (B) and the thermoplastic resin (X), those described in the first resin composition of the present disclosure can be used.
[0091] The first resin composition of the present disclosure can be produced, for example, by melt-kneading the amorphous resin (A) and the fluorine-containing copolymer (B) while applying a high shear force, and the second resin composition of the present disclosure can be produced, for example, by melt-kneading the thermoplastic resin (X) and the fluorine-containing copolymer (B) while applying a high shear force. Specifically, the composition can be produced by melt-kneading under conditions where the shear rate calculated from the following formula 1 is 600 / sec or more. The present disclosure also provides a method for producing a resin composition, comprising a step of melt-kneading an amorphous resin (A) and a fluorine-containing copolymer (B) at a shear rate calculated from the following formula 1 of 600 / sec or more. Equation 1: γ = πDr / C γ: Shear rate ( / sec) D: Screw outer diameter (mm) r: screw rotation speed (rpm) C: Tip clearance (mm) The present disclosure also provides a method for producing a resin composition, comprising the step of melt-kneading a thermoplastic resin (X) and a fluorine-containing copolymer (B) at a shear rate calculated from the above formula 1 of 600 / sec or more.
[0092] The shear rate is preferably 700 / sec or more, more preferably 800 / sec or more, even more preferably 900 / sec or more, even more preferably 1400 / sec or more, even more preferably 1500 / sec or more, and even more preferably 1600 / sec or more. This makes the obtained resin composition more excellent in fluidity, and also makes it possible to obtain a molded product with more excellent impact strength. The upper limit is not particularly limited, but may be, for example, 3000 / sec.
[0093] The melt kneading is preferably carried out while applying a high shear force to the amorphous resin (A) and the fluorine-containing copolymer (B), or to the thermoplastic resin (X) and the fluorine-containing copolymer (B). The device used for the melt kneading is not particularly limited, but by adjusting the kneading conditions that can apply shear more effectively, such as a special screw, high rotation speed, and narrow clearance, it is possible to carry out the melt kneading with a conventionally used twin-screw extruder, single-screw extruder, multi-screw extruder, tandem extruder, or a batch kneader such as a roll kneader, a lab plastomill, a Banbury mixer, a pressure kneader, or a compounding mill. This makes it possible to disperse the fluorine-containing copolymer in the amorphous resin or thermoplastic resin (X), or the amorphous resin or thermoplastic resin (X) in the fluorine-containing copolymer on the submicron order, and further to suppress the behavior of the amorphous resin or the fluorine-containing copolymer agglomerating during molding. As a result, it is possible to give a molded product with even better impact strength. As a device capable of applying a high shear force, it is preferable to use a twin-screw extruder or a high shear processor having an internal feedback screw in the kneading section (a reflux-type high shear processor). The internal feedback screw is a screw in which a feedback hole is formed along the screw central axis from the tip to the rear end. In a high shear processing machine having an internal feedback screw in the kneading section, the molten resin injected into the kneading section is sent to the tip side with the rotation of the internal feedback screw, flows into the feedback hole from the inlet at the tip, flows backward, is discharged from the discharge port, and is sent back to the tip side with the rotation of the internal feedback screw. This circulation allows the molten resin to be highly dispersed and mixed, and the size of the dispersed phase can be reduced. Examples of the high shear processing machine include devices described in JP 2005-313608 A and JP 2011-046103 A. When a twin-screw extruder is used as a kneader, it is preferable to use a twin-screw extruder having a screw configuration with a large L / D. The screw configuration of the twin-screw extruder is preferably L / D=30 or more, more preferably L / D=35 or more, and even more preferably L / D=40 or more. Here, L / D is the effective length (L) of the screw divided by the screw diameter (D). From the viewpoint of kneading properties and improving productivity, melt kneading using a twin-screw extruder is most preferable.
[0094] The melt-kneading time is preferably 1 to 600 seconds, more preferably 5 to 300 seconds. If the melt-kneading time is longer than the above time, the resin may deteriorate significantly and the desired performance may not be achieved. If the melt-kneading time is shorter than the above time, the dispersibility may be deteriorated and the desired performance may not be achieved. The melt kneading temperature must be equal to or higher than the glass transition temperature of the amorphous resin (A) and the melting point of the fluorine-containing copolymer (B), and is preferably from 240 to 450°C, more preferably from 260 to 400°C.
[0095] The form of the first and second resin compositions of the present disclosure is not particularly limited, and may be pellets. That is, pellets obtained by molding the first and second resin compositions of the present disclosure also constitute the present disclosure.
[0096] The pellets of the present disclosure may be obtained by kneading the amorphous resin (A) and the fluorine-containing copolymer (B) to obtain the first resin composition of the present disclosure, or by kneading the thermoplastic resin (X) and the fluorine-containing copolymer (B) to obtain the second resin composition of the present disclosure, removing the kneaded mixture from a kneader and then molding it into a pellet shape; alternatively, the pellets may be obtained by kneading the amorphous resin (A) and the fluorine-containing copolymer (B), or the thermoplastic resin (X) and the fluorine-containing copolymer (B), using a kneader, and then extruding the mixture from the kneader by melt extrusion or the like to mold it.
[0097] The molding method is not particularly limited, but examples thereof include melt extrusion using a twin-screw extruder or the like.
[0098] The pellets may be added after molding into a pellet shape, or may have known components added thereto. Known methods can be used for adding the additives to the pellets, and examples of such methods include spraying the pellets with a spray or dry blending the pellets with powders of the additives. For example, the pellets may have a lubricant (e.g., magnesium stearate) added thereto after molding. Molded products formed from the pellets have excellent impact strength. The pellets may also be further kneaded after adding known ingredients (eg, lubricants) which may be added later. The present disclosure also includes pellets obtained by molding the resin composition obtained by the above-mentioned production method, and pellets to which a lubricant has been added after molding.
[0099] Components other than the amorphous resin (A) and the fluorine-containing copolymer (B) may be added to and mixed with the amorphous resin (A) and the fluorine-containing copolymer (B) in advance, or may be added when blending the amorphous resin (A) and the fluorine-containing copolymer (B). The same applies when a thermoplastic resin (X) is used instead of the amorphous resin (A).
[0100] The present disclosure also includes a molded article formed from the first resin composition, the second resin composition, or the pellets of the present disclosure.
[0101] A molded article made of the first resin composition or the second resin composition of the present disclosure can be obtained by injection molding such pellets. In such injection molding, not only a normal cold runner type molding method but also a hot runner that enables runnerless manufacturing can be used. In addition to normal molding methods, injection molding can also use gas-assisted injection molding, injection compression molding, ultra-high speed injection molding, injection press molding, two-color molding, sandwich molding, in-mold coating molding, insert molding, foam molding (including those using supercritical fluids), rapid heating and cooling mold molding, adiabatic mold molding, and in-mold remelting molding, as well as molding methods consisting of combinations thereof. Film molding, extrusion molding, wire molding by extrusion, tube molding, and sheet molding can also be used.
[0102] The molded product of the present disclosure has a Charpy strength of 5KJ / m 2 It is preferable that the concentration is 10KJ / m or more. 2 The higher the Charpy impact strength, the better. There is no upper limit, but it is preferably 100 KJ / m 2 may be also possible. The Charpy strength is a value measured using an impact tester in accordance with ASTM D6110-02.
[0103] The molded article of the present disclosure preferably has a flexural modulus of 1000 MPa or more, more preferably 2000 MPa or more. There is no upper limit, but it may be, for example, 3000 MPa. The flexural modulus is a value measured in accordance with ASTM D 790 using a universal material testing machine.
[0104] The molded article of the present disclosure has high flexibility and a low relative dielectric constant and dielectric tangent, and is therefore suitable for use as a material requiring dielectric properties (particularly, a material for high-frequency circuit boards).
[0105] The high-frequency circuit board is a circuit board that can operate in a high-frequency band. The high-frequency band may be a band of 1 GHz or more, preferably a band of 3 GHz or more, and more preferably a band of 5 GHz or more. There is no particular upper limit, but it may be a band of 100 GHz or less.
[0106] When the molded article of the present disclosure is used as a material for high-frequency circuit boards, etc., it is preferable to use a metal foil and the molded article of the present disclosure as a laminate. The present disclosure also includes a laminate including a metal foil and the molded article of the present disclosure.
[0107] Examples of the metal foil include copper, stainless steel, aluminum, iron, silver, gold, and ruthenium. In addition, alloys of these materials can also be used. Of these, copper is preferred. As the copper, rolled copper, electrolytic copper, etc. can be used.
[0108] The laminate of the present disclosure is preferably a sheet. The thickness of the laminate may be, for example, 1 μm to 1 mm, and is preferably 1 to 500 μm. More preferably, it is 150 μm or less, and even more preferably, it is 100 μm or less.
[0109] The laminate of the present disclosure may be one in which other layers are further laminated on the metal foil and the molded article of the present disclosure. EXAMPLES
[0110] Next, the present disclosure will be described with reference to examples, but the present disclosure is not limited to only these examples.
[0111] <Glass transition temperature (Tg)> The measurement was performed using a differential scanning calorimeter (DSC) in accordance with JIS K7121 at a temperature rise rate of 20° C. / min.
[0112] <Continuous use temperature> Measured in accordance with UL746B.
[0113] <Melt flow rate (MFR)> The MFR of the fluorocopolymer and the amorphous resin was measured using a melt indexer under the conditions of a preheating time of 5 minutes, 380°C or 400°C, and a load of 5000g in accordance with ASTM D1238. The MFR of the resin composition obtained by mixing the fluorocopolymer and the amorphous resin was also measured in the same manner as above. The measurement temperature was 380° C. in the example using the amorphous resin (1), and 400° C. in the example using the amorphous resin (2).
[0114] <Melting point> Using a differential scanning calorimetry (DSC) device, the temperature was determined as the temperature corresponding to the maximum value in the heat of fusion curve when the temperature was increased at a rate of 10° C. / min.
[0115] <Calculation of average dispersed particle size> The kneaded products (resin compositions) obtained in the examples and comparative examples, the strands of the kneaded products obtained in the examples and comparative examples after MFR measurement, and the sections cut out from the injection molded products (molded products) obtained in the examples and comparative examples were cut perpendicular to the flow direction, the cross sections were photographed with a confocal laser microscope, and the obtained microscopic images were analyzed with image analysis software (Image J). The dispersed phase was selected, and the circle equivalent diameter was obtained. The circle equivalent diameters of 20 dispersed phases were calculated, and the average was calculated to obtain the average dispersed particle diameter r1 and the average dispersed particle diameter r2.
[0116] <Shear rate during mixing> The shear rate (γ) during kneading was calculated using the following formula 1. Equation 1: γ = πDr / C D: Screw outer diameter (mm) r: screw rotation speed (rpm) C: Tip clearance (mm)
[0117] <Impact strength (Charpy impact strength)> A notch was made in the injection molded article produced by the above-mentioned method, and measurements were performed using an impact tester in accordance with ASTM D6110-02.
[0118] <Flexural modulus> The injection molded product produced by the above-mentioned method was measured using a universal material testing machine in accordance with ASTM D 790. The measurement was performed at a test speed of 2 mm / min.
[0119] <Dielectric constant and dielectric loss tangent> The injection molded product produced by the above-mentioned method was cut into a rectangular shape with a width of 2 mm and a length of 100 mm, and the relative dielectric constant and dielectric loss tangent at 25°C and 20 GHz were measured by the cavity resonator perturbation method (network analyzer).
[0120] <IRピーク> The dispersed phase isolated from the resin composition was subjected to IR in accordance with JIS K0117: 2017. The results were expressed according to the following criteria. ○: Not only the peaks of the dispersed phase components but also the peaks of the continuous phase components are detected ×: Only peaks of dispersed phase components were detected In addition, in Comparative Example 2 and Comparative Example 5 in which no dispersed phase was present, and in Examples 3, 4, 5, and 8 in which the dispersed phase could not be isolated, IR could not be measured, and therefore are indicated as "-".
[0121] In the examples and comparative examples, the following materials were used. Amorphous resin (1): PEI (Tg: 217°C, continuous use temperature: 170°C, MFR: 58g / 10min) Amorphous resin (2): TPI (Tg: 250°C, continuous use temperature: 240°C, MFR: 50g / 10min) Fluorine-containing copolymer (1): FEP (TFE / HFP / PPVE copolymer (with reactive functional groups), MFR: 30g / 10min, melting point: 260℃) Fluorine-containing copolymer (2): PFA (TFE / PAVE copolymer (with reactive functional groups), MFR: 16 g / 10 min, melting point: 306°C) Fluorine-containing copolymer (3): FEP (TFE / HFP / PPVE copolymer (no reactive functional groups), MFR: 37 g / 10 min, melting point: 260°C)
[0122] Examples 1 to 6, Comparative Examples 1 to 4 The materials were dry-blended in the ratios (mass%) shown in Tables 1 and 2, and dried at 120°C for 8 hours, and then melt-kneaded under the following conditions using a reflux-type high-shear processing machine (manufactured by Niigata Machine Techno Co., Ltd.) to produce a resin composition. The diameter of the return hole used was φ2.5 mm. Screw L / D: 1.8 Mixing temperature: 360℃ Shear rate during kneading: See Tables 1 and 2 Mixing time: 10 seconds
[0123] Example 7 The materials were premixed in the ratios (mass%) shown in Table 2, and then extruded in a twin-screw extruder (φ25 mm, L / D=52.5) at a cylinder temperature of 360°C and a shear rate of 2090 sec. -1 The mixture was melt-kneaded under the above conditions to produce a resin composition.
[0124] Comparative Example 5, Example 8 A resin composition was produced under the same conditions as in Example 1, except that the materials were dry-blended in the ratio (mass %) shown in Table 2 and the kneading temperature was 400°C.
[0125] <Production of injection molded products> The resin compositions produced in the examples and comparative examples were dried at 120° C. for 8 hours, and then injection molded using a small injection molding machine to obtain ASTM multipurpose test pieces (127 mm×12.7 mm×3.2 mm).
[0126] [Table 1]
[0127] [Table 2]
[0128] Comparing the Examples and Comparative Examples with the same composition, the Examples with r2 / r1 less than 1.70 had good impact strength. Also, the Examples 1 to 7 tended to have high flexibility and low relative dielectric constant and dielectric loss tangent compared to the Comparative Example 2 using only amorphous resin. The same tendency was observed in the comparison between the Example 8 and the Comparative Example 6.
[0129] In Examples 1, 2, 4, 6, 7 and 8 and Comparative Examples 1 and 3, where the content of amorphous resin (A) was greater than the content of fluorinated copolymer (B), the amorphous resin (A) formed a continuous phase, and the fluorinated copolymer (B) formed a dispersed phase. In Examples 3, 5 and Comparative Example 4, where the content of amorphous resin (A) was greater than the content of fluorinated copolymer (B), the fluorinated copolymer (B) formed a continuous phase, and the amorphous resin (A) formed a dispersed phase.
[0130] In Examples 1, 2, 4, 6, and 7, the IR peak results were ◯, and continuous phase components were present in the dispersed phase. In Examples 3, 5, and 8, IR could not be performed, but the same improvement effects as in the other Examples were obtained, so it is presumed that continuous phase components are present in the dispersed phase.
Claims
1. The composition comprises an amorphous resin (A) belonging to super engineering plastics and a fluorine-containing copolymer (B), A resin composition in which a ratio r2 / r1 of an average dispersed particle size r1 of the amorphous resin (A) or the fluorinated copolymer (B) to an average dispersed particle size r2 of the amorphous resin (A) or the fluorinated copolymer (B) after a melt flow rate is measured in accordance with ASTM D1238 at 380°C or higher or a temperature at which the resin composition melts, under a load of 5,000 g, and with a preheating time of 5 minutes is less than 1.
70. (However, r1 and r2 were measured for the same resin or the same copolymer.)
2. 2. The resin composition according to claim 1, wherein the amorphous resin (A) has a glass transition temperature of 190°C to 290°C.
3. 3. The resin composition according to claim 1, wherein the amorphous resin (A) has a continuous use temperature of 140° C. or higher.
4. 3. The resin composition according to claim 1, wherein the amorphous resin (A) has an imide structure.
5. The resin composition according to claim 4, wherein the amorphous resin (A) has an amide structure and an imide structure.
6. 5. The resin composition according to claim 4, wherein the amorphous resin (A) is a thermoplastic polyimide.
7. 5. The resin composition according to claim 4, wherein the amorphous resin (A) is a polyetherimide.
8. 3. The resin composition according to claim 1, wherein the melting point of the fluorine-containing copolymer (B) is from 200 to 323°C.
9. The fluorine-containing copolymer (B) is a copolymer composed of tetrafluoroethylene and the following general formula (1): CF 2 =CF-Rf 1 (1) (wherein, Rf 1 is -CF 3 Or -ORf 2Rf 2 3. The resin composition according to claim 1, which is a copolymer of a perfluoroethylenically unsaturated compound represented by the formula:
10. 10. The resin composition according to claim 9, wherein the perfluoroethylenically unsaturated compound is at least one selected from the group consisting of hexafluoropropylene and perfluoro(alkyl vinyl ether).
11. The resin composition according to claim 9, wherein the fluorine-containing copolymer (B) is at least one selected from the group consisting of tetrafluoroethylene / hexafluoropropylene copolymers and tetrafluoroethylene / perfluoro(alkyl vinyl ether) copolymers.
12. When r1 and r2 are measured for the amorphous resin (A), r2 is 2.0 μm or less, 3. The resin composition according to claim 1, wherein, when r1 and r2 are values measured for said fluorine-containing copolymer (B), r2 is 1.0 μm or less.
13. 3. The resin composition according to claim 1, wherein the mass ratio (A):(B) of the amorphous resin (A) to the fluorine-containing copolymer (B) is from 99:1 to 10:
90.
14. The resin composition according to claim 13, wherein the mass ratio (A):(B) is 80:20 to 20:
80.
15. 3. The resin composition according to claim 1, which has a phase structure composed of a continuous phase and a dispersed phase, and components of the continuous phase are present in the dispersed phase.
16. A resin composition having a phase structure in which one of the thermoplastic resin (X) and the fluorine-containing copolymer (B) is a continuous phase and the other is a dispersed phase, and components of the continuous phase are present in the dispersed phase.
17. A method for producing the resin composition according to claim 1 or 2, A production method comprising the step of melt-kneading an amorphous resin (A) and a fluorine-containing copolymer (B) at a shear rate calculated from the following formula 1 of 600 / sec or more: Equation 1: γ=πDr / C γ: shear rate ( / sec) D: Screw outer diameter (mm) r: screw rotation speed (rpm) C: Tip clearance (mm)
18. The method according to claim 17, wherein the shear rate is 800 / sec or more and 3000 / sec or less, the melt-kneading time is 5 to 300 seconds, and the melt-kneading temperature is 260 to 400°C.
19. A pellet obtained by molding the resin composition according to claim 1 or 2.
20. A molded article formed from the resin composition according to claim 1 or 2.
21. The Charpy impact strength measured using an impact tester in accordance with ASTM D6110-02 is 5 kJ / m 2 The molded article according to claim 20.
22. The molded article according to claim 20, which is used in materials where dielectric properties are required.
23. The molded article according to claim 20, which is a material for a high-frequency circuit board.
24. A laminate comprising a metal foil and the molded article according to claim 20.
25. 25. The laminate of claim 24, wherein the metal foil is copper.
Citation Information
Patent Citations
Fluorine-containing resin composition
JP2001072882A