Mounting table and components for plasma processing device
The use of a conductive-ceramic boundary layer and 3D printing for plasma processing parts addresses the lead time issue by enhancing heat transfer and power efficiency, resulting in faster production of complex parts.
Patent Information
- Application Number
- JP2024157538
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-11-28
- Estimated Expiration
- 2038-05-15
AI Technical Summary
The manufacturing of complex plasma processing parts with hollow structures requires a long production and development period, leading to increased lead times and man-hours.
A mounting table with a base made of a conductive material and an electrostatic chuck made of ceramic material, featuring a boundary layer with a changing blend ratio of conductive and ceramic materials, and a 3D printing process to form these parts without adhesives, ensuring efficient heat transfer and high-frequency power feeding.
This approach reduces lead time in manufacturing by improving heat transfer and high-frequency power efficiency, allowing for faster production of complex parts with uniform temperature distribution and reduced manufacturing steps.
Smart Images

Figure 2024166325000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a mounting table and a component for a plasma processing apparatus. [Background technology]
[0002] In recent years, parts installed in plasma processing apparatuses have become more complex in structure in order to provide higher functionality, and may be manufactured by adhering or joining different members (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2018-46185 A Summary of the Invention [Problem to be solved by the invention]
[0004] The manufacturing of such parts requires a long production and development period due to their complex structures, such as hollow structures, and therefore increases in lead time during part manufacturing are an issue. There is a demand to reduce the number of steps in the parts manufacturing process and shorten the lead time.
[0005] In response to the above problem, one object of the present invention is to shorten the lead time when manufacturing parts. [Means for solving the problem]
[0006] In order to solve the above problem, according to one aspect, there is provided a mounting table comprising: a base formed of a conductive material; an electrostatic chuck formed of a ceramic material and disposed on an upper surface of the base; and a boundary layer provided between the base and the electrostatic chuck, wherein the boundary layer contains a mixture of the conductive material and the ceramic material, and a composition ratio of the conductive material to the ceramic material in the mixture changes in the boundary layer from the base toward the electrostatic chuck. Effect of the Invention
[0007] According to one aspect, the lead time for manufacturing parts can be shortened. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a diagram showing an example of a plasma processing apparatus according to an embodiment. [Diagram 2] 2 is an enlarged view of a portion of a mounting table of the plasma processing apparatus shown in FIG. 1; [Diagram 3] FIG. 1 is a diagram showing an example of the configuration of a 3D printer according to an embodiment. [Figure 4] 10 is a flowchart illustrating an example of a part forming process according to an embodiment. [Diagram 5] 1A to 1C are diagrams for explaining a method of forming a component according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings. In this specification and the drawings, substantially identical components are designated by the same reference numerals, and redundant description will be omitted.
[0010] [Plasma processing equipment] The plasma processing apparatus 100 shown in FIG. 1 is a capacitively coupled plasma processing apparatus. The plasma processing apparatus 100 includes a processing vessel 112 and a mounting table 116. The processing vessel 112 has a substantially cylindrical shape, and its internal space serves as a processing chamber 112c. The processing vessel 112 is made of, for example, aluminum. A ceramic film having plasma resistance, such as an alumite film and / or an yttrium oxide film, is formed on the surface of the processing vessel 112 facing the internal space. The processing vessel 112 is grounded. An opening 112p is formed on the sidewall of the processing vessel 112 for loading and unloading a wafer W into and from the processing chamber 112c. The opening 112p can be opened and closed by a gate valve GV.
[0011] The mounting table 116 is configured to support the wafer W in the processing chamber 112c. The mounting table 116 has a function of adsorbing the wafer W, a function of adjusting the temperature of the wafer W, and a structure for transmitting high frequency waves to a base 117 of the electrostatic chuck. The mounting table 116 will be described in detail later.
[0012] The plasma processing apparatus 100 has an upper electrode 130. The upper electrode 130 is disposed in an upper opening of the processing vessel 112, and is disposed approximately parallel to the mounting table 116 that functions as a lower electrode. An insulating support member 132 is interposed between the upper electrode 130 and the processing vessel 112.
[0013] The upper electrode 130 has a top plate 134 and a support 136. The top plate 134 has a substantially disk-like shape. The top plate 134 may be conductive. The top plate 134 is made of, for example, silicon or aluminum, and a plasma-resistant ceramic film is formed on the surface of the top plate 134. A plurality of gas discharge holes 134a are formed in the top plate 134. The gas discharge holes 134a extend in a substantially vertical direction.
[0014] The support 136 detachably supports the top plate 134. The support 136 is made of, for example, aluminum. A gas diffusion chamber 136a is formed in the support 136. A plurality of holes 136b extend from the gas diffusion chamber 136a, each of which communicates with a plurality of gas discharge holes 134a. A pipe 138 is connected to the gas diffusion chamber 136a via a port 136c. A gas supply unit 139 is connected to the pipe 138.
[0015] The plasma processing apparatus 100 includes an exhaust device 150. The exhaust device 150 includes one or more pumps, such as a turbo molecular pump or a dry pump, and a pressure control valve. The exhaust device 150 is connected to an exhaust port formed in the processing vessel 112.
[0016] The plasma processing apparatus 100 has a first control unit 151. A storage unit of the first control unit 151 stores a control program and recipe data for controlling various processes executed by the plasma processing apparatus 100 using a processor. For example, the storage unit of the first control unit 151 stores a control program and recipe data for executing a plasma process such as an etching process in the plasma processing apparatus 100.
[0017] 2 in addition to Fig. 1, the mounting table 116 and components of the plasma processing apparatus 100 associated with the mounting table 116 will be described in detail below. Fig. 2 is an enlarged cross-sectional view showing a part of the mounting table 116 of the plasma processing apparatus 100 shown in Fig. 1.
[0018] The mounting table 116 has a base 117 and an electrostatic chuck 120. The base 117 is made of, for example, an aluminum alloy (Al), titanium (Ti), silicon carbide (SiC), or the like. The base 117 is supported by a support member 114 extending upward from the bottom of the processing vessel 112. The support member 114 is an insulating member and is made of, for example, aluminum oxide (alumina). The support member 114 has a substantially cylindrical shape.
[0019] The base 117 is formed from a conductive metal, for example, aluminum. The base 117 has a substantially disk shape. The base 117 has a central portion 117a and a peripheral portion 117b. The central portion 117a has a substantially disk shape. The central portion 117a provides a first upper surface 117c of the base 117. The first upper surface 117c is a substantially circular surface.
[0020] The peripheral portion 117b is continuous with the central portion 117a and extends in the circumferential direction (circumferential direction with respect to the axis Z) outside the central portion 117a in the radial direction (radial direction with respect to the axis Z extending in the vertical direction). In one embodiment, the peripheral portion 117b, together with the central portion 117a, provides the lower surface 117d of the base 117. The peripheral portion 117b also provides the second upper surface 117e. The second upper surface 117e is a band-shaped surface, is outside the first upper surface 117c in the radial direction, and extends in the circumferential direction. The second upper surface 117e is closer to the lower surface 117d than the first upper surface 117c in the vertical direction.
[0021] A power feeder 119 is connected to the base 117. The power feeder 119 is, for example, a power feed rod, and is connected to a lower surface 117d of the base 117. The power feeder 119 is made of aluminum or an aluminum alloy. A first high frequency power supply 62 is connected to the power feeder 119 via a matching device 66. In addition, a second high frequency power supply 64 is connected to the power feeder 119 via a matching device 68.
[0022] A flow path 117f for the coolant is formed in the base 117. The flow path 117f extends, for example, in a spiral shape within the base 117. A coolant is supplied to the flow path 117f from a chiller unit. In one embodiment, the coolant supplied to the flow path 117f is a coolant that absorbs heat by vaporizing and performs cooling. The coolant may be, for example, a hydrofluorocarbon-based coolant.
[0023] The electrostatic chuck 120 has an adsorption portion 123. The adsorption portion 123 is provided on a base 121 on a base 117. The base 121 constitutes a lower electrode, and is provided on the base 117. The base 121 has electrical conductivity. The base 121 may be made of ceramics, such as aluminum nitride or silicon carbide, which is made electrically conductive, or may be made of a metal (such as titanium).
[0024] The base 121 has a substantially disc shape. The base 121 has a central portion 121a and a peripheral portion 121b. The central portion 121a has a substantially disc shape. The central portion 121a provides a first upper surface 121c of the base 121. The first upper surface 121c is a substantially circular surface.
[0025] The peripheral portion 121b is continuous with the central portion 121a and extends in the circumferential direction outside the central portion 121a in the radial direction. In one embodiment, the peripheral portion 121b, together with the central portion 121a, provides the lower surface 121d of the base 121. The peripheral portion 121b also provides a second upper surface 121e. The second upper surface 121e is a strip-shaped surface and extends in the circumferential direction outside the first upper surface 121c in the radial direction. The second upper surface 121e is closer to the lower surface 121d than the first upper surface 121c in the vertical direction.
[0026] A boundary layer 129 is formed between the adsorption portion 123 and the base 121. The adsorption portion 123 has a substantially disk shape and is made of ceramics. The ceramics constituting the adsorption portion 123 has a melting point of 1×10 15 The ceramic may be one having a volume resistivity of Ω·cm or more. As such a ceramic, for example, aluminum oxide (alumina) may be used.
[0027] The electrostatic chuck 120 includes a plurality of regions RN concentric with respect to the axis Z, i.e., the central axis of the electrostatic chuck 120. In one embodiment, the electrostatic chuck 120 includes a first region R1, a second region R2, and a third region R3. The first region R1 intersects with the axis Z, the third region R3 is a region including an edge of the electrostatic chuck 120, and the second region R2 is between the first region R1 and the third region R3. In one example, the first region R1 is a region from the center of the electrostatic chuck 120 to a radius of 120 mm, the second region R2 is a region in the electrostatic chuck 120 from a radius of 120 mm to a radius of 135 mm, and the third region R3 is a region in the electrostatic chuck 120 from a radius of 135 mm to a radius of 150 mm. The number of regions in the electrostatic chuck 120 may be any number equal to or greater than one.
[0028] The adsorption portion 123 of the electrostatic chuck 120 incorporates an electrode film 125. A DC power supply is electrically connected to the electrode film 125. When a DC voltage from the DC power supply is applied to the electrode film 125, the adsorption portion 123 generates an electrostatic force such as a Coulomb force, and holds the wafer W by the electrostatic force.
[0029] The adsorption unit 123 further includes a plurality of built-in heaters HN. The plurality of heaters HN are provided in the plurality of regions RN of the electrostatic chuck, respectively. In one embodiment, the plurality of heaters HN include a first heater 156, a second heater 157, and a third heater 158. The first heater 156 is provided in the first region R1, the second heater 157 is provided in the second region R2, and the third heater 158 is provided in the third region R3. The plurality of heaters HN are connected to a heater power source.
[0030] A plurality of first elastic members EM1 are provided between the base 121 and the base 117. The plurality of first elastic members EM1 separate the electrostatic chuck 120 upward from the base 117. Each of the plurality of first elastic members EM1 is an O-ring. The plurality of first elastic members EM1 have different diameters from each other and are provided concentrically with respect to the axis Z. The plurality of first elastic members EM1 are provided below the boundary between adjacent regions of the electrostatic chuck 120 and the edge of the electrostatic chuck 120. In one embodiment, the plurality of first elastic members EM1 include an elastic member 165, an elastic member 167, and an elastic member 169. The elastic member 165 is provided below the boundary between the first region R1 and the second region R2, the elastic member 167 is provided below the boundary between the second region R2 and the third region R3, and the elastic member 169 is provided below the edge of the electrostatic chuck 120.
[0031] The plurality of first elastic members EM1 are partially disposed in grooves provided by the first upper surface 117c of the base 117 and are in contact with the first upper surface 117c and the lower surface 121d of the base 121. The plurality of first elastic members EM1, together with the base 117 and the base 121, define a plurality of heat transfer spaces DSN between the first upper surface 117c of the base 117 and the lower surface 121d of the base 121. The plurality of heat transfer spaces DSN extend below each of the plurality of regions RN of the electrostatic chuck 120 and are separated from each other. In one embodiment, the plurality of heat transfer spaces DSN include a first heat transfer space DS1, a second heat transfer space DS2, and a third heat transfer space DS3. The first heat transfer space DS1 is located inside the elastic member 165, the second heat transfer space DS2 is located between the elastic member 165 and the elastic member 167, and the third heat transfer space DS3 is located between the elastic member 167 and the elastic member 169. As described later, a heat transfer gas (e.g., He gas) is supplied to the heat transfer spaces DSN. The length of each of the heat transfer spaces DSN in the vertical direction is set to, for example, 0.1 mm or more and 2.0 mm or less.
[0032] The first elastic members EM1 are configured to have a higher thermal resistance than the thermal resistance of each of the heat transfer spaces DSN to which He gas is supplied. The thermal resistance of the heat transfer spaces DSN depends on the thermal conductivity of the heat transfer gas, its vertical length, and its area. The thermal resistance of each of the first elastic members EM1 depends on its thermal conductivity, its vertical thickness, and its area. Therefore, the material, thickness, and area of each of the first elastic members EM1 are determined according to the thermal resistance of each of the heat transfer spaces DSN. The first elastic members EM1 may be required to have low thermal conductivity and high heat resistance. Therefore, the first elastic members EM1 may be formed of, for example, perfluoroelastomer.
[0033] The mounting table 116 has a fastening member 171. The fastening member 171 is formed from a metal, and is configured to hold the base 121 and the multiple first elastic members EM1 between the fastening member 171 and the base 117. The fastening member 171 is formed from a material having low thermal conductivity, such as titanium, in order to suppress heat conduction between the base 121 and the base 117 via the fastening member 171.
[0034] In one embodiment, the fastening member 171 has a tubular portion 171a and an annular portion 171b. The tubular portion 171a has a generally cylindrical shape and provides a first lower surface 171c at its lower end. The first lower surface 171c is a band-shaped surface extending in the circumferential direction.
[0035] The annular portion 171b has a generally annular plate shape, is continuous with the inner edge of the upper part of the cylindrical portion 171a, and extends radially inward from the cylindrical portion 171a. The annular portion 171b provides a second lower surface 171d. The second lower surface 171d is a band-shaped surface extending in the circumferential direction.
[0036] The fastening member 171 is disposed such that the first lower surface 171c contacts the second upper surface 117e of the base 117, and the second lower surface 171d contacts the second upper surface 121e of the base 121. The fastening member 171 is fixed to the peripheral portion 117b of the base 117 by a screw 173. The amount of squeezing of the multiple first elastic members EM1 is adjusted by adjusting the engagement of the screw 173 with the fastening member 171. This adjusts the vertical length of the multiple heat transfer spaces DSN.
[0037] In one embodiment, a second elastic member 175 is provided between the lower surface of the inner edge of the annular portion 171b of the fastening member 171 and the second upper surface 121e of the base 121. The second elastic member 175 is an O-ring, and prevents particles (e.g., metal powder) that may be generated by friction between the second lower surface 171d of the fastening member 171 and the second upper surface 121e of the base 121 from moving toward the adsorption portion 123.
[0038] Moreover, the second elastic member 175 generates a reaction force smaller than the reaction force generated by the plurality of first elastic members EM1. In other words, the plurality of first elastic members EM1 are configured so that the reaction force generated by the plurality of first elastic members EM1 is larger than the reaction force generated by the second elastic member 175. Furthermore, the second elastic member 175 may be formed from a perfluoroelastomer, which is a material having high heat resistance and low thermal conductivity.
[0039] A heater 176 is provided on the fastening member 171. The heater 176 extends in the circumferential direction and is connected to a heater power supply via a filter. The filter is provided to prevent high frequency waves from entering the heater power supply.
[0040] The heater 176 is provided between the first film 180 and the second film 182. The first film 180 is provided on the fastening member 171 side of the second film 182. The first film 180 has a thermal conductivity lower than that of the second film 182. For example, the first film 180 may be a thermally sprayed film made of zirconia, and the second film 182 may be a thermally sprayed film made of yttrium oxide (yttria). The heater 176 may also be a thermally sprayed film of tungsten.
[0041] An edge ring FR is provided on the second film 182. The edge ring FR is made of, for example, Si. The edge ring FR is heated by heat from the heater 176. In addition, most of the heat flux from the heater 176 is directed toward the second film 182 rather than the first film 180, and then directed toward the edge ring FR via the second film 182. Therefore, the edge ring FR is efficiently heated.
[0042] Further, the base 117 of the mounting table 116, the fastening member 171, etc. are covered on their outer peripheries with one or more insulating members 186. The one or more insulating members 186 are formed of, for example, aluminum oxide or quartz.
[0043] As described above, in the mounting table 116, the base 117 and the base 121 are separated from each other by the plurality of first elastic members EM1. In addition, in the mounting table 116, no adhesive is used to bond the base 121 and the adsorption unit 123. Therefore, the temperature of the electrostatic chuck 120 can be set to a high temperature. In addition, since heat exchange between the electrostatic chuck 120 and the base 117 can be performed through the heat transfer gas supplied to the plurality of heat transfer spaces DSN, the temperature of the electrostatic chuck 120 can also be set to a low temperature. In addition, in the mounting table 116, a high-frequency power supply route to the base 121 of the electrostatic chuck 120 is secured by the power supply body 119, the base 117, and the fastening member 171. Furthermore, since the power supply body 119 is connected to the base 121 of the electrostatic chuck 120, not directly, but to the base 117, aluminum or an aluminum alloy can be used as a constituent material of the power supply body 119. Therefore, even when a high frequency of 13.56 MHz or more is used, the loss of the high frequency in the power feeder 119 is suppressed.
[0044] As described above, in one embodiment, the second elastic member 175 is provided between the lower surface of the inner edge of the annular portion 171b of the fastening member 171 and the second upper surface 121e of the base 121. Since the second upper surface 121e of the peripheral portion 121b of the base 121 and the second lower surface 171d of the fastening member 171 are in contact with each other, friction occurs at the contact points, and particles (e.g., metal powder) may be generated. Even if such particles are generated, the second elastic member 175 can suppress the particles from adhering to the adsorption portion 123 and the wafer W placed on the adsorption portion 123.
[0045] Further, the plurality of first elastic members EM1 are configured so that the reaction force generated by the plurality of first elastic members EM1 is greater than the reaction force generated by the second elastic member 175. This allows the electrostatic chuck 120 to be reliably separated from the base 117.
[0046] In one embodiment, the first elastic members EM1 are configured to have a higher thermal resistance than the thermal resistance of the heat transfer spaces DSN when He gas is supplied to the heat transfer spaces DSN. The first elastic members EM1 are formed of, for example, perfluoro elastomer. With the first elastic members EM1, the thermal conduction between the electrostatic chuck 120 and the base 117 is dominant through the heat transfer spaces DSN rather than through the first elastic members EM1. Therefore, the temperature distribution of the electrostatic chuck 120 can be made uniform.
[0047] In one embodiment, the gas line 190 for the heat transfer gas supplied between the wafer W and the adsorption unit 123 is formed without using an adhesive. A surface 121f of the base 121 defining the storage space in which the sleeve 192 that partially constitutes the gas line 190 is disposed is covered with a coating 194, and an insulating third elastic member 196 is provided between the coating 194 and the base 117 so as to seal the storage space. This prevents the plasma from penetrating between the base 121 and the base 117, and prevents the dielectric breakdown of the base 121 from occurring as a result.
[0048] Furthermore, the plasma processing apparatus 100 having the above-described mounting table 116 can perform plasma processing on the wafer W in a wide temperature range from low to high temperatures.
[0049] [3D printer configuration] Next, an example of the configuration of the 3D printer 200 will be described with reference to FIG. 3. FIG. 3 shows an example of the configuration of the 3D printer 200 according to an embodiment. The 3D printer 200 according to this embodiment is an example of an apparatus that forms (manufactures) parts used in a plasma processing apparatus. However, the apparatus that forms the parts is not limited to the configuration of the 3D printer 200 shown in FIG. 3.
[0050] In this embodiment, the mounting table 116 that functions as a lower electrode having a complex structure will be described as an example of a part formed by the 3D printer 200. However, the part formed by the 3D printer 200 is not limited to this, and may be, for example, the upper electrode 130. For example, it may be a part that includes different materials or a part that is fixed by screws using different materials that cannot be bonded. In addition, any part that is arranged in the plasma processing apparatus 100 may be used.
[0051] The 3D printer 200 is capable of forming a three-dimensional object in the chamber 210. In the 3D printer 200 according to this embodiment, three-dimensional data for forming the mounting table 116 as a three-dimensional object is stored in a storage unit such as a RAM 256, and the mounting table 116 is manufactured based on the three-dimensional data. The mounting table 116 is formed on a mounting surface of a stage 202 provided on the table. The stage 202 can be raised and lowered, for example, so as to gradually lower it, as the formation of the mounting table 116 progresses.
[0052] In this embodiment, raw material powder for forming the mounting table 116 is stored in a raw material storage section 203 provided on the table. The raw material may be the same as the material of each component constituting the mounting table 116. For example, when, among the components constituting the mounting table 116, the bases 117 and 121 are made of an aluminum alloy and the electrostatic chuck 120 is made of SiC, the raw material storage section 203 stores aluminum alloy powder and SiC powder separately.
[0053] However, the material of the bases 117 and 121 is not limited to aluminum alloy, and may be ceramics such as SiC. The material of the electrostatic chuck 120 is not limited to SiC, and may be ceramics such as alumina. When the bases 117 and 121 are made of SiC and the electrostatic chuck 120 is made of alumina, SiC powder and alumina powder are separately stored in the raw material storage unit 203. The raw materials of the materials constituting the bases 117, 121, and the electrostatic chuck 120 are not limited to powder form, and may be wire form. In this embodiment, the bases 117 and the electrostatic chuck 120 are made of different materials.
[0054] In the chamber 210, an energy beam is irradiated while a raw material powder is being supplied, thereby melting the raw material powder. In this embodiment, a laser beam A (optical laser) is used as the energy beam to be irradiated.
[0055] Laser light A is output from a light source 206 and irradiated onto a predetermined position determined by a laser scanning device 204 that performs two-dimensional scanning. The light source 206 and the laser scanning device 204 are preferably disposed outside the chamber 210. The second control unit 250 drives a laser driving unit 208 to move the laser scanning device 204 to a predetermined position.
[0056] The laser scanning device 204 scans the stage 202 with the laser light A in at least two-dimensional (XY) directions. For example, the laser scanning device 204 is controlled to move the irradiation spot of the laser light A on the stage 202 in accordance with three-dimensional data indicating the three-dimensional structure of the mounting table 116. Specifically, under the control of the second control unit 250, the laser scanning device 204 scans in two-dimensional (XY) directions in accordance with the progress of formation of parts such as the bases 117 and 121 and the electrostatic chuck 120 that constitute the mounting table 116.
[0057] The second control unit 250 controls the roller driving unit 207 to drive the roller 205. As a result, the aluminum alloy powder which is the material of the base 117 and / or the SiC powder which is the material of the electrostatic chuck 120 are supplied to the laser light scanning space 209.
[0058] It is preferable that the temperature of the raw material storage unit 203 is adjusted by a heating means. It is also preferable that the chamber 210 is provided with a mechanism capable of supplying an inert gas and evacuating the chamber 210.
[0059] The laser beam A scanned in two-dimensional directions by the laser scanning device 204 is irradiated onto an irradiation area on the stage 202 through a laser transmission window 211 provided on the ceiling of the chamber 210, for example, directly above the center of the stage 202. The laser beam A heats the aluminum alloy powder and / or SiC powder on the stage 202 (see B in FIG. 3), melting and solidifying the powder to form the mounting table 116. In this manner, the base 117 and the electrostatic chuck 120 are three-dimensionally formed in this order, and the manufacture of the mounting table 116 is completed.
[0060] The second control unit 250 has a CPU 252, a ROM 254, and a RAM 256. The second control unit 250 controls the supply of raw material powder from the raw material storage unit 203, and the elevation of the stage 202. The second control unit 250 also controls the lighting of the light source 206, the scanning of the laser scanning device 204, and the roller driving unit 207 and the laser driving unit 208. In this way, the second control unit 250 controls the operation of manufacturing the mounting table 116.
[0061] The control program executed by the CPU 252 is stored in, for example, the ROM 254. The CPU 252 executes the control program based on, for example, three-dimensional data stored in the RAM 256, thereby controlling the manufacture of the mounting table 116. The control program may be stored in a fixed recording medium, or in a removable, computer-readable recording medium such as various flash memories or optical (magnetic) disks.
[0062] Furthermore, the second control unit 250 has a display 258 and an input device 260 such as a keyboard or a pointing device. The display 258 is used to display the restoration progress state of the edge ring 87. The input device 260 is used to input commands such as starting and stopping the restoration operation of the edge ring 87 and control parameters during setting.
[0063] The three-dimensional data is data for manufacturing the mounting table 116, and is stored in a storage unit such as the RAM 256. The three-dimensional data includes data on various parts constituting the mounting table 116, such as the three-dimensional structure of the base 117, the hollow structure of the flow path 117f and the like in the base 117, the base 121, and the electrostatic chuck 120. The three-dimensional data also includes data on the three-dimensional structure of the electrostatic chuck 120, and the heater HN and electrode film 125 embedded in the electrostatic chuck 120. The three-dimensional data also includes data on a boundary layer formed between the bases 117, 121, and the electrostatic chuck 120.
[0064] [3D printer operation] Next, an example of the operation of the 3D printer 200 will be described with reference to Fig. 4 and Fig. 5. Fig. 4 is a flowchart showing an example of a part forming process according to an embodiment. Fig. 5 is a diagram for explaining a part forming method according to an embodiment.
[0065] When this process is started, the second control unit 250 acquires the three-dimensional data stored in the RAM 256 (step S10). Based on the three-dimensional data, the second control unit 250 irradiates the aluminum alloy powder with a laser beam while supplying the aluminum alloy powder to the laser beam scanning space 209 (step S12). At this time, the second control unit 250 controls the roller driving unit 207 to operate the roller 205 to supply the aluminum alloy powder to the laser beam scanning space 209. In addition, the second control unit 250 controls the laser driving unit 208 to move the laser scanning device 204 to a predetermined position and irradiates the aluminum alloy powder with a laser beam. The second control unit 250 repeatedly executes the above-mentioned operation of supplying the aluminum alloy powder using the roller 205 and melting and solidifying it with the laser beam. In this way, the second control unit 250 completes the formation of the bases 117, 121 (step S14).
[0066] 5(1) shows a part of the process for forming the bases 117, 121. This process is an example of a first process for forming the bases by supplying aluminum alloy powder, which is an example of a metal raw material, and irradiating the powder with laser light. This allows the hollow structure of the flow channel 117f inside the base 117 to be precisely formed based on the three-dimensional data.
[0067] Returning to FIG. 4, next, the second control unit 250 irradiates the aluminum alloy powder and the SiC powder with the laser light while changing the blending ratio and supplying the powder to the laser light scanning space 209 (step S16). At this time, the second control unit 250 gradually decreases the blending ratio of the aluminum alloy powder from 100% based on the three-dimensional data and continuously changes it to 0% before supplying it. Also, the second control unit 250 gradually increases the blending ratio of the SiC powder from 0% based on the three-dimensional data and continuously changes it to 100% before supplying it.
[0068] As a result, the blending ratio of the aluminum alloy powder and the SiC powder supplied to the laser light scanning space 209 changes from a state in which there is a large amount of aluminum alloy to a state in which there is a large amount of SiC. The second control unit 250 repeatedly executes the operation of supplying the aluminum alloy powder and the SiC powder blended at a predetermined ratio to the laser light scanning space 209 using the roller 205, irradiating the aluminum alloy powder and the SiC powder with the laser light, and melting and solidifying them. As a result, the second control unit 250 completes the formation of the boundary layer 129 (step S18).
[0069] 5(2) shows an example of a step of forming the boundary layer 129. This step is an example of a second step in which a powder in which an aluminum alloy powder, which is an example of a metal raw material, and a SiC powder, which is an example of a ceramic raw material, are mixed in a predetermined ratio is supplied onto the base 121, and the powder is irradiated with a laser beam to form a boundary layer on the base.
[0070] 4, next, the second control unit 250 irradiates the SiC powder with laser light while supplying the SiC powder to the laser light scanning space 209 (step S20). The second control unit 250 repeatedly executes the above-mentioned operation of supplying the SiC powder using the roller 205 and melting and solidifying the powder with the laser light. As a result, the ceramic layer forming the adsorption portion 123 of the electrostatic chuck 120 is formed up to below the heater layer (step S22).
[0071] 5(3) shows an example of the step of forming the ceramic layer. This step is an example of the third step in which a ceramic layer (adsorption portion 123) is formed on the boundary layer 129 by supplying SiC powder, which is an example of a ceramic raw material, and irradiating the powder with laser light.
[0072] 4, next, the second control unit 250 irradiates the heater raw material powder with laser light while supplying the powder to the laser light scanning space 209 (step S24). The second control unit 250 supplies the heater raw material powder using the roller 205, and performs an operation of melting and solidifying the powder with the laser light to form a heater layer in the adsorption unit 123.
[0073] 5(4) shows an example of a process for forming the heater HN. This process is an example of the fourth process in which the heater HN is formed by irradiating the heater HN raw material with an energy beam while supplying the heater HN raw material powder.
[0074] Returning to Fig. 4, next, the second control unit 250 irradiates the SiC powder with laser light while supplying the SiC powder to the laser light scanning space 209 (step S26). The second control unit 250 repeats the above-mentioned operation of supplying the SiC powder using the roller 205 and melting and solidifying it with the laser light. As a result, the ceramic layer that forms the adsorption unit 123 is formed up to under the electrode film (step S28).
[0075] Next, the second control unit 250 irradiates the powder with laser light while supplying the powder as the raw material of the electrode film to the laser light scanning space 209 (step S30). The second control unit 250 supplies the powder as the raw material of the electrode film using the roller 205, and performs an operation of melting and solidifying the powder with the laser light to form an electrode layer in the electrostatic chuck 120.
[0076] 5(5) shows an example of a process for forming an electrode layer (electrode film 125). This process is an example of a fifth process in which the electrode film 125 is formed by irradiating the raw material of the electrode film 125 with a laser beam while supplying the raw material powder of the electrode film 125.
[0077] Returning to FIG. 4, next, the second control unit 250 irradiates the SiC powder with laser light while supplying the powder to the laser light scanning space 209 (step S32). The second control unit 250 repeatedly executes the operation of supplying the SiC powder using the roller 205 and melting and solidifying it with the laser light. This forms the remaining ceramic layer of the adsorption portion 123 (step S34), and ends this process. This completes the formation of the adsorption portion 123 of the electrostatic chuck 120 shown in FIG. 5(6), and ends the manufacture of the mounting table 116.
[0078] According to this method of forming a component, a boundary layer 129 is provided between the base 121 and the adsorption portion 123, which is formed by changing the compounding ratio of the materials of each component. At this time, by forming the boundary layer 129 of different materials smoothly and in a gradational shape, it is possible to eliminate the need for an adhesive layer on the mounting table 116. This can increase the heat transfer coefficient between the different materials of the mounting table 116, improving the thermal characteristics.
[0079] With regard to the blending ratio of each material of the boundary layer 129, the blending ratio of the aluminum alloy which is the material of the base 121 becomes higher than the blending ratio of the SiC which is the material of the adsorption portion 123, the closer to the base 121. Conversely, the blending ratio of the SiC which is the material of the adsorption portion 123 becomes higher than the blending ratio of the aluminum alloy which is the material of the base 121, the closer to the adsorption portion 123.
[0080] In this way, the boundary layer 129 is formed by melting and solidifying a material in which the blending ratio of aluminum alloy and SiC changes in a gradational manner, and laminating the material. The formation of the boundary layer 129 in which the blending ratio of different materials changes in a gradational manner and lamination is also called "gradient lamination."
[0081] In the process of forming the boundary layer 129, the boundary layer 129 between the base 121 and the adsorption portion 123 is laminated at an angle, thereby making it possible to improve the heat transfer coefficient between the different materials of the mounting table 116 compared to a case where the boundary layer 129 is not laminated at an angle. Furthermore, in the process of forming the boundary layer 129, the manufacturing man-hours can be reduced by eliminating the adhesive layer that bonds the base 121 and the adsorption portion 123, and the manufacturing lead time can be shortened.
[0082] Furthermore, by arranging the flow channel structure, wiring structure, and the like three-dimensionally, the mounting table 116 can be made highly functional.
[0083] In the 3D printer 200, the steps may be executed in the order of the first step, the second step, and the third step, or the third step, the second step, and the first step. This allows the 3D printer 200 to manufacture the upper electrode 130 that functions as the upper electrode, similar to the mounting table 2 that functions as the lower electrode.
[0084] [Boundary Layer 129 Variations] The boundary layer 129 is not limited to a slope-like (gradient-like) inclined lamination in which the blending ratio of the aluminum alloy powder and the SiC powder changes linearly. The boundary layer 129 may be a step-like inclined lamination in which the blending ratio of the aluminum alloy powder and the SiC powder changes stepwise. In addition, the inclination of the boundary layer 129 (the blending ratio of each material) may be changed according to the linear expansion coefficient of each material of the base 121 and the adsorption portion 123.
[0085] [Type of 3D printer] In this embodiment, a powder bed fusion type 3D printer is used as an example of the 3D printer 200 that manufactures the mounting table 116. In a powder bed fusion type 3D printer, a part is formed by repeating the process of spreading powdered raw material on the stage 202, melting it with a laser beam or the like, and spreading the powdered raw material again and melting it with a laser beam or the like. For this reason, a powder bed fusion type 3D printer is suitable for manufacturing the mounting table 116 and upper electrode 130 structures in which the three-dimensional structure to be formed in advance is clear and which have a complex structure such as a hollow structure.
[0086] However, the 3D printer 200 is not limited to such a configuration, and may be, for example, a directed energy 3D printer, or a 3D printer using other methods. Examples of 3D printers using other methods include binder injection 3D printers, sheet lamination 3D printers, photopolymerization curing (photolithography) 3D printers, and material extrusion (fused deposition modeling) 3D printers.
[0087] Furthermore, when the material of the parts to be manufactured is a resin material or ceramics, ultraviolet light is used as the energy beam in the process of irradiating the energy beam while supplying the raw material of the resin material, which is performed by the 3D printer. As a result, according to the part forming method of this embodiment, not only parts made of metal materials but also parts made of resin or ceramic materials can be formed. As an example of a 3D printer when the material of the parts is a resin or ceramic material, a material jet type 3D printer that solidifies and layers resin jetted from an inkjet head with ultraviolet light can be cited.
[0088] [Layered structure of different ceramics] Finally, a brief description will be given of the manufacture of a part having a laminated structure of different ceramics using a 3D printer. For example, when the material of the base 121 is SiC and the material of the adsorption part 123 is alumina, the mounting table 116 is an example of a part having a laminated structure of different ceramics. In this case, the material of the base 121 is an example of a raw material of a first ceramic, and the material of the adsorption part 123 is an example of a raw material of a second ceramic different from the first ceramic.
[0089] In this method of forming a part having a laminated structure of different ceramics using the 3D printer 200, first, a process of irradiating an energy beam onto one of the raw materials, the first ceramic and the second ceramic, while supplying the raw material. For example, the second control unit 250 in FIG. 3 irradiates ultraviolet light onto the SiC powder while supplying the SiC powder into the laser light scanning space 209 based on three-dimensional data. The energy beam irradiated in this process and the following processes is not limited to ultraviolet light, and may be light of other frequency bands.
[0090] Next, a step of irradiating the raw materials with an energy beam while supplying the first ceramic raw material and the second ceramic raw material is executed. For example, the second control unit 250 irradiates the SiC powder and the alumina powder with ultraviolet light while supplying the SiC powder and the alumina powder to the laser beam scanning space 209 based on the three-dimensional data.
[0091] Finally, a step of irradiating the other raw material of the first ceramic and the second ceramic with an energy beam is executed while supplying the other raw material. For example, the second control unit 250 irradiates the alumina powder with ultraviolet light while supplying the alumina powder to the laser light scanning space 209 based on the three-dimensional data. As a result, the mounting table 116 having a layered structure of the SiC base 121, the boundary layer 129, and the alumina adsorption portion 123 is formed using the 3D printer 200.
[0092] In the process of irradiating ultraviolet rays while supplying two types of ceramic powder, the second control unit 250 irradiates ultraviolet rays onto the powder while changing the blending ratio of SiC powder and alumina powder and supplying the powder to the laser light scanning space 209. At this time, the second control unit 250 gradually decreases the blending ratio of SiC powder, which is the same as the material of the base, from 100% based on the three-dimensional data, and continuously changes it to 0% before supplying it. Also, the second control unit 250 gradually increases the blending ratio of alumina powder, which is the same as the material of the electrostatic chuck 120, from 0% based on the three-dimensional data, and continuously changes it to 100% before supplying it.
[0093] As a result, the SiC powder and the alumina powder are supplied to the laser beam scanning space 209 while changing in the mixture ratio from a state with a high SiC content to a state with a high alumina content. The second control unit 250 repeatedly performs an operation of irradiating the SiC and alumina powder with the changing mixture ratio with ultraviolet light to melt and solidify the powder. As a result, the boundary layer 129 formed between the SiC base 121 and the alumina adsorption portion 123 is inclinedly laminated.
[0094] In this manufacturing process, the boundary layer 129 between the base 121 and the adsorption unit 123 is laminated at an angle, thereby improving the heat transfer coefficient between the different materials of the mounting table 116. In addition, in this manufacturing process, the boundary layer 129 is laminated at an angle, thereby eliminating the adhesive layer that bonds the base 121 and the adsorption unit 123, thereby reducing the number of manufacturing steps and shortening the manufacturing lead time.
[0095] Although the plasma processing apparatus and the parts for the plasma processing apparatus have been described above with reference to the above-mentioned embodiments, the plasma processing apparatus and the parts for the plasma processing apparatus according to the present invention are not limited to the above-mentioned embodiments, and various modifications and improvements are possible within the scope of the present invention. The matters described in the above-mentioned embodiments can be combined to the extent that they are not inconsistent.
[0096] The plasma processing apparatus according to the present invention can be applied to any type of plasma processing apparatus, including Capacitively Coupled Plasma (CCP), Inductively Coupled Plasma (ICP), Radial Line Slot Antenna, Electron Cyclotron Resonance Plasma (ECR), and Helicon Wave Plasma (HWP).
[0097] In this specification, the wafer W has been described as an example of the substrate, but the substrate is not limited to this and may be various substrates used in LCDs (Liquid Crystal Displays) and FPDs (Flat Panel Displays), CD substrates, printed circuit boards, etc.
[0098] The following is a summary: [Appendix 1] A plasma treatment vessel; a plasma generating means for performing plasma processing in the plasma processing vessel; a component disposed in the plasma processing vessel; The part comprises: The first ceramic; formed from a second ceramic different from the first ceramic, A plasma processing apparatus comprising: a boundary layer formed while a blending ratio of the first ceramic and the second ceramic changes. [Appendix 2] The part comprises: a first ceramic layer formed of the first ceramic; a second ceramic layer formed of the second ceramic; The boundary layer is provided between the first ceramic layer and the second ceramic layer. 2. The plasma processing apparatus according to claim 1. [Appendix 3] The boundary layer is formed by continuously or stepwise changing the blending ratio of the first ceramic and the second ceramic. 3. The plasma processing apparatus according to claim 1 or 2. [Appendix 4] the first ceramic is alumina; The second ceramic is silicon carbide. 4. The plasma processing apparatus according to claim 1, wherein the plasma processing apparatus comprises: [Appendix 5] A plasma treatment vessel; a plasma generating means for performing plasma processing in the plasma processing vessel; a part to be placed in the plasma processing vessel; The part comprises: Metal and It is made of ceramics, The plasma processing apparatus includes a boundary layer formed while the compounding ratio of the metal to the ceramics changes. [Appendix 6] The part comprises: a metal layer formed of the metal; a ceramic layer formed of the ceramic, The boundary layer is provided between the metal layer and the ceramic layer. 6. The plasma processing apparatus according to claim 5. [Appendix 7] The ceramic layer is It has a heater layer inside. 7. The plasma processing apparatus according to claim 6. [Appendix 8] The ceramic layer is With an electrode layer inside, 8. The plasma processing apparatus according to claim 6 or 7. [Appendix 9] The metal layer is A flow path is formed inside. 9. The plasma processing apparatus according to any one of claims 6 to 8. [Appendix 10] The boundary layer is formed by changing the compounding ratio of the metal and the ceramic continuously or stepwise. 10. The plasma processing apparatus according to any one of claims 5 to 9. [Appendix 11] the metal is aluminum; The ceramic is alumina or silicon carbide. 11. The plasma processing apparatus according to any one of claims 5 to 10. [Appendix 12] The first ceramic; formed from a second ceramic different from the first ceramic, A boundary layer is formed while the blending ratio of the first ceramic and the second ceramic changes. Parts for plasma processing equipment. [Appendix 13] a first ceramic layer formed of the first ceramic; a second ceramic layer formed of the second ceramic; The boundary layer is provided between the first ceramic layer and the second ceramic layer. 13. A part for a plasma processing apparatus according to claim 12. [Appendix 14] The boundary layer is formed by continuously or stepwise changing the blending ratio of the first ceramic and the second ceramic. 14. A part for a plasma processing apparatus according to claim 12 or 13. [Appendix 15] the first ceramic is alumina; The second ceramic is silicon carbide. The part for a plasma processing apparatus according to any one of claims 12 to 14. [Appendix 16] Metal and It is made of ceramics, A boundary layer is formed while the blending ratio of the metal and the ceramic changes. Parts for plasma processing equipment. [Appendix 17] a metal layer formed of the metal; a ceramic layer formed of the ceramic, The boundary layer is provided between the metal layer and the ceramic layer. 17. A part for a plasma processing apparatus according to claim 16. [Appendix 18] The ceramic layer is It has a heater layer inside. 18. A part for a plasma processing apparatus according to claim 17. [Appendix 19] The ceramic layer is With an electrode layer inside, 19. A part for a plasma processing apparatus according to claim 17 or 18. [Appendix 20] The metal layer is A flow path is formed inside. 20. The part for a plasma processing apparatus according to any one of claims 17 to 19. [Appendix 21] The boundary layer is formed by changing the compounding ratio of the metal and the ceramic continuously or stepwise. 21. The part for a plasma processing apparatus according to any one of claims 16 to 20. [Appendix 22] the metal is aluminum; The ceramic is alumina or silicon carbide. 22. The part for a plasma processing apparatus according to any one of claims 16 to 21. [Explanation of symbols]
[0099] 62 First high frequency power source 64 Second high frequency power source 100 Plasma treatment device 112 Processing vessel 116 Placement table 117 Foundation 120 Electrostatic Chuck 121 Foundation 123 Adsorption part 125 Electrode membrane 129 Boundary layer 130 Upper electrode 139 Gas Supply Section 151 First Control Section 200 3D Printers 202 Stage 203 Raw Material Storage Section 204 Laser Scanner 205 Lola 206 Light source 207 Roller drive unit 208 Laser driver 209 Laser Light Scanning Space 210 Chamber 250 Second Control Section HN Heater
Claims
1. A base formed of a conductive material; an electrostatic chuck disposed on an upper surface of the base and made of a ceramic material; a boundary layer provided between the base and the electrostatic chuck, the boundary layer includes a mixture of the conductive material and the ceramic material; a compounding ratio of the conductive material to the ceramic material in the mixture changes from the base to the electrostatic chuck in the boundary layer; Mounting stand.
2. a mixing ratio of the conductive material to the ceramic material in the mixture gradually decreases from the base toward the electrostatic chuck; The mounting table according to claim 1 .
3. a mixing ratio of the conductive material to the ceramic material in the mixture linearly decreases from the base to the electrostatic chuck; The mounting table according to claim 2 .
4. a mixing ratio of the conductive material to the ceramic material in the mixture is decreased in a stepwise manner from the base to the electrostatic chuck; The mounting table according to claim 2 .
5. a mixing ratio of the conductive material to the ceramic material in the mixture decreases from 100% to 0% toward the electrostatic chuck; The mounting table according to any one of claims 2 to 4.
6. The boundary layer is formed by melting and solidifying. The mounting table according to any one of claims 2 to 5.
7. the conductive material is an aluminum alloy, aluminum nitride, silicon carbide or titanium; The ceramic material is aluminum oxide or silicon carbide. The mounting table according to any one of claims 2 to 6.
8. a first component formed from a first material; a second component formed from a second material; a boundary layer provided between the first component and the second component, the boundary layer comprises a mixture of the first material and the second material; a blending ratio of the first material to the second material in the mixture varies from the first component to the second component at the boundary layer; Parts for plasma processing equipment.
9. a mixing ratio of the first material to the second material in the mixture gradually decreases from the first part to the second part; The part for a plasma processing apparatus according to claim 8.
10. a ratio of the first material to the second material in the mixture decreases linearly from the first part to the second part; The part for a plasma processing apparatus according to claim 9.
11. a ratio of the first material to the second material in the mixture decreases in a stepwise manner from the first part to the second part; The part for a plasma processing apparatus according to claim 9.
12. the blend ratio of the first material to the second material in the mixture decreases from 100% to 0% toward the second part; The part for a plasma processing apparatus according to any one of claims 9 to 11.
13. The boundary layer is formed by melting and solidifying. The part for a plasma processing apparatus according to any one of claims 9 to 12.
14. the first material is an aluminum alloy, aluminum nitride, silicon carbide or titanium; The second material is aluminum oxide or silicon carbide. The part for a plasma processing apparatus according to any one of claims 9 to 13.
Citation Information
Patent Citations
Film forming method
JP1989011960A
Surface-coated tungsten carbide-based cemented carbide cutting tip obtained by forming hard coating layer free of interlayer bonded surface
JP1992246174A
Alumina-based composite ceramic sintered body
JP1993170522A
Stage structure and processor using it
JP1997213781A
Electrostatic chuck
JP1998041377A